A polyolefin hollow fiber membrane for asymmetric degassing and its preparation method and use
By optimizing the melt stretching method and air-cooled crystallization process, an asymmetric polyolefin hollow fiber membrane with high porosity and mechanical properties was prepared, which solved the problem of insufficient porosity and mechanical properties of existing membranes in ultrapure water degassing. problem, achieving the effects of efficient degassing and long life.
Patent Information
- Application Number
- CN202210809824.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-11
AI Technical Summary
Existing polyolefin hollow fiber membranes have problems such as low porosity, insufficient mechanical properties, and diluent residue during the degassing process, which limits their application in ultrapure water degassing.
Asymmetric polyolefin hollow fiber membranes are prepared by melt stretching method. By controlling the length and width of microfibers, a dense outer surface and a porous inner surface are formed to improve porosity and mechanical properties, and through air-cooled crystallization and hot drawing pore expansion processes Optimize membrane structure.
The polyolefin hollow fiber membrane achieves high porosity, high degassing efficiency and long service life. It is suitable for degassing ultrapure water and ensures both rapid gas permeation and mechanical strength.
Smart Images

Figure CN115155329B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of membrane materials, and more particularly to a polyolefin hollow fiber membrane for asymmetric degassing and a preparation method and application thereof. Background Art
[0002] In many applications in the industrial, biochemical or medical fields, there is a problem of separating gas components from liquids; for example, in the process of preparing ultrapure water, it is necessary to remove oxygen and carbon dioxide in the ultrapure water as much as possible, because the presence of these gases will have an adverse effect on the subsequent preparation of electronic devices such as silicon wafers (Chinese patent CN1090042C has a corresponding description); currently the most common way to remove gases is to use membrane separation technology, which uses various degassing membranes to effectively remove various gases in liquids at room temperature, which is safe and efficient.
[0003] Currently, the existing degassing membranes are generally polyolefin hollow fiber membranes, and the common polyolefins are PP, PE and PMP. The main methods for preparing polyolefin hollow fiber membranes are melt stretching and thermally induced phase separation. The basic principle of thermally induced phase separation is that a mixture of a polymer and a high boiling point, low molecular weight diluent forms a homogeneous solution at high temperature, which is then extruded through a hollow die head. The molded product undergoes liquid-liquid or solid-liquid phase separation in the coolant, and the position occupied by the diluent is removed to form micropores. This method is described in detail in patents such as US6409921, US6497752 and US7429343. This method has a good porosity, which can be as high as 75%. The membrane filaments produced by this process have high degassing performance and mechanical properties, meeting the needs of practical applications; but since diluents and other substances are added during the preparation process, even after subsequent purification and other treatments, a small amount of diluent will still remain in the membrane; in the process of degassing the liquid during membrane formation, these diluents will dissolve and enter the corresponding liquid; these diluents have basically no effect on general liquids; but in some high-precision fields such as microelectronics, even a small amount of pollution will have a significant impact on the surface of the silicon wafer, then these small amounts of diluents will cause great damage to the silicon wafer, and ultrapure water is mainly used in the field of microelectronics to rinse various types of dirt that appear in the preparation process of silicon wafers. Therefore, the polyolefin hollow fiber membrane prepared by thermotropic phase cannot be used for the degassing of ultrapure water.
[0004] The basic principle of the melt stretching method is to melt extrude pure polymer melt. The formation of micropores is mainly related to the hard elasticity of the polymer material. During the stretching process, the lamellar structure of the hard elastic material arranged perpendicular to the extrusion direction is pulled apart to form micropores, and then the pore structure is fixed by a heat setting process. Its preparation process mainly includes melt spinning, drawing, heat treatment, stretching, heat setting and other steps. For example, this method is described in detail in patents such as US3558764, US4055696 and US4664681. The hollow fiber membrane prepared by this method does not contain diluent, so it is particularly suitable for the degassing of ultrapure water, ensuring that new impurities (such as diluents) are basically not introduced during the degassing process; but the existing hollow fiber membrane prepared by the melt stretching method also has a major disadvantage that the porosity is too low, generally only up to about 30%, which greatly restricts the exchange efficiency between gas and liquid, thereby resulting in too low deoxidation efficiency / decarbonization (carbon dioxide) efficiency. The existence of the above problems greatly limits the development of degassing membranes. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a polyolefin hollow fiber membrane for asymmetric degassing, and a preparation method and use thereof. The hollow fiber membrane is prepared by a melt stretching method, has a high porosity, high deoxygenation efficiency / decarbonization (carbon dioxide) efficiency, and has high mechanical properties and a long service life, and is particularly suitable for degassing of ultrapure water.
[0006] To achieve the above object, the present invention provides the following technical solution: an asymmetric degassing polyolefin hollow fiber membrane, comprising a main body, one side of the main body is an inner surface facing the inner cavity, and the other side is an outer surface, the main body has a non-directional tortuous passage, and the inner surface has a plurality of microfibers for forming a porous structure, the average length of the microfibers is 100-400nm, and the average width is 15-60nm;
[0007] The length direction of the microfiber is consistent with the length direction of the hollow fiber membrane, and the width direction of the microfiber is consistent with the circumferential direction of the hollow fiber membrane;
[0008] The surface energy of the outer surface is 15-40 mN / m, and the outer surface is a dense surface.
[0009] In the membrane structure of the hollow fiber membrane provided by the present invention, it can be clearly seen that the pore size and distribution of the pores on the inner and outer surfaces of the membrane are completely different, and there is a large gap; the outer surface of the membrane is very dense, and "dense" in the present invention means that the pore area ratio of the outer surface (i.e., pore area: outer surface area) is not more than 5% when photographed by a scanning electron microscope at 50,000 times, that is, there are two situations in which the pore structure cannot be observed or a very small number of pore structures can be observed. Since the hollow fiber membrane of the present invention is mainly used to remove various gas components in liquids, such as removing oxygen and carbon dioxide from ultrapure water, these liquids to be treated will be in direct contact with the outer surface of the hollow fiber membrane, and the dense outer surface ensures the service life of the hollow fiber membrane, and there is no risk of leakage (i.e., the liquid will not penetrate the membrane wall thickness into the membrane cavity), thereby ensuring that the hollow fiber membrane has a good degassing efficiency;
[0010] As is known to all, the surface energy of water at 20°C is 72.8 mN / m. If the surface energy of the membrane is lower than 72.8 mN / m, it means that the outer surface of the membrane has a certain hydrophobic property. The greater the hydrophobic property of the membrane, the surface energy of the outer surface of the hollow fiber membrane of the present invention at 20°C is 15-40 mN / m, which means that the outer surface of the membrane has a strong hydrophobic property and is not easily wetted by hydrophilic liquids such as water, further improving the service life of the hollow fiber membrane of the present invention when used as a degassing membrane; At present, one of the biggest reasons for the failure of the degassing membrane is that the outer surface gradually becomes hydrophilic (some liquids contain amphiphilic substances, which easily cause the membrane to penetrate the liquid, or some Substances with low surface tension, such as ethanol, will directly pass through, and using it in pure water will cause bacteria to grow, resulting in the membrane being hydrophilic). The combined effect of a dense outer surface and a relatively strong hydrophobic outer surface will make the process of hydrophilizing the outer surface of the membrane very long, that is, the degassing membrane has a long service life and can perform degassing for a long time; but if there are many holes on the outer surface of the degassing membrane and it is not dense enough, then even if the outer surface of the membrane has a strong hydrophobicity, the membrane filaments are easily hydrophilized during the degassing process, that is, they are wetted by the liquid in a relatively short time, and the service life of the membrane filaments with such a structure will be very short; in addition, a dense outer surface is conducive to improving the mechanical strength of the membrane filaments;
[0011] On the inner surface of the membrane, there are many microfibers (fiber structures of a certain length and thickness). These microfibers are evenly distributed on the inner surface of the membrane, and corresponding holes are formed between the microfibers, so that a certain number of holes with a certain pore size appear on the inner surface of the membrane. The existence of these holes ensures that the hollow fiber membrane has a high porosity, which is convenient for the rapid penetration of gases such as oxygen. The pore size on the inner surface is related to the length of the microfibers. Generally, the longer the microfibers are, the larger the pore size of the membrane pores (that is, there is a positive correlation between the length of the microfibers and the pore size of the holes on the inner surface). Therefore, when the length of the microfibers is too small, the pore size of the holes on the inner surface will be too small, which will affect the gas permeation rate and then affect the corresponding degassing efficiency (this The degassing efficiency in the invention mainly refers to the deoxygenation efficiency and the decarbonation efficiency, and other gases are not considered in the present invention), which cannot meet the needs of practical applications; and the length of the microfiber is too long, which, on the one hand, indicates that the pore size on the inner surface is too large, which will make the mechanical strength of the membrane too low and cannot meet practical needs; on the other hand, in the long-term degassing process, the overly long microfiber is easy to break, thereby greatly reducing the service life of the degassing membrane; and the average length of the microfiber in the present invention is 100-400nm (the length direction of the microfiber is consistent with the length direction of the hollow fiber membrane), so that the inner surface has holes with suitable pore size, thereby ensuring that the degassing membrane has a high degassing rate and degassing efficiency, and at the same time ensuring that the degassing membrane has a high mechanical strength and a long service life;
[0012] The length of the microfiber reflects the size of the holes on the inner surface; the width of the microfiber (i.e., thickness) reflects to a certain extent the number of holes on the inner surface, because in the circumferential direction of the membrane, the width of the microfiber is the spacing between adjacent holes. The larger the width of the microfiber, the larger the distance between adjacent holes, and the fewer the holes. If the number of holes on the inner surface is too small, it will affect the degassing rate and degassing efficiency of the degassing membrane, so the width of the microfiber cannot be too large. If the width of the microfiber is too small, it means that the microfiber is very thin, and these very thin microfibers are easy to break during the degassing process, and the holes are also easy to collapse, resulting in the degassing membrane being unable to continue to have a degassing effect and having a too low service life. The average width is 15-60nm (the width direction of the microfiber is consistent with the circumferential direction of the hollow fiber membrane), which ensures that there are a suitable number of holes on the inner surface, further ensuring that the degassing membrane has a high degassing rate and degassing efficiency, while ensuring that the degassing membrane has a high mechanical strength and a long service life.
