Laminated body and method for producing the same
By adjusting the storage modulus of the hydrogenated block copolymer adhesive layer, the problem of insufficient adhesion between styrene-based thermoplastic elastomers and ceramics or metals was solved, achieving a strong bond effect without the need for primer treatment.
Patent Information
- Application Number
- CN202180017336.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-27
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-02-25
AI Technical Summary
In the prior art, styrene-based thermoplastic elastomers have insufficient adhesion to ceramics or metals, and require additional application of adhesives or primers, resulting in a complicated process and insufficient adhesion.
By using an adhesive layer containing hydrogenated block copolymers, and adjusting the storage modulus at 100°C to the range of 1.20×10⁵ to 4.00×10⁵ Pa, a strong bond between substrates can be achieved, eliminating the need for primer treatment.
Even without primer treatment, it can achieve a strong bond between metal and resin substrates, improving adhesion and molding processability.
Smart Images

Figure CN115135497B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminate having an adhesive layer containing a hydrogenated block copolymer obtained by hydrogenating a block copolymer containing a polymer block composed of a structural unit derived from an aromatic vinyl compound and a polymer block composed of a structural unit derived from a conjugated diene, and a method for producing the same. Background Art
[0002] Ceramics, metals, and synthetic resins are used in various applications such as home appliances, electronic components, machine components, and automobile components due to their excellent durability, heat resistance, and mechanical strength. These components are sometimes used as a laminated body laminated with an elastomer having excellent flexibility for purposes such as fixing to other structural components, shock absorption, damage prevention, and sealing, depending on the application, component composition, and usage method.
[0003] As such an elastomer, a styrene-based thermoplastic elastomer having excellent flexibility, mechanical properties and molding processability can be suitably used. Here, the styrene-based thermoplastic elastomer refers to a block copolymer having a polymer block formed by a structural unit derived from an aromatic vinyl compound and a polymer block formed by a structural unit derived from a conjugated diene, or a hydrogenated product thereof.
[0004] However, conventional styrene-based thermoplastic elastomers have problems such as insufficient adhesive strength to ceramics, metals, etc., and difficulty in melt bonding when used directly. Therefore, in order to bond ceramics or metals to styrene-based thermoplastic elastomers, methods of applying an adhesive separately or performing primer treatment on the surface of ceramics, metals, or synthetic resins are disclosed (see Patent Documents 1 to 6).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2006-291019
[0008] Patent Document 2: Japanese Patent Application Publication No. 2006-206715
[0009] Patent Document 3: Japanese Patent Application Publication No. 63-25005
[0010] Patent Document 4: Japanese Patent Application Laid-Open No. 9-156035
[0011] Patent Document 5: Japanese Patent Application Publication No. 2009-227844
[0012] Patent document 6: Japanese Patent Application Publication No. 2010-1364. Summary of the invention
[0013] Problems to be solved by the invention
[0014] As described above, the methods described in Patent Documents 1 to 6 require additional application of an adhesive or primer treatment, which is complicated and also results in insufficient adhesive strength, and thus improvement is desired.
[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminate in which substrates formed of metal and resin or the like can be firmly bonded to each other even without primer treatment or the like, and a method for producing the laminate.
[0016] Solutions to Solve Problems
[0017] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by adjusting the storage modulus at 100° C. measured by dynamic viscoelasticity measurement of an adhesive layer containing a hydrogenated block copolymer to a specific range, thereby completing the present invention.
[0018] That is, the present invention is an invention based on the following [1] to
[19] as its main purpose.
[0019] [1] A laminate comprising, in this order, a substrate (X), an adhesive layer (Y), and a substrate (Z), characterized in that:
[0020] The adhesive layer (Y) comprises a hydrogenated block copolymer (A) obtained by hydrogenating a block copolymer (P), wherein the block copolymer (P) comprises a polymer block (a) composed of a structural unit derived from an aromatic vinyl compound and a polymer block (b) composed of a structural unit derived from a conjugated diene.
[0021] The mass ratio of the polymer block (a) to the polymer block (b) [(a) / (b)] is 1 / 99 to 50 / 50,
[0022] The storage modulus G' of the adhesive layer (Y) at 100°C is 1.20×10 5 ~4.00×10 5 Pa.
[0023] [2] The laminate according to [1], wherein the loss modulus G" of the adhesive layer (Y) at 100°C is 3.00×10 4 ~2.50×10 5 Pa.
[0024] [3] The laminate according to [1] or [2], wherein the adhesive layer (Y) is formed from a thermoplastic elastomer composition containing a hydrogenated block copolymer (A).
[0025] [4] The laminate according to any one of [1] to [3], wherein the polymer block (b) contains 1 to 100% by mass of a structural unit (b1) derived from farnesene and contains 0 to 99% by mass of a structural unit (b2) derived from a conjugated diene other than farnesene.
[0026] [5] The laminate according to [4], wherein the conjugated diene other than farnesene is at least one selected from butadiene, isoprene, and myrcene.
[0027] [6] The laminate according to any one of [1] to [5], wherein the hydrogenation rate of carbon-carbon double bonds in the polymer block (b) is 70 mol % or more.
[0028] [7] The laminate according to any one of [1] to [6], wherein the peak molecular weight (Mp) of the hydrogenated block copolymer (A) is 4,000 to 1,500,000.
[0029] [8] The laminate according to any one of [1] to [7], wherein the molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer (A) is 1.00 to 4.00.
[0030] [9] The laminate according to any one of [1] to [8], wherein the aromatic vinyl compound is styrene.
[0031]
[10] The laminate according to [9], wherein the peak molecular weight of the polymer block (a) formed from the structural unit derived from styrene is 2,000 to 55,000.
[0032]
[11] The laminate according to any one of [1] to
[10] , wherein the substrate (X) and the substrate (Z) are each independently at least one selected from metal, polar resin, polyolefin resin, carbon fiber, glass, and ceramic.
[0033]
[12] The laminate according to any one of [1] to
[11] , wherein the adhesive layer (Y) satisfies the following relational expression (i):
[0034] [(0℃ hardness / 23℃ hardness)×100≤140] (i)
[0035]
[13] The laminate according to any one of [1] to
[12] , wherein the hydrogenated block copolymer (A) is a mixture of two or more hydrogenated block copolymers, and the content of the diblock copolymer in the hydrogenated block copolymer (A) is 50% by mass or less.
[0036]
[14] The laminate according to any one of [1] to
[13] , wherein when a stainless steel plate is used as the substrate (X) and a polyacetal resin is used as the substrate (Z), the shear adhesion of the adhesive layer (Y) at 23°C is 10 N / cm 2 above.
[0037]
[15] The laminate according to any one of [1] to
[14] , wherein the arithmetic mean roughness (Ra) of the substrate (X) and the substrate (Z) is 0.010 to 10 μm.
[0038]
[16] A method for manufacturing a laminate, which is the method for manufacturing a laminate as described in any one of [1] to
[15] , characterized in that it comprises: a step (Ia) of press-molding the adhesive layer (Y) on the substrate (X), and a step (II) of injection-molding the substrate (Z) on the adhesive layer (Y) after the step (Ia).
[0039]
[17] A method for producing a laminated body according to any one of [1] to
[15] , characterized in that it comprises: a step (Ib) of applying a solution and / or aqueous emulsion containing the hydrogenated block copolymer (A) onto the substrate (X) and then drying the solution and / or aqueous emulsion to form the adhesive layer (Y); and a step (II) of injection molding the substrate (Z) onto the adhesive layer (Y) after the step (Ib).
[0040]
[18] A method for manufacturing a laminate, which is the method for manufacturing a laminate as described in any one of [1] to
[15] , characterized in that it comprises: a step (Ic) of press-molding the adhesive layer (Y) on the substrate (X), and a step (II-c) of press-molding the substrate (Z) on the adhesive layer (Y) after the step (Ic).
[0041]
[19] The method for producing a laminate according to any one of
[16] to
[18] , wherein the substrate (X) is a metal and the substrate (Z) is a polar resin or a polyolefin resin.
[0042] Effects of the Invention
[0043] According to the present invention, a laminated body capable of firmly bonding substrates formed of metal and resin or the like even without primer treatment or the like, and a method for producing the laminated body can be provided.
[0044] Brief description of the attached figure
[0045] Figure 1 This is a cross-sectional view of a laminate (test piece) used for measuring the adhesive strength of Examples.
[0046] Figure 2 This is a diagram of a test piece used for measuring the adhesive strength in Examples, observed from the substrate (Z) side. DETAILED DESCRIPTION
[0047] [1] Laminated body
[0048] The laminate of the present invention comprises a substrate (X), an adhesive layer (Y) and a substrate (Z) in this order, wherein the adhesive layer (Y) comprises a hydrogenated block copolymer (A) obtained by hydrogenating a block copolymer (P), wherein the block copolymer (P) comprises a polymer block (a) formed of a structural unit derived from an aromatic vinyl compound and a polymer block (b) formed of a structural unit derived from a conjugated diene, wherein the mass ratio of the polymer block (a) to the polymer block (b) [(a) / (b)] is 1 / 99 to 50 / 50, and the storage modulus G' of the adhesive layer (Y) at 100°C is 1.20×10 5 ~4.00×10 5 Pa.
[0049] Hereinafter, the configuration of the present invention will be described in detail.
[0050] [Adhesive layer (Y)]
[0051] The adhesive layer (Y) in the present invention is a layer comprising a hydrogenated block copolymer (A) described below, and its storage modulus G' at 100°C measured by dynamic viscoelasticity measurement is 1.20×10 5 ~4.00×10 5 Pa.
[0052] In the present invention, since the storage modulus G' at 100°C is 1.20×10 5 ~4.00×10 5 The layer of Pa is an adhesive layer, and therefore exhibits excellent adhesion even to substrates with low polarity such as acrylic resins that are difficult to bond with conventional methods. It should be noted that the reason why the excellent effect is achieved when the storage modulus at 100°C is within the above range is not determined, but it is believed that when the storage modulus at 100°C is within the range, which is close to the temperature when the laminate is manufactured by injection molding or press molding, the hydrogenated block copolymer and the substrate become compatible and closely attached, so the adhesion between the adhesive layer (Y) and the substrate is improved.
