Packaging structure and fabrication method for bare copper bonding wire

By forming a layer of metal solder paste and creating solder balls on the bare copper area of ​​the leadframe, the problem of electrical connection between small-sized chips and the leadframe is solved, resulting in shorter solder wire lengths and stronger solder bonding, while reducing the risk of solder wire tipping.

CN115172174BActive Publication Date: 2026-11-17JCET SEMICON (SUQIAN) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210864628.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-21
Publication Date
2026-11-17
Estimated Expiration
2042-07-21

AI Technical Summary

Technical Problem

Existing technologies cannot effectively achieve electrical connections between the bare copper area of ​​small-sized chips or pads and the lead frame, and existing soldering processes have problems such as long wire lengths, difficulty in wire bonding, and high risk of wire tipping.

Method used

A metal solder paste layer is formed on the upper surface of the bare copper area of ​​the lead frame, and solder balls are made in a semi-molten state. The solder balls and the metal solder paste layer form a eutectic structure, and electrical connection is achieved by connecting the solder balls with the bonding wires between the chip pads and pins.

Benefits of technology

It reduces the length of the welding wire, enhances the welding bond strength, reduces the risk of the welding wire tipping over, and improves the reliability and stability of the welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172174B_ABST
    Figure CN115172174B_ABST
Patent Text Reader

Abstract

This invention discloses a packaging structure and its fabrication method for implementing bare copper area bonding wires. The fabrication method includes the following steps: providing a lead frame and at least one chip; forming a solder layer on the upper surface of the pins; forming a metal solder paste layer in a portion of the bare copper area on the lead frame surface; mounting the chip on the upper surface of the bare copper area; heating the metal solder paste layer to a semi-molten state; when the metal solder paste layer is in a semi-molten state, fabricating at least a first solder ball and a second solder ball on the upper surface of the metal solder paste layer, so that the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer; electrically connecting the first solder ball and the pad through a first bonding wire, and electrically connecting the second solder ball and the solder layer through a second bonding wire; the chip is electrically connected to the pins in sequence through the first bonding wire, the metal solder paste layer, and the second bonding wire, thereby shortening the bonding wire length and enhancing the stability of the packaging structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor packaging technology, and in particular to a packaging structure for implementing bare copper bonding wires and its fabrication method. Background Technology

[0002] As a chip carrier for integrated circuits, the lead frame is a key structural component that uses bonding wires to achieve electrical connection between the internal circuit leads of the chip and the external leads, forming an electrical circuit. It acts as a bridge connecting to external wires. Most semiconductor integrated circuits require the use of lead frames, making it an important basic material in the electronics and information industry.

[0003] There are two existing leadframe soldering technologies: one is aluminum wire or aluminum strip soldering, which can achieve electrical connection between the chip and the bare copper surface on the leadframe. However, due to the large size of aluminum wire / aluminum strip, this soldering technology is limited to chips with large pads and large bare copper areas. For small chips or chips with small pads, effective soldering cannot be achieved using aluminum wire or aluminum strip soldering. The second is gold-copper wire soldering, which can be used to solder chips with small pads. However, it can only achieve direct interconnection between the chip and silver-plated pins, and cannot solder wires in the bare copper area. Furthermore, the wire length from the chip lead bonding to the pin is relatively long, making wire bonding difficult, and it is prone to the risk of wire tilting or sinking during subsequent packaging processes. Summary of the Invention

[0004] The purpose of this invention is to provide a packaging structure for bonding wires in bare copper areas and a method for manufacturing the same.

[0005] To achieve one of the above-mentioned objectives, one embodiment of the present invention provides a method for fabricating a bare copper area bonding wire package structure, the method comprising the following steps:

[0006] A lead frame is provided, the lead frame including at least one base island and pins distributed around the base island, the surface of the base island being a bare copper area;

[0007] A weld layer is formed on the upper surface of the pin;

[0008] A metal solder paste layer is formed in a portion of the upper surface of the bare copper area;

[0009] Provide at least one chip and mount the chip above the bare copper area;

[0010] Heating causes the metal solder paste layer to be in a semi-molten state. When the metal solder paste layer is in a semi-molten state, at least a first solder ball and a second solder ball are made on the upper surface of the metal solder paste layer, so that the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer.

