Polyester rubber composite tire with biodegradable tread and preparation method thereof

By introducing a polar transition layer material into the tire, the bonding problem between the polar polyester rubber tread and the non-polar rubber carcass is solved, and a polyester rubber composite tire with a biodegradable tread is prepared, which solves the problem of waste tires and tire wear debris pollution problems, and implemented solutions suitable for industrial production.

CN115109401BActive Publication Date: 2024-10-11BEIJING UNIV OF CHEM TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210201490.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-19
Filing Date
2022-03-02
Publication Date
2024-10-11
Estimated Expiration
2042-03-02

AI Technical Summary

Technical Problem

In the existing technology, polar polyester rubber treads and non-polar traditional rubber carcasses are difficult to bond, resulting in bonding problems during tire preparation and affecting tire performance and environmental friendliness.

Method used

Using polar transition layer materials, the polar polyester rubber tread and the non-polar rubber carcass are co-vulcanized to form a polyester rubber composite tire with a biodegradable tread, using butylene glycol-based polyester elastomer and polar rubber and other materials to prepare treads with excellent mechanical properties, and solve the adhesion problem through transition layer materials.

Benefits of technology

It achieves effective bonding of polar polyester rubber tread and non-polar rubber carcass, provides polyester rubber composite tires with biodegradable treads, solves the problem of waste tires and tire wear debris pollution, and is suitable for large quantities Industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003527599380000021
    Figure BDA0003527599380000021
  • Figure BDA0003527599380000031
    Figure BDA0003527599380000031
  • Figure BDA0003527599380000041
    Figure BDA0003527599380000041
Patent Text Reader

Abstract

The present invention provides a polyester rubber composite tire with a biodegradable tread and a preparation method. The composite tire includes a tread, a transition layer and a carcass. The tread is made of a biodegradable butene glycol-based polyester elastomer composite material, the transition layer is made of a polar rubber composite material, the carcass is a commercial carcass or is made by mixing a common carcass formula, and the finished product of the biodegradable polyester rubber composite tire with a tread is formed by pre-assembly molding of the tread, the transition layer and the carcass and synchronous co-vulcanization. The composite tire prepared by the present invention has excellent mechanical properties, can meet the performance requirements of the tire in actual use, and can be biodegraded and environmentally friendly. By introducing the polar transition layer material for co-vulcanization, the bonding problem between the polar polyester rubber tread material and the non-polar traditional carcass material is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of tires, and more particularly to a polyester rubber composite tire with a biodegradable tread and a preparation method thereof. Background Art

[0002] Tires are the most widely used area for rubber materials. About 1.5 billion tires are scrapped every year in the world, and only 15-20% can be recycled. A large number of discarded tires will cause great harm to the environment, occupy a lot of land resources, and cause environmental pollution; at the same time, a large number of tires in motion will also produce countless tire debris every day, which cannot be degraded for a long time and will threaten human health. Therefore, the development of degradable tires or partially degradable tires is of great significance to reality and can further improve the living environment of mankind. Due to the low recycling rate of waste tires, the development of biodegradable tires is one of the best strategies to jointly solve the pollution problems of waste tires and tire debris.

[0003] Polyester rubber, also known as polyester elastomer, is a new type of rubber that has emerged in recent years. Structurally, the main chain of polyester rubber molecules contains a large number of ester groups, which gives it biodegradable properties. When polyester rubber is used as the matrix material, a biodegradable polyester rubber composite material can be developed. Because the main chain of the molecule contains a large number of ester groups, polyester rubber is also a polar rubber material. Similar to polar polyurethane elastomers, tires prepared using polyester rubber can also be divided into two categories according to their structure: full polyester rubber tires and polyester rubber tread-traditional rubber carcass composite tires (referred to as polyester rubber composite tires). From an environmental perspective, full polyester rubber tires are more meaningful, but there are still many technical problems to be overcome. Compared with full polyester rubber tires, the preparation technology of polyester rubber composite tires is relatively simple, and when biodegradable polyester rubber materials are used as tread rubber, the pollution problem of waste tires and tire debris can be well solved. In view of this, it is of great significance to develop polyester rubber composite tires with biodegradable treads.

[0004] When preparing polyester rubber composite tires, the most important problem to be solved is the bonding problem between the polar polyester rubber tread and the non-polar traditional rubber tire body. In view of this, the present invention develops a polar transition layer material, which effectively solves the bonding problem between the polar polyester rubber tread and the non-polar traditional rubber tire body, and then prepares a polyester rubber composite tire with a biodegradable tread, filling the gap in related technologies at home and abroad. Summary of the invention

[0005] In order to solve the technical problems existing in the prior art, the present invention provides a polyester rubber composite tire with biodegradable tread and a preparation method thereof.

[0006] The present invention provides a polyester rubber composite tire with a biodegradable tread. The tread is made of a biodegradable butene glycol-based polyester elastomer composite material, has excellent mechanical properties, can meet the performance requirements of the tire in actual use, and is biodegradable and environmentally friendly. However, polyester rubber tread materials are polar materials, while currently common tire body materials are non-polar materials. The two are difficult to co-vulcanize due to the large difference in interface polarity. The present invention mainly solves the problem of bonding between a polar polyester rubber tread and a non-polar rubber tire body, and provides a method for preparing the above-mentioned polyester rubber composite tire with a biodegradable tread.