[0053] From the viewpoint of further improving the adhesiveness of the adhesive layer (Y), the storage modulus G' at 100°C is preferably 3.50×10 5 Pa or less, more preferably 3.00×10 5Pa or less, more preferably 2.80×10 5 Pa or less. In addition, the storage modulus G' is preferably 1.30×10 5 Pa or more, more preferably 1.50×10 5 Pa or more, more preferably 1.70×10 5 Pa or above.
[0054] In addition, in this invention, the storage modulus G' at 100 degreeC means the value measured by the method described in an Example.
[0055] In addition, the storage modulus G' of the adhesive layer (Y) at 0°C measured by dynamic viscoelasticity measurement is preferably 4.00×10 5 ~5.00×10 8 When the storage modulus G' at 0°C is less than the upper limit, the laminate of the present invention exhibits strong adhesion even when exposed to an atmosphere at 0°C. From this viewpoint, the storage modulus G' at 0°C is preferably 5.00×10 7 Pa or less, more preferably 5.00×10 6 Pa or less, more preferably 8.00×10 5 In addition, from the viewpoint of adhesiveness in an atmosphere at 0°C, the storage elastic modulus G' of the adhesive layer (Y) at 0°C is preferably 4.00×10 5 Pa or above.
[0056] In addition, in this invention, the storage modulus G' at 0 degreeC means the value measured by the method described in an Example.
[0057] In addition, from the viewpoint of further improving the adhesiveness of the adhesive layer (Y), the loss modulus G" of the hydrogenated block copolymer (A) described below at 100°C measured by dynamic viscoelasticity measurement is preferably 3.00×10 4 Pa~2.50×10 5 Pa. The loss modulus G" at 100°C is preferably 3.50×10 4 Pa or more, more preferably 4.00×10 4 Pa or more, more preferably 4.50×10 4 Pa or more. In addition, the loss modulus G" at 100°C is preferably 2.00×10 5 Pa or less, more preferably 1.50×10 5 Pa or less, more preferably 1.00×10 5 Below Pa.
[0058] In addition, in the present invention, the loss modulus G" at 100°C refers to a value measured by the method described in the Examples.
[0059] The shear adhesive strength of the adhesive layer (Y) at 23°C is preferably 10 N / cm 2 More preferably 15N / cm 2 More preferably, 20 N / cm 2 .
[0060] The shear bond strength of the adhesive layer (Y) at 23°C refers to the shear bond strength of the adhesive layer (Y) when a stainless steel plate is used as the substrate (X) and a polyacetal resin is used as the substrate (Z), and can be specifically measured by the measurement method described in the Examples.
[0061] From the viewpoint of use in a wide temperature range, the adhesive layer (Y) preferably has a lower hardness increase in a low temperature atmosphere than in a high temperature atmosphere. When the hardness increase is large in a low temperature atmosphere, the rubber elasticity decreases, and it becomes easy to peel off when impacted. From the above viewpoints, as one of the preferred embodiments of the resin composition of this embodiment, s in the following relational formula (i) is preferably 140 or less, more preferably 130 or less, further preferably 120 or less, and particularly preferably 115 or less.
[0062] [(0℃ hardness / 23℃ hardness)×100≤s] (i)
[0063] In the above relational expression (i), “23° C. hardness” indicates hardness measured at an ambient temperature of 23° C. by the type A durometer method of JIS K 6253-2:2012.
[0064] In addition, "0°C hardness" means the hardness measured at an ambient temperature of 0°C by the type A durometer method of JIS K 6253-2:2012.
[0065] The thickness of the adhesive layer (Y) is not particularly limited, but is preferably 0.001 to 10.00 mm, more preferably 0.005 to 5.00 mm, further preferably 0.01 to 2.50 mm, particularly preferably 0.01 to 1.50 mm, and most preferably 0.01 to 1.00 mm, from the viewpoint of reducing the weight of the laminate and improving the degree of freedom in design.
[0066] <Hydrogenated block copolymer (A)>
[0067] The adhesive layer (Y) is a layer containing the hydrogenated block copolymer (A). When the adhesive layer (Y) contains the hydrogenated block copolymer (A), the substrate (X) and the substrate (Z) can be firmly bonded due to the flexibility of the hydrogenated block copolymer (A).
[0068] The hydrogenated block copolymer (A) includes a polymer block (a) composed of a structural unit derived from an aromatic vinyl compound and a polymer block (b) composed of a structural unit derived from a conjugated diene.
[0069] Examples of the aromatic vinyl compound constituting the polymer block (a) include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-tert-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, and divinylbenzene. These aromatic vinyl compounds may be used alone or in combination of two or more.
[0070] Among them, styrene, α-methylstyrene, and 4-methylstyrene are more preferred, and styrene is further preferred.
[0071] When the polymer block (a) is composed of structural units derived from styrene, its peak molecular weight (Mp) is preferably 2000 to 55000, more preferably 4000 to 20000, and even more preferably 5000 to 10000 from the viewpoint of improving the adhesion and molding processability of the adhesive layer (Y). It should be noted that the peak molecular weight (Mp) in this specification refers to a value measured by the method described in the Examples described below.
[0072] It should be noted that all “peak molecular weights” described in the present specification and claims are peak molecular weights calculated in terms of standard polystyrene obtained by gel permeation chromatography (GPC), and more specifically, are values measured by the method described in the Examples.
[0073] The peak molecular weight of each polymer block possessed by the block copolymer (P) can be obtained by measuring the liquid sampled at the end of each polymerization of each polymer block in the manufacturing process. For example, when a triblock copolymer having an a1-b-a2 structure is synthesized by sequentially polymerizing a1, b, and a2, the peak molecular weight of the initial polymer block a1 can be obtained by GPC determination of the liquid sampled at the end of the polymerization of a1. In addition, the peak molecular weight of polymer block b can be obtained as follows: the peak molecular weight of the diblock copolymer having the structure of a1-b is obtained by GPC determination of the liquid sampled at the end of the polymerization of b, and the peak molecular weight of the polymer block a1 is obtained by subtracting the peak molecular weight of the polymer block a1 from the value thereof. Furthermore, the peak molecular weight of polymer block a2 can be obtained as follows: the peak molecular weight of the triblock copolymer having the structure of a1-b-a2 is obtained by GPC determination of the liquid sampled at the end of the polymerization of a2, and the peak molecular weight of the diblock copolymer having the structure of a1-b is obtained by subtracting the peak molecular weight of the diblock copolymer having the structure of a1-b from the value thereof.
[0074] Examples of the conjugated diene constituting the polymer block (b) include butadiene, isoprene, 2,3-dimethylbutadiene, 2-phenyl-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, myrcene, farnesene, and chloroprene, etc. These may be used alone or in combination of two or more.
[0075] Among them, butadiene, isoprene, myrcene, and farnesene are more preferred, and farnesene is even more preferred.
[0076] The farnesene used as the conjugated diene may be α-farnesene or β-farnesene represented by the following formula (I), and β-farnesene is preferably used from the viewpoint of the ease of production of the hydrogenated block copolymer. α-farnesene and β-farnesene may also be used in combination.
[0077] [Chemical formula 1]
[0078]
[0079] The polymer block (b) in the present invention may contain a structural unit (b1) derived from farnesene and a structural unit (b2) derived from a conjugated diene other than farnesene in combination from the viewpoint of improving the adhesiveness of the adhesive layer (Y).
[0080] The content of the farnesene-derived structural unit (b1) in the polymer block (b) is preferably 1 to 100 mass %, more preferably 30 to 95 mass %, further preferably 45 to 90 mass %, and further preferably 50 to 80 mass %.
[0081] On the other hand, the content of the structural unit (b2) derived from a conjugated diene other than farnesene in the polymer block (b) is preferably 0 to 99% by mass, more preferably 5 to 70% by mass, further preferably 10 to 55% by mass, and further preferably 20 to 50% by mass.
[0082] In addition, as a conjugated diene other than farnesene, at least one selected from butadiene, isoprene and myrcene is preferable.
[0083] The mass ratio of the aforementioned polymer block (a) to the aforementioned polymer block (b) [(a) / (b)] is 1 / 99 to 50 / 50. When the content of the polymer block (a) is less than the aforementioned lower limit, a hydrogenated block copolymer having excellent flexibility and molding processability and strong adhesion cannot be obtained. On the other hand, when the content of the polymer block (a) exceeds the aforementioned upper limit, the molding processability and adhesion are reduced. From this viewpoint, the mass ratio of the aforementioned polymer block (a) to the aforementioned polymer block (b) [(a) / (b)] is preferably 5 / 95 to 40 / 60, more preferably 8 / 92 to 30 / 70, and further preferably 10 / 90 to 25 / 75.
[0084] The hydrogenated block copolymer (A) is a hydrogenated product of a block copolymer (P) comprising at least one polymer block (a) and one polymer block (b), and preferably a hydrogenated product of a block copolymer (P) comprising two or more polymer blocks (a) and one or more polymer blocks (b).
[0085] The bonding mode of polymer block (a) and polymer block (b) is not particularly limited, and may be linear, branched, radial, or a combination of two or more thereof. Among them, it is preferred that each block is bonded in a linear chain. When polymer block (a) is represented by a and polymer block (b) is represented by b, (ab) is preferably used. l 、a-(ba) m or b-(ab) n It should be noted that the aforementioned l, m and n each independently represent an integer greater than 1.
[0086] As the aforementioned bonding form, copolymers represented by babab or aba are preferred from the viewpoints of flexibility, molding processability, and handling properties.
[0087] It should be noted that the hydrogenated block copolymer (A) may be composed of one hydrogenated block copolymer, or may be a mixture of two or more hydrogenated block copolymers, for example, a mixture of the above-mentioned triblock or higher block copolymer and the so-called diblock copolymer represented by (ab). However, from the viewpoint of improving the adhesion durability (heat resistance, etc.) of the adhesive layer (Y), the content of the diblock copolymer in the hydrogenated block copolymer (A) is preferably 50% by mass or less, more preferably 40% by mass or less, particularly preferably 30% by mass or less, and most preferably 20% by mass or less.