[0011] The first solder ball and the pad on the upper surface of the chip are electrically connected by a first bonding wire, and the second solder ball and the solder layer are electrically connected by a second bonding wire. The chip is electrically connected to the pin in sequence through the first bonding wire, the metal solder paste layer and the second bonding wire.

[0012] As a further improvement of one embodiment of the present invention, the formation of a metal solder paste layer in a partial area on the upper surface of the bare copper area specifically includes:

[0013] A solder paste layer with a thickness of 5-25 μm is formed on a portion of the upper surface of the bare copper area by printing / dot / laser spraying to create the metal solder paste layer.

[0014] As a further improvement of one embodiment of the present invention, the heating causes the metal solder paste layer to be in a semi-molten state. When the metal solder paste layer is in a semi-molten state, at least a first solder ball and a second solder ball are formed on the upper surface of the metal solder paste layer, so that the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer, specifically including:

[0015] Set the welding temperature so that the metal solder paste layer is in a semi-molten state;

[0016] The reserved solder lines of the wedge are melted in a portion of the upper surface of the metal solder paste layer to form a first solder ball and a second solder ball. At the welding temperature, the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer. The upper surface of the first solder ball and the second solder ball is higher than the upper surface of the metal solder paste layer.

[0017] The welding wire connecting the first solder ball and the second solder ball is cut using the cutting tool.

[0018] As a further improvement of one embodiment of the present invention, the step of forming a welding layer on the surface of the pin specifically includes:

[0019] A silver plating layer is formed on the upper surface of the pin using an electroplating process.

[0020] As a further improvement of one embodiment of the present invention, the step of forming a welding layer on the surface of the pin specifically includes:

[0021] Using printing / dot / laser processes, solder paste is sprayed onto the upper surface of the pin to form another layer of metal solder paste.

[0022] As a further improvement to one embodiment of the present invention, the step of electrically connecting the first solder ball and the pad on the upper surface of the chip via a first bonding wire, and electrically connecting the second solder ball and the pin via a second bonding wire, specifically includes:

[0023] The cutter is controlled to deliver the first bonding wire to the solder pad to melt and form a third solder ball, and the first bonding wire is wire-bonded to the first solder ball;

[0024] The control cutter delivers the second bonding wire to the silver plating layer to melt and form a fourth solder ball, and then wirebonds the second bonding wire to the second solder ball.

[0025] As a further improvement to one embodiment of the present invention, the step of electrically connecting the first solder ball and the pad on the upper surface of the chip via a first bonding wire, and electrically connecting the second solder ball and the pin via a second bonding wire, specifically includes:

[0026] The cutter is controlled to deliver the first bonding wire to the solder pad to melt and form a third solder ball, and the first bonding wire is wire-bonded to the first solder ball;

[0027] The cutting tool is controlled to deliver the second welding wire to melt on the other metal solder paste layer to form a fourth solder ball. At the welding temperature, the bottom surface and part of the side surface of the fourth solder ball form a eutectic structure with the other metal solder paste layer, and the upper surface of the fourth solder ball is higher than the upper surface of the other metal solder paste layer.

[0028] The cutting tool is controlled to bond the second wire lead to the second solder ball.

[0029] This invention provides a packaging structure for bonding wires in bare copper areas, which is fabricated using the method for fabricating a packaging structure for bonding wires in bare copper areas as described in any of the above embodiments.

[0030] This invention provides a packaging structure for bonding wires in a bare copper area, including a lead frame and at least one chip. The lead frame includes at least one base island and pins distributed around the base island. A bare copper area is formed on the surface of the base island. The chip is disposed above the bare copper area. At least one solder pad is formed on the upper surface of the chip, and a solder layer is formed on the upper surface of the pins.

[0031] A metal solder paste layer is also provided on a portion of the upper surface of the bare copper area. At least a first solder ball and a second solder ball are provided on the upper surface of the metal solder paste layer. The bottom surface and part of the side surface of the first solder ball and the second solder ball are disposed in the metal solder paste layer and form a eutectic structure with the metal solder paste layer.