[0007] One of the objects of the present invention is to provide a polyester rubber composite tire having a biodegradable tread.

[0008] The polyester rubber composite tire with biodegradable tread is formed by assembling and preforming the tread, transition layer and carcass, and then co-vulcanizing them simultaneously;

[0009] The tread is based on 100 parts by weight of the butene glycol-based polyester elastomer, and the components are calculated by weight:

[0010]

[0011] After the components are uniformly mixed, the tread is obtained;

[0012] The transition layer is based on 100 parts by weight of the total rubber content, and the components are calculated by weight:

[0013]

[0014]

[0015] The rubber includes polar rubber and non-polar rubber;

[0016] The polar rubber accounts for 40% to 1% of the total rubber mass; preferably 60% to 1%.

[0017] After mixing the components evenly, the transition layer is obtained;

[0018] The tire body is a commercial tire body or is prepared by mixing a common tire body formula;

[0019] In a preferred embodiment of the present invention,

[0020] The polar rubber is at least one of epoxy natural rubber, nitrile rubber, and hydrogenated nitrile rubber; preferably epoxy natural rubber; more preferably epoxy natural rubber with an epoxy degree of 35% to 75%;

[0021] The non-polar rubber is at least one of natural rubber, styrene-butadiene rubber and butadiene rubber;

[0022] The nanofiller A and the nanofiller B are independently selected from at least one of white carbon black and carbon black; white carbon black and carbon black are both common grades of rubber compositions for tire treads, wherein white carbon black is preferably one of A200 and VN3, and carbon black is preferably one of N330 and N234;

[0023] The peroxide crosslinking agent A and the peroxide crosslinking agent B are independently selected from at least one of dicumyl peroxide, di-tert-butyl diisopropyl peroxide, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane;

[0024] The other compounding aids A and the other compounding aids B are independently selected from at least one of rubber processing aids, cross-linking aids, silane coupling agents, and colorants; other compounding aids can be used in combination according to the commonly used amount of rubber as long as they do not violate the purpose of the present invention.

[0025] In a preferred embodiment of the present invention,

[0026] The rubber processing aid is at least one of stearic acid, palmitic acid and oleic acid; and / or,

[0027] The auxiliary cross-linking agent is at least one of triallyl isocyanurate (TAIC), trimethylolpropane trimethacrylate, and N,N'-m-phenylene bismaleimide; and / or,

[0028] The silane coupling agent is at least one of γ-methacryloxypropyltrimethoxysilane (KH570), γ-aminopropyltriethoxysilane (KH550), and bis-γ-triethoxysilylpropyl tetrasulfide (Si69); and / or,

[0029] The colorant is at least one of titanium dioxide, phthalocyanine green and permanent yellow.

[0030] In a preferred embodiment of the present invention,

[0031] The butene glycol-based polyester elastomer is a butene glycol-based aliphatic polyester elastomer or a butene glycol-based aliphatic-aromatic copolyester elastomer.

[0032] In a preferred embodiment of the present invention,

[0033] The butene glycol-based aliphatic polyester elastomer of the present invention is a polyester elastomer in a patent application (application number 202010045414.1, invention name “A butene glycol-based polyester elastomer and preparation method”), which is cited in its entirety herein.

[0034] The structure of the butene glycol-based polyester elastomer is as follows:

[0035]

[0036] R m1 , R m2 is a branched or unbranched chain alkyl group, R m1 , R m2 can be the same or different; wherein m1, m2 represent the number of carbon atoms, 2≤m1≤14; preferably 2≤m1≤10; 2≤m2≤14; preferably 2≤m2≤10; m1, m2 can be equal or unequal;

[0037] R n1 , R n2 is a branched or unbranched chain alkyl group, R n1 , R n2 Can be the same or different; wherein n1, n2 represent the number of carbon atoms, 2≤n1≤12, preferably 2≤n1≤8; 2≤n2≤12; preferably 2≤n2≤8;; n1, n2 can be equal or different;

[0038] x and y are integers of 1 to 3, and x and y may be equal or different.

[0039] a, b, c, d, e, f, g, h, i, j, k, l, m, n, and o represent the degree of polymerization;

[0040] Among them, a, c, m, o are not 0 at the same time; e and k are not 0 at the same time; the others can be 0 at the same time;

[0041] The preparation method comprises:

[0042] The diol, dibasic acid and / or lactic acid, antioxidant and polymerization inhibitor are subjected to esterification reaction and polymerization reaction under the action of a catalyst to obtain a butene glycol-based polyester elastomer;

[0043] The diols are 1,4-butene diol and other diols; the other diols are HO-R m -OH, diethylene glycol, triethylene glycol, tetraethylene glycol or a combination thereof;

[0044] Among them, R m is a branched or unbranched chain alkyl group, wherein m represents the number of carbon atoms, 2≤m≤14; preferably 2≤m≤10;

[0045] The dibasic acid is HOOC-R n -One or a combination of COOH;

[0046] Among them, R n It is a branched or unbranched chain alkyl group, wherein n represents the number of carbon atoms, 2≤n≤12, preferably 2≤n≤8.

[0047] Among them, preferred:

[0048] The molar percentage of 1,4-butenediol in the diol is 2% to 60%, more preferably 5% to 30%.

