Pb-doped SmFeO3 gas-sensitive material with hollow tubular structure and its application

Pb-doped SmFeO3 gas-sensitive material was prepared by electrospinning to form a hollow tubular structure, which solved the problem of high energy consumption and insufficient response of SmFeO3 sensors at high temperatures, and achieved high sensitivity detection of acetone gas, suitable for diabetes Prediagnosis.

CN115128135BActive Publication Date: 2024-11-22TAISHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210724263.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-11-22
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

The existing SmFeO3 gas sensors need to operate at higher temperatures, resulting in increased energy consumption and safety hazards, and insufficient response at extremely low gas concentrations, which cannot meet the detection needs of diabetes prediagnosis.

Method used

Electrospinning method was used to prepare Pb-doped SmFeO3 gas-sensitive material to form a hollow tubular structure, increasing specific surface area and porosity, improving responsiveness, and further improving the RH adaptability and long-term stability of the material under light conditions.

Benefits of technology

It reduces the optimal operating temperature of the sensor, significantly improves the detection sensitivity and selectivity of acetone gas, and has an error of less than 10%. It is suitable for industrial production and reduces the cost of non-invasive diagnosis of diabetes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115128135B_ABST
    Figure CN115128135B_ABST
Patent Text Reader

Abstract

The invention discloses a Pb-doped SmFeO3 gas-sensitive material with a hollow tubular structure and its application. The Pb-doped SmFeO3 gas-sensitive material is a nano powder with a hollow tubular structure, and the doping amount of Pb is 2wt%. The preparation method thereof is as follows: Fe(NO3)3, Sm2O3, PdCl2, DMF, PVP, anhydrous ethanol and nitric acid are added into deionized water to obtain a mixed solution, the mixed solution is heated and stirred until transparent to obtain a precursor solution; the precursor solution is electrostatically spun to obtain nanofibers, and the nanofibers are sintered to obtain the Pb-doped SmFeO3 gas-sensitive material. The invention prepares the Pd-doped SmFeO3 gas-sensitive material by an electrostatic spinning method, which has a large specific surface area and a high porosity, and can increase the adsorption sites and percolation channels of gas molecules. The RH adaptability, selectivity and long-term stability of the Pd-doped SmFeO3 are also greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor gas sensitive materials, and in particular to a Pb-doped SmFeO3 gas sensitive material with a hollow tubular structure and applications thereof. Background Art

[0002] As a non-invasive detection method, breath analysis has been increasingly valued for its advantages such as being painless and suitable for home use. Among them, using acetone gas to detect diabetes is the most likely disease detection method to be realized at this stage. It has been reported that the acetone concentration in the exhaled gas of healthy people is about 0.3-0.9ppm, while the acetone concentration in the exhaled gas of diabetic patients is about 0.9-1.8ppm, and even exceeds 1.8ppm in severe cases. Such a significant difference in acetone concentration makes it a biomarker for pre-diagnosis of diabetes.

[0003] In recent years, there have been more and more reports on gas detection using metal oxide semiconductor (MOS) gas sensors. MOSs, especially ABO3 perovskite materials, have the unique advantages of large specific surface area and abundant active sites, which can increase the diffusion path and enhance the adsorption of gas molecules, thereby improving its sensing ability. 0.9 Mg 0.1 The detection range of O3 is 353-300ppm, the detection range of ZnFe2O4 is 25-100ppm, the detection range of NiFe2O4 is 24.3-100ppm, the detection range of PrFeO3 is 44.94-50ppm, the detection range of CoFe2O4 is 17.3-100ppm, the detection range of Pd-NdFeO3 is 50-300ppm, the detection range of Pt-Zn2SnO4 is 500-680ppm, the detection range of Ca-YbFeO3 is 1.42-3ppm, LaNi 0.5 Ti 0.5 The detection range of O3 is 5-29ppm, LaFeO3, Gd 0.9 Ca 0.1 The detection range of FeO3 is 117.7-600ppm, La 0.68 Pb 0.32The detection range of FeO3 is 7-50ppm. As a typical p-type MOS, SmFeO3 is widely used in the field of gas sensing with its excellent performance: the detection range of NO2 is 0.2-10.2ppm, the detection range of CO is 1.40-100ppm, the detection range of ozone is 1.1-8ppm, and the detection range of methanol is 18.19-100ppm. However, the sensor based on SmFeO3 needs to work at a higher operating temperature, which increases energy consumption and safety hazards. When the gas concentration is ppb, the response is low and cannot meet the requirements of pre-diagnosis of diabetes using exhaled breath. Therefore, there is a need for a sensor with low operating temperature, high detection sensitivity, and the ability to respond to acetone at PPb concentration. Summary of the invention

