Adsorbent and method for producing the same
By combining iron and alkali metal carbonates on porous carbides, a stable adsorbent is formed, which solves the problems of adsorbent stability in water and carbon dioxide sequestration, achieving water quality improvement and the provision of low-cost fertilizers, while reducing greenhouse gas emissions.
Patent Information
- Application Number
- CN202210124732.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-10
- Filing Date
- 2022-02-10
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-02-10
AI Technical Summary
Existing adsorbents are difficult to maintain their shape in water for a long time, and cannot effectively fix carbon dioxide in the atmosphere, resulting in poor greenhouse effect gas storage effects.
Using porous carbide as the basic skeleton, combined with carbonates and bicarbonates of iron and alkali metals or alkaline earth metals, it forms a stable adsorbent by treating it with carbon dioxide gas, inhibiting disintegration in water, and using biomass to create low-cost adsorbents agent.
It has realized an adsorbent that improves water quality in the long term, manufactures fertilizers at low cost, effectively sequesters carbon dioxide in the atmosphere, and reduces the greenhouse effect.
Smart Images

Figure CN115069213B_ABST
Abstract
Description
Technical Field
[0001] One embodiment of the present invention relates to an adsorbent and a method for producing the same. Background Art
[0002] It is known that the adsorbent of porous carbide with iron carried in carbon prepared with biomass as basic material can adsorb the phosphate ion from phosphoric acid, thus can be used for water quality improvement in waters such as rivers, lakes, and oceans. In addition, the adsorbent having adsorbed phosphate ions can also be used as fertilizer, therefore by spreading the adsorbent after having adsorbed phosphate ions to soil, it is possible to effectively utilize the carbon dioxide fixed by plants, carbon dioxide is sequestered (Carbon Sequestration) in soil. Therefore, the adsorbent obtained by biomass plays a main role in the carbon sequestration of greenhouse effect gases in the fixed atmosphere (with reference to patent documentation 1, non-patent documentation 1).
[0003] (Prior art literature)
[0004] (Patent Document)
[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 2007-75706
[0006] Non-patent document 1: Shibata Akira, "COOLVEGETM, a vegetable that can be used for simple carbonization and carbon sequestration of biomass for regional revitalization", Journal of the High Temperature Society, March 2011, Vol. 37, No. 2, pp. 37-42 Summary of the invention
[0007] (Problems to be solved by the invention)
[0008] One of the problems of one embodiment of the present invention is to provide an adsorbent and a method for manufacturing the same. Alternatively, one of the problems of one embodiment of the present invention is to provide an adsorbent that can be used to improve water quality and can maintain its shape in water for a long time and a method for manufacturing the same. Alternatively, one of the problems of one embodiment of the present invention is to provide a system for sequestering carbon by fixing carbon dioxide in the atmosphere.
[0009] (Measures taken to solve the problem)
[0010] One embodiment of the present invention is an adsorbent, which includes porous carbide, a binder, and iron, and further includes at least one of a carbonate and a bicarbonate of a metal selected from alkali metals and alkaline earth metals.
[0011] One embodiment of the present invention is a method for producing an adsorbent, which includes: a step of mixing a porous carbide, a binder, and an iron powder to prepare a precursor; and a step of treating the precursor with a gas containing carbon dioxide.
[0012] (Effects of the Invention)
[0013] According to an embodiment of the present invention, an adsorbent and a method for manufacturing the same can be provided, wherein the adsorbent can be used for long-term improvement of water quality in water bodies such as rivers, lakes, and oceans. In addition, a fertilizer effective for plant growth can be manufactured at low cost. Furthermore, carbon dioxide in the atmosphere can be sealed underground in the form of carbon, which helps to suppress the greenhouse effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a flow chart showing a method for producing an adsorbent according to one embodiment of the present invention.
[0015] Figure 2 This is a scheme showing a method for producing an adsorbent according to one embodiment of the present invention.
[0016] Figure 3 This is a conceptual diagram showing a carbon dioxide storage system which is one embodiment of the present invention.
[0017] Figure 4 This is a photograph of the adsorbent after phosphoric acid is adsorbed in the example. DETAILED DESCRIPTION
[0018] Hereinafter, various embodiments of the present invention will be described with reference to the drawings, etc. However, the present invention can be implemented in various forms within the scope not departing from the gist thereof, and should not be construed as being limited to the description of the embodiments shown below.
[0019] <First Embodiment>
[0020] In this embodiment, an adsorbent and a method for producing the adsorbent according to one embodiment of the present invention will be described.
[0021] 1. Adsorbent
[0022] The adsorbent has a porous carbide as a basic skeleton, and carries iron (0-valent iron) on its surface and pores. The carried iron can convert phosphoric acid and its ions present in water into iron phosphate and adsorb it to the porous carbide. Therefore, the adsorbent can be used as an adsorbent for effectively improving the water quality of rivers, lakes, oceans and other water bodies. The adsorbent also includes a binder and contains at least one of a carbonate and a bicarbonate of a metal selected from an alkali metal and an alkaline earth metal. The adsorbent may also contain an iron compound, or a compound of a metal selected from an alkali metal and an alkaline earth metal other than a carbonate and a bicarbonate, and water.