[0049] The catalyst can be a conventional catalyst in the prior art, and in the present invention, it can be preferably one or a combination of selenium dioxide, antimony trioxide, ethylene glycol antimony, p-toluenesulfonic acid, acetate, alkyl aluminum with 1 to 12 carbon atoms, organic tin compounds and titanate; in view of the problem of heavy metal residues in polyester products, titanate catalysts without heavy metal elements, such as tetrabutyl titanate, tetraisopropyl titanate, etc., are preferred. It can be added in the esterification section or in the pre-condensation section, and the amount of the catalyst is 0.02 to 0.5% of the total mass of the diol, dibasic acid and / or lactic acid.

[0050] The antioxidant can be a conventional antioxidant in the prior art, and in the present invention, it can be preferably a phosphoric acid or phosphorous acid compound, preferably one or two of phosphoric acid, phosphorous acid, phosphate ester, phosphite ester, phenyl phosphate, and phenyl phosphite. The amount of the antioxidant is 0.01-0.2% of the total mass of the diol, dibasic acid and / or lactic acid; preferably 0.04-0.08%;

[0051] The polymerization inhibitor can be a conventional polymerization inhibitor in the prior art, and in the present invention, it can be preferably a phenolic polymerization inhibitor, an ether polymerization inhibitor, a quinone polymerization inhibitor or an aromatic amine polymerization inhibitor, preferably one or two of hydroquinone, p-tert-butylcatechol, p-hydroxyanisole, benzoquinone, diphenylamine, and p-phenylenediamine. The amount of the polymerization inhibitor is 0.01-0.5% of the total mass of the diol, dibasic acid and / or lactic acid; preferably 0.05-0.2%.

[0052] The molar ratio of the alcohol to the acid of the diol, the dibasic acid and / or the lactic acid is 1.05:1 to 1.8:1, preferably 1.1 to 1.5:1, wherein the molar ratio of the alcohol to the acid refers to the molar ratio of the number of -OH and -COOH functional groups.

[0053] The esterification reaction is preferably:

[0054] The temperature is raised to 130-240° C. under protective gas conditions for esterification reaction, and the esterification reaction time is 1-5 hours; wherein the protective gas is a gas that does not affect the reaction process and does not react with the raw materials, preferably an inert gas or nitrogen.

[0055] The polymerization reaction is preferably:

[0056] Pre-condense at 190-250°C and 3kPa-10kPa for 1-4h; then evacuate to below 500Pa at 200-250°C and perform final condensation for 0.5-10h.

[0057] In a preferred embodiment of the present invention,

[0058] The butene glycol-based aliphatic-aromatic copolyester elastomer of the present application is a polyester elastomer in a patent application (application number 202110281347.8, invention name “A butene glycol-based aliphatic-aromatic copolyester elastomer and preparation method”), which is cited in its entirety herein.

[0059] The structural formula of the butene glycol-based aliphatic-aromatic copolyester elastomer is:

[0060]

[0061] R m , R n is a branched or unbranched chain alkyl or alkoxy group, R m , R n can be the same or different; wherein m, n represent the number of carbon atoms, 2≤m≤14; preferably 2≤m≤6; 2≤n≤14; preferably 2≤n≤6; the number of alkoxy groups is preferably 0 to 3;

[0062] R x , R y is a branched or unbranched chain alkyl group, R x , R y Can be the same or different; wherein x, y represent the number of carbon atoms, 4≤x≤14, preferably one of 4, 6, 10, 12; 4≤y≤14, preferably one of 4, 6, 10, 12;

[0063] R z is an aromatic ring or a furan ring; the aromatic ring is one of a benzene ring, a biphenyl ring, and a naphthalene ring;

[0064] a, b, c, d, e, f, g, h, i, and j represent the degree of polymerization;

[0065] Among them, a, b, e, f are not 0 at the same time; c and j are not 0 at the same time; g is not 0; d can be 0;

[0066] The butene glycol-based aliphatic-aromatic copolyester elastomer is prepared by subjecting a diol, an organic acid, an antioxidant, and a polymerization inhibitor to an esterification reaction and a polymerization reaction under the action of a catalyst to obtain the butene glycol-based aliphatic-aromatic copolyester elastomer;

[0067] The diols are 1,4-butene diol and saturated aliphatic diols;

[0068] The saturated aliphatic diol is C2~C 14 A branched or unbranched diol, preferably at least one of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2,3-butanediol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, and tetraethylene glycol;

[0069] The organic acid is a dibasic acid and lactic acid, or a dibasic acid;

[0070] The dibasic acid is a saturated aliphatic dibasic acid and an aromatic dibasic acid;

[0071] The saturated aliphatic dibasic acid is C4~C 14 A branched or unbranched dibasic acid, preferably at least one of succinic acid, adipic acid, sebacic acid, and dodecanedioic acid;

[0072] The aromatic dibasic acid is at least one of terephthalic acid, phthalic acid, isophthalic acid, biphenyl dicarboxylic acid, naphthalene dicarboxylic acid and furan dicarboxylic acid;

[0073] The molar percentage of 1,4-butenediol to diol is 2% to 60%, preferably 5% to 30%;

[0074] The molar percentage of the aromatic dibasic acid in the dibasic acid is 3% to 50%, preferably 5% to 40%;

[0075] The molar ratio of -OH to -COOH functional groups in diols and organic acids is (1.1-2):1; preferably (1.1-1.7):1;