[0088] In addition, in the present invention, a polymer having a bonding structure represented by b1-a-b2-a-b1 obtained by coupling using a coupling agent after producing a polymer arm having a bonding structure represented by b1-a-b2-Li by anionic polymerization ("Li" represents an active end when BuLi is used for anionic polymerization) can also be used. In this case, the content of the block copolymer having a bonding structure represented by b1-a-b2 derived from the polymer arm remaining without coupling is preferably 50% by mass or less, more preferably 40% by mass or less, further preferably 30% by mass or less, and further preferably 20% by mass or less in the hydrogenated block copolymer (A) from the viewpoint of not reducing the adhesion durability (heat resistance, etc.).
[0089] In addition, when the block copolymer (P) has two or more polymer blocks (a) or two or more polymer blocks (b), each polymer block may be a polymer block formed by the same structural unit or a polymer block formed by different structural units. For example, in the two polymer blocks (a) in the triblock copolymer represented by [aba], the types of the aromatic vinyl compounds in each of them may be the same or different.
[0090] The peak molecular weight (Mp) of the hydrogenated block copolymer (A) is preferably 4,000 to 1,500,000, more preferably 10,000 to 1,200,000, further preferably 50,000 to 800,000, and further preferably 80,000 to 500,000, from the viewpoint of improving the adhesiveness and molding processability of the adhesive layer (Y). It should be noted that the peak molecular weight (Mp) in this specification refers to a value measured by the method described in the Examples described below.
[0091] The molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer (A) is preferably 1.00 to 4.00, more preferably 1.00 to 3.00, and even more preferably 1.00 to 2.00. When the molecular weight distribution is within the above range, the hydrogenated block copolymer (A) has a small viscosity variation and is easy to handle.
[0092] The block copolymer (P) may contain a polymer block (c) composed of other monomers in addition to the polymer block (a) and the polymer block (b) as long as the effects of the present invention are not impaired.
[0093] As the other monomers, for example, unsaturated hydrocarbon compounds such as propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene; unsaturated compounds containing functional groups such as acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, acrylonitrile, methacrylonitrile, maleic acid, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid, 2-methacrylamide-2-methylpropanesulfonic acid, vinyl sulfonic acid, vinyl acetate, and methyl vinyl ether can be mentioned. These can be used alone or in combination of two or more.
[0094] When the block copolymer (P) has the polymer block (c), the content thereof is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less.
[0095] <Method for producing hydrogenated block copolymer (A)>
[0096] The hydrogenated block copolymer (A) can be preferably produced by, for example, a polymerization step of obtaining a block copolymer (P) by anionic polymerization and a step of hydrogenating the carbon-carbon double bonds in the polymer block (b) in the block copolymer (P).
[0097] 〔Polymerization process〕
[0098] The block copolymer (P) can be manufactured by a solution polymerization method or the method described in Japanese Patent Publication No. 2012-502135 and Japanese Patent Publication No. 2012-502136. Among them, the solution polymerization method is preferred, and for example, known methods such as anionic polymerization or cationic polymerization, free radical polymerization, etc. can be applied. Among them, the anionic polymerization method is preferred. As the anionic polymerization method, an aromatic vinyl compound, farnesene and / or a conjugated diene other than farnesene are successively added in the presence of a solvent, an anionic polymerization initiator, and a Lewis base as required to obtain a block copolymer (P).
[0099] Examples of anionic polymerization initiators include alkali metals such as lithium, sodium, and potassium; alkaline earth metals such as beryllium, magnesium, calcium, strontium, and barium; lanthanide rare earth metals such as lanthanum and neodymium; and compounds containing the above alkali metals, alkaline earth metals, and lanthanide rare earth metals. Among them, alkali metals and compounds containing alkali metals are preferred, and organic alkali metal compounds are more preferred.
[0100] Examples of the organic alkali metal compound include organic lithium compounds such as methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexyl lithium, phenyl lithium, distyrene lithium, dilithium methane, dilithium naphthalene, 1,4-dilithium butane, 1,4-dilithium-2-ethylcyclohexane, 1,3,5-trilithium benzene, and the like; sodium naphthyl, potassium naphthyl, and the like. Among them, organic lithium compounds are preferred, and n-butyl lithium and sec-butyl lithium are more preferred, and sec-butyl lithium is particularly preferred. It should be noted that the organic alkali metal compound can be reacted with a secondary amine such as diisopropylamine, dibutylamine, dihexylamine, and dibenzylamine to be used as an organic alkali metal amide.
[0101] The amount of the organic alkali metal compound used in the polymerization varies depending on the molecular weight of the block copolymer (P), but is generally in the range of 0.01 to 3% by mass based on the total amount of the aromatic vinyl compound, farnesene and conjugated diene other than farnesene.
[0102] As the solvent, there is no particular limitation as long as it has no adverse effect on the anionic polymerization reaction, and examples thereof include saturated aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, n-heptane, isooctane, etc.; saturated alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc., etc. These can be used alone or in combination of two or more. The amount of the solvent used is not particularly limited.
[0103] Lewis base has the function of controlling the microstructure in the structural unit derived from farnesene and the structural unit derived from conjugated diene other than farnesene. Examples of the Lewis base include ether compounds such as dibutyl ether, diethyl ether, tetrahydrofuran, dioxane, ethylene glycol diethyl ether, di(tetrahydrofuranyl)propane, pyridine, tertiary amines such as N,N,N',N'-tetramethylethylenediamine and trimethylamine, alkali metal alkoxides such as potassium tert-butoxide, phosphine compounds, etc. When a Lewis base is used, its amount is usually preferably in the range of 0.01 to 1000 molar equivalents relative to 1 mole of the anionic polymerization initiator.
[0104] The temperature of the polymerization reaction is usually -80 to 150°C, preferably 0 to 100°C, and more preferably in the range of 10 to 90°C. The polymerization reaction may be carried out in a batch or continuous manner. The block copolymer (P) can be produced by continuously or intermittently supplying monomers in a polymerization reaction solution in such a manner that the amount of the aromatic vinyl compound, farnesene and / or conjugated diene other than farnesene in the polymerization reaction system is within a specific range, or by sequentially polymerizing in such a manner that each monomer is in a specific ratio in the polymerization reaction solution.
[0105] The polymerization reaction can be terminated by adding an alcohol such as methanol or isopropanol as a polymerization terminator. The obtained polymerization reaction liquid can be injected into a poor solvent such as methanol to precipitate the block copolymer (P), or the polymerization reaction liquid can be washed with water, separated, and then dried to separate the block copolymer (P).
[0106] In this polymerization step, an unmodified block copolymer (P) can be obtained as described above, but before the hydrogenation step described below, a block copolymer (P) modified by introducing a functional group into the block copolymer (P) can also be obtained. Examples of the functional group that can be introduced include amino, alkoxysilyl, hydroxyl, epoxy, carboxyl, carbonyl, mercapto, isocyanate, chloro, and acid anhydride.
[0107] As a method for modifying the block copolymer (P), for example, before adding a polymerization terminator, a modifying agent such as tin tetrachloride, tetrachlorosilane, dichlorodimethylsilane, dimethyldiethoxysilane, tetramethoxysilane, tetraethoxysilane, 3-aminopropyltriethoxysilane, tetraglycidyl-1,3-bisaminomethylcyclohexane, 2,4-toluene diisocyanate, 4,4'-bis(diethylamino)benzophenone, N-vinylpyrrolidone, etc., which can react with the polymerization active terminal, or other modifying agents described in Japanese Patent Application Laid-Open No. 2011-132298 can be mentioned. In addition, maleic anhydride or the like can be grafted onto the separated copolymer for use.
[0108] The position where the functional group is introduced may be the polymerization end of the block copolymer (P) or the side chain. In addition, the functional group may be a single type or a combination of two or more types. The modifier is preferably used in an amount of 0.01 to 10 molar equivalents relative to the anionic polymerization initiator.
[0109] 〔Hydrogenation process〕
[0110] A hydrogenated block copolymer (A) can be obtained by imparting a process of hydrogenating the block copolymer (P) or the modified block copolymer (P) obtained by the above method. A known method can be used for the hydrogenation method. For example, a block copolymer (P) is dissolved in a solvent that has no effect on the hydrogenation reaction to form a solution, in which a Ziegler catalyst; a nickel, platinum, palladium, ruthenium or rhodium metal catalyst supported on carbon, silica, diatomaceous earth, etc.; an organic metal complex having cobalt, nickel, palladium, rhodium or ruthenium metal, etc. are present as a hydrogenation catalyst to carry out a hydrogenation reaction. In the hydrogenation step, a hydrogenation catalyst can be added to a polymerization reaction liquid containing a block copolymer (P) obtained by the method for producing the block copolymer (P) described above, and a hydrogenation reaction is carried out. In the present invention, it is preferred that palladium is supported on carbon as palladium carbon.
[0111] In the hydrogenation reaction, the hydrogen pressure is preferably 0.1 to 20 MPa, the reaction temperature is preferably 100 to 200° C., and the reaction time is preferably 1 to 20 hours.
[0112] The hydrogenation rate of the carbon-carbon double bonds in the polymer block (b) is preferably 70 to 100 mol%, more preferably 80 to 100 mol%, and further preferably 85 to 100 mol%, from the viewpoint of obtaining a thermoplastic elastomer composition having excellent flexibility and molding processability. 1 It was calculated by H-NMR.
[0113] <Thermoplastic elastomer composition constituting adhesive layer (Y)>
[0114] The adhesive layer (Y) of the present invention may be formed only of the hydrogenated block copolymer (A), but may also be formed of a thermoplastic elastomer composition comprising the hydrogenated block copolymer (A) and other components such as the polar group-containing polymer (B).
[0115] [Polar group-containing polymer (B)]
[0116] The thermoplastic elastomer composition may contain a polymer (B) containing a polar group. By containing a polymer containing a polar group, the adhesive layer (Y) has both appropriate flexibility and moldability, and forms strong adhesion with ceramics, metals, resins, concrete, asphalt, etc. even without primer treatment.
[0117] The reason why the adhesive force is improved by using the polar group-containing polymer (B) is considered to be because: when the thermoplastic elastomer composition contains the polar group-containing polymer (B), the thermoplastic elastomer composition becomes compatible with a substrate such as ceramics, metals, and resins; and when the adherend has a polar group, a chemical bond is generated between the polar group contained in the polar group-containing polymer (B) and the polar group on the surface of the adherend.