[0013] The surface energy test method of the outer surface of the hollow fiber membrane is to test the hollow fiber membrane with a dyne pen, brush a 10 cm long ink strip on the hollow fiber membrane with the dyne pen, and observe whether more than 90% of the ink strip shrinks and forms ink drops within 2 seconds, until it stops shrinking and ink drops appear, and the surface energy of the ink tested is the surface energy of the outer surface of the membrane; the measurement method of the microfiber on the membrane surface can be through the use of a scanning electron microscope to characterize the morphology of the membrane structure, and then use computer software (such as Matlab, NIS-Elements, etc.) or manual measurement, and perform corresponding calculations; During the preparation of the membrane, in the direction perpendicular to the membrane thickness (if the membrane is a hollow fiber membrane, this direction is perpendicular to the radial direction), its various characteristics such as the length and width of the microfibers are roughly uniform and basically consistent; therefore, the average length and average width of the microfibers in a certain area on the corresponding plane can be used to reflect the average length and average width of the overall microfibers on the plane; when actually measuring, the membrane surface can be characterized by an electron microscope to obtain the corresponding SEM image, and since the microfibers on the membrane surface are roughly uniform, a certain area can be selected, such as 1μm 2 (1μm times 1μm) or 25μm 2 (5 μm multiplied by 5 μm), the specific area size depends on the actual situation, and then the length and width of all microfibers on the area are measured by corresponding computer software or manually, and then calculated to obtain the average length and average width of the microfibers on the surface; of course, those skilled in the art can also obtain the above parameters by other measurement methods, and the above measurement methods are for reference only. In addition, the average spacing between adjacent microfibers, the hole area ratio of the inner surface, the average width of the lamellar area and the average length of the air permeable area in the present invention can all be measured by the above method;
[0014] As a further improvement of the present invention, the difference between the maximum length and the minimum length of the microfiber does not exceed 350nm; the difference between the maximum width and the minimum width of the microfiber does not exceed 70nm;
[0015] The average length of the microfibers is 4-10 times the average width of the microfibers;
[0016] In the circumferential direction of the hollow fiber membrane, the average spacing between adjacent microfibers is 20-80 nm.
[0017] In the present invention, there is a positive correlation between the length of the microfiber and the size of the holes on the inner surface. When the length of some microfibers is too long, some holes with too large holes (defective holes) will appear on the inner surface. These holes with too large holes are more likely to collapse under the action of external forces (stress is more likely to concentrate), which also greatly reduces the overall mechanical strength of the membrane. Therefore, the length of the microfibers cannot be too long. When the length of some microfibers is too short, some holes with too small holes will appear on the inner surface. These holes with too small holes are regarded as "false holes". Although the existence of "false holes" increases the hole area ratio on the inner surface of the membrane, However, the degassing efficiency is not increased because the aperture of the "pseudo-pores" is too small. Compared with other pores, these "pseudo-pores" have greater resistance to gas penetration, so that the gas will not pass through these "pseudo-pores", and then the degassing efficiency cannot be increased. Therefore, the length of the microfiber cannot be too small; and the difference between the maximum length and the minimum length of the microfiber in the present invention does not exceed 350nm, which can explain that the aperture size of the holes on the outer surface is relatively uniform, and there are neither holes with particularly large apertures (defective holes) nor holes with particularly small apertures (pseudo-pores), which ensures that the membrane as a whole has greater mechanical strength and high degassing efficiency.
[0018] In the present invention, the width (i.e., thickness) of the microfiber reflects to a certain extent the number of holes on the inner surface. When the width of the microfiber is too large, the number of holes in a certain area of the inner surface is too small. Too few holes will inevitably affect the degassing efficiency, and at the same time greatly increase the resistance to gas permeation and the pressure loss during the degassing process. If the width of the microfiber is too small, more holes will appear in a certain area of the inner surface (i.e., in this area, the hole area ratio is too high, and the solid area ratio is too low), which is bound to be a big defect. When external forces act, it is easy to cause the collapse of the holes, so that the degassing membrane cannot continue to degas, and the service life is short. In the present invention, the difference between the maximum width and the minimum width of the microfiber does not exceed 70nm, which means that the thickness of the microfiber is relatively uniform (there are no particularly thick microfibers, nor are there particularly thin microfibers), and it also means that in a certain area of the inner surface, the distribution of holes is relatively uniform (the hole distribution is neither too dense nor too sparse), further ensuring that the membrane has high degassing performance and mechanical properties.
[0019] The main function of the microfibers in the present invention is to maintain the stability of the pores, ensuring that the pores on the inner surface are not prone to collapse and other restrictions during the degassing process, thereby making the membrane as a whole have higher mechanical strength and can have excellent degassing performance for a long time; then what kind of microfibers can better control the stability of the pores? After research, it was found that one of the important characteristics is that there needs to be a suitable ratio between the length and width of the microfibers, because the larger the pore size, the stronger the support required (generally, the thicker the microfiber, the stronger its support for the pore), because when the ratio is too large, it means that the length of the microfiber is too long (in fact, it also means that the pore size of the hole is too large) or the width of the microfiber is too small (very thin, and the supporting effect on the pore is very weak), then the microfibers cannot provide good support for the pores, and the membrane fibers are in the process of degassing. During the degassing process, the holes are prone to collapse, and the service life is greatly reduced; when the ratio is too small, it means that the length of the microfiber is too small (in fact, it also means that the hole diameter is too small) or the width of the microfiber is too large (very thick, resulting in too few holes). At this time, although the microfiber can improve the stability of the holes, the hole diameter on the inner surface is too small and the number is too small, resulting in too low degassing efficiency and unable to meet the needs of practical applications; the average length of the microfiber in the present invention is 4-10 times the average width of the microfiber. Under this ratio, the microfiber can maintain the stability of the holes for a long time and efficiently, ensuring that the hollow membrane has a long service life and mechanical strength. At the same time, the inner surface has a suitable pore diameter and a suitable number of holes, so that the membrane has a large degassing efficiency and meets the needs of practical applications;
[0020] In the membrane structure provided by the present invention, it can be clearly seen that elliptical holes are formed between adjacent microfibers on the inner surface of the membrane; that is, in the circumferential direction of the hollow fiber membrane, the spacing between adjacent microfibers reflects the width of the hole. Generally, the larger the spacing between the microfibers, the larger the width of the hole (that is, the circumferential spacing between the microfibers is positively correlated with the width of the hole); when the circumferential spacing between the microfibers is too large, the width of the hole will be too large, the microfibers cannot maintain the stability of the hole effectively, and the membrane filament cannot be guaranteed to be able to degas for a long time. When the circumferential spacing between the microfibers is too small, the width of the hole will be too small. Even if the long diameter of the hole on the inner surface is very long, the area of the hole is still very small (that is, the hole area ratio on the inner surface of the membrane is too low), then the degassing rate of the membrane filament is too low at this time, and it cannot meet the needs of time application; the average circumferential spacing between adjacent microfibers in the present invention is 20-80nm, so that the hole has a suitable width, which further ensures that the hollow fiber membrane has an excellent degassing rate, as well as high mechanical properties and service life.
[0021] As a further improvement of the present invention, the average length of the microfibers is 2-8 times the average spacing between adjacent microfibers in the circumferential direction of the membrane; the average width of the microfibers is 50%-95% of the average spacing between adjacent microfibers in the circumferential direction of the membrane; and the pore area ratio of the inner surface is 10-35%.
[0022] In the present invention, elliptical holes are formed between adjacent microfibers, wherein the length of the microfibers is positively correlated with the long diameter (length) of the holes, and the circumferential spacing between the microfibers is positively correlated with the short diameter (width) of the holes; and we all hope that the ratio between the long diameter and the short diameter of the holes should not be too large or too small (when the ratio is too low or too high, the degassing rate and degassing efficiency of the entire membrane are not high); and in the present invention, the average length of the microfibers and the circumferential spacing between the microfibers are controlled to ensure that holes with ideal long and short diameters appear on the inner surface of the membrane. It has been found through research that when the average length of the microfibers is 2-8 times the average spacing between adjacent microfibers in the circumferential direction of the membrane, holes with ideal long and short diameters can appear on the inner surface, further improving the degassing efficiency of the polyolefin hollow fiber;
[0023] The main function of microfibers is to maintain the stability of the holes. Generally speaking, the larger the average width of the microfibers, the stronger the supporting effect on the holes. In addition to the length of the microfibers, the circumferential spacing between the microfibers will also affect the supporting effect of the microfibers on the holes. Generally speaking, the larger the circumferential spacing between the microfibers, the stronger the supporting effect of the microfibers on the holes (that is, when the circumferential spacing between the microfibers is larger, the thicker the microfibers are required); and the larger the circumferential spacing between the microfibers, the smaller the pore size of the holes on the inner surface. The larger the width of the microfiber, the more conducive it is to improving the degassing rate and degassing efficiency; therefore, through research, it is found that when the average width of the microfiber is 50%-95% of the average circumferential spacing between adjacent microfibers, it further ensures that the microfiber can support the holes for a long time, ensuring that the degassing membrane can effectively degas for a long time without affecting the efficient degassing of the membrane; in addition, through research, it is found that the pore area rate of the inner surface of the hollow fiber membrane of the present invention is 10-35%, which further ensures that the hollow fiber membrane has a high mechanical strength, and at the same time, the gas can quickly enter the inner cavity of the membrane through the membrane thickness, thereby achieving the purpose of rapid degassing.
[0024] As a further improvement of the present invention, in the circumferential direction of the membrane, a plurality of microfibers are regularly arranged to form a permeable zone for ventilation; the permeable zone is in the shape of a long strip; the average length of the permeable zone is 400-1100 nm, and the average length of the permeable zone is greater than the average width of the permeable zone;
[0025] The length direction of the air permeable zone is consistent with the circumferential direction of the hollow fiber membrane; the width direction of the air permeable zone is consistent with the length direction of the hollow fiber membrane.
[0026] By further observing the inner surface of the hollow fiber membrane, it was found that the microfibers were relatively evenly distributed on the inner surface (this should be related to the fact that the membrane was made by the melt stretching method), and in the circumferential direction of the membrane, several microfibers were regularly arranged, and finally formed a long strip area. There are many holes in this area, and the hole area ratio is high. Gases (such as oxygen, carbon dioxide, etc.) mainly enter the inner cavity of the membrane through this area, so this area is called the permeable zone; further observations found that the width direction of the permeable zone is basically consistent with the length direction of the hollow fiber membrane, and the width of the permeable zone is basically the same as the length of the microfiber, so The main factor affecting the size of the breathable zone is the length of the breathable membrane. The longer the breathable zone is, the larger the area of the breathable zone is. The larger the area of the breathable zone is, the easier it is for gas to pass through, thereby increasing the gas permeation rate and further improving the degassing efficiency of the membrane filament. However, an excessively large breathable zone will cause the local pore area rate on the inner surface of the hollow fiber membrane to be too large, and then there is the possibility of structural damage due to stress concentration, resulting in a greatly reduced service life of the membrane filament. The average length of the breathable zone in the present invention is 400-1100nm, which not only ensures the degassing rate, but also makes the membrane filament have higher mechanical strength and service life.
