A method for preparing large-size TC18 titanium alloy bars
By employing a method of low-heat forging, high-low temperature cyclic forging, and reversible upsetting, the problems of long cycle time and high cost in the preparation of large-size TC18 titanium alloy bars have been solved. This method enables the efficient preparation of TC18 titanium alloy bars that meet aerospace standards and exhibits good microstructure uniformity and ultrasonic flaw detection uniformity.
Patent Information
- Application Number
- CN202210685128.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-06-14
AI Technical Summary
Existing technologies for preparing large-size TC18 titanium alloy bars suffer from problems such as long forging cycles, high costs, poor batch stability, and unsatisfactory microstructure and performance.
TC18 titanium alloy bars with diameters of Φ500mm to Φ600mm were prepared by using a method of low-temperature cyclic forging combined with reversible upsetting and drawing, and by continuously reheating in the furnace to prevent grain growth and ensure fine and uniform microstructure.
It shortens the production cycle, reduces the manufacturing cost, and meets the mechanical properties and microstructure uniformity requirements of aviation standards, while also providing good uniformity in ultrasonic flaw detection.
Smart Images

Figure CN115121752B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonferrous metal processing technology and relates to a method for preparing a large-size TC18 titanium alloy bar. Background Art
[0002] TC18 titanium alloy is a high-strength, high-toughness near-β-type titanium alloy with a nominal composition of Ti-5Al-5Mo-5V-1Cr-1Fe. It is currently widely used in key load-bearing components such as aircraft fuselages, landing gears, load-bearing frame beams, and pillars. With the development of the aviation industry, new demands are put forward for the integration and large-scale of aircraft load-bearing components. To this end, high-quality, large-size TC18 titanium alloy bars are required. TC18 titanium alloy has a low phase transition point, high resistance to forging deformation, poor forging permeability of large-size bars, and a large "deformation dead zone". Traditional processes usually use small deformation, multiple fire times and other methods to match the relationship between deformation and organization. The disadvantages are long forging cycle, high cost, and poor batch stability. Based on the hot working characteristics of near-β-type titanium alloys, this patent proposes a new preparation method for large-size TC18 titanium alloy bars, which can obtain high-quality large-size TC18 titanium alloy bars while reducing production cycle and cost. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and propose a method for preparing large-size TC18 titanium alloy bars. The preparation method has fewer forging times and fewer grinding times, thereby avoiding the problem of long production cycle. The prepared bars have a unit weight of 2000kg to 4000kg and a diameter of Φ500mm to Φ600mm. Their mechanical properties meet the requirements of aviation standards, and they also have the advantages of good uniformity of high and low magnification structures and ultrasonic flaw detection.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] A method for preparing a large-size TC18 titanium alloy bar is characterized by being implemented in the following steps:
[0006] S1. Open forging
[0007] Select TC18 titanium alloy ingot, heat and keep warm, and perform 2 to 4 fire forging to obtain an intermediate billet;
[0008] S2. Intermediate billet forging
[0009] The intermediate billet is heated and kept warm, and forged 4 to 6 times to obtain a bar billet;
[0010] S3, finished product forging
[0011] The rod blank is heated and kept warm, forged for 1 to 2 times, and rounded to obtain the TC18 titanium alloy rod.
[0012] Furthermore, in step S1, the ingot is heated to 250°C to 350°C above the phase transformation point for a holding time of 400min to 600min, and the first fire forging is performed, and then the ingot is returned to the furnace to 250°C to 350°C above the phase transformation point for a holding time of 200min to 300min, and the second fire forging is performed. The final forging temperature is not less than 800°C. After forging, the billet is cooled in air to obtain an intermediate billet.
[0013] Furthermore, the TC18 titanium alloy ingot selected in step S1 has a unit weight of 4.5 to 6 t and a diameter of Φ690 to Φ720 mm.
[0014] Furthermore, in the 2nd to 4th forging of step S1, the ingot is heated and kept warm before being upset and drawn, the forging ratio during upsetting is controlled between 1.5 and 2.5, and the deformation during drawing is controlled between 30% and 80%;
[0015] After returning to the furnace for heat preservation, the steel is upset and drawn. The forging ratio is controlled between 1.5 and 2.5 during upsetting, and the deformation is controlled between 30% and 80% during drawing. Reversing upsetting is used in some firings during the forging process to ensure that the β grains are fully refined and homogenized.