[0118] As the olefin constituting the polymer (B) containing a polar group, an olefin having 2 to 10 carbon atoms is preferred, and an olefin having 2 to 8 carbon atoms is preferred. Examples of such olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 4-methyl-1-pentene, and cyclohexene. These olefins may be used alone or in combination of two or more thereof. Among them, ethylene and propylene are preferred, and propylene is more preferred.
[0119] In addition, examples of the polar group possessed by the polar group-containing polymer (B) include a (meth)acryloyloxy group, a hydroxyl group, an amide group, an amino group, a halogen atom such as a chlorine atom, a carboxyl group, an ester group, an acid anhydride group, etc. Among them, from the viewpoint of improving the adhesive force, a (meth)acryloyloxy group, a carboxyl group, an ester group, and an acid anhydride group are preferred, and a carboxyl group and an acid anhydride group are more preferred.
[0120] The method for producing the polar group-containing polymer (B) is not particularly limited, and the polymer can be obtained by random copolymerization, block copolymerization or graft copolymerization of an olefin and a comonomer containing a polar group by a known method. Among them, random copolymerization and graft copolymerization are preferred, and graft copolymerization is more preferred. In addition, the polymer can also be obtained by oxidation or chlorination of a polyolefin resin by a known method. In addition, the polymer can be produced by modifying a commercially available polyolefin by reacting a compound containing a polar group with the polyolefin.
[0121] As copolymerizable monomers containing polar groups, for example, vinyl acetate, vinyl chloride, ethylene oxide, propylene oxide, acrylamide, unsaturated carboxylic acid or its ester or anhydride can be mentioned. Among them, unsaturated carboxylic acid or its ester or anhydride is preferred. As unsaturated carboxylic acid or its ester or anhydride, for example, (meth) acrylic acid, (meth) acrylate, maleic acid, maleic anhydride, fumaric acid, itaconic acid, itaconic anhydride, humic acid, humic anhydride, etc. can be mentioned. Among them, maleic acid and maleic anhydride are more preferred. These copolymerizable monomers containing polar groups can be used alone or in combination of two or more.
[0122] Specific examples of the (meth)acrylates as the copolymerizable monomers containing polar groups include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, isohexyl acrylate, n-octyl acrylate, isooctyl acrylate, and 2-ethylhexyl acrylate; and alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, isohexyl methacrylate, n-octyl methacrylate, isooctyl methacrylate, and 2-ethylhexyl methacrylate. These (meth)acrylates may be used alone or in combination of two or more.
[0123] From the viewpoint of improving adhesiveness, the polar group-containing polymer (B) is preferably a polyolefin containing a carboxyl group or an acid anhydride group as a polar group, that is, a carboxylic acid-modified olefin polymer or a carboxylic acid anhydride-modified olefin polymer, and more preferably a maleic acid-modified olefin polymer or a maleic anhydride-modified olefin polymer.
[0124] The polar group of the polar group-containing polymer (B) may be post-treated after polymerization. For example, the (meth)acryloyloxy group and the carboxyl group may be neutralized with metal ions to form an ionomer, or may be esterified with methanol, ethanol, etc. In addition, vinyl acetate may be hydrolyzed.
[0125] The melt flow rate (MFR) of the polymer (B) containing a polar group at 230°C and a load of 2.16 kg (21 N) is preferably 0.1 to 300 g / 10 minutes, more preferably 0.1 to 100 g / 10 minutes, further preferably 0.1 to 80 g / 10 minutes, and further preferably 0.1 to 50 g / 10 minutes. If the MFR of the polymer (B) containing a polar group under the above conditions is 0.1 g / 10 minutes or more, good molding processability can be obtained. On the other hand, if the MFR is 300 g / 10 minutes or less, mechanical properties are easily expressed.
[0126] The melting point of the polar group-containing polymer (B) is preferably 100° C. or higher, more preferably 110 to 170° C., and even more preferably 120 to 145° C., from the viewpoint of heat resistance.
[0127] The amount of the structural unit containing a polar group in the polymer (B) containing a polar group is preferably 0.01 to 10% by mass in all the structural units. If it is 0.01% by mass or more, the adhesion to ceramics and the like is further improved. If the proportion of the structural unit containing a polar group is 10% by mass or less, the affinity with the hydrogenated block copolymer (A) is improved, the mechanical properties become good, and the resulting thermoplastic elastomer composition becomes a composition with excellent flexibility and molding processability. The above ratio is more preferably 0.01 to 7% by mass, and further preferably 0.01 to 5% by mass. A substance obtained by diluting a polyolefin resin containing a structural unit containing a polar group at a high concentration with a polyolefin resin having no structural unit containing a polar group can be used as the polymer (B) containing a polar group so as to optimize the proportion of the structural unit containing a polar group. The total content of the structural unit containing a polar group and the structural unit derived from an olefin relative to the structural unit of the polar group-containing polymer (B) is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and further preferably 100% by mass.
[0128] The content of the polymer (B) containing a polar group in the thermoplastic elastomer composition is preferably 5 to 100 parts by mass relative to 100 parts by mass of the hydrogenated block copolymer (A). If the polymer (B) containing a polar group is above the aforementioned lower limit, it can be firmly bonded to ceramics and the like. On the other hand, when the polymer (B) containing a polar group is below the aforementioned upper limit, sufficient adhesion can be obtained while flexibility and molding processability also become good. From this viewpoint, the content of the polymer (B) containing a polar group is preferably 10 to 90 parts by mass, and more preferably 15 to 80 parts by mass relative to 100 parts by mass of the hydrogenated block copolymer (A).
[0129] 〔Softener〕
[0130] The thermoplastic elastomer composition may further contain a softener as long as it does not hinder the effect of the present invention. As the softener, generally, a softener used for rubber or plastic can be used. Examples thereof include paraffin-based, cycloalkane-based, and aromatic-based process oils; phthalic acid derivatives such as dioctyl phthalate and dibutyl phthalate; white oil; mineral oil; liquid copolymers of ethylene and α-olefins; liquid paraffin; polybutene; low molecular weight polyisobutylene; liquid polybutadiene, liquid polyisoprene, liquid polyisoprene / butadiene copolymer, liquid styrene / butadiene copolymer, liquid styrene / isoprene copolymer, and liquid polydienes and their hydrogenates. Among them, from the viewpoint of compatibility with the hydrogenated block copolymer (A), preferred are paraffin-based process oils; liquid copolymers of ethylene and α-olefins; liquid paraffin; low molecular weight polyisobutylene and hydrogenates thereof, and more preferred are hydrogenates of paraffin-based process oils.
[0131] In addition, known softeners generally used with polyvinyl acetal resins, for example, organic acid ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters; phosphoric acid plasticizers such as organic phosphates and organic phosphites, etc., can also be used.
[0132] Examples of the monobasic organic acid esters include diol esters obtained by reacting a diol such as triethylene glycol, tetraethylene glycol, tripropylene glycol, and a monobasic organic acid such as butyric acid, isobutyric acid, hexanoic acid, 2-ethylbutyric acid, heptanoic acid, n-octanoic acid, 2-ethylhexanoic acid, nonanoic acid (n-nonanoic acid), and decanoic acid, represented by triethylene glycol-dihexanoic acid, triethylene glycol-di(2-ethylhexyl acid) ester.
[0133] Examples of the polybasic acid organic esters include esters of polybasic organic acids such as adipic acid, sebacic acid, and azelaic acid, represented by dibutyl sebacate, dioctyl azelate, and dibutyl carbitol adipate, and linear or branched alcohols.
[0134] Examples of the organic phosphate include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.
[0135] The softeners may be used alone or in combination of two or more.
[0136] When the thermoplastic elastomer composition contains a softener, the content thereof is preferably in the range of 0.1 to 100 parts by mass relative to 100 parts by mass of the hydrogenated block copolymer (A). When the softener is within this range, the flexibility and molding processability of the thermoplastic elastomer composition are further improved. From this viewpoint, the content of the softener is more preferably 1 to 90 parts by mass relative to 100 parts by mass of the hydrogenated block copolymer (A).
[0137] 〔Other optional ingredients〕
[0138] The adhesive layer (Y) may contain other thermoplastic polymers, inorganic fillers, tackifying resins, antioxidants, lubricants, light stabilizers, processing aids, colorants such as pigments or dyes, flame retardants, antistatic agents, matting agents, silicone oils, antiblocking agents, ultraviolet absorbers, release agents, foaming agents, antibacterial agents, mildew inhibitors, and fragrances as needed, within a range that does not hinder the effects of the present invention.
[0139] As the aforementioned other thermoplastic polymers, for example, olefin polymers without polar groups, styrene polymers, polyphenylene ether resins, polyethylene glycol, etc. can be cited. Among them, from the viewpoint of improving the molding processability of the adhesive layer (Y), olefin polymers without polar groups are preferred. As such olefin polymers without polar groups, for example, one or more of polyethylene, polypropylene, polybutene, block copolymers or random copolymers of propylene and other α-olefins such as ethylene or 1-butene can be used.
[0140] When other thermoplastic polymers are contained, the content thereof is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 10 parts by mass or less, based on 100 parts by mass of the hydrogenated block copolymer (A).
[0141] The aforementioned inorganic filler may be contained for the purpose of improving the physical properties of the adhesive layer (Y), such as heat resistance and weather resistance, adjusting the hardness, improving the economic efficiency as an extender, etc. Examples of the inorganic filler include calcium carbonate, talc, magnesium hydroxide, aluminum hydroxide, mica, clay, natural silicate, synthetic silicate, titanium oxide, carbon black, barium sulfate, glass hollow spheres, glass fibers, etc. The inorganic filler may be used alone or in combination of two or more.
[0142] When an inorganic filler is contained, the content thereof is preferably within a range that does not impair the flexibility of the thermoplastic elastomer composition, and is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, further preferably 30 parts by mass or less, and particularly preferably 10 parts by mass or less, based on 100 parts by mass of the hydrogenated block copolymer (A).