[0027] As a further improvement of the present invention, in the length direction of the hollow fiber membrane, a lamellar crystal area with a solid structure is formed between adjacent permeable areas; the average width of the lamellar crystal area is 80-280nm; the average width of the lamellar crystal area is 0.3-1.5 times the average width of the permeable area; the width direction of the lamellar crystal area is consistent with the length direction of the hollow fiber membrane.
[0028] On the inner surface of the hollow fiber membrane, in addition to the air permeable area with several holes, there are also corresponding solid areas, which are called lamellar areas. The lamellar areas are located between adjacent air permeable areas (it can also be considered that the stretching effect between the lamellar areas forms the air permeable area with several holes inside). Generally, we believe that microfibers are used to maintain the stability of the holes, and the existence of the lamellar area is used to maintain the stability of the air permeable area. Therefore, if the width of the lamellar area is too small, the stability of the air permeable area cannot be maintained, which affects both the mechanical strength of the membrane and the membrane. The degassing efficiency of the filaments is improved; if the width of the lamellar crystal zone is too large, although the overall mechanical strength of the membrane is guaranteed, the area of the breathable zone will be too small, and the gas will not be able to quickly penetrate the membrane thickness into the inner cavity of the membrane filaments; and the average width of the lamellar crystal zone on the inner surface of the membrane of the present invention is 80-280nm, and the average width of the lamellar crystal zone is controlled to be 0.3-1.5 times (preferably 0.4-1.2 times) of the average width of the breathable zone. Such a membrane inner surface structure not only ensures that the hollow fiber membrane has a high dimensional stability, but also further ensures that the membrane filaments have a high degassing effect.
[0029] As a further improvement of the present invention, the average length of the breathable zone is 2-5 times the average width of the breathable zone; the hole area ratio in the breathable zone is 30-70%, and the hole area ratio of the breathable zone is 20-50% higher than the overall hole area ratio of the inner surface.
[0030] The ratio of the length to the width of the breathable zone can reflect the degree of stretching sufficiency in the preparation process of the hollow fiber membrane. When the ratio of the length to the width of the breathable zone is too small, it means that the hollow fiber membrane is stretched excessively. Excessive stretching is likely to cause the breakage of the microfiber tie structure of the hollow fiber membrane, the collapse of the micropores and the increase of the porosity of the surface, thereby resulting in a decrease in both the degassing effect and the mechanical properties; and when the ratio of the length to the width of the breathable zone is too large, it means that the hollow fiber membrane is not stretched enough or the heat setting process is not suitable, resulting in the shrinkage of the breathable zone, and it is impossible to form a sufficient porosity, so the degassing effect is often poor; since the breathable zone is the main area for gas permeation on the inner surface, the pore area ratio of the breathable zone should be higher, so that the membrane filament has a higher degassing rate; but the pore area ratio in the breathable zone cannot be too high, otherwise there will still be a risk of pore collapse and the service life is too short; in the present invention, the pore area ratio in the breathable zone is 30-70%, and the pore area ratio of the breathable zone is 20-50% higher than the overall pore area ratio of the inner surface. Such a pore area ratio further ensures that the hollow fiber membrane has both a high degassing rate and strong dimensional stability.
[0031] As a further improvement of the present invention, the main body includes a cortex and a support layer, one side of the support layer is an inner surface, one side of the cortex is an outer surface, the thickness of the cortex is 0.5-4 μm, and the thickness of the cortex accounts for 1-8% of the overall thickness of the membrane; the porosity of the cortex is not higher than 10%.
[0032] By further observing the cross-sectional structure of the membrane, it is found that the main body of the membrane mainly includes two regions. In the region close to the outer surface, the number of holes is small, relatively dense, and the thickness of the region is small. In the present invention, the region is called the cortex; and in the region close to the inner surface, the pore size of the holes is relatively large, the number of holes is relatively large, and the number of holes is relatively large. In the present invention, it is called the support layer; in the present application, the cortex and the support layer are composed of the same material, the two layers are combined into an integral structure, and are directly formed during the membrane preparation process. In the transition from the cortex to the support layer, there is only a change in the membrane structure. Therefore, the membrane prepared in the present application is an asymmetric membrane; in contrast, for example, a composite membrane has a multi-layer structure, which is a dense layer as a separation layer applied to a porous, often microporous support layer or support membrane in a separate process step, and the materials constituting the support layer and the cortex in the composite membrane are often different;
[0033] It is well known that under the same conditions, the permeation rate of gas in the cortex must be lower than the diffusion rate of gas in the microporous structure. Therefore, it can be expected that the degassing effect of the asymmetric hollow fiber membrane with a dense cortex must be much lower than the degassing effect of the hollow fiber membrane with a microporous structure that penetrates inside and outside.
[0034] However, the inventors of the present application unexpectedly discovered that, based on the relatively good microporous structure of the hollow fiber membrane body, it is only necessary to control the thickness of the cortex of the hollow fiber membrane and the ratio of the cortex to the wall thickness of the hollow fiber membrane within a certain range (the thickness of the cortex is 0.5-4 μm, and the thickness of the cortex accounts for 1-8% of the total thickness of the membrane).
[0035] The degassing effect of the asymmetric hollow fiber membrane with a dense cortex is only slightly reduced compared to the hollow fiber membrane with an inner and outer through-microporous structure; but the presence of the dense cortex will greatly extend the service life of the membrane fiber, and can achieve efficient degassing for a long time, with high economic benefits; in addition, in the process of degassing ultrapure water, in addition to paying attention to some conventional degassing indicators, people also control an additional indicator-water vapor permeation rate, that is, they hope that the water vapor permeation rate (water vapor permeation amount per unit time) can be reduced as soon as possible, but in general, the higher the oxygen permeation rate, the higher the water vapor permeation rate; and in the present invention, it is surprisingly found that through the presence of a certain thickness of dense cortex, although the oxygen permeation rate also decreases slightly, the water vapor permeation rate has a significant decrease, and only a small amount of water vapor will pass through the wall thickness into the inner cavity.
[0036] As a further improvement of the present invention, the thickness of the support layer is 38-58 μm, and the support layer is at least 35 μm thicker than the skin layer; the porosity of the support layer is 40-70%; the average pore size in the support layer gradually decreases from the area close to the inner surface to the area close to the skin layer.
[0037] In the main structure of the membrane, most of the area is the support layer; therefore, the various properties of the support layer will have a great impact on the overall performance of the membrane; after observation, it was found that the thickness of the support layer in the present invention is 38-58μm, and the support layer is at least 35μm thicker than the skin layer, that is, the thickness of the support layer is much greater than the thickness of the skin layer, and the porosity in the support layer is 40%-70%. Such a support layer structure makes the polyolefin hollow fiber membrane not only have higher mechanical properties, but also have higher porosity, thereby ensuring the overall degassing efficiency of the membrane.
[0038] As a further improvement of the present invention, the average pore size variation gradient of the support layer is 1.5-4 nm / μm; the support layer contains porous fibers for forming a porous structure, and the average diameter of the porous fibers is 60-300 nm.
[0039] In the present invention, the speed of the change of the pore size in the support layer with the thickness is reflected by the size of the average pore size change gradient. The larger the value, the faster the pore size changes, and the smaller the value, the smaller the pore size changes. The value can be obtained by (average pore size close to the inner surface-average pore size close to the cortex) / thickness, so the unit is nm (representing the average pore size) / 1μm (representing the thickness). In the present invention, the average pore size change gradient in the support layer is 1.5-4nm / μm; the pore size change gradient value is very small, which shows that the membrane pore size in the support layer of the present invention changes with the thickness in a small gradient, the pore size in the support layer is very small and changes too fast, and there are no excessively large holes, so that the membrane as a whole has good mechanical strength, and at the same time has a high porosity, degassing rate and degassing. The efficiency is relatively high; in addition, the support layer structure with a gradient pore size change and the suitable microfiber structure on the inner surface further ensure that the degassing efficiency is not affected as much as possible while the water vapor permeability is further reduced; at the same time, the support layer also has a number of porous fibers for forming a porous structure, and the presence of the porous fibers ensures the stability of the holes in the support layer; the average diameter (thickness) of the porous fibers is closely related to the pore size and porosity of the holes in the support layer; the average diameter of the porous fibers in the present invention is 60-300nm, and porous fibers of such a thickness are conducive to ensuring that the membrane as a whole has a high mechanical strength, and at the same time can perform efficient degassing for a long time, so it is suitable for use as a degassing membrane, especially for the degassing of ultrapure water.
[0040] As a further improvement of the present invention, the thickness of the hollow fiber membrane is 40-60 μm, the porosity is 30-50%, and the inner diameter is 175-225 μm; the overall crystallinity of the hollow fiber membrane is 30-55%;
[0041] The membrane-forming material of the hollow fiber membrane is at least one of PP, PE and PMP.
[0042] When the thickness of the membrane is too small, the mechanical strength of the membrane will be low; when the thickness of the membrane is too large, the actual time for the gas to pass through the membrane will be too long, and the time cost will be too high. In addition, when the wall thickness is too large, the resistance will be large, so the gas removal rate will be greatly reduced; therefore, the thickness of the hollow fiber membrane in the present invention is 40-60μm, which is relatively thin and is particularly suitable for use as a degassing membrane. On the basis of ensuring the mechanical strength of the membrane fiber, it has excellent degassing rate and degassing efficiency; the gas to be removed in the liquid (such as oxygen, carbon dioxide, etc.) will enter the inner cavity of the membrane fiber after passing through the wall thickness, and then these gases will be removed by vacuum or purge gas, thereby achieving the purpose of long-term and efficient degassing; therefore, the size of the inner diameter will also affect the amount of degassing per unit time less; the larger the inner cavity, the greater the degassing amount per unit time; but if the inner cavity is too large, the overall compressive strength of the membrane will be too low; the inner cavity diameter of the hollow fiber membrane of the present invention is 175-225μm, which not only ensures that the membrane as a whole has a high compressive strength, but also enables more gas to be removed per unit time, with high economic benefits; when the porosity of the membrane is too high, the tensile strength of the membrane will be too low, its mechanical properties will be poor, its industrial practical value will be low, and it will not be able to meet market demand; and when the porosity of the membrane is too low, the degassing rate and degassing efficiency of the membrane filament will be too low, and the economic benefits will be too low; the porosity of the membrane filament in the present invention is 30-50%, so that the membrane not only has good tensile strength, but also has a large degassing rate and degassing efficiency, with high economic benefits;
[0043] Through DSC measurement, it was found that the overall crystallinity of the prepared hollow fiber membrane was 30-55%, and the membrane fiber had a high degree of crystallinity as a whole, which further ensured that the membrane fiber had a high mechanical strength and could be subjected to various processing treatments; the hollow fiber membrane of the present invention is made of polyolefin materials, containing only carbon and hydrogen elements, and no other elements; further, it can be any one of PP, PE and PMP, and the raw materials are widely available and easy to obtain; the thickness and inner diameter of the hollow fiber membrane of the present invention can be obtained by using a scanning electron microscope to characterize the morphology of the membrane structure, and then using computer software (such as Matlab, NIS-Elements, etc.) or manually measuring; the volume porosity of the membrane can be obtained using a mercury intrusion instrument according to the mercury intrusion method.