[0004] In view of the above-mentioned prior art, the purpose of the present invention is to provide a Pb-doped SmFeO3 gas-sensitive material with a hollow tubular structure and its application. The present invention adopts an electrospinning method to prepare a Pd-doped SmFeO3 gas-sensitive material, which is a hollow tubular microstructure, so that it has a large specific surface area and high porosity, which can increase the adsorption sites and percolation channels of gas molecules. The RH adaptability, selectivity and long-term stability of Pd-doped SmFeO3 are also greatly improved. After illumination, the RH adaptability, selectivity and long-term stability are further increased.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] According to a first aspect of the present invention, a Pb-doped SmFeO3 gas-sensitive material is provided. The Pb-doped SmFeO3 gas-sensitive material is a nano powder with a hollow tubular structure. The doping amount of Pb in the Pb-doped SmFeO3 gas-sensitive material is 2 wt%.

[0007] Preferably, the average particle size of the Pb-doped SmFeO3 gas-sensitive material is 64.1 nm and the average pore size is 11.8 nm.

[0008] The second aspect of the present invention provides a method for preparing a Pb-doped SmFeO3 gas-sensitive material, comprising the following steps:

[0009] (1) adding Fe(NO3)3, Sm2O3, PdCl2, DMF, PVP, anhydrous ethanol and nitric acid into deionized water to obtain a mixed solution, heating and stirring the mixed solution until transparent to obtain a precursor solution;

[0010] (2) The precursor solution obtained in step (1) is subjected to electrospinning to obtain nanofibers, and the nanofibers are sintered to obtain a powdered Pb-doped SmFeO3 gas-sensitive material.

[0011] Preferably, in step (1), the mass ratio of Fe(NO3)3, Sm2O3, PdCl2, DMF, PVP, ethanol and nitric acid to deionized water is 242:174.4:177.4:100:100:50:50:200.

[0012] Preferably, the weight average molecular weight of the PVP is 1,300,000; and the volume concentration of the nitric acid is 97%.

[0013] Preferably, in step (1), the heating is water bath heating at a temperature of 60° C.; and the stirring is magnetic stirring.

[0014] Preferably, in step (2), during the electrospinning process, the voltage is maintained at 12 kV, the distance between the needle tip of the syringe used for electrospinning and the collector is 20 cm, and the injection rate is 0.4 mL / h.

[0015] Preferably, in step (2), the sintering temperature is 800° C. and the sintering time is 6 hours.

[0016] The third aspect of the present invention provides the use of Pb-doped SmFeO3 gas-sensitive material in the preparation of a gas sensor.

[0017] A fourth aspect of the present invention provides a Pb-doped SmFeO3 gas sensor, wherein the sensor is prepared by the following method:

[0018] The Pb-doped SmFeO3 gas-sensitive material is added into deionized water to prepare a paste-like slurry, and the slurry is placed on a gas-sensitive film, and after drying, a Pb-doped SmFeO3 gas-sensitive sensor is obtained.

[0019] A fifth aspect of the present invention provides the use of a Pb-doped SmFeO3 gas sensor in detecting acetone or in non-invasively diagnosing diabetes.

