Spherical single crystal 3-nitro-1,2,4-triazol-5-one and preparation method thereof
By controlling the cooling and stirring rate in the aqueous solvent and combining appropriate additives, high-quality NTO spherical single crystals were successfully prepared, which solved the morphology and defect problems of NTO polycrystalline in the prior art, and significantly improved its density and purity. and mechanical properties, suitable for high-performance explosives.
Patent Information
- Application Number
- CN202210853143.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-06
- Filing Date
- 2022-07-07
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-07-07
AI Technical Summary
It is difficult to prepare high-quality NTO spherical single crystals in the prior art, resulting in the prepared NTO crystals being polycrystalline, with poor morphology and high defect content, which limits its application in mixed explosives.
By controlling the cooling rate and stirring rate in the aqueous solvent, and combining appropriate additives to regulate the growth process of NTO crystals, the preparation of high-quality NTO spherical single crystals is achieved. The specific steps include dissolving NTO in the solvent heated in the water bath, and adding additives after Stir under constant temperature conditions, control the cooling rate and stirring rate, gradually precipitate the crystals, and realize the molding of single crystals by static and supersaturation control.
The prepared NTO spherical single crystal has high density, low porosity, low mechanical sensitivity, excellent chemical purity and mechanical properties. The impact sensitivity and friction sensitivity are significantly reduced, and the thermal decomposition activation energy is improved. It is suitable for high-performance explosives.
Smart Images

Figure CN115142117B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a spherical single crystal 3-nitro-1,2,4-triazole-5-one and a preparation method thereof, and belongs to the field of quality control of single-substance explosive crystals. Background Art
[0002] The high-tech development of weapons and equipment has put forward increasingly higher requirements on the destructive power, operability, battlefield survivability and safety of elemental explosives. The crystal quality control of elemental explosives is an important breakthrough point for improving the comprehensive performance of elemental explosives.
[0003] 3-nitro-1,2,4-triazol-5-one (NTO) is a high-energy, insensitive single-element explosive. NTO crystals, produced directly from the nitration reaction of TO, are jagged, rod-like crystals that easily aggregate and are sensitive to shock waves. When used in mixed explosives, the mixed explosive charge has poor molding properties, low charge density, and reduced solids content, limiting NTO's application in mixed explosives. Existing technologies use rapid cooling to tightly aggregate fine, rod-like NTO particles to produce spherical NTO polycrystals. This allows for control of particle size and sphericity, reducing impact sensitivity to 20% and friction sensitivity to 16%, lowering viscosity during charging and increasing charge capacity. Compared to polycrystals, single crystals have fewer internal defects and impurities, higher crystal purity, and better mechanical properties. Reaction hotspots are reduced when the crystals are subjected to external mechanical forces, effectively improving safety. While explosives researchers at home and abroad have produced quasi-spherical single crystals of CL-20, HMX, and RDX, currently produced NTO crystals are all polycrystalline. Therefore, the preparation of high-quality spherical NTO single crystals has become a challenge for those skilled in the art.
[0004] Preparation and Characterization of Quasi-Spherical NTO (Energetic Materials, 2005, 13(z1):4-6) reported that quasi-spherical NTO was prepared under conditions of rapid cooling and high-speed stirring. Scanning electron microscopy (SEM) images of the spherical particles showed that the spherical NTO was composed of densely aggregated rod-like fine structures with a diameter of several microns.
[0005] In the article "Preparation and Mechanical Sensitivity Study of Spherical NTO Crystals" (Chemical Propellants and Polymer Materials, 2019, 17(02): 23-26), spherical NTO was obtained by heating and rapidly cooling under the action of the surfactant polyvinyl alcohol. From the SEM images, it can be seen that the spherical NTO prepared when the polyvinyl alcohol content is 0.001% to 0.01% has a smooth surface and few edges and corners. The spherical NTO is prepared by polyvinyl alcohol coating the NTO surface.
[0006] The patent "A high crystal density spherical NTO crystal and preparation method" (CN201510673200.8) discloses a high crystal density spherical NTO crystal and a preparation method thereof. The spherical NTO formed by cooling crystallization appears as a spherical polycrystal formed by the agglomeration of small crystals under a low-magnification electron microscope.
[0007] The patent "A spherical NTO crystal and its preparation method" (CN202111613994.0) discloses a method for preparing spherical NTO crystals by limiting the parameters of solvent type, saturated solution temperature, cooling rate and stirring rate during the cooling process. The SEM provided shows that the crystals are polycrystals formed by the aggregation of small crystals.