[0044] The present invention also provides a method for preparing a polyolefin hollow fiber membrane for asymmetric degassing, comprising the following steps:
[0045] S1, spinning, melt-extrude polyolefin in a die head to form a molded product having an inner surface and an outer surface; the polyolefin is at least one of PP, PE and PMP;
[0046] S2, pre-crystallization, placing the molded product in an air section for pre-crystallization; the melting point of the polyolefin material is Tm, the outer surface temperature of the molded product after pre-crystallization is Tm-(Tm+15)°C, the temperature of the inner surface is greater than the temperature of the outer surface, and the average temperature change gradient of the molded product after pre-crystallization is 0.01-0.2°C / 1um;
[0047] S3, air-cooling crystallization, the molded product obtained in step S2 is subjected to air-cooling crystallization by means of air-blowing cooling, the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, the molded product is sequentially passed through the rapid cooling zone and the slow cooling zone and then rolled up to obtain spun fibers; wherein the outer surface temperature of the molded product is reduced to (Tg+80)-(Tg+120)°C after passing through the rapid cooling zone; and in the rapid cooling zone, the cooling rate of the outer surface of the molded product is not less than 80°C / mm@(100-200)m / min, and the cooling rate of the inner surface of the molded product is 20-60°C / m@(100-200)m / min;
[0048] S4, primary shaping, subjecting the spun fiber to a first heat-setting treatment to obtain a heat-set semi-finished product;
[0049] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product;
[0050] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product;
[0051] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane.
[0052] As a further improvement of the present invention, the melt index of the polyolefin in S1 is 1-7 g / min@(Tm+20°C, 5kg); the crystallinity of the polyolefin is 40-70%;
[0053] The die aspect ratio in S1 is 2-5; the die temperature is (Tm+10)-(Tm+40)°C.
[0054] As a further improvement of the present invention, the length of the air section in S2 is 30-1000mm; the temperature of the air section is 40-70°C; the speed of the cooling air flow during blowing cooling in S3 is 30-60m / min, the temperature of the cooling air flow is 30-70°C, and the path length of the slow cooling zone is 4-8m.
[0055] As a further improvement of the present invention, the cold drawing temperature in S5 is (Tg+30)-(Tg+80)°C, the cold drawing elongation is 20-40%, and the cold drawing rate is (10-30)% / min;
[0056] The hot drawing temperature in S6 is (Tm-60)-(Tm-30)°C, the hot drawing elongation is 2-6 times the cold drawing elongation, and the hot drawing rate is not higher than 15% of the cold drawing rate.
[0057] As a further improvement of the present invention, the first heat setting temperature in S4 is (Tm-60)-(Tm-20)°C, and the setting time is 20-40min; the second heat setting temperature in S7 is 10-30°C higher than the first heat setting temperature, and the setting time is 0.5-3min.
[0058] The present invention prepares the polyolefin hollow fiber membrane by melt stretching method, that is, no corresponding diluent needs to be added in the preparation process, and the raw material used is only the membrane-forming material polyolefin, such as any one of PP, PE and PMP; thus, the prepared membrane is very pure, and when the corresponding liquid is degassed, impurities such as the diluent will not be dissolved, thereby ensuring the purity of the liquid; that is, the polyolefin hollow fiber membrane prepared by the present invention is suitable for degassing various liquids, and is particularly suitable for degassing in ultrapure water.
[0059] In the present invention, the first step is to melt-treat the polyolefin at a suitable temperature and then extrude it to form a molded product with an inner surface and an outer surface; in the process of extruding the molded product, a cavity-forming fluid is introduced at the same time. Common cavity-forming fluids are inert gases, such as nitrogen, argon and other gases. The introduction of the cavity-forming fluid can effectively avoid the concave deformation of the molded product and ensure that the film has a relatively uniform wall thickness; it is well known that the relevant properties of the raw materials are the basis of the surface properties of the membrane filaments and the related microporous morphological structure; after research, it is found that parameters such as the crystallinity and melt index of the raw materials have a great influence on the performance of the film; the crystallinity of the polyolefin raw material in this application is 40-70% (measured by the DSC method), and too low crystallinity of the raw material polyolefin will lead to too low porosity of the film, which in turn makes the gas permeation rate too low and the degassing efficiency too low; therefore, the selection of a polyolefin raw material with high crystallinity is conducive to ensuring that the film has a higher porosity and excellent mechanical properties;
[0060] The melt index is a value that indicates the fluidity of the material during processing; the larger the melt index value, the better the processing fluidity of the material, and vice versa; when the melt index is too small, the obstacles to the arrangement of the molecular chains increase, the molecular chains diffuse, and the activation energy required for the crystal phase structure increases, resulting in a decrease in the ability of the molecular chains to arrange regularly, thereby reducing the crystallinity. When the melt index is large, the plasticity of the material deteriorates and it is not easy to form; when the melt index is too large, the mechanical strength of the film will be too low (generally, the lower the molecular weight, the greater the melt index, and too low a molecular weight will make the mechanical strength of the film too low), which cannot meet the needs of practical applications; the polyolefin melt index in this application is 1-7g / min@(Tm+20℃, 5kg), where Tm is the melting point of the polyolefin raw material, that is, the polyolefin melt index of the present invention is measured at 20℃ above the melting point of the corresponding raw material polyolefin; by selecting raw materials with such a melt index, it is shown that the raw material has good processing fluidity, makes the film thickness more uniform, improves the raw material processing efficiency, and reduces energy consumption and production costs; at the same time, it is also beneficial for the film to obtain higher mechanical properties;
[0061] The die extrusion temperature of the present application is (Tm+10)-(Tm+40)°C, that is, the temperature of the polyolefin extruded at the die is 10-40°C above the melting point of the polyolefin, preferably 15-35°C above the melting point of the polyolefin. The flow viscosity of the polymer melt is significantly affected by temperature, and generally the viscosity decreases with increasing temperature. When the die extrusion temperature is too low, the viscosity of the polyolefin increases, the resistance of the extrusion die increases, the energy consumption of the extrusion process increases, and the thickness of the prepared film increases, and the expansion and stretching cannot be better performed, thereby affecting the tensile strength of the film. When the extrusion temperature is too high, it is not only easy to cause thermal degradation of polyolefin, causing the main chain of polyolefin to break from the weak bond in the middle, thereby reducing its molecular weight, significantly reducing its mechanical properties, and thus reducing the mechanical properties of the film; it is also easy to increase the segment activity of the polymer molecules, expand the "free volume" of the melt, increase the fluidity of the melt, reduce its viscosity, reduce the thickness of the prepared film, and thus affect the gas throughput; the appropriate die extrusion temperature and melt index of the present application make the thickness of the prepared film more uniform, and ensure both good porosity and strong mechanical properties.
[0062] The die aspect ratio is the ratio of the effective length of the screw to the screw diameter. The die aspect ratio of the present application is 2-5. When the molten polyolefin flows in the spinneret, the macromolecular chains are oriented by the shear force. The larger the aspect ratio, the longer the polyolefin melt is subjected to the shear force, making the arrangement of the macromolecular chains more regular. The regular macromolecular structure formed under the shearing action in the channel will not disappear due to the sudden expansion at the die outlet. The polyolefin macromolecular chains have a high degree of crystallinity, a relatively complete crystal structure, and a strong bonding force between macromolecules, so that the prepared film has good crystallinity. Therefore, a suitable die aspect ratio not only has a suitable degree of crystallinity, but also has a uniform film thickness, so that the prepared film has a more uniform pore structure and a greater tensile strength.