[0020] Beneficial effects of the present invention:

[0021] (1) The present invention adopts electrospinning to prepare Pd-doped SmFeO3 gas-sensitive material, which has a hollow tubular microstructure, so that it has a large specific surface area and high porosity, which can increase the adsorption sites and percolation channels of gas molecules. Compared with SmFeO3, the response of Pd-doped SmFeO3 is significantly improved, and it is further improved under light. The RH adaptability, selectivity and long-term stability of Pd-doped SmFeO3 are also greatly improved.

[0022] (2) The Pd-doped SmFeO3 gas-sensitive material prepared by the present invention is used to make a gas sensor. After the introduction of light, the optimal operating temperature is reduced by 100° C. compared with SmFeO3.

[0023] (3) The present invention uses a Pd-doped SmFeO3 gas sensor to detect the acetone concentration in the exhaled gas of real people. Compared with the gas chromatography-mass spectrometry method, the error is less than 10%, and the error is even smaller under external light conditions.

[0024] (4) The preparation method of the present invention is simple, low-cost, and suitable for industrial production. It can reduce the cost of in vitro non-invasive diagnosis of diabetes and truly benefit the majority of diabetic patients. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 :Preparation flow chart of Pd-doped SmFeO3 sensor;

[0026] Figure 2 :(a) XRD pattern of Pd-doped SmFeO3; (b) EDS spectrum of 2wt% Pd-doped SmFeO3 Figure 3 ;(cd): SEM images of 2wt% Pd-doped SmFeO3;(ef) TEM images of 2wt% Pd-doped SmFeO3;(g) Adsorption-desorption isotherms and pore size distribution (inset) of 2wt% Pd-doped SmFeO3 nanocomposites;(h) Specific surface area of ​​SmFeO3 with different Pd doping amounts;

[0027] Figure 3 : (a) Response of Pd-doped SmFeO3 to acetone gas at operating temperature; (bd) Response of Pd-doped SmFeO3 to acetone at operating temperature; (eg) Resistance curve of Pd-doped SmFeO3 to acetone at 220°C; (hj) Change of response recovery time of Pd-doped SmFeO3 to acetone with operating temperature.

[0028] Figure 4 :(ac) Linear relationship between the response of Pd-doped SmFeO3 and acetone concentration; (df) Comparison of the selectivity of Pd-doped SmFeO3 to acetone and other gases; (g) Resistance curve of Pd-doped SmFeO3 under RH; (h) Response curve of Pd-doped SmFeO3 to RH; (i) Long-term stability of the response of Pd-doped SmFeO3.

[0029] Figure 5 : (a) Response of Pd-doped SmFeO3 under illumination; (bd) Response of Pd-doped SmFeO3 under illumination with working temperature.

[0030] Figure 6: (ac) Response recovery time of 2wt% Pd-doped SmFeO3 to acetone under illumination and operating temperature; (df) Response of Pd-doped SmFeO3 under RH illumination; (g) Resistance curve of Pd-doped SmFeO3 under RH illumination; (h) Response curve of Pd-doped SmFeO3 under RH light; (i) Long-term stability of the response of Pd-doped SmFeO3.

[0031] Figure 7 :(ab) Changes in the electronic structure of Pd-doped SmFeO3; (c) Resistance comparison of SmFeO3 and 2wt% Pd-doped SmFeO3; (d) Resistance curve of 2wt% Pd-doped SmFeO3 during the entire process under additional illumination; (e) UV-visible diffuse reflectance spectrum and energy band gap of 2wt% Pd-SmFeO3 (inset).

[0032] Figure 8 :(a) Schematic diagram of the exhaled breath measurement device; (b) Response of Pd-doped SmFeO3 to 40000 ppm CO2 under light; (c) Acetone concentration in the exhaled breath of volunteers.

[0033] Fig. 9 : Response of the sensor prepared in Comparative Example 1 to different concentrations of acetone.