[0023] 1-1. Porous carbide
[0024] Porous carbide is a carbide made by heating and carbonizing organic matter under low oxygen concentration conditions using organic matter as raw material. As an organic matter, biomass is exemplified. As porous carbides from biomass, charcoal, bamboo charcoal, white charcoal, black charcoal, sawdust charcoal, coconut shell charcoal, rice husk charcoal, etc. are exemplified. As will be described later, by using biomass as a raw material for porous carbide, a system for sealing carbon dioxide in the atmosphere can be constructed, and ions of alkali metals and alkaline earth metals can be provided at the same time, and the ions of the alkali metals and alkaline earth metals are used as reaction sites to prevent the adsorbent from disintegrating in water.
[0025] Carbonization is carried out by heating the organic matter in an inert gas atmosphere such as nitrogen or argon, an oxygen-free atmosphere, a low-oxygen atmosphere, a reducing atmosphere, or a reduced pressure atmosphere. When carbonization is carried out in a reduced pressure atmosphere, the carbonization can be carried out for 10 2 Pa and above 10 5 Pa or less, in a low vacuum state, -1 Pa and above 10 2 Pa or less in medium vacuum, at 10 -5 Pa and above 10 - 1 Pa or below, or -5 The carbonization is carried out under an ultra-high vacuum state of less than 1.5 Pa. When carbonization is carried out in a low oxygen atmosphere, it can be carried out under the condition that the oxygen concentration is 0.01% to 3%, or 0.1% to 2%. The heating temperature in the carbonization can be 400°C to 1200°C, 500°C to 1100°C, 600°C to 1000°C, or 600°C to 900°C. The heating time can be 10 minutes to 10 days, or 10 minutes to 5 hours.
[0026] Carbonization is performed using an internal combustion or external heating carbonization furnace. Examples of carbonization furnaces include intermittent sealed carbonization furnaces, continuous rotary kilns, swing carbonization furnaces, screw furnaces, and the like. While the carbonization gas is generated by the carbonization of the biomass, a porous carbide is generated in which pores of various shapes and sizes are formed by a complex mixture of pores caused by the structure of the biomass and pores formed by the desorption of the carbonization gas. The carbonization gas mainly contains hydrogen, carbon monoxide, and flammable or reducing gases such as alkanes represented by methane, propane, and butane. The carbonization gas is taken out at a high temperature (700°C to 1300°C), so its thermal energy, flammability, and the like can be used as energy for power generation, hot water supply, and the like.
[0027] Here, biomass is an organic matter, which is a substance derived from an organism and its metabolites. For example, materials from trees are listed as biomass. Specifically, wooden molded products such as board-shaped and column-shaped wood, thinning materials, pruning waste, construction waste, powdered sawdust, particleboard, etc. are listed. The type of tree is not limited, and it can be fir, cypress, bamboo. Alternatively, agricultural waste such as rice husks, bagasse, corn cobs, leaves, straw, wheat straw, hay, etc., and agricultural and sideline products such as straw can also be listed as an example of biomass. Alternatively, plants that become raw materials for fibers, such as hemp, flax, cotton, sisal, abaca, and palm hair can be listed. Alternatively, it can be algae such as seaweed. Alternatively, food scraps, silage obtained from animal feces, etc. can be cited.
[0028] The size and shape of the porous carbide are not particularly limited, but the average particle size of the porous carbide can be 1 μm to 50 mm or 1 μm to 1 mm. Since the average particle size is within this range, the porous carbide and the iron powder can be uniformly mixed in the mixing and kneading process described later.
[0029] The porous carbide has a large specific surface area due to the pores formed inside. Specifically, the specific surface area of the porous carbide is 100 m 2 / g and above 900m 2 / g or less, and can also be 100m 2 / g and above 800m 2 / g or less, or 150m 2 / g and above 400m 2 The specific surface area is measured by a gas adsorption method represented by a mercury porosimetry, a BJH method, or an HK method.
[0030] 1-2. Iron and iron compounds
[0031] As described later, iron is mixed with porous carbide as iron powder and carried. The shape of the iron powder is not limited. For example, iron powder having an average roundness of 50 or more and 100 or less, 70 or more and 95 or less, or 80 or more and 90 or less can be used. Here, the average roundness is one of the parameters representing the shape of each iron particle contained in the iron powder, and is a value obtained by analyzing an image obtained by observing the iron powder through a microscope, finding the roundness of a plurality of iron particles and averaging them. As the roundness, for example, a value obtained by dividing the circumference of a circle having an area equal to the area of the projection surface of each iron particle in the microscopic image by the circumference of the projection surface can be used. Alternatively, a value obtained by dividing the area of the projection surface by the area of the circle inscribed in the projection surface can be used as the roundness.