[0143] Examples of the tackifier resin include rosin resins, terpene phenolic resins, terpene resins, aromatic hydrocarbon-modified terpene resins, aliphatic petroleum resins, alicyclic petroleum resins, aromatic petroleum resins, coumarone-indene resins, phenolic resins, and xylene resins.
[0144] When the tackifier resin is contained, the content thereof is preferably in a range that does not impair the mechanical properties of the thermoplastic elastomer composition, and is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 30 parts by mass or less, based on 100 parts by mass of the hydrogenated block copolymer (A).
[0145] Examples of the antioxidant include hindered phenol-based, phosphorus-based, lactone-based, and hydroxy-based antioxidants. Among them, hindered phenol-based antioxidants are preferred. When an antioxidant is contained, its content is preferably within a range that does not color the obtained thermoplastic elastomer composition when melt-kneaded, and is preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the hydrogenated block copolymer (A).
[0146] The method for producing the thermoplastic elastomer composition used in the adhesive layer (Y) is not particularly limited, and any method can be used as long as the hydrogenated block copolymer (A), the polar group-containing polymer (B) used as required, and other components can be uniformly mixed. When melt kneading is performed, a melt kneading device such as a single-screw extruder, a twin-screw extruder, a kneader, a batch mixer, a drum, a Banbury mixer, etc. can be used, and the thermoplastic elastomer composition can be obtained by melt kneading preferably at 170 to 270°C.
[0147] [Base material (X) and base material (Z)]
[0148] The laminate of the present invention comprises a substrate (X) and a substrate (Z).
[0149] Examples of the substrate (X) and the substrate (Z) include at least one material independently selected from metals, polar resins, polyolefin resins, carbon fibers, artificial leather, glass, and ceramics. The two substrates may be made of the same material.
[0150] Examples of metals that can be used for the substrate (X) and the substrate (Z) include iron, copper, aluminum, magnesium, nickel, chromium, zinc, and alloys containing these materials such as stainless steel. In addition, the substrate may have a metal surface formed by plating such as copper plating, nickel plating, chromium plating, tin plating, zinc plating, platinum plating, gold plating, or silver plating.
[0151] In addition, as polar resins that can be used for substrate (X) and substrate (Z), for example, polyamide resin, polyester resin, polycarbonate resin, polyphenylene sulfide resin, (meth) acrylonitrile-butadiene-styrene resin (ABS), (meth) acrylonitrile-styrene resin, (meth) acrylate-butadiene-styrene resin, (meth) acrylate-styrene resin, butadiene-styrene resin, epoxy resin, phenolic resin, diallyl phthalate resin, polyimide resin, melamine resin, polyacetal resin (POM), polysulfone resin, polyethersulfone resin, polyetherimide resin, polyphenylene ether resin, polyacrylate resin, polyetheretherketone resin, polystyrene resin, syndiotactic polystyrene resin, polyurethane (thermoplastic, thermosetting), etc. can be cited. These resins can be used alone or in combination of two or more. It should be noted that these resins can be reinforced with glass fiber or carbon fiber. As the above-mentioned polyamide resin, polyamide 6 (PA6), polyamide 66 (PA66), etc. are preferred. In addition, as the polyester resin, polylactic acid (PLA), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc. are preferable.
[0152] Further, polyolefin resins that can be used for the substrate (X) and the substrate (Z) include, for example, polyethylene, polypropylene, polybutene-1, polyhexene-1, poly-3-methyl-butene-1, poly-4-methyl-pentene-1, copolymers of one or more of ethylene and α-olefins having 3 to 20 carbon atoms (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 3-methyl-1-butene, 4-methyl-1-pentene, 6-methyl-1-heptene, isooctene, isooctadiene, decadiene, etc.), ethylene / propylene / diene copolymers (EPDM), ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, etc., and cycloolefin (co)polymers such as ethylene-norbornene copolymers are also preferred. It should be noted that these resins may be reinforced with glass fibers or carbon fibers.
[0153] The ceramics that can be used for the substrate (X) and the substrate (Z) are not particularly limited as long as they are non-metallic inorganic materials, and examples thereof include metal oxides, metal carbides, metal nitrides, etc. Specifically, examples thereof include glass, cement, aluminum oxide, zirconium oxide, zinc oxide-based ceramics, barium titanate, lead zirconate titanate, silicon carbide, silicon nitride, ferrites, etc.
[0154] As the substrate (X) and the substrate (Z), from the viewpoint of adhesion with the above-mentioned adhesive layer (Y), metals such as copper, aluminum, and stainless steel, polar resins such as polyacetal resin (POM) and polyamide 6 (PA6), polyester resins such as polybutylene terephthalate, polycarbonate resins, (meth)acrylonitrile-styrene resin (AS), (meth)acrylonitrile-butadiene-styrene resin (ABS), and polyolefin resins such as polyethylene and polypropylene are preferred.
[0155] It should be noted that the laminate of the present invention may have a substrate other than the substrate (X) and the substrate (Z), or an adhesive layer (Y), but is preferably a laminate in which only the substrate (X), the adhesive layer (Y) and the substrate (Z) are laminated.
[0156] The thickness of the substrate (X) and the substrate (Z) is not particularly limited. In the case of the following "First Manufacturing Method", "Second Manufacturing Method", "Third Manufacturing Method" and "Fifth Manufacturing Method", the thickness of each of the substrate (X) and the substrate (Z) is preferably 0.01 to 5.00 mm, more preferably 0.03 to 3.00 mm, particularly preferably 0.04 to 2.00 mm, and most preferably 0.05 to 1.00 mm. On the other hand, in the case of the "Fourth Manufacturing Method", the thickness of the substrate (X) is preferably 0.01 to 1.00 mm, more preferably 0.02 to 0.50 mm, particularly preferably 0.03 to 0.40 mm, and most preferably 0.03 to 0.03 mm, and the thickness of the substrate (Z) is preferably 0.01 to 5.00 mm, more preferably 0.03 to 3.00 mm, particularly preferably 0.04 to 2.00 mm, and most preferably 0.05 to 1.00 mm. When the thickness of the substrate (X) and the substrate (Y) is within the above range, it is easier to maintain the interlayer adhesive force of the laminate of the present invention at a high level, which is preferred.
[0157] The surface roughness of the substrate (X) and the substrate (Z) is not particularly limited. When the substrate (X) and the substrate (Z) are polar materials (e.g., polar resins, metals, etc.), there is a tendency that a small arithmetic mean roughness (Ra) shows a high adhesive force. Therefore, the arithmetic mean roughness (Ra) in this case is preferably 0.010 to 10 μm, more preferably 0.010 to 1 μm, further preferably 0.010 to 0.500 μm, particularly preferably 0.010 to 0.300 μm, and most preferably 0.010 to 0.200 μm.
[0158] On the other hand, when the substrate (X) and the substrate (Z) are non-polar materials (such as polyolefin resins, etc.), there is a tendency that a large arithmetic mean roughness (Ra) shows high adhesive force. Therefore, the arithmetic mean roughness (Ra) in this case is preferably 0.010 to 10 μm, more preferably 0.100 to 7 μm, and particularly preferably 0.200 to 6 μm. If it is within the above range, it is easier to show 10 N / cm 2 The above shear adhesion is therefore preferred.
[0159] In addition, in this invention, the arithmetic surface roughness (Ra) is a value measured according to JIS B 0601-2001, and is specifically a value measured according to the method described in an Example.
[0160] [2] Method for manufacturing laminate
[0161] [First Manufacturing Method]
[0162] As a first method for producing the laminate of the present invention, there can be mentioned a method comprising a step (Ia) of press-molding the adhesive layer (Y) on the substrate (X), and a step (II-a) of injection-molding the substrate (Z) on the adhesive layer (Y) after the step (Ia).
[0163] In the first production method, since the step (Ia) of performing press molding and the step (II-a) of performing injection molding are used in combination, it is possible to firmly bond resins that have not been bonded to each other, such as polyacetal resin (POM) and stainless steel plates, etc. In particular, when the hydrogenated block copolymer (A) constituting the adhesive layer (Y) has a farnesene block, the adhesive layer (Y) becomes soft, so that the adhesiveness is further improved.
[0164] <Process (Ia)>
[0165] The step (Ia) in the first production method is a step of press-molding the adhesive layer (Y) on the substrate (X).
[0166] The conditions for the press molding are not particularly limited. After laminating the adhesive layer (Y) on the substrate (X), the temperature is preferably 100 to 220°C, more preferably 120 to 200°C, and the load is preferably 10 to 100 kgf / cm 2 , more preferably 10 to 50 kgf / cm 2 , and more preferably 15 to 40 kgf / cm 2 The substrate (X) and the adhesive layer (Y) can be bonded to each other by performing compression for preferably 1 to 10 minutes, more preferably 1 to 5 minutes.
[0167] <Step (II-a)>
[0168] The step (II-a) is a step of injection-molding the substrate (Z) on the adhesive layer (Y) after the step (Ia).
[0169] The method for injection molding the substrate (Z) on the adhesive layer (Y) is not particularly limited, but the injection molding is preferably performed while setting the temperature of the mold to preferably 190 to 360° C., more preferably 200 to 330° C., and setting the cylinder temperature for injecting the resin constituting the substrate (Z) to preferably 40 to 160° C., more preferably 45 to 150° C.
[0170] [Second manufacturing method]
[0171] The second method for producing a laminate of the present invention comprises a step (Ib) of applying a solution and / or an aqueous emulsion containing the hydrogenated block copolymer (A) onto the substrate (X) and then drying the solution and / or the aqueous emulsion to form the adhesive layer (Y), and a step (II-b) of injection molding the substrate (Z) onto the adhesive layer (Y) after the step (Ib).
[0172] In the second production method, the adhesive layer (Y) can be formed by applying a solution and / or aqueous emulsion containing the hydrogenated block copolymer (A) onto the substrate (X) and drying the solution and / or aqueous emulsion. Therefore, the laminate can be produced relatively simply.
[0173] <Process (Ib)>
[0174] The step (Ib) is a step of forming the adhesive layer (Y) by applying a solution and / or an aqueous emulsion containing the thermoplastic elastomer composition onto the substrate (X) and then drying the coating.