[0034] Fig.10 : Dynamic curve of resistance of the sensor prepared in Comparative Example 1 to different concentrations of acetone at 220°C;

[0035] Fig.11 : The response recovery time of the sensor prepared in Comparative Example 1 to 1 ppm acetone varies with the operating temperature;

[0036] Fig.12 : The acetone concentration is linearly related to the response of the sensor prepared in Comparative Example 1;

[0037] Fig.13 : Comparison of the selectivity of the sensor prepared in Comparative Example 1 to 1 ppm acetone and several other common gases in human exhaled gas;

[0038] Fig.14 : Resistance curve of the sensor prepared in Comparative Example 1 under relative humidity;

[0039] Fig.15 : Response curve of the sensor prepared in Comparative Example 1 to RH;

[0040] Fig.16 : Long-term stability response of the sensor prepared in Comparative Example 1. DETAILED DESCRIPTION

[0041] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0042] As introduced in the background technology section, the SmFeO3-based sensor needs to operate at a higher operating temperature, which increases energy consumption and safety risks. When the gas concentration is ppb, the response is low and cannot meet the requirements of pre-diagnosis of diabetes using exhaled breath.

[0043] Based on this, the object of the present invention is to provide a Pb-doped SmFeO3 gas-sensitive material having a hollow tubular structure and its application. Figure 1 As shown, the present invention first mixes Fe(NO3)3, Sm2O3, PdCl2, DMF, PVP, anhydrous ethanol and nitric acid with deionized water, heats and stirs until transparent to obtain a precursor solution; the precursor solution is electrospun to obtain nanofibers, and the nanofibers are sintered to obtain a powdered Pb-doped SmFeO3 gas-sensitive material. Finally, the Pb-doped SmFeO3 nanopowder is added to deionized water to prepare a paste slurry, the slurry is placed on a gas-sensitive film, and the Pb-doped SmFeO3 gas-sensitive sensor is obtained after drying. The Pb-doped SmFeO3 nanopowder prepared by the present invention is a hollow tubular microstructure, which has a large specific surface area and high porosity, and can increase the adsorption sites and percolation channels of gas molecules. Compared with SmFeO3, the response of Pd-doped SmFeO3 is significantly improved, and further improved under light. The RH adaptability, selectivity and long-term stability of Pd-doped SmFeO3 are also greatly improved.

[0044] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.

[0045] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.

[0046] The gas-sensitive response S is defined as Rg / Ra. Ra is the resistance of the sensor in air, and Rg is the resistance of the sensor in the target gas. The response time is defined as the time required to reach 90% of the maximum response value in the rising phase, and the recovery time is defined as the time required to recover 10% of the initial response value in the falling phase.

[0047] Example

[0048] Fe(NO3)3, Sm2O3, PdCl2, DMF (99.5%), PVP (Mw = 1300000), anhydrous ethanol (99.7%), HNO3 and deionized water were weighed and mixed in a mass ratio of 242:174.4:177.4:100:100:50:50:200 ( Figure 1 a). The mixed solution was heated in a water bath at 60°C with magnetic stirring until transparent to obtain an electrospinning precursor solution ( Figure 1 b). Then the prepared precursor solution was transferred into a 10 ml syringe. During the spinning process, the voltage was maintained at 12 kV, the distance between the needle tip and the collector was about 20 cm, the injection rate was 0.4 mL / h, and the obtained nanofibers were sintered at 800 ° C in a muffle furnace for 6 hours. Finally, 2 wt% Pd-doped SmFeO3 powder was obtained.

[0049] Take a small amount of Pd-SmFeO3 powder and put it into a glass container, then add enough water to make a paste ( Figure 1 d). Place the slurry on the gas sensitive film ( Figure 1 e) The prepared planar electrode plate was aged on an aging platform for 48 hours to dry it, thereby obtaining a sensor.

[0050] Comparative Example 1

[0051] The difference from the embodiment is that PdCl2 is not added, and 0wt% Pd-doped SmFeO3 powder is prepared.

[0052] Comparative Example 2

[0053] The difference from the embodiment is that the amount of PdCl2 added is adjusted to prepare 1wt% Pd-doped SmFeO3 powder.

[0054] Comparative Example 3

[0055] The difference from the embodiment is that the amount of PdCl2 added is adjusted to prepare 3wt% Pd-doped SmFeO3 powder.