[0032] The first solder ball is connected to the solder pad via a first solder wire, and the second solder ball is connected to the solder layer via a second solder wire. The chip is electrically connected to the pin via the first solder wire, the metal solder paste layer, and the second solder wire in sequence.

[0033] As a further improvement of one embodiment of the present invention, the upper surfaces of the first solder ball and the second solder ball are higher than the upper surface of the metal solder paste layer.

[0034] As a further improvement of one embodiment of the present invention, the thickness of the metal solder paste layer is 5 to 25 μm.

[0035] As a further improvement of one embodiment of the present invention, the first bonding wire has a third solder ball formed at one end connected to the solder pad, and the other end is connected to the first solder ball.

[0036] As a further improvement of one embodiment of the present invention, the welding layer is a silver-plated layer, and the second solder ball is connected to the silver-plated layer by a second solder wire.

[0037] As a further improvement of one embodiment of the present invention, the soldering layer is another metal solder paste layer, and a fourth solder ball is formed at one end of the second solder wire that is connected to the other metal solder paste layer. The bottom surface and part of the side surface of the fourth solder ball are disposed in the other metal solder paste layer and form a eutectic structure with the other metal solder paste layer. The upper surface of the fourth solder ball is higher than the upper surface of the other metal solder paste layer, and the other end of the second solder wire is connected to the second solder ball.

[0038] The beneficial effects of this invention are as follows: a layer of metal solder paste is formed on the upper surface of a portion of the bare copper area of ​​the lead frame, and at least two solder balls are fabricated on the metal solder paste layer. The two solder balls are wire-bonded to the chip pad and the pin respectively, so that the chip and the pin can be electrically connected through the bare copper area, which greatly reduces the wire length of the direct wire bonding from the chip pad to the pin in the prior art; and, the metal solder paste layer is in a semi-molten state when heated, and the bottom surface and part of the surface of the solder balls fabricated on it can form a eutectic structure with the metal solder paste layer, which enhances the welding bonding force. Attached Figure Description

[0039] Figure 1 This is a schematic diagram of the fabrication process of the bare copper area bonding wire package structure in Embodiments 1 and 2 of the present invention.

[0040] Figures 2(a) to (f) are schematic diagrams of the fabrication steps for realizing the bare copper area bonding wire package structure in Embodiments 1 and 2 of the present invention.

[0041] Figure 3 This is a side view of the packaging structure for implementing bare copper bonding wires in Embodiment 3 of the present invention.

[0042] Figure 4 This is a top view of the packaging structure for implementing bare copper bonding wires in Embodiment 3 of the present invention.

[0043] Figure 5This is a side view of the packaging structure for implementing bare copper bonding wires in Embodiment 4 of the present invention.

[0044] Figure 6 This is a top view of the packaging structure for implementing bare copper area bonding wires in Embodiment 4 of the present invention. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments and corresponding drawings. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0046] Embodiments of the present invention are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0047] For ease of explanation, this document uses terms indicating relative spatial position, such as "above," "below," "behind," and "front," to describe the relationship of one unit or feature shown in the accompanying drawings relative to another unit or feature. Terms indicating relative spatial position can include different orientations of the device during use or operation besides those shown in the figures. For example, if the device in the figures is flipped, a unit described as being "below" or "above" other units or features will be located "below" or "above" other units or features. Therefore, the exemplary term "below" can encompass both "below" and "above" spatial orientations.

[0048] Example 1

[0049] like Figure 1 As shown, this embodiment provides a method for fabricating a bare copper area bonding wire package structure, including the following steps:

[0050] S1: A lead frame is provided, the lead frame includes at least one base island and pins distributed around the base island, the surface of the base island is a bare copper area;

[0051] S2: A solder layer is formed on the upper surface of the pin;

[0052] S3: A metal solder paste layer is formed in a portion of the upper surface of the bare copper area;

[0053] S4: Provide at least one chip and mount the chip above the bare copper area;

[0054] S5: Heating causes the metal solder paste layer to be in a semi-molten state. When the metal solder paste layer is in a semi-molten state, at least a first solder ball and a second solder ball are made on the upper surface of the metal solder paste layer, so that the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer.

[0055] S6: Electrically connect the first solder ball and the pad on the upper surface of the chip through the first bonding wire, and electrically connect the second solder ball and the pin through the second bonding wire.