[0076] The amount of the catalyst used is 0.05% to 1.0% of the total mass of the diol and the organic acid; preferably 0.1% to 0.6%;

[0077] The amount of antioxidant used is 0.01% to 0.5% of the total mass of diol and organic acid; preferably 0.05% to 0.2%;

[0078] The amount of the polymerization inhibitor is 0.01% to 0.5% of the total mass of the diol and the organic acid; preferably 0.05% to 0.2%;

[0079] The catalyst is at least one of selenium dioxide, antimony trioxide, antimony glycol, p-toluenesulfonic acid, acetate, alkyl aluminum with 1 to 12 carbon atoms, organic tin compounds, and titanate; preferably at least one of tetrabutyl titanate and tetraisopropyl titanate; and / or,

[0080] The antioxidant is at least one of phosphoric acid and phosphorous acid compounds; preferably at least one of phosphoric acid, phosphorous acid, phosphate ester, phosphite ester, phenyl phosphate, and phenyl phosphite; and / or,

[0081] The polymerization inhibitor is at least one of phenolic polymerization inhibitors, etheric polymerization inhibitors, quinone polymerization inhibitors, and aromatic amine polymerization inhibitors; preferably at least one of hydroquinone, p-tert-butylcatechol, p-hydroxyanisole, benzoquinone, diphenylamine, and p-phenylenediamine;

[0082] Preferably, 30% to 40% of the total mass of the catalyst is added in the esterification reaction stage, and the remaining catalyst is added in the pre-condensation stage of the polymerization reaction;

[0083] The esterification reaction is carried out by heating the temperature to 130°C to 240°C under protective gas conditions, and the esterification reaction time is 2h to 6h;

[0084] The polymerization reaction is performed by pre-condensation at 190°C to 250°C and 3kPa to 10kPa for 1h to 4h; then, at 200°C to 250°C, vacuum is drawn to below 500Pa, and final condensation is performed for 0.5h to 10h.

[0085] The second object of the present invention is to provide a method for preparing a polyester rubber composite tire with a biodegradable tread, comprising:

[0086] (1) mixing the tread and transition layer components according to the amounts to obtain a tread rubber mix and a transition layer rubber mix;

[0087] (2) preparing a tread rubber sheet and a transition layer rubber sheet from the tread rubber mixture and the transition layer rubber mixture obtained in step (1), respectively;

[0088] (3) preparing a rubber composite material carcass;

[0089] (4) assembling the tread rubber sheet, the transition layer rubber sheet, and the rubber composite material carcass to preform a green composite tire;

[0090] (5) vulcanizing the green composite tire to obtain the polyester rubber composite tire with biodegradable tread.

[0091] In a preferred embodiment of the present invention,

[0092] The specific process of step (1) includes preparing the tread rubber compound and the transition layer rubber compound by using a conventional mixing process in a conventional rubber mixing equipment;

[0093] The specific process of step (2) comprises extruding the tread rubber compound and the transition layer rubber compound obtained in step (1) from a roller extruder respectively, and then discharging the sheets through the die plate of the roller extruder, or directly discharging the sheets through an open mill, to obtain semi-finished tread and transition layer rubber sheets;

[0094] The specific process of step (3) includes processing the base rubber, the sidewall and other parts of the tire;

[0095] The specific process of step (4) includes assembling the tread, transition layer, base rubber, sidewall and other tire components into a green tire on a molding machine;

[0096] The specific process of step (5) includes placing the green tire on a shaping vulcanizer equipped with a mold, and vulcanizing to obtain a degradable polyester rubber composite tire product.

[0097] Considering that during the assembly process, the polar transition layer is in direct contact with the base rubber in many parts of the tire body, the bonding strength between the two is tested to express the bonding performance between the polar transition layer and the rubber tire body.

[0098] Compared with the prior art, the present invention has the following advantages:

[0099] First, the present invention prepares a polyester rubber composite tire with a biodegradable tread for the first time, providing an effective solution to the environmental pollution problem caused by a large number of waste tires and tire scraps;

[0100] 2. The present invention solves the bonding problem between the polar polyester rubber tread and the non-polar traditional rubber tire body by introducing a polar transition layer material, and provides a universal method for preparing a polyester rubber composite tire with a biodegradable tread that does not require special equipment and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0101] Figure 1 This is a finished product picture of the biodegradable polyester rubber composite tire with tread prepared in Example 1;

[0102] 1 is the tread;

[0103] Figure 2 A cross-sectional view of a biodegradable polyester rubber composite tire with tread prepared in Example 1;

[0104] 2 is the transition layer; 3 is the carcass;

[0105] Figure 3 is a scanning electron microscope image of the tread rubber surface prepared in Example 1;

[0106] Figure 4 is a scanning electron microscope image of the surface of the tread rubber prepared in Example 1 after being buried in the soil for 3 months;

[0107] SEM scanning electron microscope: magnification 400 times. DETAILED DESCRIPTION

[0108] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0109] The butene glycol-based aliphatic polyester elastomer and the butene glycol-based aliphatic-aromatic copolyester elastomer used in the examples are homemade in the laboratory; the other raw materials used in the examples and comparative examples are conventional commercially available raw materials.

[0110] Rubber mechanical properties test: GB / T 528-1998;

[0111] Scanning electron microscope (SEM), model S-4800, produced by Hitachi, Japan;

[0112] Adhesion strength test: GB / T 2791-1995.