[0032] The average particle size of the iron powder is not limited, and for example, an iron powder having an average particle size in the range of 20 μm to 500 μm, or 50 μm to 200 μm can be used. Furthermore, iron powder having the following particle size distribution can also be used: 1) the proportion of iron particles with a particle size in the range of 1 μm to 150 μm is 3% to 70% by mass, 2) the proportion of iron particles with a particle size in the range of 1 μm to 75 μm is 0% to 25% by mass, 3) the proportion of iron particles with a particle size in the range of 1 μm to 45 μm is 0% to 15% by mass, 4) the proportion of iron particles with a particle size in the range of 150 μm to 2000 μm is 30% to 99% by mass, and 5) the proportion of iron particles with a particle size in the range of 600 μm to 2000 μm is 0% to 15% by mass, and at the same time, the sum of the proportion of at least any one of 1) to 3) and the proportion of iron particles in 4) or 5) is 100% by mass. Here, the average particle size of the iron powder is a value obtained by analyzing an image obtained by observing the iron powder through a microscope, finding the particle sizes of a plurality of iron particles, and averaging the obtained values. As the particle size of each iron particle, for example, the diameter of a circle inscribed in the projection plane of each iron particle in the microscopic image or the length of one side of a square can be used.
[0033] The iron powder may contain trace amounts of other elements, such as carbon, oxygen, sulfur, phosphorus, manganese, silicon, vanadium, copper, titanium, etc. Therefore, the purity of the iron powder may be 90.0% to 99.9%, or 95.0% to 99.0%.
[0034] In addition, a part of the iron powder can be carried on the porous carbide in an oxidized state, that is, as an iron compound. As the iron compound, iron oxide and iron hydroxide can be exemplified. The iron contained in the iron compound can exist in a state of divalent, trivalent, or a mixed valence of a mixture of divalent and trivalent atomic valences. Therefore, when the iron compound is iron hydroxide, it can be ferrous hydroxide or ferric hydroxide. When the iron compound is iron oxide, it can be wurtzite (FeO), hematite or maghemite (Fe2O3), or magnetite (Fe3O4).
[0035] 1-3 Adhesive
[0036] The binder is used to effectively disperse the porous carbide and the iron powder in the kneading process to be described later, and to integrate the iron, the iron compound and the porous carbide. The type of binder is not limited, and an organic binder and / or an inorganic binder can be used. As an organic binder, for example, one or more selected from molasses, waste molasses, starch, dextrin, corn starch, rice bran, polyvinyl alcohol, copolymers of vinyl acetate and ethylene or saponified products thereof, waste pulp liquid, lignin sulfonate, carboxymethyl cellulose, hydroxypropyl methyl cellulose, sodium alginate, phenolic resin and tar pitch can be cited. Among them, molasses is cheap, has few harmful components and many solid components, so the use of molasses can make the molding of the adsorbent easy. As an inorganic binder, for example, cement, blast furnace slag powder, fly ash, gypsum (calcium sulfate), plaster obtained by heating and dehydrating gypsum, sodium silicate, etc. can be cited.
[0037] 1-4. Carbonates and bicarbonates
[0038] Biomass is used as the raw material of porous carbide, so that the alkali metal and alkaline earth metal compounds contained in the biomass remain in the porous carbide. The metal compound is included in the porous carbide in the form of halides, oxides, hydroxides, sulfates, and nitrates, for example. As described later, in the manufacturing process of adsorbent, the alkali metal and alkaline earth metal compounds are converted into carbonates and / or bicarbonates by reacting with carbon dioxide, and are carried on the porous carbide (carbonation). In other words, the alkali metal and alkaline earth metal compounds play the role of the reaction site of carbon dioxide.
[0039] Specific examples of alkali metals include sodium, potassium, lithium, and cesium. Alkaline earth metals include magnesium and calcium. Therefore, examples of carbonates and bicarbonates contained in the adsorbent include sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, sodium bicarbonate, potassium bicarbonate, lithium bicarbonate, cesium bicarbonate, magnesium bicarbonate, and calcium bicarbonate.
[0040] The adsorbent may contain compounds of alkali metals and alkaline earth metals other than carbonates and bicarbonates, which do not react with carbon dioxide and remain. That is, the adsorbent may contain carbonates or bicarbonates of metals selected from alkali metals and alkaline earth metals, and one or more of chlorides, oxides, hydroxides, sulfates, and nitrates of the above metals.
[0041] In addition, the carbonate or hydrogen carbonate of an alkali metal or alkaline earth metal can be formed by adding a compound of an alkali metal and / or alkaline earth metal separately when manufacturing the adsorbent and then reacting the compound with carbon dioxide. In this case, the content of the carbonate or hydrogen carbonate of an alkali metal or alkaline earth metal is not limited to the compound of an alkali metal or alkaline earth metal contained in the biomass and can be adjusted arbitrarily.