[0008] The above patent studied the preparation of NTO crystals and obtained NTO spherical polycrystals of different sizes by adjusting the cooling crystallization process conditions. However, due to the particularity of NTO crystals, high-quality NTO spherical single crystals were not obtained. Summary of the Invention
[0009] The purpose of the present invention is to solve the problem that the NTO obtained by recrystallization of NTO is polycrystalline, has poor morphology, and contains a large number of defects in the prior art, and to provide a spherical single crystal of 3-nitro-1,2,4-triazol-5-one and a preparation method thereof. The high-quality NTO spherical single crystal is prepared by finely controlling the cooling crystallization process; the unit cell parameters of the NTO spherical single crystal prepared by this method are β=106.61°, which is consistent with the α-type crystal structure, and the density reaches 1.941g / cm 3 (100K), porosity less than 0.3%, chemical purity greater than 99.5%, obvious black cross extinction phenomenon under polarizing microscope, typical spherulite, aspect ratio less than 1.1, impact sensitivity reaches 20-28%, friction sensitivity reaches 8-12%, thermal decomposition activation energy reaches 393.7kJ / mol, and elastic modulus reaches 20MPa.
[0010] To achieve the above object, the present invention provides the following technical solutions:
[0011] A spherical control scheme for high-quality NTO single crystals, with the following specific steps:
[0012] Step 1: Dissolve the raw material NTO in a solvent heated in a water bath, and then keep it at 70-90°C for 1 hour to obtain solution A.
[0013] The solvent is an aqueous solvent commonly used in industry, such as N-methylpyrrolidone and ethanol, with a water mass ratio of 10-90% and a NTO to solvent material ratio of 20-50%. Compared with the solvent system used in the prior art, the selection range is wider and the cost is lower.
[0014] Step 2: While maintaining the temperature constant and stirring continuously, add an additive to the solution A obtained in step 1. After the solute is completely dissolved, keep the temperature constant for 20 to 40 minutes; the mass ratio of the additive to the total mass of solution A and the additive is 0.01-0.03%;
[0015] The additive is one or more combinations of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, polyvinylpyrrolidone, lecithin, ethylene glycol, formic acid, acetic acid, amino acids, etc.;
[0016] Step 3: Control the cooling rate at 3-10°C / min and the stirring rate at 200-500 r / min. After the crystals are precipitated, keep the mixture at 0°C for 30 minutes to obtain a mixed system B.
[0017] Step 4: Let the mixed system B stand for 24 hours, take the supernatant into a beaker, control the supernatant supersaturation to 1.3% to 1.8%, control the stirring rate to 200 to 500 r / min, and the cooling rate to 0.2 to 0.5°C / min until the crystals are completely precipitated, filter, wash, and dry.
[0018] Compared with the spherical NTO polycrystals prepared by the existing technology, the preparation of spherical NTO single crystals is realized, which greatly improves and expands the performance of NTO.
[0019] Beneficial effects
[0020] 1. The present invention is a preparation method for high-quality NTO spherical single crystals, and the product density reaches 1.941g / cm 3 (100K), porosity less than 0.3%, chemical purity greater than 99.5%, obvious black cross extinction phenomenon under polarizing microscope, typical spherulite, aspect ratio less than 1.1, impact sensitivity reaches 20%-28%, friction sensitivity reaches 8-12%, thermal decomposition activation energy reaches 393.7kJ / mol, elastic modulus reaches 20MPa. Compared with the raw material and spherical NTO polycrystals (see Table 1), the density, porosity, mechanical sensitivity, thermal safety and mechanical properties are significantly improved.
[0021] 2. The recrystallization technology commonly used in modern industrial production is used to control the NTO spherical single crystals. The preparation conditions are mild. The aqueous solvents of N-methylpyrrolidone and ethanol, which are commonly used solvents for NTO recrystallization, are selected, with a water mass ratio of 10-90%. Single or mixed additive components such as hexadecyltrimethylammonium bromide, lecithin, ethylene glycol, formic acid, acetic acid, and amino acids are selected, and the mass is 0.01-0.03% of the total mass of the system. This can achieve the preparation of high-quality NTO spherical single crystals.
[0022] 3. The present invention is a method for preparing high-quality NTO spherical single crystals. The quality of NTO crystals is controlled by controlling the temperature, cooling rate and stirring rate in an aqueous solvent system. The entire process is simple to operate, does not require additional precision equipment, and has mild reaction conditions, is safe, reliable, green and efficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Scanning electron microscope image of NTO spherical single crystals prepared in NMP system;
[0024] Figure 2 Polarizing microscope image of NTO spherical single crystals prepared in NMP system;
[0025] Figure 3 Optical microscope image of NTO bulk single crystals prepared in the NMP system.