[0056] Performance characterization:

[0057] The X-ray diffraction analysis of SmFeO3 doped with Pd at different doping amounts prepared in Example 1 to Comparative Examples 1 to 3 is as follows: Figure 2 As shown in a. Compared with the standard card (PDF card: 39-1490), it shows a single phase. The average particle size can be calculated using the Scherrer method. The Scherrer equation is as follows:

[0058]

[0059] Where λ is the wavelength of the x-ray, β is the integral width of the diffraction peak, and θ is the Bragg diffraction angle. The average particle sizes of Pd-doped SmFeO3 are 76.3nm (Comparative Example 1), 73.8nm (Comparative Example 2), 64.1nm (Example), and 61.9nm (Comparative Example 3). This shows that the Pd element can inhibit the growth of MOSs grains. Due to the low doping amount of the Pd element, the characteristic peak cannot be reflected in the XRD spectrum, so the EDS (energy dispersive spectroscopy) spectrum of 2wt% Pd-SmFeO3 was performed to confirm the presence of the Pd element. From Figure 2 b It can be seen that Pd element is doped in the material.

[0060] Figure 2 cd is a scanning electron microscope image of 2wt% Pd-SmFeO3 at different magnifications. It can be seen that the material presents a nanotube-like microstructure. During the material preparation stage, after sintering, as PVP decomposes at high temperatures, the material surface becomes rough and the nanotubes become hollow. The TEM image of 2wt% Pd-SmFeO3 is shown in Figure 2 As shown in Figure ef: the interplanar spacings are 0.195nm and 0.349nm, respectively, pointing to the (221) and (111) planes of the SmFeO3 hexagonal lattice.

[0061] Example The specific surface area and porosity of the prepared 2 wt % Pd-SmFeO 3 hollow nanofibers were further analyzed by nitrogen adsorption-desorption measurements. Figure 2 g shows the BET curve of 2 wt% Pd-SmFeO3 prepared in Example 1 and the corresponding Barrett-Joyner-Halenda (BJH) pore size distribution (inset). The specific surface area of ​​2 wt% Pd-SmFeO3 is 28.68 m 2 / g, the average pore size is 11.8nm. The specific surface area of ​​SmFeO3 with different Pd doping amounts is as follows Figure 2 h. It can be seen that when the Pd element doping amount is 2wt%, the composite powder presents the largest specific surface area. Since the Pd element can inhibit the growth of MOSs grains, the smaller the grain size, the larger the specific surface area. However, when the doping amount is too high, the particles will agglomerate in a small range, and the specific surface area of ​​the material will decrease. Specific surface area is an important factor affecting the sensitivity of the material. A larger specific surface area can provide more adsorption sites, which can enhance the reaction between the sensing material and the gas molecules, resulting in a higher response to the target gas.

[0062] Test example:

[0063] 1. Gas sensing performance

[0064] For gas-sensitive materials, sensitivity to target gas has always been the most important characteristic. The response of SmFeO3 with different Pd doping amounts to 1ppm acetone is shown in Figure 2. Figure 3 As shown in a. For all samples, the highest response was obtained at 220°C. The highest responses to 1 ppm acetone were 3.36 (Comparative Example 1), 4.16 (Comparative Example 2), 10.73 (Example) and 7.38 (Comparative Example). Figure 3 bd and Fig. 9 The response of all samples to 0.01-1 ppm acetone at operating temperature is shown. It can also be seen that the optimum operating temperature is 220°C for any concentration of acetone.

[0065] For Pd-SmFeO3, the repeatability of the response to acetone gas at different concentrations is shown in Figure 3 For example, Fig.10 As shown in Figure 2, it can be seen that for different concentrations of acetone gas, the resistance of the gas-sensitive material can recover to the initial value each time the acetone gas is removed, indicating that the material has excellent repeatability. The response recovery time of all samples is shown in Figure 2. Figure 3 hj and Fig.11 It can be seen that before reaching 220°C, the response recovery time increases with the increase of operating temperature, and after 220°C, the response recovery time decreases with the further increase of operating temperature.