[0016] Furthermore, the specific process of step S2 is: heating and keeping the intermediate billet at 100°C to 200°C above the phase transformation point and 30°C to 60°C below the phase transformation point, performing 4 rounds of forging respectively, controlling the forging ratio during upsetting between 1.5 and 2.5, controlling the deformation during drawing between 20% and 60%, using the reversing upsetting and drawing operation mode for some rounds, the final forging temperature is not less than 600°C, and air cooling the billet after each forging to finally obtain a rod billet.
[0017] Furthermore, the specific process of the 4-fire forging in step S2 is as follows: the heating temperature of the first fire is 100°C to 200°C above the phase transformation point, and the holding time is 400min to 600min before upsetting; the heating temperature of the second fire is 30°C to 60°C below the phase transformation point, and the holding time is 400min to 600min before upsetting; the heating temperature of the third fire is 100°C to 200°C above the phase transformation point, and the holding time is 400min to 600min before upsetting; the heating temperature of the fourth fire is 30°C to 60°C below the phase transformation point, and the holding time is 400min to 600min before upsetting.
[0018] Furthermore, the specific process of the first fire forging in step S3 is: heating the billet to 30°C to 60°C below the phase transformation point, keeping the temperature for 400min to 600min, and then stretching and shaping the billet to a round diameter of Φ510mm to Φ610mm, controlling the deformation amount to 5% to 30%, and the final forging temperature not less than 600°C.
[0019] Furthermore, the TC18 titanium alloy prepared in step S3 has a unit weight of 2 t to 4 t and a diameter of Φ500 mm to Φ600 mm.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] This preparation method has fewer forging times and fewer grinding times, avoiding the problem of long production cycles; this preparation method adopts a continuous re-furnace forging heating method for blank heating to prevent the grains from growing due to long heating time after crushing, fully ensuring the degree of organizational refinement and effectively guaranteeing the uniformity of organizational structure and performance; this preparation method adopts a high-low-high cycle forging process, the traditional high-low-high process is 1 high-low cycle, and this preparation method adopts 2-3 high-low cycles to improve organizational uniformity; this preparation method adopts a reversing upsetting forging method for some fires to ensure the horizontal and vertical organizational refinement and uniformity. The single weight of the prepared bar is 2 to 4 tons, and the diameter is Φ500mm to Φ600mm. Its mechanical properties meet the requirements of aviation standards, and it also has the advantages of good uniformity of high-low organization and ultrasonic flaw detection.
[0022] Other features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0025] Figure 1 (a) is a schematic diagram of the macrostructure of the head of the Φ550 mm rod prepared in Example 1 of the present invention;
[0026] Figure 1 (b) is a schematic diagram of the macrostructure of the tail of the Φ550 mm rod prepared in Example 1 of the present invention;
[0027] Figure 2 (a) is a high-magnification structural diagram of the edge of a Φ550 mm rod prepared in Example 1 of the present invention;
[0028] Figure 2 (b) is a high-magnification structural diagram of the R / 2 portion of the Φ550 mm rod prepared in Example 1 of the present invention;
[0029] Figure 2 (c) is a high-magnification structural diagram of the core of the Φ550 mm rod prepared in Example 1 of the present invention;
[0030] Figure 3 (a) is a schematic diagram of the empty burning structure of the head of the Φ550 mm rod prepared in Example 1 of the present invention;
[0031] Figure 3 (b) is a schematic diagram of the empty burning structure of the tail of the Φ550 mm rod prepared in Example 1 of the present invention; DETAILED DESCRIPTION
[0032] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices consistent with some aspects of the present invention as detailed in the appended claims.