[0063] The second step is to naturally cool the molded product after extrusion from the die head through an air section, thereby performing preliminary molding and giving the molded product a certain strength; in the air section, the overall temperature of the molded product will be reduced to a certain extent, wherein the cooling rate of the outer surface is relatively faster, while the cooling rate of the inner surface is relatively slower; through research, it is found that controlling the temperature of the inner and outer surfaces of the molded product after natural cooling can affect the number of overall lamellae to a certain extent, thereby enabling the support layer in the hollow fiber membrane to form a larger number of microporous structures, while the skin layer forms a relatively dense membrane pore structure (generally, the more lamellae, the easier it is to form holes); in the present invention, the outer surface temperature of the molded product after natural cooling is Tm-(Tm+15)°C (Tm is the melting point of the polyolefin raw material), the temperature of the inner surface is greater than the temperature of the outer surface, and the average temperature change gradient of the molded product after pre-crystallization is 0.01-0.2°C / 1um; in such an outer Under the combined effect of the surface temperature and the temperature gradient of the molded product, combined with the subsequent blowing crystallization and the corresponding cold-drawing and hot-drawing processes, it is beneficial to obtain an ideal membrane structure, which changes the situation that the existing stretching method cannot obtain a higher porosity, and truly makes the film have a higher porosity, and then has a high degassing rate and degassing efficiency; further research found that the temperature of the outer surface of the molded product after natural cooling cannot be too high or too low, because if the temperature of the outer surface is too high at this time, then when entering the subsequent air-cooling crystallization, the entire molded product will cool down rapidly (the cooling rate during air-cooling crystallization is greater than the cooling rate during natural cooling), which will easily cause the wall thickness of the final film to be uneven and unable to meet practical needs; and if the temperature of the outer surface is too low, it means that more crystal nuclei have appeared on the outer surface at this time. After the subsequent cold-drawing and hot-drawing treatments, more holes will appear on the outer surface of the film, which is not dense enough, and then the service life of the membrane filament is short;
[0064] In order to ensure that the molded product has an ideal temperature gradient and outer surface temperature after natural cooling, it is necessary to strictly control the path length during natural cooling and the corresponding atmosphere temperature. In the present invention, the air segment length is 30-1000mm, the air segment temperature is 40-70°C, and the gas in the air segment can be air, preferably an inert gas (such as nitrogen), so that the molded product has an ideal temperature gradient after natural cooling. In addition, it is found that the cooling behavior of the molded product during natural cooling will greatly affect the magnitude and uniformity of the tensile stress on the subsequent membrane filaments, and the tensile stress is an important factor affecting the growth and orientation of the lamellae; if the natural cooling speed is too slow, The polyolefin material maintains a low viscosity for a long time, the tensile stress is reduced, and the crystallization power of the polyolefin material is insufficient, resulting in low crystallinity and crystal orientation of the inner layer of the molded product (i.e., the porous layer of the product); if the natural cooling speed is too fast, although the tensile stress of the fiber becomes larger, the tensile stress is too concentrated, the uniformity of the tensile stress becomes worse, and the crystallinity and crystal orientation of the molded product are also low; the inner surface temperature and outer surface temperature of the molded product of the present invention can be measured by a depth thermal imager, and of course, can also be measured by other methods; the average temperature change gradient of the molded product in the present invention is obtained by (inner surface temperature-outer surface temperature) / thickness of the molded product;
[0065] Then, the molded product is subjected to air-cooling crystallization. In the present application, the air-cooling crystallization is divided into two stages with different cooling rates, that is, the molded product after pre-crystallization will first pass through a rapid cooling zone for rapid cooling, and then quickly enter a slow cooling zone for slow cooling, wherein the cooling rate of the molded product during rapid cooling is not less than 80°C / mm@(100-200)m / min, and the temperature of the outer surface of the molded product after rapid cooling is (Tg+80)-(Tg+120)°C, wherein Tg is the glass transition temperature of the polyolefin raw material. By limiting the cooling rate during rapid cooling and the outer surface temperature after the end of the rapid cooling zone, it is explained that in the rapid cooling zone The temperature of the outer surface of the inner molded product drops rapidly, resulting in a small number of crystal nuclei on the outer surface and a low degree of crystallinity (at low temperatures, the macromolecular chain segments on the outer surface of the molded product have poor mobility and cannot be fully adjusted, resulting in difficult nucleation and incomplete crystallization. Therefore, the faster the cooling rate, the less likely the crystal nuclei will grow, resulting in a small number of crystal nuclei on the outer surface and a low degree of crystallinity); and the number of crystal nuclei is one of the key factors affecting the number of holes. Generally, the fewer the number of crystal nuclei on the outer surface, the fewer the number of holes that appear on the outer surface after the step of cold drawing and hole formation; and since the number of crystal nuclei on the outer surface in the present invention is small,
[0066] Then, after the cold drawing and hole forming step, the number of holes on the outer surface is very small, so that a dense outer surface is finally obtained; if the cooling speed of the outer surface of the molded product is too slow, the macromolecular segments in the outer surface have enough time to move and adjust, resulting in an increase in the crystallinity of the outer surface, and under the action of the drawing stress, its crystal orientation degree will also increase; then, in the stretching and hole forming step, a porous structure will appear on the outer surface and the area near the outer surface, and it will become no longer dense; therefore, it is necessary to control the cooling speed of the outer surface of the molded product in the rapid cooling zone to be no less than 80℃ / mm@(100-200)m / min;
[0067] It should be noted that the cooling rate in this application is not less than 80°C / mm@(100-200)m / min, which means that under the condition that the line speed of the molded product is 100-200m / min, in the cooling path of 1mm, the temperature reduction value is not less than 80°C, so the length of the rapid cooling zone is very short, generally at the millimeter level; in the present invention, the speed of the cooling air flow during the blowing cooling is 30-60m / min, and the temperature of the cooling air flow is 30-70°C, so that the molded product can be quickly cooled in the rapid cooling zone;
[0068] In the rapid cooling zone, the area near the inner surface will cool down and solidify quickly, thus hindering the heat exchange between the rest of the inner area of the molded product (subsequently forming the support layer) and the outside world. Therefore, in the rapid cooling zone, the cooling rate of the inner surface is much lower than that of the outer surface, generally 20-60℃ / m@(100-200)m / min. Such a cooling rate ensures that more crystal nuclei can appear on the inner surface, and further, more crystal nuclei will appear in the rest of the inner area of the molded product (subsequently forming the support layer); after the molded product passes through the rapid cooling zone, it will enter a slow cooling zone (rapid cooling and slow cooling are mainly for the cooling of the outer surface of the molded product, while the cooling rates of the inner surface in the two zones are different Not that big), at this time, the outer surface and its vicinity are basically solidified and the temperature difference with the external environment becomes smaller, so they are slowly cooled down, but the outer surface is basically no longer conducive to the formation and growth of crystal nuclei. Therefore, the outer surface of the membrane filaments finally obtained is still dense and the ratio of the skin thickness to the membrane wall thickness is low (the skin will not be formed too thick); while in the slow cooling zone, the rest of the molded product will still be cooled continuously. By setting the path length of the slow cooling zone to 4-8 meters, as many crystal nuclei as possible are generated in the rest of the molded product, thereby finally obtaining a high-porosity support layer; in the present invention, the specific two-stage air-cooled crystallization can form a sudden temperature change in the wall thickness direction of the molded product, rather than the conventionally recognized gradual temperature gradient. Among them, the temperature of the area near the inner surface of the molded product is lower, while the temperature of the remaining area (the area where the support layer is subsequently formed) is higher and the temperature gradient in the wall thickness direction is smaller; that is, the molded product is divided into two inner and outer areas with relatively uniform temperature distribution. Although the temperature distribution is relatively uniform in each area, the temperature difference between the two areas is large; therefore, the macromolecular chain segments in the remaining areas of the molded product (the areas where the support layer is subsequently formed) are more active, which is convenient for nucleation and crystal growth; it should be noted that in the air-cooled crystallization stage, the molded product cannot be continuously cooled rapidly, otherwise the proportion of the skin thickness to the membrane wall thickness will be too high, or even the entire membrane wall will be cooled rapidly, resulting in low crystallinity of the entire membrane wall. This is also one of the important reasons why this application does not adopt cooling methods such as liquid rapid extraction.
[0069] The fourth step is to perform the first heat setting treatment on the nascent fiber after air cooling crystallization and winding. The first heat setting temperature is (Tm-60)-(Tm-20)℃ and the setting time is 20-40min. The one-time setting process determines the crystallinity, crystal form, orientation and lamella size of the fiber before stretching and hole forming. The one-time setting can eliminate the structural defects in the nascent fiber (similar to annealing treatment), improve the structural integrity of the fiber, and reduce the possibility of excessive concentration of tensile stress in the subsequent stretching and hole forming process.
[0070] Then, cold drawing and hot drawing treatment are carried out. The present application specifically adopts a cold drawing process of less pulling and faster drawing in combination with a hot drawing process of more pulling and slower drawing, so that the support layer has a higher porosity and a better pore structure. The main function of cold drawing is to pull the lamellae apart and form an initial microfiber ligament structure and pore structure; the main function of hot drawing is to further pull the lamellae that have not been pulled apart in the cold drawing stage apart, and to expand the micropores generated in the cold drawing stage; therefore, cold drawing and hot drawing are interrelated and mutually influential processes, and there is a high degree of correlation between the process parameters of the two, rather than two isolated steps. When adjusting the process parameters, the overall process parameters of the two must be uniformly adjusted; for example, the hot drawing rate must be compatible with the cold drawing rate, because different cold drawing rates produce different pore structures, different internal residual stress conditions, different degrees of separation of the lamellae and different structures of the microfiber ligaments, and these conditions will affect the hot drawing rate, therefore, the cold drawing rate or the hot drawing rate cannot be adjusted in isolation.
[0071] Similarly, the hot stretch elongation and cold stretch elongation must also be compatible. The degree of lamellar separation in the inner layer of the fiber, the length and thickness of the microfiber ligaments, etc. are all different under different cold stretch elongations. Correspondingly, the hot stretch elongation also needs to be adjusted based on the fiber structure caused by different cold stretch elongations. When the ratio of the hot stretch elongation to the cold stretch elongation is too small, it indicates excessive cold stretching and / or insufficient hot stretching; when the ratio of the hot stretch elongation to the cold stretch elongation is too large, it indicates insufficient cold stretching and / or excessive hot stretching, both of which may lead to deterioration of the pore structure; finally, a second heat setting is performed, the second heat setting temperature is 10-30°C higher than the first heat setting temperature, and the setting time is 0.5-3min; at this temperature and this treatment time, the residual stress in the stretching pore-forming stage can be well eliminated without destroying the lamellae and pore structure (too high temperature, too long treatment time, etc. are likely to cause melting recrystallization of thin lamellae and microfiber tie structures, thereby causing destruction of the lamellae structure and pore structure; too low temperature is likely to cause fiber shrinkage, resulting in deterioration of the pore structure); finally, a high-porosity hollow fiber membrane is obtained, which has high degassing performance, high mechanical strength and a long service life.
[0072] The present invention also provides a use of a polyolefin hollow fiber membrane for asymmetric degassing, wherein the polyolefin hollow fiber membrane is used to remove oxygen and carbon dioxide from ultrapure water; the O2 permeation rate of the polyolefin hollow fiber membrane is 15-30 L / (min·bar·m 2 ), CO2 permeation rate is 20-35L / (min·bar·m 2 );
[0073] The deoxidation efficiency of the polyolefin hollow fiber membrane is not less than 80%, and the carbon dioxide removal efficiency is not less than 70%; the tensile strength of the polyolefin hollow fiber membrane is not less than 150CN, and the elongation at break is 30-150%.
[0074] The membrane filaments prepared by the present invention can be used for degassing various liquids, and are particularly suitable for degassing high-purity water, and can achieve long-term and efficient degassing.