[0113] The parts described in the examples and comparative examples are all parts by weight.

[0114] Embodiment 1:

[0115] The tread biodegradable polyester rubber composite tire comprises a tread, a transition layer and a carcass, wherein the tread is made of a butene glycol-based polyester elastomer composite material, the transition layer is made of a polar rubber composite material, and the carcass is made by mixing a common carcass formula.

[0116] Preparation of tread rubber:

[0117] Preparation of butene glycol based polyester elastomer:

[0118] In a reaction kettle equipped with a mechanical stirrer, a heating device, a temperature measuring device, a nitrogen system and a vacuum system, 565 g (7.43 mol) of 1,3-propylene glycol, 669 g (7.43 mol) of 1,4-butanediol, 145 g (1.65 mol) of 1,4-butenediol, 1050 g (8.89 mol) of succinic acid, 770 g (3.81 mol) of sebacic acid, 0.32 g of phosphorous acid and 1.28 g of hydroquinone were added; then, the temperature was raised to 180° C. under a nitrogen atmosphere, and esterification was carried out at normal pressure for 2 hours; then, 0.1% of the total weight of the monomers was added with tetrabutyl titanate as a catalyst, and the temperature was raised to 220° C. and 3 kPa, and pre-condensation was carried out for 1 hour; finally, the temperature was evacuated to below 500 Pa at 220° C., and final condensation was carried out for 9 hours to obtain a butenediol-based polyester elastomer.

[0119] The structure of the prepared butene glycol-based polyester elastomer is as follows:

[0120]

[0121] Among them, m1=3, m2=4; n1=2, n2=8;

[0122] In addition, (a+c+e):(k+m+o)≈9.52:4.08.

[0123] The tread rubber is based on 100 parts by weight of the prepared butene glycol-based polyester elastomer, and the components are calculated by weight:

[0124]

[0125] The components are mixed according to weight to obtain the tread rubber.

[0126] Preparation of transition layer:

[0127] The weight parts of each component are:

[0128]

[0129] The carcass is the HL746 rubber carcass of Linglong Tire.

[0130] Preparation method:

[0131] (1) mixing the tread and transition layer components according to the amounts to obtain a tread rubber mix and a transition layer rubber mix;

[0132] (2) preparing a tread rubber sheet and a transition layer rubber sheet from the obtained tread rubber mix and transition layer rubber mix, respectively;

[0133] (3) preparing a rubber composite material carcass, which is the HL746 rubber carcass of Linglong tire;

[0134] (4) assembling the tread rubber sheet, the transition layer rubber sheet, and the rubber carcass to preform a green composite tire;

[0135] (5) vulcanizing the green composite tire to obtain the polyester rubber composite tire with biodegradable tread.

[0136] The tread-polar transition layer composite film and the polar transition layer-base rubber composite film were prepared on a conventional flat-plate vulcanizer at 160°C. After being fully vulcanized, the composite films were taken out and cut into 25 mm wide films to test the T-peel strength of the composite films.

[0137] Embodiment 2:

[0138] The tread biodegradable polyester rubber composite tire comprises a tread, a transition layer and a carcass, wherein the tread is made of a butene glycol-based polyester elastomer composite material, the transition layer is made of a polar rubber composite material, and the carcass is made by mixing a common carcass formula.

[0139] Preparation of tread rubber:

[0140] Preparation of butene glycol based polyester elastomer:

[0141] Into a reaction kettle equipped with mechanical stirring, heating device, temperature measuring device, nitrogen system and vacuum system, 598g (6.63mol) 1,4-butanediol, 212g (2.41mol) 1,4-butenediol, 931g (10.33mol) lactic acid, 153g (1.29mol) succinic acid, 1306g (6.46mol) sebacic acid, 3.2g tri-(2,4-di-tert-butylphenyl) )-phosphite and 12.8g of p-hydroxyanisole; then, under a nitrogen atmosphere, the temperature was raised to 130°C, and esterification was carried out at normal pressure for 2h, and then the temperature was raised to 190°C, and esterification was continued at normal pressure for 2h; then, 0.05% of the total weight of the monomers was added with tetraisopropyl titanate as a catalyst, and the temperature was raised to 190°C and 10kPa, and pre-condensation was carried out for 4h; finally, vacuum was evacuated to below 500Pa at 210°C, and final condensation was carried out for 6h to obtain a butene glycol-based polyester elastomer.

[0142] The structure of the prepared butene glycol-based polyester elastomer is as follows:

[0143]

[0144] Among them, m1=4, m2=0 (equivalent to m1=m2=4); n1=2, n2=8;

[0145] In addition, (b+d+f):(a+e):(k+m)≈10.33:1.29:6.46.

[0146] The tread rubber is based on 100 parts by weight of the prepared butene glycol-based polyester elastomer, and the components are calculated by weight:

[0147]

[0148]

[0149] The components are mixed according to weight to obtain the tread rubber.

[0150] Preparation of transition layer:

[0151] The weight parts of each component are:

[0152]

[0153] The carcass is the HL746 rubber carcass of Linglong Tire.