[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0034] A method for preparing a large-size TC18 titanium alloy bar is specifically implemented according to the following steps:
[0035] S1. Open forging
[0036] Select TC18 titanium alloy ingots with a unit weight of 4.5-6t and a diameter of Φ690-Φ720mm, heat and keep them warm, and perform 2-4 fire forgings. First, heat the ingot to 250℃-350℃ above the phase transformation point, keep it warm for 400min-600min, perform the first fire forging, then return it to 250℃-350℃ above the phase transformation point, keep it warm for 200min-300min, perform the second fire forging, and the final forging temperature is not less than 800℃. After forging, cool the billet in the air to obtain the intermediate billet. The selected TC18 titanium alloy ingot. During forging, the ingot is heated and kept warm, and then upsetting is performed. The forging ratio is controlled between 1.5 and 2.5 during upsetting, and the deformation is controlled between 30% and 80% during elongation. Some fires in the forging process adopt the operation mode of reversing upsetting to ensure that the β grains are fully refined and homogenized.
[0037] S2. Intermediate billet forging
[0038] The intermediate billet is heated and kept at 100℃~200℃ above the phase transformation point and 30℃~60℃ below the phase transformation point, and forged for 4 to 6 times. The forging ratio is controlled between 1.5 and 2.5 during upsetting, and the deformation is controlled between 20% and 60% during drawing. Reversing upsetting and drawing are used in some of the fires. The final forging temperature is not less than 600℃. After the holding time is 400min~600min, upsetting and drawing are carried out. After each forging, the billet is air-cooled to finally obtain a rod billet.
[0039] S3, finished product forging
[0040] The bar billet is heated and kept warm, and then forged 1 to 2 times, and then rounded to obtain TC18 titanium alloy bar. The prepared TC18 titanium alloy has a unit weight of 2t to 4t and a diameter of Φ500mm to Φ600mm. The bar billet is heated to 30℃ to 60℃ below the phase transition point, and after the holding time is 400min to 600min, it is stretched and shaped, and the rounded diameter is Φ510mm to Φ610mm, the deformation is controlled at 5% to 30%, and the final forging temperature is not less than 600℃.
[0041] The following is an explanation of the specific process:
[0042] Embodiment 1:
[0043] The present invention provides a method for preparing a large-size TC18 titanium alloy bar, which is implemented according to the following steps:
[0044] Open forging: Select TC18 titanium alloy ingots with a 4.5-ton specification of Φ690mm and chemical composition that meet the requirements, and perform two-stage forging: first heat the ingot to 250℃ above the phase transition point, keep it warm for 400min, perform the first stage forging, perform upsetting, control the forging ratio at 1.8 during upsetting, and control the deformation at 50% during elongation, return to the furnace to 250℃ above the phase transition point, keep it warm for 200min, perform upsetting, control the forging ratio at 1.8 during upsetting, and control the deformation at 50% during elongation. The specifications after forging are square with a side length of 600mm, and the final forging temperature is controlled at above 800℃. The material after forging is cooled by air cooling to obtain an intermediate billet. Open billet heating adopts a continuous re-furnace forging heating method to prevent the grains from growing due to excessive heating time after crushing, fully guarantee the degree of organizational refinement, and effectively guarantee the uniformity of organization and performance.
[0045] Intermediate billet forging: The intermediate billet forging is completed in 4 fires. The heating temperature of the first fire is 1000℃, and it is upsetting after being kept warm for 500min; the heating temperature of the second fire is 820℃, and it is upsetting after being kept warm for 500min; the heating temperature of the third fire is 1000℃, and it is upsetting after being kept warm for 500min; the heating temperature of the fourth fire is 820℃, and it is upsetting after being kept warm for 420min. The forging ratio of the above fire upsetting is controlled at 1.8, and the deformation during drawing is controlled at 40%. The specification after the fourth fire forging is a cross-sectional diameter of 580mm, and the final forging temperature is controlled at above 600℃. Air cooling is used for cooling after each fire forging.
[0046] Finished product forging: Finished product forging is completed in 1 fire. The heating temperature of the first fire is 820℃. After keeping warm for 420min, it is directly drawn and shaped to Φ560mm. The deformation of the straight drawing is 8%. The final forging temperature is controlled at above 600℃. After the finished product forging fire is completed, it is cooled by air cooling and turned into Φ550mm bars by lathe.
[0047] The Φ550 mm rod prepared in Example 1 was observed at low magnification. Figure 1 It can be seen that there is no delamination, cracks, pores, segregation, metal and non-metallic inclusions and other metallurgical defects visible to the naked eye at the head and tail of the rod macrostructure; there is no clear grain visible to the naked eye, and the macrostructure is uniform and blurred, meeting the requirements of aviation standards.