[0026] Figure 4 Optical microscope image of NTO spherical polycrystals prepared in NMP system; DETAILED DESCRIPTION
[0027] The present invention will be further described below with reference to the embodiments and accompanying drawings.
[0028] Example 1
[0029] A method for preparing high-quality NTO crystals, the specific steps are as follows:
[0030] Step 1: Add 18g of a mixed solution of ethanol and water (80% ethanol, 20% water) to a three-necked flask, add 0.03% acetic acid to the mixed solvent, add 1g of ordinary NTO, and slowly heat the resulting mixture to 50°C. Stir continuously during the dissolution and heating process at a stirring rate of 500 rpm until the solute is completely dissolved to obtain Solution A;
[0031] Step 2: Under continuous stirring, keep the solution A obtained in step 1 at a constant temperature for 40 minutes;
[0032] Step 3: Using cooling water to cool the solution A obtained in step 2 at a rate of 10°C / min, cool it to 0°C and keep it warm for 20 minutes, stirring at a speed of 500 r / min to obtain a mixed system B.
[0033] Step 4: Let the mixed system B stand for 24 hours, take the supernatant into a beaker, measure the temperature at 25°C, reduce it by 0.5°C, control the supernatant supersaturation to 1.3%, control the stirring rate to 500r / min, and the cooling rate to 0.3°C / min until the crystals are completely precipitated, filter, wash, and dry to obtain high-quality NTO crystals HQ-NTO-1.
[0034] Example 2
[0035] A method for preparing high-quality NTO crystals, the specific steps are as follows:
[0036] Step 1: Add 12g of a mixed solution of NMP and water (25% NMP, 75% water) to a three-necked flask, add 0.02% formic acid to the mixed solvent, add 1g of ordinary NTO, and slowly heat the resulting mixture to 90°C. Stir continuously during the dissolution and heating process at a stirring rate of 300 r / min until all the solute is dissolved to obtain Solution A;
[0037] Step 2: Under continuous stirring, keep the solution A obtained in step 1 at a constant temperature for 30 minutes;
[0038] Step 3: Using cooling water to cool the solution A obtained in step 2 at a rate of 5°C / min, cool it to 0°C and keep it warm for 20 minutes, stirring at a speed of 300 r / min to obtain a mixed system B.
[0039] Step 4: Let the mixed system B stand for 24 hours, take the supernatant into a beaker, control the supernatant supersaturation to 1.5%, control the stirring rate to 300r / min, and the cooling rate to 0.2℃ / min until the crystals are completely precipitated, filter, wash and dry to obtain high-quality NTO crystals HQ-NTO-2, such as Figure 1 As shown in the SEM image of spherical single crystal, NTO is a micron-level single crystal with high sphericity and smooth surface. Figure 2 As shown in the polarizing microscope image of the spherical single crystal, NTO exhibits obvious black cross extinction phenomenon, which is a typical feature of spherulites.
[0040] Example 3
[0041] A method for preparing high-quality NTO crystals, the specific steps are as follows:
[0042] Step 1: Add 15g of a mixed solution of ethanol and water (90% ethanol, 10% water) to a three-necked flask, add 0.02% tetrabutylammonium bromide to the mixed solvent, add 1g of ordinary NTO, and slowly heat the resulting mixture to 75°C. Stir continuously during the dissolution and heating process at a stirring rate of 300 r / min until the solute is completely dissolved to obtain Solution A;
[0043] Step 2: Under continuous stirring, keep the solution A obtained in step 1 at a constant temperature for 40 minutes;
[0044] Step 3: Using cooling water to cool the solution A obtained in step 2 at a rate of 3°C / min, cool it to 0°C and keep it warm for 20 minutes, stirring at a speed of 300 r / min to obtain a mixed system B.
[0045] Step 4: Let the mixed system B stand for 24 hours, take the supernatant into a beaker, control the supernatant supersaturation to 1.5%, control the stirring rate to 300r / min, and the cooling rate to 0.5℃ / min until the crystals are completely precipitated, filter, wash, and dry to obtain high-quality NTO crystals HQ-NTO-3.
[0046] Example 4
[0047] A method for preparing high-quality NTO crystals, the specific steps are as follows:
[0048] Step 1: Add 12g of NMP-water mixed solution (NMP 25%, water 75%) to a three-necked flask, add 0.02% lecithin to the mixed solvent, add 1g of NTO ordinary product, slowly heat the resulting mixture to 90°C, and continue stirring during the dissolution and heating process at a stirring rate of 300r / min until the solute is completely dissolved to obtain solution A;
[0049] Step 2: Under continuous stirring, keep the solution A obtained in step 1 at a constant temperature for 40 minutes;
[0050] Step 3: Using cooling water to cool the solution A obtained in step 2 at a rate of 8°C / min, cool it to 0°C and keep it warm for 20 minutes, stirring at a speed of 300 r / min to obtain a mixed system B.