[0066] The relationship between the sensitivity of the material and the gas concentration is very important, and a highly fitted relationship can be used to predict the response value at a given gas concentration. It can be seen that the response value has a good linear relationship with the gas concentration, and all R 2 Value greater than 94% ( Figure 4 ac and Fig.12 ). Comparison of the selectivity of Pd-SmFeO3 to 1ppm acetone and several other common gases exhaled by humans. Figure 4 -f and Fig.13 As shown. It can be seen that Pd-SmFeO3 shows higher selectivity for acetone gas compared to other gases. In particular, for common gases in human exhaled breath such as N2, O2, NO, CO2, CO, the reaction can be ignored, so that acetone in human exhaled breath can be detected more accurately. For Pd-SmFeO3, the resistance decreases with RH, but the reduction ratio is different ( Figure 4 g and Fig.14 ). In the range of 20%-90% RH, the decrease ratios are: 78.5% (Comparative Example 1), 77.2% (Comparative Example 2), 57.1% (Example 1) and 69.2% (Comparative Example 3). This shows that the resistance of 2wt% Pd-SmFeO3 shows the highest RH adaptability. RH will also affect the response of gas-sensitive materials to target gases. Figure 4 h and Fig.15 The response of Pd-SmFeO3 to 1ppm acetone under RH conditions is shown. It can be seen that the response decreases with increasing RH. Before 50% RH, the response is little affected by it. But after 50% RH, the response drops sharply. This means that the gas sensor in this study can be used in a low RH environment without considering the influence of RH. This will greatly expand its practical application areas.

[0067] Long-term stability is another important characteristic of gas-sensitive materials. The higher the long-term stability, the longer the replacement cycle of the gas-sensitive material, and the greater the economic and energy advantages. Figure 4 i and Fig.16 The long-term stability of Pd-SmFeO3 for 30 days is shown. Experimental data are obtained every 2 days. It can be seen that all responses decrease slightly over time, but the proportion of decrease is different. The proportion of decrease is: 34.5% (Comparative Example 1), 25.9% (Comparative Example 2), 2.6% (Example) and 7.5% (Comparative Example 3). It can be seen that the long-term stability of 2wt% Pd-SmFeO3 is more than 13 times that of pure SmFeO3. SmFeO3 doped with Pd element shows higher advantages in long-term stability.

[0068] In order to lower the optimal working temperature of the gas-sensitive material and further improve the sensitivity of the gas-sensitive material, light is introduced to irradiate the gas-sensitive material during the experiment. Figure 5 a shows the response of Pd-SmFeO3 to 1PPM acetone under illumination of different wavelengths. The dotted line represents the response of the same material in the absence of illumination. In this study, a total of six different wavelengths of light (365, 410, 450, 535, 590 and 635nm) were used to irradiate Pd-SmFeO3. The response of all samples decreases with increasing illumination wavelength. When the illumination wavelength exceeds 535nm, the effect of light on the material response is very small and almost negligible. In addition, the effect of different wavelengths of light on the response of Pd-SmFO3 at any operating temperature is also studied. In addition, the present invention also studies the effect of different wavelengths of light on the response of Pd-SmFO3 at operating temperature. The optimal operating temperature of the sensor prepared in the embodiment is reduced to 120°C under illumination. Figure 5 bd shows the response of Pd-SmFO3 to 1 PPM acetone at the operating temperature. Illumination improves the response of all samples to acetone at any operating temperature, and short-wavelength illumination improves the response of Pd-SmFeO3 more.

[0069] Illumination not only enhances the material's response, but also reduces its response recovery time, improving RH adaptability and long-term stability. Figure 6Figures ac show the response recovery time of 2wt% Pd-SmFeO3 under different wavelengths of light as a function of operating temperature. Compared to the response recovery time of 2wt% Pd-SmFeO3 without light, the response recovery time is now significantly shorter. Most notably, under 356nm light, the response recovery time is shortened by nearly half. Under light, the RH adaptability of Pd-SmFeO3 is also improved, such as Figure 6 df. It can be seen that at 50% RH, the response drops sharply again. However, the percentage of the drop is significantly reduced, for example, from 57.2% to 19.24% (365nm, Example). In addition, illumination also greatly improves the long-term stability of Pd-SmFeO3, as shown in Figure 2. Figure 6 Although the reaction slowly decreased after 30 days, the percentage of decrease decreased significantly, from 2.6% to 2.23% (365 nm, Example).