[0175] In step (Ib), first, a solution and / or aqueous emulsion containing the thermoplastic elastomer composition is prepared. Specifically, the thermoplastic elastomer composition is dissolved or dispersed in an organic solvent or water by a known method.
[0176] When obtaining the aqueous emulsion, for example, there may be mentioned methods using a homogenizer, a homomixer, a disper mixer, a colloid mill, a pipeline mixer, a high-pressure homogenizer, an ultrasonic emulsifier, etc. These may be used alone or in combination.
[0177] In the present invention, various additives may be further added to the aqueous emulsion used according to the application, within a range that does not impair the effects of the present invention.
[0178] Examples of additives include anionic surfactants, cationic surfactants, nonionic surfactants, fillers, modifiers, pigments, etc. However, if too much surfactant is added, the resistance of the thin molded body is impaired, so it is necessary to limit the amount to the minimum necessary.
[0179] The content of the thermoplastic elastomer composition in the solution and / or aqueous emulsion containing the thermoplastic elastomer composition is preferably 5 to 50% by mass, more preferably 10 to 40% by mass, and even more preferably 15 to 30% by mass.
[0180] After the solution or aqueous emulsion is prepared by the above method, the solution or aqueous emulsion is applied to the substrate (X) by one or more methods selected from coating, dipping, nozzle (spray) coating, and brush coating.
[0181] Next, the adhesive layer (Y) can be formed by drying the mixture at preferably 30 to 80° C., more preferably 40 to 70° C., for preferably 15 minutes to 2 hours, more preferably 20 minutes to 1 hour.
[0182] <Step (II-b)>
[0183] The step (II-b) in the second manufacturing method is a step of injection molding the substrate (Z) on the adhesive layer (Y) after the step (Ib). A suitable method for injection molding the substrate (Z) on the adhesive layer (Y) is the same as the conditions described in the step (II-a) in the first manufacturing method.
[0184] [Third Manufacturing Method]
[0185] The third method for producing a laminate of the present invention is a method for producing a laminate, which comprises a step (Ic) of press-molding the adhesive layer (Y) on the substrate (X), and a step (II-c) of press-molding the substrate (Z) on the adhesive layer (Y) after the step (Ic).
[0186] In the third production method, since press molding is performed a total of two times in step (Ic) and step (II-c), the substrate (X), the adhesive layer (Y), and the substrate (Z) can be firmly bonded together.
[0187] <Process (Ic)>
[0188] The step (Ic) in the third production method is a step of press-molding the adhesive layer (Y) on the substrate (X), and a suitable mode is the same as the conditions described in the step (Ia) in the first production method.
[0189] <Step (II-c)>
[0190] The step (II-c) in the third manufacturing method is a step of press-molding the substrate (Z) on the adhesive layer (Y) after the step (Ic). A suitable method for press-molding the substrate (Z) on the adhesive layer (Y) is the same as the conditions described in the step (Ia) in the first manufacturing method.
[0191] [Fourth Manufacturing Method]
[0192] The fourth method for producing a laminate of the present invention is a method for producing a laminate, comprising a step (Id) of co-extruding the substrate (X) and the adhesive layer (Y), and a step (II-d) of press-molding the substrate (Z) on the adhesive layer (Y) after the step (Id).
[0193] In the fourth manufacturing method, in step (Id), the substrate (X) and the adhesive layer (Y) are firmly bonded by co-extrusion, and further in step (II-d), press molding is performed, so that the substrate (X), the adhesive layer (Y) and the substrate (Z) as a whole can be firmly bonded.
[0194] <Process(Id)>
[0195] The step (Id) in the fourth production method is a step of co-extruding the substrate (X) and the adhesive layer (Y).
[0196] The co-extrusion method is not particularly limited, and examples thereof include a method using a film-forming apparatus such as a T-die extruder and an inflation molding machine.
[0197] The barrel temperature of the substrate (X) side during coextrusion is preferably set to 150 to 250° C., and the barrel temperature of the substrate (Y) side is preferably set to 140 to 240° C. In the case of T-die extrusion molding, the temperature of the T-die is more preferably 130 to 230° C.
[0198] <Step (II-d)>
[0199] The step (II-d) in the fourth manufacturing method is a step of press-molding the substrate (Z) on the adhesive layer (Y) after the step (Id). A suitable method for press-molding the substrate (Z) on the adhesive layer (Y) is the same as the conditions described in the step (Ia) in the first manufacturing method.
[0200] [Fifth Manufacturing Method]
[0201] The fifth method for manufacturing a laminate of the present invention is a method for manufacturing a laminate, which comprises a step (Ie) of injection molding the adhesive layer (Y) on the substrate (X), and a step (II-e) of injection molding the substrate (Z) on the adhesive layer (Y) after the step (Ie).
[0202] In the fifth production method, the characteristics of the adhesive layer (Y) are fully utilized and two injection moldings are performed simultaneously, so that base materials that cannot be bonded by the conventional method can be firmly bonded.
[0203] <Process (Ie)>
[0204] The step (Ie) in the fifth manufacturing method is a step of injection molding the adhesive layer (Y) on the substrate (X). A suitable method for injection molding the adhesive layer (Y) on the substrate (X) is the same as the conditions described in the step (II-a) in the first manufacturing method.
[0205] <Step (II-e)>
[0206] The step (II-e) in the fifth manufacturing method is a step of injection molding the substrate (Z) on the adhesive layer (Y) after the step (Ie). A suitable method for injection molding the substrate (Z) on the adhesive layer (Y) is the same as the conditions described in the step (II-a) in the first manufacturing method.
[0207] In the production method of the present invention, in any production method, there is no limitation on the substrate (X) and the substrate (Z), but from the viewpoint of more firmly bonding the two substrates, it is preferred that the substrate (X) is a metal and the substrate (Z) is a polar resin or a polyolefin resin.
[0208] [Application of laminated body]
[0209] The laminate of the present invention can be widely used in various applications. For example, in the outer shell materials of electronic and electrical equipment, OA equipment, household appliances, automotive components, etc., synthetic resins, synthetic resins containing glass fibers, aluminum, magnesium alloys and other light metals are used, and the laminate of the present invention can be used for these outer shell materials. More specifically, it is preferably bonded to the outer shells of large displays, notebook personal computers, portable phones, PHS, PDA (portable information terminals such as electronic notebooks), electronic dictionaries, video cameras, digital cameras, portable radio cassette players, converters, etc., and used for impact cushioning materials, coating materials with anti-slip functions, waterproof materials, design materials, etc.
[0210] In addition, it is used for the purposes of a wide range of molded bodies or structures bonded to glass such as window moldings or gaskets, sealing materials, anti-corrosion materials, etc. of automobiles or buildings. In addition, it can also be suitable for the sealing agent of the joint between the glass of the window of an automobile or a building and an aluminum window frame or a metal opening, the connecting part of the glass in the solar cell module, etc. and the metal frame, etc. And then, it can also be suitable for the separator of the secondary battery used in various information terminal devices such as notebook personal computers, portable phones, cameras, etc. or hybrid electric vehicles, fuel cell vehicles, etc. Example
[0211] The present invention is described below by way of examples, but the present invention is not limited to these examples. It should be noted that β-farnesene (purity 97.6 mass % AMRS, manufactured by Incomoleitide Co., Ltd.) was purified by passing through a 3Å molecular sieve and distilled under a nitrogen atmosphere to remove hydrocarbon impurities such as zingiberene, bisabolene, epoxidized farnesene, farnesol isomers, E,E-farnesol, squalene, ergosterol, and various dimers of farnesene, and was used for the following polymerization.
[0212] The components used in Examples and Comparative Examples are as follows.
[0213] <Hydrogenated block copolymer (A)>
[0214] [Production Example 1: Production of hydrogenated block copolymer (A-1)]
[0215] A hydrogenated block copolymer (A-1) was produced by the method described in Production Example 6 of JP-A-2018-024776 except that the composition was as shown in Table 1 below. The details are as follows.
[0216] In a nitrogen-purged and dried pressure vessel, 50.0 kg of cyclohexane as a solvent, 190.5 g of sec-butyl lithium (10.5 mass % cyclohexane solution) as an anionic polymerization initiator, and 0.40 kg of tetrahydrofuran as a Lewis base were placed, and after heating to 50° C., 6.34 kg of β-farnesene was added, and polymerization was carried out for 2 hours. Subsequently, 2.50 kg of styrene (1) was added, and polymerization was carried out for 1 hour. Further, 3.66 kg of butadiene was added, and polymerization was carried out for 1 hour. Subsequently, 0.02 kg of dichlorodimethylsilane was added to the polymerization reaction solution as a coupling agent, and the reaction was carried out for 1 hour, thereby obtaining a reaction solution containing a poly(β-farnesene)-polystyrene-polybutadiene-polystyrene-poly(β-farnesene) pentablock copolymer (hereinafter referred to as “block copolymer (P1)”). To the reaction solution, 5% by mass of palladium carbon (palladium loading: 5% by mass) as a hydrogenation catalyst was added relative to the block copolymer (P1), and the reaction was carried out under the conditions of a hydrogen pressure of 2 MPa and 150° C. for 10 hours. After cooling and depressurization, the palladium carbon was removed by filtration, the filtrate was concentrated, and then vacuum dried to obtain a hydrogenated product (A-1) of a poly(β-farnesene)-polystyrene-polybutadiene-polystyrene-poly(β-farnesene) pentablock copolymer (hereinafter referred to as "hydrogenated block copolymer (A-1)"). The obtained hydrogenated block copolymer (A-1) is a mixture containing 90% by mass of a hydrogenated product of a poly(β-farnesene)-polystyrene-polybutadiene-polystyrene-poly(β-farnesene) pentablock copolymer and 10% by mass of a hydrogenated product of a polybutadiene-polystyrene-poly(β-farnesene) triblock copolymer. The above-mentioned physical properties were measured for the obtained hydrogenated block copolymer (A-1). The results are shown in Table 1.
[0217] [Production Example 2: Production of hydrogenated block copolymer (A-2)]
[0218] In addition, a hydrogenated block copolymer (A-2) was produced by the method described in Example 1 of International Publication No. 2019 / 103048 except that the compounding was performed as shown in Table 1 below. The details are as follows.