[0051] Step 4: Let the mixed system B stand for 24 hours, take the supernatant into a beaker, control the supernatant supersaturation to 1.8%, control the stirring rate to 300r / min, and the cooling rate to 0.3℃ / min until the crystals are completely precipitated, filter, wash, and dry to obtain high-quality NTO crystals HQ-NTO-4.
[0052] The chemical purity, porosity (true density method), aspect ratio, decomposition peak temperature (DSC, 10°C / min), and mechanical properties of the prepared crystals were tested. The results are shown in Table 1.
[0053] Table 1 NTO sample performance test
[0054]
[0055] Comparative Example 1
[0056] To investigate the effect of the cooling crystallization process conditions on the morphology of NTO crystals, NTO crystals were prepared according to the method of Example 3. The specific process parameters are shown in Table 2.
[0057] Table 2 Effect of cooling crystallization process conditions of ethanol and water (9:1) system on NTO crystal morphology
[0058]
[0059] As shown in Table 2, NTO spherical single crystals can be prepared when the additive content is 0.01% to 0.03%, the cooling rate of the supernatant is controlled at 0.2 to 0.5°C / min, and the supersaturation is 1.3% to 1.8%. NTO single crystals prepared outside this range are blocky or rod-shaped and easily aggregated. Figure 3 This is an optical microscope image of NTO bulk single crystal prepared in the NMP system, with poor sphericity.
[0060] Comparative Example 2
[0061] Add 2g NMP and 6g distilled water to a three-necked flask, add 1g NTO to the mixed solution, stir, and heat at 95°C until it is completely dissolved. Rapidly introduce a low-temperature medium into the jacket to quickly cool the crystallization solution, and control the cooling rate to 10°C / min. Maintain high-speed stirring to keep the crystallization solution in a turbulent state until the crystallization solution cools to room temperature. Filter and dry to obtain a spherical polycrystalline sample of NTO, see Figure 4 , the degree of sphericalization of NTO spherical polycrystals under optical microscope is lower than that of spherical single crystals.
[0062] The above specific description further illustrates the purpose, technical solutions and beneficial effects of the invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A spherical single crystal 3-nitro-1,2,4-triazol-5-one, Features: Under a polarizing microscope, it shows an obvious black cross extinction phenomenon, which is a spherical single crystal; at 100K, the crystal density reaches 1.941g / cm 3 ; The crystal porosity is less than 0.3%, and the chemical purity is greater than 99.5%; the crystal aspect ratio is less than 1.1, the impact sensitivity reaches 20%-28%, the friction sensitivity reaches 8-12%, the thermal decomposition activation energy reaches 393.7 kJ / mol, and the elastic modulus reaches 20MPa.
2. A method for preparing spherical single crystal 3-nitro-1,2,4-triazol-5-one according to claim 1, Features: The steps include: Step 1: dissolve the raw material NTO in a solvent heated in a water bath, and then keep the temperature at 70-90°C until it is fully dissolved to obtain solution A; Step 2: Keep the temperature constant, add additives to solution A under continuous stirring, and keep the temperature constant until the additives are completely dissolved; the mass ratio of the additive to the total mass of solution A and additives is 0.01-0.03%; Step 3, controlling the cooling rate at 3-10°C / min, stirring, and after crystals are precipitated, keeping the mixture at 0°C for 30 minutes to obtain a mixed system B; Step 4: After the mixed system B is allowed to stand, the supernatant is collected; The mixture was stirred continuously, the supernatant was controlled to have a supersaturation of 1.3% to 1.8%, and the temperature was lowered until all the crystals were precipitated, with a cooling rate of 0.2 to 0.5°C / min. The mixture was filtered, washed, and dried to obtain spherical single crystals of 3-nitro-1,2,4-triazol-5-one. In step 1, the solvent is an aqueous solvent of N-methylpyrrolidone or ethanol, wherein the water content is 10% to 90%; The additive in step 2 is at least one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, polyvinylpyrrolidone, lecithin, ethylene glycol, formic acid, acetic acid and amino acid.
3. The method according to claim 2, Features: The stirring rate in steps 2, 3 and 4 is 200-500 r / min.
Citation Information
Cited By
Ultrasonic-assisted NTO crystallization granulation method
CN117886765A
An ultrasonic-assisted NTO crystallization granulation method
CN117886765B