[0056] Corresponding to steps S1 and S2, as shown in Figure 2(a), a lead frame 1 is provided. Specifically, the lead frame 1 includes a base island 11 and pins 12 distributed around the base island 11. The upper surface of the base island 11 is a bare copper area 13. A solder layer 2 is formed on the upper surface of the pins, specifically including:

[0057] The solder layer 2 is a silver plating layer formed on the upper surface of pin 12 using an electroplating process. The main process steps include: material loading, electrolytic degreasing, activation, pre-plating silver, localized silver plating, silver stripping, preventing silver paste diffusion, preventing copper discoloration, drying, and material collection. This step is existing technology and will not be elaborated upon here. The thickness of the silver plating layer 2 can be designed according to actual needs; it should not be too thin or too thick. If the silver plating layer 2 is too thin, there is a risk of peeling and soldering failure; if it is too thick, it will affect subsequent wire bonding processes, and increasing the wire bonding height increases the risk of product packaging.

[0058] In step S3, a metal solder paste layer 3 is formed on a portion of the upper surface of the bare copper area 13, specifically including:

[0059] As shown in Figure 2(b), a layer of solder paste is formed on a portion of the upper surface of the bare copper area 13 using processes such as printing / dot / laser jetting. This solder paste layer serves as the metal solder paste layer 3. The thickness of the metal solder paste layer 3 should not be too thick or too thin. Excessive thickness can affect subsequent wire bonding processes, increasing the wire height and thus increasing the risk of product packaging. Insufficient thickness, on the other hand, will affect the bonding strength with the wires. Therefore, the thickness of the metal solder paste layer 3 should be controlled between 5 and 25 μm. In other embodiments of this invention, the metal solder paste layer 3 can also be other solderable materials that are in a semi-molten state at the soldering temperature.

[0060] In step S4, at least one chip 4 is provided and mounted on top of the bare copper area 13, specifically including:

[0061] As shown in Figure 2(c), before mounting the chip 4 above the bare copper area 13, an adhesive layer 5 is first applied to the surface of the chip 4 where it needs to be attached to the bare copper area 13, so that the chip 4 is connected and fixed to the lead frame 1. In some embodiments of the present invention, the adhesive layer 5 can be a composite material of one or more of the following: non-conductive / conductive adhesive, film, or solder paste.

[0062] Furthermore, the upper surface of chip 4 has at least one solder pad for wire bonding operations to achieve electrical connection between chip 4 and external circuitry.

[0063] The present invention does not limit the specific dimensions of the provided lead frame 1 and chip 4, which can be selected according to the actual needs of the product.

[0064] In step S5, heating causes the metal solder paste layer 3 to be in a semi-molten state. When the metal solder paste layer 3 is in a semi-molten state, at least a first solder ball 61 and a second solder ball 62 are formed on the upper surface of the metal solder paste layer 3, so that the bottom surface and part of the side surface of the first solder ball 61 and the second solder ball 62 form a eutectic structure with the metal solder paste layer 3, specifically including:

[0065] A wire bonding apparatus is provided, including a cleaver and a wire bonder. The cleaver is used for wire bonding operations. In some embodiments of the present invention, the wire bonder is made of one or more of the following materials: gold, copper, aluminum, silver and palladium. In this embodiment, the wire bonder is a gold-copper wire, and the cleaver is made of ceramic. Specifically, the cleaver includes two symmetrical clamping parts, which clamp the wire bonder in two directions to fix and move the wire bonder.

[0066] The packaging structure in Figure 2(c) is placed inside the equipment, and the soldering temperature is set. Here, the soldering temperature can be set according to the characteristics of the metal solder paste layer 3. In this embodiment, according to the characteristics of the solder paste, the soldering temperature can be set to 180 degrees, so that the solder paste, i.e. the metal solder paste layer 3, is in a semi-molten state.