[0154] Preparation method:

[0155] (1) mixing the tread and transition layer components according to the amounts to obtain a tread rubber mix and a transition layer rubber mix;

[0156] (2) preparing a tread rubber sheet and a transition layer rubber sheet from the obtained tread rubber mix and transition layer rubber mix, respectively;

[0157] (3) preparing a rubber composite material carcass, which is the HL746 rubber carcass of Linglong tire;

[0158] (4) assembling the tread rubber sheet, the transition layer rubber sheet, and the rubber carcass to preform a green composite tire;

[0159] (5) vulcanizing the green composite tire to obtain the polyester rubber composite tire with biodegradable tread.

[0160] The tread-polar transition layer composite film and the polar transition layer-base rubber composite film were prepared on a conventional flat-plate vulcanizer at 160°C. After being fully vulcanized, the composite films were taken out and cut into 25 mm wide films to test the T-peel strength of the composite films.

[0161] Embodiment 3:

[0162] The tread biodegradable polyester rubber composite tire comprises a tread, a transition layer and a carcass, wherein the tread is made of a butene glycol-based polyester elastomer composite material, the transition layer is made of a polar rubber composite material, and the carcass is made by mixing a common carcass formula.

[0163] Preparation of tread rubber:

[0164] Preparation of butene glycol-based aliphatic-aromatic copolyester elastomers:

[0165] 560 g (7.36 mol) of 1,3-propylene glycol, 663 g (7.36 mol) of 1,4-butanediol, 144 g (1.64 mol) of 1,4-butene glycol, 936 g (7.93 mol) of succinic acid, 687 g (3.40 mol) of sebacic acid, 209 g (1.26 mol) of terephthalic acid, 2.24 g of phosphorous acid and 2.56 g of hydroquinone were added to a reaction kettle equipped with a mechanical stirrer, a heating device, a temperature measuring device, a nitrogen system and a vacuum system; then, the temperature was raised to 190° C. in a nitrogen atmosphere, and esterification was performed at normal pressure for 3 hours; then, 0.2% of the total weight of the monomers was added with tetrabutyl titanate as a catalyst, and the temperature was raised to 200° C. and 8 kPa, and pre-condensation was performed for 3 hours; finally, the temperature was evacuated to below 500 Pa at 220° C., and final condensation was performed for 9 hours to obtain a butene glycol-based aliphatic-aromatic copolyester elastomer.

[0166] The structure of the prepared butene glycol-based aliphatic-aromatic copolyester elastomer is as follows:

[0167]

[0168] Among them, HO-R m -OH, HO-R n -OH corresponds to 1,3-propylene glycol and 1,4-butanediol; HOOC-Rx -COOH, HOOC-R y -COOH corresponds to succinic acid and sebacic acid; HOOC-R z -COOH corresponds to terephthalic acid;

[0169] In addition, (a+e+h):(b+f+i):(c+g+j)≈7.93:3.4:1.26.

[0170] The tread rubber is based on 100 parts by weight of the prepared butene glycol-based polyester elastomer, and the components are calculated by weight:

[0171]

[0172]

[0173] The components are mixed according to weight to obtain the tread rubber.

[0174] Preparation of transition layer:

[0175] The weight parts of each component are:

[0176]

[0177] The carcass is the HL746 rubber carcass of Linglong Tire.

[0178] Preparation method:

[0179] (1) mixing the tread and transition layer components according to the amounts to obtain a tread rubber mix and a transition layer rubber mix;

[0180] (2) preparing a tread rubber sheet and a transition layer rubber sheet from the obtained tread rubber mix and transition layer rubber mix, respectively;

[0181] (3) preparing a rubber composite material carcass, which is the HL746 rubber carcass of Linglong tire;

[0182] (4) assembling the tread rubber sheet, the transition layer rubber sheet, and the rubber carcass to preform a green composite tire;

[0183] (5) vulcanizing the green composite tire to obtain the polyester rubber composite tire with biodegradable tread.

[0184] The tread-polar transition layer composite film and the polar transition layer-base rubber composite film were prepared on a conventional flat-plate vulcanizer at 160°C. After being fully vulcanized, the composite films were taken out and cut into 25 mm wide films to test the T-peel strength of the composite films.

[0185] Comparative Example 1:

[0186] It includes two parts, a tread and a carcass, and does not contain a polar rubber transition layer. The tread rubber is a natural rubber / styrene-butadiene rubber composite material, and the carcass is the same as that in Examples 1 to 3, which is the HL746 rubber carcass of Linglong tire.

[0187] The tread compound is:

[0188]

[0189] Preparation method:

[0190] (1) mixing the tread rubber according to the amount to obtain a tread rubber mix;

[0191] (2) preparing a tread rubber sheet from the obtained tread rubber mixture;

[0192] (3) preparing a rubber composite material carcass, which is the HL746 rubber carcass of Linglong tire;

[0193] (4) assembling the tread rubber sheet and the rubber carcass to preform a green composite tire;

[0194] (5) vulcanizing the green composite tire to obtain a rubber composite tire.

[0195] The tread-base rubber composite film was prepared on a conventional flat-plate vulcanizer at 160°C. The base rubber was the base rubber of the HL746 rubber carcass of Linglong Tire. After being fully vulcanized, it was taken out and cut into 25 mm wide films to test the T-peel strength of the composite film.

[0196] Table 1 Performance test results of Examples 1 to 3 and Comparative Example 1

[0197]

[0198] a : The bonding strength between the traditional rubber tread and the traditional rubber base rubber.