[0075] Beneficial effects of the present invention: the polyolefin hollow fiber membrane provided by the present invention has a dense outer surface, and the surface energy of the outer surface is 15-40mN / m, so that the hollow fiber membrane has a long service life and is not easily wetted by hydrophilic liquids; there are a number of microfibers on the inner surface for forming a porous structure, the average length of the microfibers is 100-400nm, and the average width is 15-60nm; the length direction of the microfibers is consistent with the length direction of the hollow fiber membrane, and the width direction of the microfibers is consistent with the circumferential direction of the hollow fiber membrane; the inner surface of such a structure ensures that the hollow fiber membrane has a high porosity, thereby having a large degassing (oxygen and carbon dioxide) rate and degassing efficiency, and at the same time the membrane as a whole has large mechanical properties, and is suitable for use as a degassing membrane; in addition, the present invention also provides a melt stretching method to prepare the hollow fiber membrane, which does not contain a diluent, thereby further making the hollow fiber membrane suitable for degassing in ultrapure water; the preparation method is fast and effective, simple to operate, and suitable for large-scale promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 This is a scanning electron microscope (SEM) image of the inner surface of the hollow fiber membrane prepared in Example 1, wherein the magnification is 10000×;
[0077] Figure 2 This is a further enlarged scanning electron microscope (SEM) image of the inner surface of the hollow fiber membrane prepared in Example 1, wherein the magnification is 20000×;
[0078] Figure 3 This is a scanning electron microscope (SEM) image of the outer surface of the hollow fiber membrane prepared in Example 1, wherein the magnification is 10000×;
[0079] Figure 4 This is a further enlarged scanning electron microscope (SEM) image of the outer surface of the hollow fiber membrane prepared in Example 1, wherein the magnification is 20000×;
[0080] Figure 5 Schematic diagram of the device for testing the degassing efficiency of the present invention. DETAILED DESCRIPTION
[0081] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0082] Example 1 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0083] S1. Spinning, melt-extrude polyolefin in a die to form a molded product having an inner surface and an outer surface, wherein the die aspect ratio is 3; the die extrusion temperature is 190° C.; the polyolefin is PP, the PP is homoisotactic PP, the crystallinity of the PP is 55% (measured by DSC method), the isotacticity is 99.9%, and the melt index is 4 g / min@(190° C., 5 kg); the melting point Tm of the PP is 170° C., and the glass transition temperature Tg is -10° C.;
[0084] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 400 mm; the temperature of the air section is 55°C; after pre-crystallization, the outer surface temperature of the molded product is 175°C, and the average temperature change gradient of the molded product after pre-crystallization is 0.062°C / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 183°C);
[0085] S3, air cooling crystallization, air cooling crystallization is performed on the molded product by blowing cooling, the air cooling crystallization includes a rapid cooling zone and a slow cooling zone, the molded product passes through the rapid cooling zone and the slow cooling zone in sequence and then is rolled up to obtain nascent fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 90°C; and in the rapid cooling zone, the cooling air flow speed is 50m / min, and the cooling air flow temperature is 45°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@150m / min, and the cooling speed of the inner surface of the molded product is controlled to be 40°C / m@150m / min; and the path length of the slow cooling zone is 6m;
[0086] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 130° C., and the setting time is 30 minutes;
[0087] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 40° C., the cold drawing elongation is 30%, and the cold drawing rate is 20% / min;
[0088] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 125° C., the hot drawing elongation is 100%, and the hot drawing rate is 2% / min;
[0089] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0090] The second heat setting temperature is 155°C and the setting time is 2 minutes.
[0091] Example 2 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0092] S1, spinning, melt-extrude polyolefin in a die to form a molded product with an inner surface and an outer surface, wherein the die aspect ratio is 5; the die extrusion temperature is 205°C; the polyolefin is PP, the PP is homopolymer isotactic PP, the crystallinity of the PP is 65% (measured by DSC method), the isotacticity is 99.9%, and the melt index is 2g / min@(190°C, 5kg); the melting point Tm of the PP is 170°C, and the glass transition temperature Tg is -10°C;
[0093] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 600 mm; the temperature of the air section is 65°C; after pre-crystallization, the outer surface temperature of the molded product is 185°C, and the average temperature change gradient of the molded product after pre-crystallization is 0.067°C / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 198°C);
[0094] S3, air-cooling crystallization, air-cooling crystallization is performed on the molded product by means of air-blowing cooling, and the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, and the molded product is successively passed through the rapid cooling zone and the slow cooling zone before being rolled up to obtain nascent fibers; wherein, the outer surface temperature of the molded product drops to 100°C after passing through the rapid cooling zone; and in the rapid cooling zone, the speed of the cooling airflow is 30m / min, and the temperature of the cooling airflow is 70°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@120m / min, and the cooling speed of the inner surface of the molded product is controlled to be 25°C / m@120m / min; and the path length of the slow cooling zone is 8m;
[0095] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 140° C., and the setting time is 25 minutes;
[0096] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 50° C., the cold drawing elongation is 35%, and the cold drawing rate is 18% / min;
[0097] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 135° C., the hot drawing elongation is 140%, and the hot drawing rate is 1.8% / min;
[0098] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0099] The second heat setting temperature is 165°C and the setting time is 1.5 minutes.
[0100] Example 3 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0101] S1, spinning, melt-extrude polyolefin in a die to form a molded product with an inner surface and an outer surface, wherein the die aspect ratio is 4; the die extrusion temperature is 200°C; the polyolefin is PP, the PP is homoisotactic PP, the crystallinity of the PP is 60% (measured by DSC method), the isotacticity is 99.9%, and the melt index is 3g / min@(190°C, 5kg); the melting point Tm of the PP is 170°C, and the glass transition temperature Tg is -10°C;
[0102] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 500 mm; the temperature of the air section is 60°C; after pre-crystallization, the outer surface temperature of the molded product is 180°C, and the average temperature change gradient of the molded product after pre-crystallization is 0.070°C / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 192°C);
[0103] S3, air-cooling crystallization, air-cooling crystallization is performed on the molded product by means of air-blowing cooling, and the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, and the molded product is successively passed through the rapid cooling zone and the slow cooling zone before being rolled up to obtain nascent fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 95°C; and in the rapid cooling zone, the cooling air flow speed is 35m / min, and the cooling air flow temperature is 65°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@130m / min, and the cooling speed of the inner surface of the molded product is controlled to be 30°C / m@130m / min; and the path length of the slow cooling zone is 7m;
[0104] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 145° C., and the setting time is 20 minutes;
[0105] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 60° C., the cold drawing elongation is 40%, and the cold drawing rate is 14% / min;
[0106] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 140° C., the hot drawing elongation is 120%, and the hot drawing rate is 1.2% / min;
[0107] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0108] The second heat setting temperature is 180°C and the setting time is 1 minute.
[0109] Example 4 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0110] S1, spinning, melt-extrude polyolefin in a die to form a molded product with an inner surface and an outer surface, wherein the die aspect ratio is 3; the die extrusion temperature is 195°C; the polyolefin is PP, the PP is homopolymer isotactic PP, the crystallinity of the PP is 50% (measured by DSC method), the isotacticity is 99.9%, and the melt index is 5g / min@(190°C, 5kg); the melting point Tm of the PP is 170°C, and the glass transition temperature Tg is -10°C;
[0111] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 300 mm; the temperature of the air section is 50°C; after pre-crystallization, the outer surface temperature of the molded product is 178°C, and the average temperature change gradient of the molded product after pre-crystallization is 0.068°C / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 188°C);
[0112] S3, air-cooling crystallization, air-cooling crystallization is performed on the molded product by means of air-blowing cooling, and the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, and the molded product is successively passed through the rapid cooling zone and the slow cooling zone before being rolled up to obtain spun fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 85°C; and in the rapid cooling zone, the cooling air flow speed is 40m / min, and the cooling air flow temperature is 60°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@140m / min, and the cooling speed of the inner surface of the molded product is controlled to be 35°C / m@140m / min; and the path length of the slow cooling zone is 6.5m;
[0113] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 125°C, and the setting time is 35 minutes;
[0114] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 25° C., the cold drawing elongation is 28%, and the cold drawing rate is 22% / min;
[0115] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 130° C., the hot drawing elongation is 120%, and the hot drawing rate is 2.2% / min;
[0116] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0117] The second heat setting temperature is 145°C and the setting time is 2.5 minutes.
[0118] Example 5 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0119] S1, spinning, melt-extrude polyolefin in a die to form a molded product with an inner surface and an outer surface, wherein the die aspect ratio is 2; the die extrusion temperature is 185°C; the polyolefin is PP, the PP is homoisotactic PP, the crystallinity of the PP is 48% (measured by DSC method), the isotacticity is 99.9%, and the melt index is 6g / min@(190°C, 5kg); the melting point Tm of the PP is 170°C, and the glass transition temperature Tg is -10°C;
[0120] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 200 mm; the temperature of the air section is 48°C; after pre-crystallization, the outer surface temperature of the molded product is 174°C, and the average temperature change gradient of the molded product after pre-crystallization is 0.054°C / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 182°C);
[0121] S3, air-cooling crystallization, air-cooling crystallization is performed on the molded product by means of air-blowing cooling, and the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, and the molded product is successively passed through the rapid cooling zone and the slow cooling zone before being rolled up to obtain nascent fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 80°C; and in the rapid cooling zone, the cooling air flow speed is 52m / min, and the cooling air flow temperature is 43°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@160m / min, and the cooling speed of the inner surface of the molded product is controlled to be 45°C / m@160m / min; and the path length of the slow cooling zone is 5.5m;
[0122] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 120° C., and the setting time is 40 minutes;
[0123] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 30° C., the cold drawing elongation is 24%, and the cold drawing rate is 24% / min;
[0124] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 120° C., the hot drawing elongation is 150%, and the hot drawing rate is 2% / min;
[0125] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0126] The second heat setting temperature is 140°C and the setting time is 3 minutes.
[0127] Example 6 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0128] S1, spinning, melt-extrude polyolefin in a die to form a molded product with an inner surface and an outer surface, wherein the die aspect ratio is 2; the die extrusion temperature is 180°C; the polyolefin is PP, the PP is homopolymer isotactic PP, the crystallinity of the PP is 44% (measured by DSC method), the isotacticity is 99.9%, and the melt index is 7g / min@(190°C, 5kg); the melting point Tm of the PP is 170°C, and the glass transition temperature Tg is -10°C;
[0129] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 80 mm; the temperature of the air section is 45°C; after pre-crystallization, the outer surface temperature of the molded product is 172°C, and the average temperature change gradient of the molded product after pre-crystallization is 0.050°C / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 177°C);
[0130] S3, air cooling crystallization, the molded product is air cooled and crystallized by blowing air cooling, the air cooling crystallization includes a rapid cooling zone and a slow cooling zone, the molded product passes through the rapid cooling zone and the slow cooling zone in sequence and then is rolled up to obtain nascent fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 75°C; and in the rapid cooling zone, the cooling air flow speed is 55m / min, and the cooling air flow temperature is 40°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@180m / min, and the cooling speed of the inner surface of the molded product is controlled to be 50°C / m@180m / min; and the path length of the slow cooling zone is 5m;
[0131] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 135° C., and the setting time is 32 minutes;
[0132] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 35° C., the cold drawing elongation is 20%, and the cold drawing rate is 28% / min;
[0133] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 115° C., the hot drawing elongation is 100%, and the hot drawing rate is 2% / min;
[0134] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0135] The second heat setting temperature is 150°C and the setting time is 2 minutes.