[0219] Into a nitrogen-purged and dried pressure vessel were placed 50 kg of cyclohexane as a solvent and 87 g of a cyclohexane solution of sec-butyllithium having a concentration of 10.5 mass % as an anionic polymerization initiator (substantially added amount of sec-butyllithium: 9.1 g).
[0220] After the temperature in the pressure vessel was raised to 50° C., 1.0 kg of styrene (1) was added and polymerized for 1 hour. At the temperature in the vessel of 50° C., 63 g of 2,2-di(2-tetrahydrofuryl)propane (DTHFP) as a Lewis base was added. A mixed solution of 8.16 kg of isoprene and 6.48 kg of butadiene was added over 5 hours and polymerized for 2 hours. Furthermore, 1.0 kg of styrene (2) was added and polymerized for 1 hour, thereby obtaining a reaction solution containing a polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer.
[0221] In the reaction solution, a Ziegler hydrogenation catalyst formed by nickel octanoate and trimethylaluminum was added under a hydrogen atmosphere, and the reaction was carried out for 5 hours under the conditions of a hydrogen pressure of 1 MPa and 80°C. After the reaction solution was cooled and depressurized, the catalyst was removed by washing with water, and vacuum dried to obtain a hydrogenated product (A-2) of a polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer (hereinafter referred to as "hydrogenated block copolymer (A-2)"). The obtained (A-2) is composed of 100% by mass of the hydrogenated product of the polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer, and does not substantially contain the hydrogenated product of the polystyrene-poly(isoprene / butadiene) diblock copolymer. The above-mentioned physical properties were measured for the obtained hydrogenated block copolymer (A-2). The results are shown in Table 1.
[0222] [Production Example 3: Production of hydrogenated block copolymer (A-3)]
[0223] SEBS having a molecular weight (Mp) of 66,500, a vinyl bond content of 38 mol% in the diene block and a styrene content of 30% by mass and SEB having a molecular weight (Mp) of 33,500, a vinyl bond content of 38 mol% in the diene block and a styrene content of 30% by mass were mixed so that the mass ratio [SEBS / SEB] was 3 / 7 to produce a hydrogenated block copolymer (A-3).
[0224] The mass ratio [(a) / (b)] of SEBS was 30 / 70, and the hydrogenation rate was 99 mol %. The mass ratio [(a) / (b)] of SEB was 30 / 70, and the hydrogenation rate was 99 mol %. The content of the diblock copolymer in the hydrogenated block copolymer (A-3) was 30 mass %.
[0225] The following measurements were performed on the obtained hydrogenated block copolymers (A-1), (A-2) and (A-3).
[0226] (1) Determination of molecular weight distribution and peak molecular weight (Mp), etc.
[0227] The peak molecular weight (Mp) and molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer were determined by GPC (gel permeation chromatography) using standard polystyrene-equivalent molecular weights, and the peak molecular weight (Mp) was determined from the top position of the peak of the molecular weight distribution. The measuring apparatus and conditions are as follows.
[0228] The peak molecular weight of the polymer block (a) is determined by measuring a liquid sampled after completion of the polymerization of the polymer block (A).
[0229] ・Device: GPC device "GPC8020" manufactured by Tosoh Corporation
[0230] ・Separation column: "TSKgelG4000HXL" manufactured by Tosoh Corporation
[0231] ・Detector: "RI-8020" manufactured by Tosoh Corporation
[0232] ・Eluent: Tetrahydrofuran
[0233] ・Eluent flow rate: 1.0ml / min
[0234] ・Sample concentration: 5mg / 10ml
[0235] ・Column temperature: 40℃.
[0236] (2) Method for determining hydrogenation rate
[0237] In each of the preparation examples, the block copolymer before hydrogenation and the block copolymer after hydrogenation (hydrogenated block copolymer) were dissolved in deuterated chloroform solvent, and the reaction mixture was measured at 50° C. using Lambda-500 manufactured by JEOL Ltd. 1 H-NMR: The hydrogenation rate of the polymer block (b) in the hydrogenated block copolymer (A) was calculated by the following formula from the peak of protons in the carbon-carbon double bond appearing at 4.5 to 6.0 ppm in the obtained spectrum.
[0238] Hydrogenation rate = {1-(the number of moles of carbon-carbon double bonds contained in 1 mole of the block copolymer after hydrogenation) / (the number of moles of carbon-carbon double bonds contained in 1 mole of the block copolymer before hydrogenation)}×100 (mol%)
[0239] [Table 1]
[0240] .
[0241] [Examples 1 to 39 and Comparative Examples 1 to 15]
[0242] Laminated bodies were produced by laminating the materials described in Table 2 using the materials described in Tables 3 to 10. The steps and conditions of the respective production methods described in Tables 3 to 10 are as follows.
[0243] <First Manufacturing Method (〔1〕 Pressurization Molding Step,〔2〕 Injection Molding Step)>
[0244] (1) Production of Adhesive Layer (Y)
[0245] The compression molding machine "NF-37" manufactured by Shindo Metal Industry Co., Ltd. was used, and a Teflon (registered trademark) coated metal frame was used as a spacer. The pressure was adjusted at 200°C and 100 kgf / cm 2 The hydrogenated block copolymer (A) was compressed and pressed for 3 minutes under a load of 15 kgf / cm 2 Compression molding was performed under a load of 1 minute to obtain an adhesive layer (Y) having a thickness of 1 mm.
[0246] (2) Process (Ia)
[0247] The two sides of a substrate (X) with a length of 100 mm, a width of 35 mm, and a thickness of 1 mm were washed with a surfactant aqueous solution and distilled water in sequence, and then dried. Then, the substrate (X) and the adhesive layer (Y) prepared in the above (1) were arranged in the center of a metal spacer with an outer dimension of 200 mm × 200 mm, an inner dimension of 150 mm × 150 mm, and a thickness of 2 mm.
[0248] The laminated substrate (X) and adhesive layer (Y) were sandwiched between polytetrafluoroethylene sheets and subjected to compression molding at a temperature of 180° C. and a load of 20 kgf / cm 2 (2N / mm 2 ) was press-formed for 3 minutes, thereby laminating the base material (X) and the adhesive layer (Y).
[0249] (3) Step (II-a)
[0250] After the laminate of the substrate (X) and the adhesive layer (Y) was placed in an injection molding machine ("EC75SX; 75 tons" manufactured by Toshiba Machine Co., Ltd.), the material constituting the substrate (Z) was laminated by injection insert molding to produce a laminate in which the substrate (X), the adhesive layer (Y) and the substrate (Z) were laminated in this order. The thickness of the substrate (Z) was 2.0 mm.
[0251] <Second manufacturing method (〔1〕coating and drying step, 〔2〕injection molding step)>
[0252] (1) Process (Ib)
[0253] A 25 mass % solution of the hydrogenated block copolymer (A) was prepared using cyclohexane as a solvent. The substrate (X) (thickness 1.0 mm) was dipped twice in the above solution for coating. Then, the substrate (X) and the adhesive layer (Y) were laminated after drying in a Gill oven at 60°C for 30 minutes. The thickness of the adhesive layer (Y) after drying was 0.2 mm.
[0254] (3) Step (II-a)
[0255] A laminate was obtained by the same method as that described in the above-mentioned first production method. The thickness of the substrate (Z) was 2.8 mm.
[0256] <Third manufacturing method (〔1〕pressing and molding step,〔2〕pressing and molding step)>
[0257] (1) Production of Adhesive Layer (Y)
[0258] The adhesive layer (Y) was obtained by the same method as that described in the first production method. The thickness of the substrate (Y) was 1.0 mm.
[0259] (2) Process (Ic)
[0260] The substrate (X) and the adhesive layer (Y) were laminated by the same method as the method (Ia) described in the first production method. The thickness of the substrate (X) was 1.0 mm.
[0261] (3) Step (II-c)
[0262] The adhesive layer (Y) and the substrate (Z) were laminated by the same method as the method (Ia) described in the first production method. The thickness of the substrate (Z) was 1.0 mm.
[0263] <Fourth Manufacturing Method (〔1〕Co-extrusion Step,〔2〕Pressure Molding Step)>
[0264] (1) Process (Id)
[0265] The substrate (X) was supplied from a single screw extruder with a screw diameter of 30 mm (GM30-28, manufactured by GM Engineering Co., Ltd.), and the adhesive layer (Y) was supplied from a single screw extruder with a screw diameter of 25 mm (GM-25-25, manufactured by GM Engineering Co., Ltd.), and the film discharged from the T-die (T300 coat hanger die) was wound to obtain a coextruded film of the substrate (X) and the adhesive layer (Y). The thickness of the substrate (X) was 0.03 to 0.05 mm, and the thickness of the substrate (Y) was 0.005 to 0.03 mm.
[0266] (2) Step (II-d)
[0267] The coextruded film obtained in the above step (Id) was press-formed with a substrate (Z) on the adhesive layer (Y) by the same method as the method (Ia) described in the above first manufacturing method. The layer structure of the obtained laminated body was a structure having a substrate (X), an adhesive layer (Y) and a substrate (Z) in this order. It should be noted that the thickness of the substrate (Z) was 1.0 mm.
[0268] <Fifth Manufacturing Method (〔1〕Injection Molding Step,〔2〕Injection Molding Step)>
[0269] (1) Process (Ie)
[0270] After the substrate (X) was placed in an injection molding machine (EC75SX; 75 tons manufactured by Toshiba Machine Co., Ltd.), the material constituting the adhesive layer (Y) was laminated by injection insert molding. The thickness of the substrate (X) was 1.0 mm, and the thickness of the substrate (Y) was 1.0 mm.
[0271] (2) Step (II-e)
[0272] Next, a material constituting the substrate (Z) was laminated on the adhesive layer (Y) laminated on the substrate (X) by injection insert molding, thereby producing a laminated body in which the substrate (X), the adhesive layer (Y), and the substrate (Z) were laminated in this order. The thickness of the substrate (Z) was 1.0 mm.
[0273] [Table 2]
[0274] .
[0275] The following evaluations were performed on the obtained laminate. The results are shown in Tables 3 and 4.