[0199] Polyester rubber, as a polar rubber, cannot be directly prepared into a composite tire with a traditional rubber carcass. By adding a transition layer to the tread rubber and the carcass, it can be seen from the test data of Examples 1 to 3 in Table 1 that the bonding strength between the tread and the transition layer reaches 7.5 to 8.3 MPa, and the bonding strength between the transition layer and the carcass reaches 9.0 to 10.2 MPa. Although it is not as good as the bonding strength of 13.6 MPa between the tread and the carcass in Comparative Example 1, the present invention is the first to use polyester rubber to prepare a composite tire. The interface bonding strengths of the tread and the polar transition layer, and the polar transition layer and the carcass in the polyester rubber composite material are both higher than 7.5 kN / m, which fully meets the use requirements of the composite tire. Compared with the bonding between the tread and the base rubber (representing the carcass) in the traditional rubber tire, the interface bonding strength of the polyester rubber composite tire is relatively low, which is mainly because the former are all sulfur vulcanization systems, while the tread and the polar transition layer of the latter can only be cross-linked by a peroxide system.

[0200] like Figure 1 and Figure 2 As shown, the finished product of the biodegradable polyester rubber composite tire has a good appearance, a clear tread pattern, and a good bonding effect between the tread, transition layer, and carcass.

[0201] Depend on Figure 3 and Figure 4 As shown, after the tread rubber of Example 1 was buried in the soil for 3 months, holes appeared on the surface of the tread rubber due to destruction by microorganisms, which shows that the tread rubber material developed based on polyester elastomer is biodegradable, so it can alleviate the environmental pollution problem caused by waste tires and tire debris to a certain extent.

Claims

1. A polyester rubber composite tire with a biodegradable tread, characterized in that: The polyester rubber composite tire with biodegradable tread is formed by assembling and preforming the tread, transition layer and carcass, and then co-vulcanizing them simultaneously; The tread is based on 100 parts by weight of the butene glycol-based polyester elastomer, and the components are calculated by weight: After the components are uniformly mixed, the tread is obtained; The transition layer is based on 100 parts by weight of the total rubber content, and the components are calculated by weight: The rubber includes polar rubber and non-polar rubber; the polar rubber is at least one of epoxy natural rubber, nitrile rubber, and hydrogenated nitrile rubber; Polar rubber accounts for 60% to 1% of the total rubber mass; After mixing the components evenly, the transition layer is obtained; The butene glycol-based polyester elastomer is a butene glycol-based aliphatic polyester elastomer or a butene glycol-based aliphatic-aromatic copolyester elastomer; The structure of the butene glycol-based aliphatic polyester elastomer is shown below: R m1 , R m2 is a branched or unbranched chain alkyl group, R m1 , R m2 can be the same or different; wherein m1, m2 represent the number of carbon atoms, 2≤m1≤14; 2≤m2≤14; m1, m2 can be equal or different; R n1 , R n2 is a branched or unbranched chain alkyl group, R n1 , R n2 can be the same or different; wherein n1, n2 represent the number of carbon atoms, 2≤n1≤12; 2≤n2≤12; n1, n2 can be equal or different; a, b, c, d, e, f, g, h, i, j, k, l, m, n, o represent the degree of polymerization; wherein a, c, m, o are not 0 at the same time; e and k are not 0 at the same time; x and y are integers from 1 to 3, and x and y may be equal or different; The structural formula of the butene glycol-based aliphatic-aromatic copolyester elastomer is: R m , R n is a branched or unbranched chain alkyl or alkoxy group, R m , R n can be the same or different; wherein m, n represent the number of carbon atoms, 2≤m≤14; 2≤n≤14; R x , R y is a branched or unbranched chain alkyl group, R x , R y Can be the same or different; wherein x, y represent the number of carbon atoms, 4≤x≤14; 4≤y≤14; R z is an aromatic ring or a furan ring; the aromatic ring is one of a benzene ring, a biphenyl ring, and a naphthalene ring; a, b, c, d, e, f, g, h, i, and j represent the degree of polymerization; Among them, a, b, e, f are not 0 at the same time; c and j are not 0 at the same time; g is not 0; and d can be 0.

2. The polyester rubber composite tire according to claim 1, characterized in that: The tread is based on 100 parts by weight of the butene glycol-based polyester elastomer, and the components are calculated by weight: The transition layer is based on 100 parts by weight of the total rubber content, and the components are calculated by weight:

3. The polyester rubber composite tire according to claim 1, characterized in that: The non-polar rubber is at least one of natural rubber, styrene-butadiene rubber and butadiene rubber.

4. The polyester rubber composite tire according to claim 3, characterized in that: The polar rubber is epoxy natural rubber with an epoxy degree of 35% to 75%.

5. The polyester rubber composite tire according to claim 1, characterized in that: The nanofiller A and the nanofiller B are independently selected from at least one of white carbon black and carbon black; and / or, The peroxide crosslinking agent A and the peroxide crosslinking agent B are independently selected from at least one of dicumyl peroxide, di-tert-butyl diisopropyl peroxide, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; and / or, The other compounding auxiliary agent A and the other compounding auxiliary agent B are independently selected from at least one of stearic acid, palmitic acid, oleic acid, a co-crosslinking agent, a silane coupling agent, and a colorant.

6. The polyester rubber composite tire according to claim 5, characterized in that: The auxiliary cross-linking agent is at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, and N,N'-m-phenylene bismaleimide; and / or, The silane coupling agent is at least one of γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and bis-γ-triethoxysilylpropyl tetrasulfide; and / or, The colorant is at least one of titanium dioxide, phthalocyanine green and permanent yellow.