[0136] Example 7 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0137] S1, spinning, melt-extrude polyolefin in a die to form a molded product with an inner surface and an outer surface, wherein the die aspect ratio is 3; the die extrusion temperature is 140°C; the polyolefin material is PE, and more preferably, commercially available mLLDPE (metallocene linear low-density polyethylene) is used, the crystallinity of the mLLDPE is 50% (measured by DSC method), and the melt index is 4g / min@(140°C, 5kg); in addition, the melting point Tm of the mLLDPE is about 120°C, and the glass transition temperature Tg is about -40°C;
[0138] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 350 mm; the temperature of the air section is 50° C.; after pre-crystallization, the outer surface temperature of the molded product is 125° C., and the average temperature change gradient of the molded product after pre-crystallization is 0.069° C. / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 134° C.);
[0139] S3, air-cooling crystallization, air-cooling crystallization is performed on the molded product by means of air-blowing cooling, and the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, and the molded product is successively passed through the rapid cooling zone and the slow cooling zone before being rolled up to obtain nascent fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 45°C; and in the rapid cooling zone, the cooling air flow speed is 45m / min, and the cooling air flow temperature is 55°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@150m / min, and the cooling speed of the inner surface of the molded product is controlled to be 30°C / m@150m / min; and the path length of the slow cooling zone is 6m;
[0140] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 80° C., and the setting time is 35 minutes;
[0141] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 20° C., the cold drawing elongation is 30%, and the cold drawing rate is 20% / min;
[0142] S6, hot-drawing and hole-expanding, hot-drawing and hole-expanding the cold-drawn semi-finished product to obtain a hot-drawn semi-finished product; wherein the hot-drawing temperature is 75° C., the hot-drawing elongation is 100%, and the hot-drawing rate is 2% / min;
[0143] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0144] The second heat setting temperature is 100°C and the setting time is 2 minutes.
[0145] Example 8 A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing:
[0146] S1, spinning, melt-extrude polyolefin in a die head to form a molded product with an inner surface and an outer surface, wherein the die head aspect ratio is 4; the die head extrusion temperature is 265°C; in this embodiment, the polyolefin material is PMP, the crystallinity of the PMP is 55% (measured by DSC method), and the melt index is 3g / min@(260°C, 5kg); the melting point Tm of the PMP is about 240°C, and the glass transition temperature Tg is about 30°C;
[0147] S2, pre-crystallization, placing the molded product in an air section (under a nitrogen atmosphere) for pre-crystallization; wherein the length of the air section is 450 mm, and the temperature of the air section is 60° C.; after pre-crystallization, the outer surface temperature of the molded product is 245° C., and the average temperature change gradient of the molded product after pre-crystallization is 0.085° C. / 1um; the inner surface temperature is higher than the outer surface temperature (the inner surface temperature is 256° C.);
[0148] S3, air-cooling crystallization, air-cooling crystallization is performed on the molded product by means of air-blowing cooling, and the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, and the molded product is successively passed through the rapid cooling zone and the slow cooling zone before being rolled up to obtain nascent fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to 155°C; and in the rapid cooling zone, the cooling air flow speed is 50m / min, and the cooling air flow temperature is 40°C, so that the cooling speed of the outer surface of the molded product is not less than 80°C / mm@150m / min, and the cooling speed of the inner surface of the molded product is controlled to be 46°C / m@150m / min; and the path length of the slow cooling zone is 6m;
[0149] S4, primary setting, subjecting the raw fiber to a first heat setting treatment to obtain a heat-set semi-finished product; the first heat setting temperature is 200°C, and the setting time is 25 minutes;
[0150] S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; wherein the cold drawing temperature is 80° C., the cold drawing elongation is 30%, and the cold drawing rate is 20% / min;
[0151] S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; wherein the hot drawing temperature is 200° C., the hot drawing elongation is 100%, and the hot drawing rate is 1.5% / min;
[0152] S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane; wherein
[0153] The second heat setting temperature is 220°C and the setting time is 2.5 minutes.
[0154] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is mainly that in step S3, the molded product is cooled rapidly by liquid cooling; that is, step S3 of Comparative Example 1 includes the following process steps:
[0155] S3, liquid cooling crystallization, in this step, the cooling medium is deionized water, the temperature of the deionized water is 40°C, and the cooling path length is 1m. After the liquid cooling is completed, the fiber enters a 70°C oven for drying, and the nascent fiber is obtained after winding; it should be noted that, due to the need to be applied to the degassing treatment of deionized water, in order to prevent the influence of solvent residues on the quality of ultrapure water, the cooling medium can only be deionized water or ultrapure water. Comparative Example 2 The main difference between Comparative Example 2 and Example 1 is that in step S3, by limiting the process parameters, the cooling rate of the fiber in the rapid cooling zone is controlled to be lower than 80°C / mm@
[0156] (150m / min); That is, step S3 of comparative example 2 includes the following process steps: further cooling the molded product by blowing cooling to make the molded product undergo cooling crystallization. In this step, the speed of the cooling airflow is 10m / min, the temperature of the cooling airflow is 90°C, and after the molded product passes through the rapid cooling zone, the outer surface is cooled to about 130°C, and then passes through the slow cooling zone with a path length of 6m, and is rolled up, and the winding speed is 150m / min;
[0157] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that in step S3, the fiber is not cooled by air blowing, but continues to be cooled by air cooling;
[0158] That is, step S3 of comparative example 3 includes the following process steps: further cooling the fiber by natural cooling, the natural cooling path length is controlled to be 6 m, and the temperature of the surrounding atmosphere is controlled to be 55° C.,
[0159] Conduct structural and performance tests on samples
[0160] 1. Structural characterization: The main structure of the membrane of each sample was characterized by scanning electron microscopy (Hitachi S-5500), and then the required data was obtained; the specific results are shown in the following table
[0161] Sample Inner diameter / μm Overall film thickness / μm Volume porosity / % Overall crystallinity of the film / % Example 1 200 50 40 44 Example 2 200 54 44 50 Example 3 200 56 46 47 Example 4 200 52 42 40 Example 5 200 48 36 38 Example 6 200 42 34 35 Example 7 180 50 38 42 Example 8 220 50 44 46 Comparative Example 1 200 50 9 10 Comparative Example 2 200 50 48 46 Comparative Example 3 200 50 55 50
[0162] It can be seen from the above table that the hollow fiber membranes prepared in Examples 1-8 have high porosity.
[0163]
[0164] It can be seen from the above table that: the hollow fibers prepared in Examples 1-8 have an ideal membrane structure, a thin and dense cortex, and a thick and porous support layer, thereby ensuring that the membrane filaments can be degassed efficiently for a long time; and for Example 1, the cortex thickness is too large due to the rapid cooling rate during the crystallization process; and for Examples 2 and 3, the cooling rate during the crystallization process is too slow, so there is no cortex, and the whole structure is porous.
[0165]
[0166]
[0167] It can be seen from the above table that an ideal microfiber structure exists on the inner surface of the hollow fiber membranes prepared in Examples 1-8 of the present invention, thereby ensuring that the membrane fibers as a whole have high mechanical properties and a high degassing rate.
[0168]
[0169] Examples 1-8 all have ideal air permeable areas and lamellar crystal areas; however, the air permeable area of comparative example 1 is too small, resulting in inefficient degassing; and the air permeable areas of comparative examples 2 and 3 are too large, resulting in very poor mechanical properties of the membrane filaments.
[0170] 2. Performance Test
[0171] 2.1 Tensile strength and elongation at break test: Use a stretching machine to uniformly stretch each sample at room temperature (stretching speed is 50 mm / min, the distance between the upper and lower clamps is 30 mm) until it breaks, so as to measure the tensile strength and elongation at break. Repeat 3 times and take the average value; the average value is the final tensile strength and elongation at break of the film;
[0172] After testing, the tensile strength of the hollow fiber membranes prepared in Examples 1-8 is not less than 150CN, and the elongation at break is 30-150%, that is, they all have large tensile strength and elongation at break, which can meet industrial requirements;
[0173] 2.2 The hollow fiber membranes prepared in Examples 1 to 8 and Comparative Examples 1-3 were tested for gas permeability. The test method was as follows: at a temperature of 25°C, a pressure of 0.1 bar, and a membrane sample area of 0.1 square meters, one side of the membrane sample was subjected to the gas to be tested (oxygen, carbon dioxide); the gas to be tested was supplied into the inner cavity of the hollow fiber membrane; the volume flow rate of the gas passing through the sample membrane wall was measured with a flow meter (Japan KOFLOC / 4800); the test was performed 3 times from the inside of the membrane to the outside of the membrane, and 3 times from the outside of the membrane to the inside of the membrane, and then the average value was taken, which was the gas permeability of the membrane. Gas permeability unit: L / min2.3 Deoxygenation efficiency, using the hollow fiber membranes prepared in each example or comparative example as raw material, assembled into a membrane area of 0.65m 2 The components are connected with the dissolved oxygen meter, water circuit and components for testing. The water circuit is used to transport the degassed liquid, the components are used to degas the degassed liquid, and the dissolved oxygen meter is used to detect the oxygen content of the degassed liquid after degassing. The degassed liquid is deionized water and the temperature of the degassed liquid is 25°C. The inside of the membrane is vacuum purged. (For example, Figure 5 (shown)
[0174] Step 1: Detect the initial oxygen content of the degassed liquid. Pump the degassed liquid into the water circuit. At this time, turn off the vacuum equipment to make the inner side of the membrane at normal pressure. The degassed liquid passes through the assembly (without degassing) and then the dissolved oxygen meter. Keep the flow rate of the degassed liquid into the dissolved oxygen meter at about 1.8 GLH. Observe the changes in the dissolved oxygen reading on the dissolved oxygen meter in real time. After the reading of the dissolved oxygen meter stabilizes (the reading of the dissolved oxygen meter changes by less than 1% within 5 minutes), read the dissolved oxygen reading on the dissolved oxygen meter. 始 .