[0048] The Φ550 mm rod prepared in Example 1 was observed under high magnification. Figure 2 It can be seen that the microstructure of the rod is a uniform structure processed in the α+β two-phase region, all the original β grain boundaries are fully broken, there is no continuous and straight grain boundary α phase, and the microstructure is uniform at high magnification, which meets the requirements of aviation standards.
[0049] The head and tail of the Φ550 mm rod prepared in Example 1 were observed for empty burning structure. Figure 3 It can be seen that there is no obvious stratified structure in the air-fired low-magnification specimen, which meets the requirements of aviation standards.
[0050] After heat treatment, the Φ550 mm rod prepared in Example 1 was taken and the room temperature performance was tested by taking a transverse sample. The results showed that the rod met the requirements of aviation standards, had good uniformity and had a certain amount of surplus, indicating that the mechanical properties of the rod were good. The mechanical properties test results are shown in Table 1.
[0051] Table 1:
[0052]
[0053] The ultrasonic flaw detection results of the Φ550mm rod prepared in Example 1 were uniform and consistent, and all met the requirement of Φ2.0-6dB or above.
[0054] Example 2
[0055] The present invention provides a method for preparing a large-size TC18 titanium alloy bar, which is implemented according to the following steps:
[0056] Open forging: select 6-ton TC18 titanium alloy ingots with a specification of Φ720mm and chemical composition that meet the requirements, and perform two-stage forging: heating temperature is 1200℃, after keeping warm for 600min, upsetting is performed, the forging ratio during upsetting is controlled at 2.5, and the deformation during drawing is controlled at 30%. After returning to 1150℃ and keeping warm for 200min, upsetting is performed, the forging ratio during upsetting is controlled at 1.5, and the deformation during drawing is controlled at 30%. The specification after forging is a square with a side length of 600mm. The final forging temperature is controlled at above 800℃ to obtain an intermediate billet. The material after forging is cooled by air cooling.
[0057] Intermediate billet forging: The intermediate billet forging is completed in 4 fires. The heating temperature of the first fire is 1050℃, and the upsetting is carried out after keeping warm for 400min; the heating temperature of the second fire is 850℃, and the upsetting is carried out after keeping warm for 400min; the heating temperature of the third fire is 1050℃, and the upsetting is carried out after keeping warm for 400min; the heating temperature of the fourth fire is 850℃, and the upsetting is carried out after keeping warm for 400min. The forging ratio of the above fire upsetting is controlled at 1.5, and the deformation during drawing is controlled at 40%. The specification after the fourth fire forging is a cross-sectional diameter of 580mm, and the final forging temperature is controlled at above 600℃. After each fire forging, air cooling is used for cooling.
[0058] Finished product forging: Finished product forging is completed in 1 fire. The heating temperature of the first fire is 850℃. After keeping warm for 400min, it is directly drawn and shaped to Φ560mm. The deformation of the straight drawing is 8%, and the final forging temperature is controlled above 600℃. After the finished product forging fire is completed, it is cooled by air cooling and turned into Φ500mm bars by lathe.
[0059] Example 3
[0060] The present invention provides a method for preparing a large-size TC18 titanium alloy bar, which is implemented according to the following steps:
[0061] Open forging: select TC18 titanium alloy ingots with a 5-ton specification of Φ700mm and chemical composition that meet the requirements, and perform two-stage forging: heating temperature is 1150℃~1200℃, after keeping warm for 600min, upsetting is performed, the forging ratio during upsetting is controlled at 2.5, and the deformation during drawing is controlled at 50%, after returning to 1150℃ and keeping warm for 300min, upsetting is performed, the forging ratio during upsetting is controlled at 2.5, and the deformation during drawing is controlled at 50%, the specification after forging is a square with a side length of 600mm, the final forging temperature is controlled at above 800℃, and the intermediate billet is obtained. The material after forging is cooled by air cooling.