7. The polyester rubber composite tire according to claim 1, characterized in that: In the structural formula of the butene glycol-based aliphatic polyester elastomer, 2≤m1≤10; 2≤m2≤10; 2≤n1≤8; 2≤n2≤8; The butene glycol-based aliphatic polyester elastomer is prepared by subjecting diol, dibasic acid, optional lactic acid, antioxidant and polymerization inhibitor to esterification reaction and polymerization reaction under the action of a catalyst.

8. The polyester rubber composite tire according to claim 1, characterized in that: In the structural formula of the butene glycol-based aliphatic-aromatic copolyester elastomer, 2≤m≤6; 2≤n≤6; the number of alkoxy groups is 0 to 3; x is one of 4, 6, 10, and 12; y is one of 4, 6, 10, and 12; The butene glycol-based aliphatic-aromatic copolyester elastomer is prepared by subjecting a diol, an organic acid, an antioxidant, and a polymerization inhibitor to an esterification reaction and a polymerization reaction under the action of a catalyst to obtain the butene glycol-based aliphatic-aromatic copolyester elastomer; The diols are 1,4-butene diol and saturated aliphatic diols; The saturated aliphatic diol is C2~C 14 Branched or unbranched diols; The organic acid is a dibasic acid and lactic acid, or a dibasic acid; The dibasic acid is a saturated aliphatic dibasic acid and an aromatic dibasic acid; The saturated aliphatic dibasic acid is C4~C 14 Branched or unbranched dibasic acids; The aromatic dibasic acid is at least one of terephthalic acid, phthalic acid, isophthalic acid, biphenyl dicarboxylic acid, naphthalene dicarboxylic acid and furan dicarboxylic acid; The molar percentage of 1,4-butenediol in diol is 2% to 60%; The molar percentage of the aromatic dibasic acid in the dibasic acid is 3% to 50%; The molar ratio of -OH to -COOH functional groups in diols and organic acids is (1.1-2):1; The amount of the catalyst used is 0.05% to 1.0% of the total mass of the diol and the organic acid; The dosage of the antioxidant is 0.01% to 0.5% of the total mass of the diol and the organic acid; The dosage of the polymerization inhibitor is 0.01% to 0.5% of the total mass of the diol and the organic acid; The catalyst is at least one of selenium dioxide, antimony trioxide, antimony glycol, p-toluenesulfonic acid, acetate, alkyl aluminum with 1 to 12 carbon atoms, organic tin compounds, and titanate; and / or, The antioxidant is at least one of phosphoric acid and phosphorous acid compounds; and / or, The polymerization inhibitor is at least one of a phenol polymerization inhibitor, an ether polymerization inhibitor, a quinone polymerization inhibitor, and an aromatic amine polymerization inhibitor; The esterification reaction is carried out by heating the temperature to 130°C to 240°C under protective gas conditions, and the esterification reaction time is 2h to 6h; The polymerization reaction is performed by pre-condensation at 190°C to 250°C and 3kPa to 10kPa for 1h to 4h; then, at 200°C to 250°C, vacuum is drawn to below 500Pa, and final condensation is performed for 0.5h to 10h.

9. The polyester rubber composite tire according to claim 8, characterized in that: The saturated aliphatic diol is at least one of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol; The saturated aliphatic dibasic acid is at least one of succinic acid, adipic acid, sebacic acid, and dodecanedioic acid; The molar percentage of 1,4-butenediol in diol is 5% to 30%; The molar percentage of the aromatic dibasic acid in the dibasic acid is 5% to 40%; The molar ratio of -OH to -COOH functional groups in diols and organic acids is (1.1-1.7):1; The amount of the catalyst used is 0.1% to 0.6% of the total mass of the diol and the organic acid; The dosage of the antioxidant is 0.05% to 0.2% of the total mass of the diol and the organic acid; The dosage of the polymerization inhibitor is 0.05% to 0.2% of the total mass of the diol and the organic acid; The catalyst is at least one of tetrabutyl titanate and tetraisopropyl titanate; and / or, The antioxidant is at least one of phosphoric acid, phosphorous acid, phosphate ester, phosphite ester, phenyl phosphate, and phenyl phosphite; and / or, The polymerization inhibitor is at least one of hydroquinone, p-tert-butylcatechol, p-hydroxyanisole, benzoquinone, diphenylamine, and p-phenylenediamine; 30% to 40% of the total mass of the catalyst is added in the esterification reaction stage, and the remaining catalyst is added in the pre-condensation stage of the polymerization reaction.

10. A method for preparing a polyester rubber composite tire with biodegradable tread as claimed in any one of claims 1 to 9, characterized in that The method comprises: (1) mixing the tread and transition layer components according to the amounts to obtain a tread rubber mix and a transition layer rubber mix; (2) preparing a tread rubber sheet and a transition layer rubber sheet from the tread rubber mixture and the transition layer rubber mixture obtained in step (1), respectively; (3) preparing a rubber composite material carcass; (4) assembling the tread rubber sheet, the transition layer rubber sheet, and the rubber composite material carcass to preform a green composite tire; (5) vulcanizing the green composite tire to obtain the polyester rubber composite tire with biodegradable tread.