[0042] 1-5. Composition ratio
[0043] The composition ratio of the above structure can be appropriately adjusted. For example, the content of porous carbide in the adsorbent can be adjusted within the range of 20 mass % to 80 mass %, 40 mass % to 80 mass %, or 60 mass % to 80 mass %. The sum of the contents of iron and iron compounds can be adjusted within the range of 5 mass % to 35 mass %, 5 mass % to 25 mass %, or 5 mass % to 20 mass %. The content of the binder can be adjusted within the range of 5 mass % to 50 mass %, 15 mass % to 50 mass %, or 20 mass % to 50 mass %. The sum of the contents of carbonates and bicarbonates of metals selected from alkali metals and alkaline earth metals can be adjusted within the range of 1 mass % to 30 mass %, 1 mass % to 15 mass %, or 1 mass % to 10 mass %.
[0044] Alternatively, the carbon content in the adsorbent can be adjusted within a range of 10% by mass or more and 80% by mass or less. The iron content (i.e., iron element containing zero-valent iron and / or iron ions) in the adsorbent can be adjusted within a range of 5% by mass or more and 35% by mass or less. The sum of the contents of alkali metals and alkaline earth metals can be adjusted within a range of 1% by mass or more and 30% by mass or less.
[0045] In the determination of the content of porous carbide in the adsorbent, the carbon content of the porous carbide in the raw material stage is first determined. For example, a combustion / infrared absorption method can be used, and a method that conforms to JIS H1617, JIS Z2615 and ASTM E1941 is adopted. Specifically, in a combustion furnace, the porous carbide in the raw material stage is burned under an oxygen flow to produce carbon dioxide. The generated carbon dioxide is introduced into an infrared analyzer using oxygen, and its absorption is measured by a detector to determine the concentration of carbon dioxide. According to the concentration of the carbon dioxide, the mass of the carbon in the porous carbide in the raw material stage is quantified as the mass of the porous carbide. Then, the content of the porous carbide can be calculated according to the mass of the porous carbide in the raw material stage, the binder mixed with the porous carbide, iron powder, water and other raw materials. The content of the binder can also be calculated according to the mass of the porous carbide, iron powder, water and other raw materials used in the manufacturing process of the adsorbent.
[0046] The sum of the contents of iron and iron oxides, and the sum of the contents of carbonates and bicarbonates of metals selected from alkali metals and alkaline earth metals, can be measured, for example, by applying inductively coupled plasma emission spectrometry (ICP-OES) or inductively coupled plasma mass spectrometry (ICP-MS) to the adsorbent. In ICP-OES, argon plasma is used as a light source, and an atomized solution sample is introduced into the plasma, thereby splitting the spectrum unique to alkali metals and alkaline earth metals, and alkali metals and alkaline earth metals can be quantitatively measured according to the measured wavelength and luminescence intensity. ICP-MS is a method of using argon plasma as an ion source to ionize the elements contained in the sample, and to separate and detect ions according to the mass-to-charge ratio. While the mass-to-charge ratio of the detected ions can be used to identify specific elements, alkali metals and alkaline earth metals can be quantitatively determined by counting the detected ions. In addition, by converting the content of the quantitative alkali metal and alkaline earth metal ions into carbonates or bicarbonates, the sum of the contents of carbonates and bicarbonates of metals selected from alkali metals and alkaline earth metals can be obtained.
[0047] In addition, in the above method, the treatment with a gas containing carbon dioxide to be described later is not considered, that is, the conversion rate of the alkali metal salt, alkaline earth metal salt and carbon dioxide contained in the porous carbide, and the mass change of the adsorbent caused by the reaction are not considered. In addition, the generation of iron compounds caused by the oxidation of iron in the manufacturing process is not considered. However, since the mass changes caused by these reactions are within a negligible range, it can be said that the measurement results of the above method have sufficiently high reliability.
[0048] On the other hand, the carbon content in the adsorbent can be obtained by applying the above-mentioned combustion / infrared absorption method to the adsorbent. In addition, the carbon content in the adsorbent is mainly derived from the carbon content of the porous carbide, the binder, and the carbonate and bicarbonate of the metal selected from the alkali metal and the alkaline earth metal. The sum of the iron content and the alkali metal and alkaline earth metal content can also be determined by applying ICP-OES or ICP-MS to the adsorbent.
[0049] By adjusting the content of each component within the above range, the function of effectively removing phosphoric acid in water can be obtained, and at the same time, the adsorbent can be prevented from disintegrating in water, so the water quality improvement function can be maintained for a long time.