[0062] Intermediate billet forging: The intermediate billet forging is completed in 4 fires. The heating temperature of the first fire is 1000℃~1050℃, and it is upsetting after 600min of heat preservation; the heating temperature of the second fire is 820℃~850℃, and it is upsetting after 600min of heat preservation. The heating temperature of the third fire is 1000℃~1050℃, and it is upsetting after 600min of heat preservation. The heating temperature of the fourth fire is 820℃~850℃, and it is upsetting after 540min of heat preservation. The forging ratio of the above fire upsetting is controlled at 2.5, and the deformation during drawing is controlled at 60%. The specification after the fourth fire forging is a cross-sectional diameter of 580mm, and the final forging temperature is controlled at above 600℃. After each fire forging, air cooling is used for cooling.
[0063] Finished product forging: Finished product forging is completed in 1 fire. The heating temperature of the first fire is 850℃, and after keeping warm for 540min, it is directly drawn and shaped to Φ560mm. The deformation of the straight drawing is 8%, and the final forging temperature is controlled above 600℃. After the finished product forging fire is completed, it is cooled by air cooling and turned into Φ600mm bars by lathe.
[0064] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0065] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A method for preparing large-size TC18 titanium alloy bars, characterized in that: Follow the steps below to implement it: S1. Billet forging Select TC18 titanium alloy ingot, heat and keep warm, and perform two-stage forging to obtain an intermediate billet; In the step S1, the ingot is heated to 250°C to 350°C above the phase transformation point, the holding time is 400min to 600min, the first fire forging is performed, and then the ingot is returned to the furnace to 250°C to 350°C above the phase transformation point, the holding time is 200min to 300min, the second fire forging is performed, the final forging temperature is not less than 800°C, and the billet is cooled in air after forging to obtain an intermediate billet; S2. Intermediate billet forging The intermediate billet is heated and kept warm, and forged four times to obtain a bar billet; The specific process of the 4-fire forging in step S2 is as follows: the heating temperature of the first fire is 100°C to 200°C above the phase transformation point, and the holding time is 400min to 600min before upsetting; the heating temperature of the second fire is 30°C to 60°C below the phase transformation point, and the holding time is 400min to 600min before upsetting; the heating temperature of the third fire is 100°C to 200°C above the phase transformation point, and the holding time is 400min to 600min before upsetting; the heating temperature of the fourth fire is 30°C to 60°C below the phase transformation point, and the holding time is 400min to 600min before upsetting; Among them, the forging ratio during upsetting is controlled between 1.5 and 2.5, the deformation during drawing is controlled between 20% and 60%, some fires adopt the operation mode of reversing upsetting and drawing, the final forging temperature is not less than 600℃, and the billet is air-cooled after each forging to finally obtain a bar billet; S3, finished product forging The bar blank is heated and kept warm, subjected to one-time forging, and rounded to obtain a TC18 titanium alloy bar; The specific process of the first fire forging in step S3 is: heating the billet to 30°C to 60°C below the phase transformation point, keeping the temperature for 400min to 600min, and then stretching and shaping the billet to a round diameter of Φ510mm to Φ610mm, controlling the deformation amount to 5% to 30%, and the final forging temperature not less than 600°C; The final prepared TC18 titanium alloy has a unit weight of 2t to 4t and a diameter of Φ500mm to Φ600mm.
2. The method for preparing a large-size TC18 titanium alloy bar according to claim 1, characterized in that: The TC18 titanium alloy ingot selected in step S1 has a unit weight of 4.5 to 6 tons and a diameter of Φ690 to Φ720 mm.
3. The method for preparing a large-size TC18 titanium alloy bar according to claim 1, characterized in that: In the second-time forging of step S1, the ingot is heated and kept warm before being upset and drawn, the forging ratio during upsetting is controlled between 1.5 and 2.5, and the deformation during drawing is controlled between 30% and 80%; After returning to the furnace for heat preservation, the steel is upset and drawn. The forging ratio is controlled between 1.5 and 2.5 during upsetting, and the deformation is controlled between 30% and 80% during drawing. Reversing upsetting is used in some firings during the forging process to ensure that the β grains are fully refined and homogenized.
Citation Information
Patent Citations
Method for processing TC18 titanium alloy large-sized section bar
CN102641978A
Preparation method of TC18 titanium alloy large-size rod
CN110205571A
Forging method for improving structure and texture uniformity of TC18 titanium alloy large-specification bar
CN112139413A
Forging method of ultrahigh-toughness TB18 titanium alloy large-specification forging stock
CN114603074A