[0070] 2. Analysis of sensing mechanism

[0071] Figure 7 The reaction mechanism of the whole experiment in this work is given. At room temperature (20℃), for p-type semiconductors, the main carriers of Pd-SmFeO3 are holes (h · )(like Figure 7 ). According to the Kroger-Vink defect notation, holes are mainly generated by the ionization of ions. The reaction might be something like this:

[0072]

[0073] Before Pd doping, few oxygen molecules capture free electrons from the material, resulting in the formation of oxygen ions on the surface of the material, and few holes are generated in the process. Since the work effect of Pd is greater than that of SmFeO3, after Pd doping, electrons will be transferred from SmFeO3 to the surrounding Pd nanoparticles, resulting in an increase in the number of holes in SmFeO3 ( Figure 7 b) The reaction may be:

[0074]

[0075]

[0076] To verify this theoretical hypothesis, the resistance of pure SmFeO3 and 2wt% Pd-SmFeO3 was tested ( Figure 7 c). It can be seen that the resistance of 2wt% Pd-SmFeO3 is lower than that of SmFeO3 at any operating temperature, which is consistent with the above theoretical assumption.

[0077] In addition, the resistance of the gas-sensitive material decreases when exposed to light ( Figure 7 d). By absorbing the energy of light, electron-hole pairs appear. More free electrons jump into the conduction band and leave a hole in the valence band. The free electrons combine with oxygen molecules on the surface of the material, resulting in more oxygen ions being adsorbed and more holes causing the resistance of the material to decrease. Figure 7 The energy band gap of 2wt% Pd-SmFeO3 was obtained in e, which is about 2.55eV. Therefore, Pd-SmFeO3 can absorb the energy of shorter wavelength light (λ<486nm), generate photogenerated holes, and enhance the sensitivity of the material. This can also explain why short-wavelength light affects the response of the material, while long-wavelength light does not. The reaction between oxygen molecules and free electrons on the surface of Pd-SmFeO3 may be like this:

[0078] Pd: SmFeO3+hv→e - +h + (6)

[0079] When acetone gas molecules are introduced, they will adsorb on the Pd-SmFeO3 surface and react with the adsorbed oxygen ions. The reaction between acetone molecules and oxygen ions may be like this:

[0080] CH3COCH3+8O - →3CO2+3H 2 O+8e - (7)

[0081] e - +h + →null (8)

[0082] Application example: Application in the detection of diabetic patients

[0083] Schematic diagram of acetone gas concentration detection in real person's exhaled breath Figure 8 As shown in a. It can be seen that the volunteers wear a breathing mask on their mouths, and a tube is connected to the inside of the operation box, and the exhaled gas is injected from the breathing mask. The RH of the exhaled gas is generally greater than 85%, but after the exhaled gas enters the glass reaction vessel through the tube, the overall RH in the glass reaction vessel is about 25% (the volume of the glass reaction vessel is about 28L).

[0084] Although the composition of the gas exhaled by each person varies greatly, the gas with the highest concentration is CO2, about 40,000 ppm. Figure 8 b shows the response of Pd-SmFeO3 to 40000 ppm CO2. Figure 8In b, AL refers to gas-sensitive materials with different Pd doping amounts and different illumination conditions. It can be seen that the response of all samples to CO2 is not negligible. Therefore, when detecting acetone concentration, the response to 40,000 ppm CO2 needs to be subtracted from the overall response to human exhaled breath. The response of all samples to acetone in the exhaled breath of four volunteers is shown in Figure 2. Figure 8 c, V1-V4 are the average values ​​of the four volunteers. The basic information of the volunteers is shown in Table 1.