[0050] The phosphate adsorption capacity of the adsorbent can be measured, for example, by batch testing. Batch testing is a method for calculating the amount of phosphate adsorption based on the difference between the phosphate concentration of a solution containing phosphate as an adsorbent and the phosphate concentration of a solution after phosphate adsorption. The determination of the phosphate concentration can be carried out by using, for example, the molybdenum blue method, the ammonium vanadium molybdate absorbance method, etc. In the former, a potassium persulfate solution is added to a certain amount of sample collected and heated, and then a mixed solution of ammonium molybdate and potassium antimony tartrate (Bis[(+)-tartrato]diantimonate(III)Dipotassium Trihydrate) is added to generate phosphomolybdic acid. L-ascorbic acid solution is added to the phosphomolybdic acid to generate molybdenum blue (hydrated mixed valence oxide of molybdenum). The absorption of molybdenum blue (for example, absorption at 880nm) is measured using a UV / visible spectrophotometer to quantify water-soluble phosphoric acid. In the latter, nitric acid (1+1) is added to a certain amount of sample collected and heated to hydrolyze non-orthophosphoric acid into orthophosphate ions. Then, ammonium metavanadate (V), ammonium heptamolybdate and nitric acid are added to generate phospho vanado molybdic acid salt. The phosphoric acid is quantified by measuring the absorption of phospho vanado molybdic acid salt (eg, absorption at 420 nm) using a UV / visible spectrophotometer.
[0051] 2. Manufacturing method
[0052] One example of a method for producing the adsorbent is described below. Figure 1 and Figure 2 A flowchart and a scheme respectively show a method for producing an adsorbent. Figure 2 M x A y It is a compound of an alkali metal or alkaline earth metal contained in a porous carbide. M is selected from Li, Na, K, Cs, Mg, and Ca, and A includes F, Cl, Br, I, OH, O, SO4, and NO3. Depending on the valence of the anion A and the metal M, x and y are each independently 1 or 2.
[0053] 2-1. Mixing and kneading
[0054] like Figure 1 , Figure 2As shown, first, porous carbide, binder, and iron (iron powder) as raw materials are mixed, and then kneaded (kneaded). As the porous carbide, as described above, it is preferred to use carbide obtained by carbonizing biomass. As the iron powder, iron powder having the above-mentioned average particle size or particle size distribution can be used. The amounts of porous carbide, binder, and iron powder are appropriately adjusted to obtain a composition ratio within the above-mentioned range. The particle size of the porous carbide can be adjusted by pre-crushing and classification. The particle size of the porous carbide is generally larger than the particle size of the iron powder, so the porous carbide can be crushed so that the particle size of the porous carbide is almost equal to the particle size of the iron powder.
[0055] When mixing or kneading, water is added to the porous carbide, binder, and iron as needed. Adding water can prevent the generation of dust and make the porous carbide and iron powder mix more evenly.
[0056] In the mixing and kneading of these raw materials, a kneader can be used. As a kneader, for example, a single-screw kneader, a twin-screw kneader, a mixing roller, a kneader or a Banbury mixer can be used. In addition, a kneader with mixing and kneading functions can be used. In this case, the porous carbide, the iron powder and the adhesive are put into the kneader, and then mixed and kneaded. Alternatively, mixing and kneading can be carried out continuously. For example, the porous carbide and the iron powder are put into a kneader for mixing, and then the adhesive is put into the kneader for kneading. The adhesive can be added all at once, can be added intermittently, and can also be added continuously. By mixing the porous carbide and the iron powder and then adding the adhesive and kneading, the aggregation of the porous carbide and the iron powder can be prevented, and foaming can be suppressed.
[0057] The kneading temperature can be set arbitrarily, for example, it can be 0° C. to 50° C. or 10° C. to 40° C. The kneading time can also be appropriately set in consideration of the mixing ratio and amount of the raw materials, the type of the binder, the capacity of the kneader, etc., for example, it can be set within the range of 1 second to 1 hour, 1 minute to 30 minutes, or 1 minute to 15 minutes.
[0058] Through the above operation, a paste-like precursor obtained by mixing porous carbide, binder and iron powder can be obtained. In addition, in this process, part of the iron powder is oxidized, and as a result, the precursor contains compounds containing divalent and / or trivalent iron (Fe(II), Fe(III)). As the iron compound, as mentioned above, iron hydroxide and iron oxide can be exemplified. In addition, during mixing and kneading, alkali metal and / or alkaline earth metal compounds other than carbonates and bicarbonates can be added.
[0059] 2-2. Granulation
[0060] As an arbitrary step, the precursor can be granulated and formed into a fixed shape. The forming of the precursor can be carried out using a granulator. As a granulator, a compression granulator, an extrusion granulator, a roller granulator, a blade granulator, a melt granulator or a spray granulator etc. can be exemplified.
[0061] When using an extrusion granulator, a paste precursor of a prescribed shape is extruded from the die installed in the granulator. The extruded precursor is cut into a prescribed length and formed into a particle shape in which the extrusion direction is a height direction. By adjusting the extrusion speed and cutting speed (if the rotary cutting method is a rotary speed of the cutter) of the precursor in the extrusion granulator, the length (the height of the particle shape) of the precursor can be adjusted. In addition, by adjusting the aperture of the die, the diameter (diameter when the cross-sectional shape is circular) of the precursor can be adjusted. Therefore, by using an extrusion granulator, a precursor with a particle shape (for example, approximately cylindrical) with controlled size can be obtained.