[0175] Step 2: Detect the final oxygen content of the degassed liquid after degassing. On the basis of step 1, turn on the vacuum equipment to vacuum purge the inner layer of the membrane to degas the degassed liquid. During the vacuum purge, keep the vacuum reading at -0.094MPa (50torr). Observe the changes in the dissolved oxygen reading on the dissolved oxygen meter in real time. When the reading of the dissolved oxygen meter stabilizes (the reading of the dissolved oxygen meter changes by less than 1% within 5 minutes), the degassing is considered to have reached equilibrium. Read the dissolved oxygen reading on the dissolved oxygen meter. 终 The deoxidation efficiency is calculated by the following formula:
[0176] 2.4 Water vapor transmission rate
[0177] On the basis of test method 2.3, after degassing begins, run the system for 5 hours and record the mass m2 of ultrapure water entering within 5 hours. After the operation is completed, collect the condensed water in the vacuum equipment and measure the mass m1 of the condensed water. Calculate the water vapor transmission rate according to the following formula:
[0178] After testing, the water vapor permeability of the hollow fiber membranes prepared in Examples 1-8 does not exceed 5‰, that is, after removing 1kg of pure water, the condensed water produced in the vacuum test does not exceed 5g.
[0179] 2.5 Acid damage sensitivity
[0180] On the basis of test method 2.3, the degassing liquid was replaced with a hydrochloric acid solution with a concentration of 5 mol / L. The condition of the component was observed every 4 hours. When leakage occurred on the inner side of the membrane, the component was considered to be breached and lost its degassing ability. The time when the component was breached was recorded.
[0181] 2.6 Alkali damage sensitivity
[0182] On the basis of test method 2.3, the degassing liquid was replaced with a sodium hydroxide solution with a concentration of 5 mol / L. The condition of the component was observed every 4 hours. When leakage occurred on the inner side of the membrane, the component was considered to be breached and lost its degassing ability. The time when the component was breached was recorded.
[0183] 2.7 Resistance to wetting damage sensitivity
[0184] On the basis of test method 2.3, the degassing liquid was replaced with 100% n-butanol (surface tension of 24.6 dynes), and the component was observed every 4 hours. When leakage occurred on the inner side of the membrane, the component was considered to be breached and lost its degassing ability. The time when the component was breached was recorded.
[0185]
[0186] It can be seen from the above table that the hollow fiber membranes prepared in Examples 1-8 of the present invention all have degassing rate and degassing efficiency, and have a long service life, while the degassing efficiency and degassing rate of Comparative Example 1 are both low, and the service life of Comparative Examples 2 and 3 is short.
[0187] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A polyolefin hollow fiber membrane for asymmetric degassing, comprising a main body, one side of the main body is an inner surface facing the inner cavity, and the other side is an outer surface, and the main body has a non-directional tortuous passage, characterized in that: The inner surface has a plurality of microfibers for forming a porous structure, wherein the average length of the microfibers is 100-400 nm and the average width is 15-60 nm; The length direction of the microfiber is consistent with the length direction of the hollow fiber membrane, and the width direction of the microfiber is consistent with the circumferential direction of the hollow fiber membrane; The surface energy of the outer surface is 15-40 mN / m, and the outer surface is a dense surface; The dense surface has a pore area ratio of no more than 5% at 50,000 times magnification; In the circumferential direction of the hollow fiber membrane, the average spacing between adjacent microfibers is 20-80 nm.
2. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 1, characterized in that: The difference between the maximum length and the minimum length of the microfiber does not exceed 350 nm; The difference between the maximum width and the minimum width of the microfiber does not exceed 70nm; The average length of the microfibers is 4-10 times the average width of the microfibers.
3. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 1, characterized in that: The average length of the microfibers is 2-8 times the average spacing between adjacent microfibers in the circumferential direction of the membrane; The average width of the microfibers is 50%-95% of the average spacing between adjacent microfibers in the circumferential direction of the membrane; and the hole area ratio of the inner surface is 10-35%.
4. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 1, characterized in that: In the circumferential direction of the membrane, a plurality of microfibers are regularly arranged to form a breathable area for ventilation; the breathable area is in the shape of a long strip; The average length of the permeable zone is 400-1100 nm, and the average length of the permeable zone is greater than the average width of the permeable zone; The length direction of the air permeable zone is consistent with the circumferential direction of the hollow fiber membrane; the width direction of the air permeable zone is consistent with the length direction of the hollow fiber membrane.
5. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 4, characterized in that: In the length direction of the hollow fiber membrane, a lamellar region of a solid structure is formed between adjacent permeable regions; the average width of the lamellar region is 80-280nm; The average width of the lamellar region is 0.3-1.5 times the average width of the air permeable region; The width direction of the lamellar crystal region is consistent with the length direction of the hollow fiber membrane.
6. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 4, characterized in that: The average length of the breathable zone is 2-5 times the average width of the breathable zone; the hole area ratio in the breathable zone is 30-70%, and the hole area ratio of the breathable zone is 20-50% higher than the overall hole area ratio of the inner surface.
7. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 1, characterized in that: The main body includes a skin layer and a support layer, one side of the support layer is an inner surface, one side of the skin layer is an outer surface, the thickness of the skin layer is 0.5-4μm, and the thickness of the skin layer accounts for 1-8% of the overall thickness of the membrane; the porosity of the skin layer is not higher than 10%.
8. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 7, characterized in that: The thickness of the support layer is 38-58 μm, and the support layer is at least 35 μm thicker than the skin layer; The porosity of the support layer is 40-70%; The average pore size in the support layer gradually decreases from the area close to the inner surface to the area close to the skin layer.
9. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 7, characterized in that: The average pore size variation gradient of the support layer is 1.5-4 nm / μm; the support layer contains porous fibers for forming a porous structure, and the average diameter of the porous fibers is 60-300 nm.
10. The polyolefin hollow fiber membrane for asymmetric degassing according to claim 1, characterized in that: The hollow fiber membrane has a thickness of 40-60 μm, a porosity of 30-50%, and an inner diameter of 175-225 μm; The overall crystallinity of the hollow fiber membrane is 30-55%; The membrane-forming material of the hollow fiber membrane is at least one of PP, PE and PMP.
11. A method for preparing a polyolefin hollow fiber membrane for asymmetric degassing according to any one of claims 1 to 10, characterized in that: The following steps are involved: S1, spinning, melt-extrude polyolefin in a die head to form a molded product having an inner surface and an outer surface; the polyolefin is at least one of PP, PE and PMP; S2, pre-crystallization, placing the molded product in an air section for pre-crystallization; the melting point of the polyolefin material is Tm, the outer surface temperature of the molded product after pre-crystallization is Tm-(Tm+15)°C, the temperature of the inner surface is greater than the temperature of the outer surface, and the average temperature change gradient of the molded product after pre-crystallization is 0.01-0.2°C / 1um; S3, air-cooling crystallization, air-cooling crystallization of the molded product obtained in step S2 by means of air-blowing cooling, the air-cooling crystallization includes a rapid cooling zone and a slow cooling zone, the molded product is successively passed through the rapid cooling zone and the slow cooling zone and then rolled up to obtain spun fibers; wherein, after the molded product passes through the rapid cooling zone, the outer surface temperature drops to (Tg+80)-(Tg+120)°C; and in the rapid cooling zone, the cooling rate of the outer surface of the molded product is not less than 80°C / mm@(100-200)m / min, and the cooling rate of the inner surface of the molded product is 20-60°C / m@(100-200)m / min; S4, primary shaping, subjecting the spun fiber to a first heat-setting treatment to obtain a heat-set semi-finished product; S5, cold drawing to form holes, cold drawing the heat-set semi-finished product to obtain a cold-drawn semi-finished product; S6, hot drawing and hole expansion, hot drawing and hole expansion of the cold drawn semi-finished product to obtain a hot drawn semi-finished product; S7, secondary shaping, subjecting the hot-drawn semi-finished product to a second heat shaping treatment to obtain a hollow fiber membrane.
12. The method for preparing a polyolefin hollow fiber membrane for asymmetric degassing according to claim 11, characterized in that: The melt index of the polyolefin in S1 is 1-7 g / min@(Tm+20°C, 5kg); the crystallinity of the polyolefin is 40-70%; The die aspect ratio in S1 is 2-5; the die temperature is (Tm+10)-(Tm+40)°C.
13. The method for preparing a polyolefin hollow fiber membrane for asymmetric degassing according to claim 11, characterized in that: The length of the air section in S2 is 30-1000 mm; the temperature of the air section is 40-70° C.; During the air blowing cooling in S3, the speed of the cooling air flow is 30-60m / min, and the temperature of the cooling air flow is 30-70℃. The path length of the slow cooling zone is 4-8m.
14. The method for preparing a polyolefin hollow fiber membrane for asymmetric degassing according to claim 11, characterized in that: The cold drawing temperature in S5 is (Tg+30)-(Tg+80)°C, the cold drawing elongation is 20-40%, and the cold drawing rate is (10-30)% / min; The hot drawing temperature described in S6 is (Tm-60)-(Tm-30)°C, the hot drawing elongation is 2-6 times the cold drawing elongation, and the hot drawing rate is not higher than 15% of the cold drawing rate.
15. The method for preparing a polyolefin hollow fiber membrane for asymmetric degassing according to claim 11, characterized in that: The first heat setting temperature in S4 is (Tm-60)-(Tm-20)℃, and the setting time is 20-40min; In S7, the second heat setting temperature is 10-30°C higher than the first heat setting temperature, and the setting time is 0.5-3min.
16. Use of a polyolefin hollow fiber membrane for asymmetric degassing according to any one of claims 1 to 10, characterized in that: The polyolefin hollow fiber membrane is used to remove oxygen and carbon dioxide from ultrapure water; The O2 permeation rate of the polyolefin hollow fiber membrane is 15-30 L / (min· bar· m 2 ), CO2 permeation rate is 20-35L / (min·bar·m 2 ); The deoxygenation efficiency of the polyolefin hollow fiber membrane is not less than 80%, and the carbon dioxide removal efficiency is not less than 70%; the tensile strength of the polyolefin hollow fiber membrane is not less than 150CN, and the elongation at break is 30-150%.
Citation Information
Patent Citations
Degassing liquids, apparatus and method
CN1090042C
Process for preparing microporous film
US3558764A
Porous polypropylene hollow filaments and method making the same
US4055696A
Heterogeneous membrane and process for production thereof
US4664681A
Integrally asymmetrical polyolefin membrane for gas exchange
US6409921B1