[0276] (1) Determination of storage modulus G' and loss modulus G" of adhesive layer (Y)
[0277] A disk-shaped test piece with a diameter of 8 mm and a thickness of 1 mm was cut out from the adhesive layer (Y) produced by the compression molding machine. The test piece was subjected to dynamic viscoelasticity measurement under the following conditions using an ARES-G2 rheometer (manufactured by TA Instruments), and the storage modulus (G') at 100°C and 0°C and the loss modulus (G") at 100°C and 0°C were measured respectively.
[0278] (Dynamic viscoelasticity measurement apparatus and measurement conditions)
[0279] ・Parallel plate: 8mm diameter
[0280] ・Vibration mode: Torsional vibration
[0281] ・Deformation: 0.1%
[0282] ・Frequency: 1Hz
[0283] ・Measurement temperature: -70~200℃
[0284] ・Heating rate: 3℃ / min.
[0285] (2) Determination of adhesion
[0286] The behavior of the obtained laminate when the substrate (X) and the substrate (Z) were peeled off by hand was evaluated based on the following criteria.
[0287] 1 (good): Cannot be peeled off by hand
[0288] 2 (Pass): Can be peeled off by hand
[0289] 3 (Unacceptable): Can be easily peeled off by hand.
[0290] (3) Method for measuring adhesive strength
[0291] <Test piece preparation method>
[0292] The two sides of a substrate (X) having a length of 50 mm, a width of 35 mm, and a thickness of 1 mm were washed with a surfactant aqueous solution and distilled water in sequence and dried. Then, the substrate (X) and the adhesive layer (Y) produced in "(1) Production of adhesive layer (Y)" in the above-mentioned <First production method [1] Press molding step, [2] Injection molding step> were cut into pieces having a length of 12.5 mm and a width of 35 mm, and were arranged in the center of a metal spacer having an outer dimension of 200 mm×200 mm, an inner dimension of 150 mm×150 mm, and a thickness of 2 mm.
[0293] Next, the laminated substrate (X) and adhesive layer (Y) were sandwiched between polytetrafluoroethylene sheets and subjected to compression molding at a temperature of 180°C and a load of 20 kgf / cm 2 (2N / mm 2 ) for 3 minutes, thereby laminating the base material (X) and the adhesive layer (Y).
[0294] Then, the laminate of the substrate (X) and the adhesive layer (Y) in which the polyimide film was attached to the portion where the adhesive layer (Y) was not laminated, and the jig to which the polyimide film was attached were placed in a mold of an injection molding machine ("EC75SX; 75 tons" manufactured by Toshiba Machine Co., Ltd.), and the materials constituting the substrate (Z) were laminated by injection insert molding, thereby producing a laminate in which the substrate (X), the adhesive layer (Y) and the substrate (Z) were laminated in this order (reference Figure 1 ).
[0295] The adhesive layer (Y) and substrate (Z) of the laminate were cut into pieces with a length of 12.5 mm and a width of 25 mm to prepare test pieces (reference Figure 2 .in, Figure 2 This is a diagram of the laminate as viewed from the substrate (Z) side. ).
[0296] <Method for measuring adhesive strength>
[0297] The substrate layer (X) and substrate layer (Z) of the test piece were sandwiched and the adhesive strength was measured at a room temperature of 23° C. and a speed of 2 mm / min using a tensile tester (3345 manufactured by Instron Corporation).
[0298] <Surface roughness of substrate>
[0299] The surface of the substrate was measured using Surfcorder SE1700α (manufactured by Kosaka Laboratory Co., Ltd.) under the following measurement conditions in accordance with JIS B 0601-2001. In addition, the surface roughness measurement values of the substrate are described only in Table 10.
[0300] (Measurement conditions)
[0301] ・Probe R: 2μm
[0302] ・Feed speed: 0.500mm / s
[0303] ・Cut-off: λc=0.800mm
[0304] ・Measuring length: 4.000mm
[0305] ・Filter: GAUSS (ASME).
[0306] [Table 3]
[0307] .
[0308] [Table 4]
[0309] .
[0310] [Table 5]
[0311]
[0312] Unmeasurable*: Adhesion is low and peeling occurred during sample preparation or during installation in a tensile tester.
[0313] [Table 6]
[0314] .
[0315] [Table 7]
[0316] .
[0317] [Table 8]
[0318] .
[0319] [Table 9]
[0320] .
[0321] [Table 10]
[0322] .
[0323] As is clear from the results of Tables 3 to 10, the laminate of the present invention has good adhesiveness.
[0324] <Reference example: Method for measuring hardness of adhesive layer (Y)>
[0325] A-1 to A-3 were used as the materials for the adhesive layer (Y), and the hardness of the adhesive layer (Y) was measured according to the following procedure. First, a compression molding machine "NF-37" manufactured by Shindo Metal Industries was used, and a Teflon (registered trademark) coated metal frame was used as a spacer. The pressure was adjusted to 200°C and 100 kgf / cm 2 After 3 minutes of compression molding under a load of 15kgf / cm 2 Compression molding was performed under a load of 1 minute to obtain an adhesive layer (Y) having a thickness of 1 mm.
[0326] The obtained sheet was cut into approximately 5 cm×5 cm, and 6 sheets were stacked to a thickness of 6 mm. The hardness was measured using an indenter of a Type A hardness tester in a thermostatic chamber at room temperature of 23° C. and 0° C. in accordance with JIS K 6253-3:2012.
[0327] INDEX is calculated based on the following relational expression (i) using the value measured at an ambient temperature of 23° C. and the value measured in a thermostatic chamber at an ambient temperature of 0° C.
[0328] (0℃ hardness / 23℃ hardness)×100≤s(INDEX) (i).
[0329] [Table 11]
[0330] .
[0331] From the results in Table 11, it is understood that the adhesive layer (Y) has a high rubber elastic modulus because the value derived from the relational expression (i) is 140 or less, and thus the substrates (X) and (Z) are firmly bonded to each other and are difficult to be peeled off.
Claims
1. A laminate comprising a substrate (X), an adhesive layer (Y) and a substrate (Z) in this order, characterized in that: The adhesive layer (Y) comprises a hydrogenated block copolymer (A) obtained by hydrogenating a block copolymer (P), wherein the block copolymer (P) comprises a polymer block (a) composed of a structural unit derived from an aromatic vinyl compound and a polymer block (b) composed of a structural unit derived from a conjugated diene, The aforementioned aromatic vinyl compound is styrene, The peak molecular weight of the polymer block (a) is 2000 to 55000, The mass ratio (a) / (b) of the polymer block (a) to the polymer block (b) is 1 / 99 to 50 / 50, The storage modulus G' of the adhesive layer (Y) at 100°C is 2.31×10 5 ~4.00×10 5 Pa.
2. The laminate according to claim 1, wherein The loss modulus G" of the adhesive layer (Y) at 100°C is 3.00×10 4 ~2.50×10 5 Pa.
3. The laminate according to claim 1 or 2, wherein: The adhesive layer (Y) is formed from a thermoplastic elastomer composition containing a hydrogenated block copolymer (A).
4. The laminate according to claim 1 or 2, wherein: The polymer block (b) contains 1 to 100% by mass of a structural unit (b1) derived from farnesene and 0 to 99% by mass of a structural unit (b2) derived from a conjugated diene other than farnesene.
5. The laminate according to claim 4, wherein The conjugated diene other than farnesene is at least one selected from the group consisting of butadiene, isoprene, and myrcene.
6. The laminate according to claim 1 or 2, wherein: The hydrogenation rate of carbon-carbon double bonds in the polymer block (b) is 70 mol% or more.
7. The laminate according to claim 1 or 2, wherein: The peak molecular weight Mp of the hydrogenated block copolymer (A) is 4,000 to 1,500,000.
8. The laminate according to claim 1 or 2, wherein: The molecular weight distribution Mw / Mn of the hydrogenated block copolymer (A) is 1.00 to 4.
00.
9. The laminate according to claim 1 or 2, wherein: The peak molecular weight of the polymer block (a) is 4,000 to 20,000.
10. The laminate according to claim 1 or 2, wherein The substrate (X) and the substrate (Z) are each independently at least one selected from the group consisting of metal, polar resin, polyolefin resin, carbon fiber, glass, and ceramic.
11. The laminate according to claim 1 or 2, wherein The adhesive layer (Y) satisfies the following relational formula (i): [(0℃ hardness / 23℃ hardness)×100≤140](i).
12. The laminate according to claim 1 or 2, wherein: The hydrogenated block copolymer (A) is a mixture of two or more hydrogenated block copolymers, and the content of the diblock copolymer in the hydrogenated block copolymer (A) is 50% by mass or less.
13. The laminate according to claim 1 or 2, wherein: When a stainless steel plate is used as the substrate (X) and a polyacetal resin is used as the substrate (Z), the shear adhesive strength of the adhesive layer (Y) at 23°C is 10 N / cm 2 above.
14. The laminate according to claim 1 or 2, wherein: The arithmetic mean roughness Ra of the substrate (X) and the substrate (Z) is 0.010 to 10 μm.
15. A method for producing a laminated body, the method for producing a laminated body according to any one of claims 1 to 14, characterized in that: The method comprises: a step (Ia) of press-molding the adhesive layer (Y) on the substrate (X); and a step (II) of injection-molding the substrate (Z) on the adhesive layer (Y) after the step (Ia).
16. A method for producing a laminated body, the method for producing a laminated body according to any one of claims 1 to 14, characterized in that: The method comprises: a step (Ib) of coating a solution and / or aqueous emulsion containing the hydrogenated block copolymer (A) on the substrate (X) and then drying the solution and / or aqueous emulsion to form the adhesive layer (Y); and a step (II) of injection molding the substrate (Z) on the adhesive layer (Y) after the step (Ib).
17. A method for producing a laminated body, the method for producing a laminated body according to any one of claims 1 to 14, characterized in that: The method comprises: a step (Ic) of press-molding the adhesive layer (Y) on the substrate (X), and a step (II-c) of press-molding the substrate (Z) on the adhesive layer (Y) after the step (Ic).
18. The method for producing a laminate according to any one of claims 15 to 17, wherein: The substrate (X) is a metal, and the substrate (Z) is a polar resin or a polyolefin resin.