[0062] The size of the particle shape can be set arbitrarily, for example, the length of each particle can be 1 mm or more and 20 mm or less, 3 mm or more and 15 mm or less, or 6 mm or more and 12 mm or less. When the cross-sectional shape is circular, the diameter of the particle can be 1 mm or more and 20 mm or less, 1 mm or more and 10 mm or less, or 3 mm or more and 8 mm or less.
[0063] The cross-sectional shape of the precursor after molding (a cross section perpendicular to the length direction) is not limited to a circle. The cross-sectional shape of the precursor can be, for example, an ellipse or a polygon. That is, the precursor after molding can be not only a cylindrical particle shape, but also an elliptical column or a multi-prism particle shape. The cross-sectional shape of the precursor can be changed by changing the opening shape of the mold. The granulation process can be carried out after the drying process to be described later.
[0064] 2-3. Carbon dioxide treatment
[0065] Next, the precursor is treated with carbon dioxide. Specifically, the precursor is contacted with a gas containing carbon dioxide, so that all or part of the compounds of alkali metals and alkaline earth metals contained in the porous carbide of the precursor are converted into carbonates or bicarbonates. The gas is carbon dioxide or a mixed gas of carbon dioxide and other gases. As other gases, rare gases such as air, nitrogen, oxygen, argon, water (water vapor), etc. can be cited. In the case of a mixed gas, the carbon dioxide concentration in the gas can be arbitrarily set, and can be appropriately set in the range of, for example, more than 1 volume % and less than 100 volume %, more than 1 volume % and less than 50 volume %, or more than 1 volume % and less than 20 volume %.
[0066] For example, a gas containing carbon dioxide can be introduced into a kneading machine so that the precursor is contacted with carbon dioxide and kneaded simultaneously. Alternatively, the precursor after kneading or molding can be arranged in a container of glass, stainless steel, etc., and the gas containing carbon dioxide can be introduced into the container. Alternatively, the precursor after molding can be rotated by a disc granulator and contacted with a gas containing carbon dioxide. The temperature in this treatment can be, for example, above 0°C and below 80°C, or above 0°C and below 50°C, typically room temperature (25°C or thereabouts). The humidity can be above 20% and below 95%, or above 50% and below 90%.
[0067] As an example of a supply source of gas containing carbon dioxide, a gas cylinder or tank containing carbon dioxide can be cited. Alternatively, waste gas from facilities that emit a large amount of carbon dioxide (chemical plants, waste incineration facilities, thermal power plants, and other various factories, etc.) or refined carbon dioxide obtained by dust removal, desulfurization, and denitrification of waste gas can be used. When facilities that emit a large amount of carbon dioxide are close to the manufacturing site of the adsorbent, these facilities act as a supply source of gas containing carbon dioxide, thereby reducing the cost of transporting carbon dioxide and preventing secondary emissions of carbon dioxide during transportation.
[0068] The adsorbent is obtained through the above steps.
[0069] 2-4. Drying
[0070] As an arbitrary process, the adsorbent obtained by the carbon dioxide treatment can be dried. The drying temperature and time are appropriately selected according to the amount of the adsorbent and the water content. For example, the drying temperature can be selected within the range of 30°C or more and less than 400°C, 50°C or more and 300°C or more and 100°C or less. The humidity during drying can be 20% or more and 95% or more, or 50% or more and 90% or less. The drying time can be appropriately selected within the range of 1 minute or more and 1 week or less, 1 hour or more and 3 days or more and 1 day or less. The atmosphere during drying can be, for example, a rare gas such as air, nitrogen, argon, or a mixture thereof.
[0071] In the manufacture of the adsorbent according to one embodiment of the present invention, calcination at high temperature is not required. That is, heating at a temperature required for carbonizing the binder (e.g., above 400°C) is not required. In other words, the maximum temperature in the manufacturing process of the adsorbent can be less than 400°C. Therefore, the time and energy required for calcination are not required, so the adsorbent can be provided at a low cost.
[0072] As described above, in the manufacturing method of the adsorbent of one embodiment of the present invention, all or part of the alkali metal and / or alkaline earth metal compounds contained in the porous carbide are converted into carbonates or bicarbonates. As a result, the adsorbent contains at least one of carbonates and bicarbonates of alkali metals and carbonates and bicarbonates of alkaline earth metals. Although the detailed mechanism is still unclear, if carbonates and / or bicarbonates of metals selected from alkali metals and alkaline earth metals are contained, the disintegration of the adsorbent in water will be suppressed. That is, even if the adsorbent is disposed in water or water containing an adsorbate for a long time, it will hardly be eroded by water and can stably maintain its shape. Therefore, it can be used as an adsorbent for long-term improvement of water quality, and can be easily recovered after adsorption.