[0085] Table 1 Basic information of volunteers

[0086]

[0087] It can be seen that Figure 8 F (Example, 365nm) in C has the highest response to the exhaled breath of the four volunteers. The acetone concentration obtained by the gas sensor of the present invention is higher than the acetone concentration measured by GC-MS, but the error is within 10%. This may be because the exhaled breath of a person contains some gas, which affects the response of the gas sensor, but the effect is small. When the acetone concentration in the exhaled gas of a person is greater than 0.9ppm, the person is identified as a diabetic patient, and when it is less than 0.9ppm, the person is identified as healthy. This result is consistent with the actual situation of the four volunteers, and also shows that the use of acetone gas sensors for pre-diagnosis of diabetes is feasible and effective.

[0088] In the present invention, Pd-modified SmFeO3 SmFeO3 was synthesized by electrospinning. It has a large specific surface area and high porosity, which improves the response of the gas-sensitive material to a certain extent. The optimal doping content of Pd is 2wt%, and the doping of Pd element as a catalyst greatly improves the gas sensitivity, RH adaptability, selectivity and long-term stability of SmFeO. In addition, when light is irradiated on Pd-SmFeO3, the shorter the wavelength of light, the greater the improvement of its response and the greater the decrease of its optimal operating temperature. When the wavelength of light increases to a certain extent, it has little effect on the response of Pd-SmFeO3. This is related to the band gap of Pd-SmFeO3. Moreover, the RH adaptability and long-term stability of the chemical properties of Pd-SmFeO3 are greatly improved under light. Finally, the Pd-SmFeO3 gas sensor was used to detect the acetone concentration in the exhaled gas of 4 volunteers, and compared with the GC-MS test results. The results show that the error is within 10%, which is acceptable. This study fully demonstrates that precious metal doping and light irradiation are two efficient ways to improve gas-sensitive response materials, and pre-diagnosis of diabetes through acetone gas sensors is feasible and effective.

[0089] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A Pd-doped SmFeO3 gas-sensitive material, characterized in that: The Pd-doped SmFeO3 gas-sensitive material is a nano powder with a hollow tubular structure; the doping amount of Pd in ​​the Pd-doped SmFeO3 gas-sensitive material is 2wt%; The preparation method of the Pd-doped SmFeO3 gas-sensitive material comprises the following steps: (1) adding Fe(NO3)3, Sm2O3, PdCl2, DMF, PVP, anhydrous ethanol and nitric acid into deionized water to obtain a mixed solution, heating and stirring the mixed solution until transparent to obtain a precursor solution; (2) The precursor solution obtained in step (1) is subjected to electrospinning to obtain nanofibers, and the nanofibers are sintered to obtain a powdered Pd-doped SmFeO3 gas-sensitive material.

2. The Pd-doped SmFeO3 gas-sensitive material according to claim 1, characterized in that: In step (1), the mass ratio of Fe(NO3)3, Sm2O3, PdCl2, DMF, PVP, anhydrous ethanol and nitric acid to deionized water is 242:174.4:177.4:100:100:50:50:

200.

3. The Pd-doped SmFeO3 gas-sensitive material according to claim 1, characterized in that: The weight average molecular weight of the PVP is 1,300,000; and the volume concentration of the nitric acid is 97%.

4. The Pd-doped SmFeO3 gas-sensitive material according to claim 1, characterized in that: In step (1), the heating is water bath heating at a temperature of 60° C.; and the stirring is magnetic stirring.

5. The Pd-doped SmFeO3 gas-sensitive material according to claim 1, characterized in that: In step (2), during the electrospinning process, the voltage was maintained at 12 kV, the distance between the needle tip of the syringe used for electrospinning and the collector was 20 cm, and the injection rate was 0.4 mL / h.

6. The Pd-doped SmFeO3 gas-sensitive material according to claim 1, characterized in that: In step (2), the sintering temperature is 800° C. and the sintering time is 6 hours.

7. Use of the Pd-doped SmFeO3 gas-sensitive material according to any one of claims 1 to 6 in the preparation of a gas sensor.