[0073] <Second Embodiment>
[0074] In this embodiment, using Figure 3 A system is described that helps reduce carbon dioxide in the atmosphere using the adsorbent described in the first embodiment.
[0075] As described in the first embodiment, in the manufacture of the adsorbent according to one embodiment of the present invention, a porous carbonized material obtained from biomass can be used as one of the raw materials. In this case, the carbonized gas obtained by carbonizing the biomass can be used as an energy source, thereby generating electricity, producing hot water, etc. ( Figure 3 , (1)).
[0076] The obtained porous carbide is mixed with iron powder and a binder and kneaded to obtain a precursor ( Figure 3 , (2)), and then treated with a gas containing carbon dioxide ( Figure 3 , (3)). As a result, an adsorbent carrying iron and iron compounds and containing carbonates, bicarbonates of alkali metals, carbonates, bicarbonates of alkaline earth metals, etc. is obtained. As described above, carbides carrying iron and iron compounds effectively adsorb pollutants in water, especially phosphorus compounds such as phosphoric acid. Therefore, by placing the adsorbent in water bodies such as rivers, lakes, and oceans, water quality can be improved ( Figure 3 , (4)).
[0077] Phosphoric acid adsorbed on an adsorbent is a representative component of nutrients that promote the growth of various plants. Therefore, an adsorbent adsorbed with phosphoric acid can be used as a fertilizer, which helps to provide fertilizer at low cost. For example, an adsorbent for water quality improvement treatment is spread on farmland as it is or after being crushed and classified. Figure 3, (5)). Alternatively, it may be spread after mixing with fertilizer adjuvants such as calcium sulfate and other fertilizer components. The fertilizer components to be added may include one or more selected from nitrogen, potassium, calcium, magnesium, manganese, silicate, and boron. Specific materials include oil cake, fermented chicken manure, fish meal, bone meal, rice bran, bat guano, bokashi compost, wood ash, lime, chemical fertilizers, and the like.
[0078] The dispersed adsorbent slowly releases the adsorbed phosphoric acid, which is used for plant growth. At this time, the plants use the carbon dioxide in the atmosphere as a carbon source to photosynthesize and grow ( Figure 3 , (6)). Thereafter, the plant is used in various forms, such as food materials, materials, etc. The utilized plant can be used as biomass and used again in the manufacture of porous carbon ( Figure 3 , (7)).
[0079] Therefore, by applying the embodiments of the present invention, a series of cycles are established, including the generation of porous carbide from biomass, the manufacture of adsorbents, the improvement of water quality and the manufacture of fertilizers, the growth of plants using fertilizers, and the regeneration of biomass. In this cycle, the carbon dioxide in the atmosphere fixed by plants is used as a carrier of iron and iron compounds that exhibit a phosphoric acid adsorption function and is sealed underground in the form of carbon. Therefore, this cycle is a system that reduces carbon dioxide in the atmosphere and seals it underground, which helps to reduce carbon dioxide in the atmosphere.
[0080] [Example]
[0081] In this example, the preparation of an adsorbent according to one embodiment of the present invention and the evaluation results of the adsorbent are described.
[0082] 1. Preparation of adsorbent
[0083] 1-1. Example
[0084] As the porous carbide of the raw material, charcoal of irregular shape (waste charcoal from wood biomass gasification power generation) is used. 15g of iron powder and 35g of gypsum, in which the proportion of iron particles with a particle size of 300μm or more and 2000μm or less is 45% by mass, the proportion of iron particles with a particle size of 75μm or more and less than 300μm is 45% by mass, and the proportion of iron particles with a particle size of 1μm or more and less than 75μm is 10% by mass, are added to the 45g of charcoal, and mixed with a spatula for 1 minute. Furthermore, 7g of molasses (solid content of 70%) and 40mL of water are added to the mixture at room temperature, and kneaded for 30 minutes to obtain a powder mixture. The solid content ratio of charcoal, iron powder, gypsum and molasses is 45:15:5:35 (total 100%).
[0085] Then, the obtained powder mixture was put into a granulator and formed into a granule shape with a diameter of 6 mm and a height of 9 mm.
[0086] Then, 50 g of the molded powder mixture was sealed in a glass container of about 5 L, and carbon dioxide (purity: 100%) was introduced into the container at 20° C. The flow rate of carbon dioxide was 5 mL / min, and the gas was introduced for 18 hours.
[0087] 1-2. Comparative Example
[0088] As a comparative example, an adsorbent was prepared by the same method as in the example, but the adsorbent was not treated with a gas containing carbon dioxide, but was allowed to stand in a container at the same temperature and for the same time.
[0089] 2. Evaluation
[0090] The adsorption capacity of phosphoric acid by the adsorbent of the example was evaluated by a batch method. 0.1 g of the adsorbent of the example was added to 50 mL of a 200 mg / L phosphoric acid solution, and the mixture was horizontally shaken at 23°C and 100 rpm until an equilibrium concentration was reached, and then filtered. The phosphorus concentration of the filtrate was quantified by molybdenum blue spectrophotometry, and the results showed that the amount of phosphorus adsorbed was 34 (mg-P / g). Therefore, it was confirmed that the adsorbent of one embodiment of the present invention exhibited a high phosphoric acid adsorption capacity. On the other hand, the phosphorus adsorption capacity of the adsorbent of the comparative example was 29 (mg-P / g).
[0091] The photo of the embodiment after phosphoric acid adsorption is as follows Figure 4 As shown in the photo, the part colored black is the adsorbent. Figure 4 As shown, it can be seen that the adsorbent of the example treated with the gas containing carbon dioxide was not disintegrated and its shape was stably maintained in water. On the other hand, the adsorbent of the comparative example disintegrated in water.
[0092] These results indicate that by bringing carbon dioxide into contact with a precursor containing porous carbide, a binder, and iron powder, carbonates of metals selected from alkali metals and alkaline earth metals can be formed in the adsorbent, and the shape stability in water can be increased without impairing the phosphate adsorption capacity of the resulting adsorbent.
[0093] As embodiments of the present invention, as long as the above-mentioned embodiments do not contradict each other, they can be appropriately combined and implemented. Addition, deletion or design changes of constituent elements appropriately made by those skilled in the art according to the embodiments are all included in the scope of the present invention as long as they have the gist of the present invention.
[0094] The effects that are obvious from the description in this specification or easily predicted by those skilled in the art, even if they are different from the effects brought about by the above-mentioned embodiments, should naturally be understood to be brought about by the present invention.
Claims
1. An adsorbent, wherein Include: Porous carbides; Adhesives; Iron; and at least one of a carbonate and a bicarbonate of a metal selected from alkali metals and alkaline earth metals, The sum of the contents of the carbonate and the bicarbonate is 1% by mass or more and 10% by mass or less, The method for producing the adsorbent comprises: a step of preparing a precursor by mixing the porous carbide with the binder and iron powder; and a step of treating the precursor with a gas containing carbon dioxide, The carbon dioxide concentration in the gas is 1% by volume or more and 100% by volume or less.
2. The adsorbent according to claim 1, wherein Also included are iron compounds.
3. The adsorbent according to claim 2, wherein The content of the porous carbide is 20 mass % or more and 80 mass % or less, The content of the binder is 5% by mass or more and 50% by mass or less, The sum of the contents of the iron and the iron compound is 5 mass % or more and 35 mass % or less.
4. The adsorbent according to claim 2, wherein The carbon content is 10 mass % or more and 80 mass % or less, The iron content is 5 mass % or more and 35 mass % or less, The content of the metal is 1 mass % or more and 30 mass % or less.
5. The adsorbent according to claim 2, wherein The iron compound is selected from iron oxide and iron hydroxide.
6. The adsorbent according to claim 1, wherein The metal is selected from the group consisting of sodium, potassium, magnesium and calcium.
7. The adsorbent according to claim 1, wherein The binder is selected from molasses, waste molasses, starch, dextrin, corn starch, rice bran, polyvinyl alcohol, copolymers of vinyl acetate and ethylene or saponified products thereof, pulp waste liquor, lignin sulfonate, carboxymethyl cellulose, hydroxypropyl methyl cellulose, sodium alginate, phenolic resin, tar pitch, cement, blast furnace slag powder, fly ash, plaster of Paris and sodium silicate.
8. A method for producing the adsorbent according to any one of claims 1 to 7, wherein: include: a process for preparing a precursor by mixing a porous carbide with a binder and iron powder; as well as a step of treating the precursor with a gas containing carbon dioxide, The carbon dioxide concentration in the gas is 1% by volume or more and 100% by volume or less.
9. The manufacturing method according to claim 8, wherein: Also includes: The step of shaping the precursor into a particle shape prior to treatment with the gas.
10. The manufacturing method according to claim 8, wherein: Also includes: A step of drying the precursor after the treatment with the gas.
11. The manufacturing method according to claim 8, wherein: The porous carbide contains a compound of a metal selected from alkali metals and alkaline earth metals.
12. The manufacturing method according to claim 11, wherein: The compound is selected from the group consisting of oxides, hydroxides, carbonates and bicarbonates of the metal.
13. The manufacturing method according to claim 8, wherein: When the porous carbide is mixed with the binder and the iron powder, water is further added.
14. The manufacturing method according to claim 9, wherein: Also includes: A process of drying the precursor after molding the precursor.
15. The manufacturing method according to claim 8, wherein: The binder is selected from molasses, waste molasses, starch, dextrin, corn starch, rice bran, polyvinyl alcohol, copolymers of vinyl acetate and ethylene or saponified products thereof, pulp waste liquor, lignin sulfonate, carboxymethyl cellulose, hydroxypropyl methyl cellulose, sodium alginate, aldehyde resin, tar pitch, cement, blast furnace slag powder, fly ash, plaster of Paris and sodium silicate.