[0067] Furthermore, the welding wire is fed to the upper surface of the metal solder paste layer 3 by controlling the cutting tool, and a certain welding power is set. Through electric spark, the reserved welding wire at the cutting tool tip is melted in the upper surface area of ​​the metal solder paste layer 3 to form the first solder ball 61 and the second solder ball 62. At the set welding temperature, since the metal solder paste layer 3 is in a semi-molten state, the bottom surface and part of the side surface of the first solder ball 61 and the second solder ball 62 combine with the metal solder paste layer 3 to form a eutectic structure, which enhances the welding bond between the welding wire and the metal solder paste layer 3.

[0068] Furthermore, after the first solder ball 61 and the second solder ball 62 are manufactured, the solder wires connecting the first solder ball 61 and the second solder ball 62 are broken using a wedge, forming the structure shown in Figure 2(d).

[0069] Specifically, the upper surfaces of the first solder ball 61 and the second solder ball 62 formed should be higher than the upper surface of the metal solder paste layer 3 to prevent the wedge from touching the metal solder paste layer 3 and to avoid wedge contamination. It should be noted that the welding power is related to the temperature, pressure, ultrasonic energy, and welding time set in the wire bonding equipment. These can be adjusted according to the actual design process. It is only necessary to ensure that at the corresponding welding temperature, the bottom surface and part of the side surface of the molten first solder ball 61 and the second solder ball 62 can bond with the metal solder paste layer 3 to form a eutectic structure, and to ensure that the formation height of the first solder ball 61 and the second solder ball 62 is higher than the metal solder paste layer 3.

[0070] In step S6, the first solder ball and the pad on the upper surface of the chip are electrically connected via a first bonding wire, and the second solder ball and the pin are electrically connected via a second bonding wire, specifically including:

[0071] As shown in Figure 2(e), the control cutter delivers the first bonding wire 71 to the upper surface of the pad of the chip 4. Through electrical discharge machining, the first bonding wire 71 pre-reserved at the cutter tip is melted on the pad of the chip 4 under a certain current to form the third solder ball 63. The control cutter then bonds the lead of the first bonding wire 71 to the first solder ball 61, cuts the bonding wire, and completes the bonding wire connection between the pad of the chip 4 and the metal solder paste layer 3, realizing the electrical connection between the chip 4 and the bare copper area 13.

[0072] As shown in Figure 2(f), the control cutter delivers the second bonding wire 72 to the upper surface of the silver plating layer 2. Through electrical discharge machining, the second bonding wire 72 pre-reserved at the cutter tip is melted on the silver plating layer 2 under a certain current to form the fourth solder ball 64. The control cutter then bonds the lead of the second bonding wire 72 to the second solder ball 62, cuts the bonding wire, and completes the bonding wire connection between the silver plating layer 2 and the metal solder paste layer 3, realizing the electrical connection between the pin 12 and the bare copper area 13.

[0073] Of course, the present invention does not limit the order of wire bonding between the solder pad and the metal solder paste layer 3 and between the pin 12 and the metal solder paste layer 3. The wire bonding process can be performed between the solder pad and the metal solder paste layer 3 first, or the wire bonding process can be performed between the pin 12 and the metal solder paste layer 3 first.

[0074] In this embodiment, the present invention is not limited to pre-planting balls on the surface of the metal solder paste layer 3, and then wire bonding them from the chip 4 and pin 12 to the balls on the metal solder paste layer 3 to complete the soldering process. In other embodiments of the present invention, the wire bonding can be first controlled to deliver the bonding wire to the pad of the chip 4. Specifically, using the same process as described above on the metal solder paste layer 3, a third solder ball 63 is formed on the pad on the upper surface of the chip 4 by melting. The wire bonding at the connection point with the third solder ball 63 is then cut by the wire bonding and the ball is pre-planted on the pad. The first bonding wire 71 is then delivered to the upper surface area of ​​the metal solder paste layer 3 by the wire bonding. The first bonding wire 71 pre-reserved at the cutting edge is melted on the metal solder paste layer 3 by electrical discharge machining under a certain current to form a first solder ball 61. The wire bonding is then controlled to bond the first bonding wire 71 to the third solder ball 63. The wire bonding is then cut off, and the wire bonding between the pad on the chip 4 and the metal solder paste layer 3 is completed, realizing the electrical connection between the chip 4 and the bare copper area 13, thus forming the structure shown in FIG2(e). Regarding the wire bonding process between the metal solder paste layer 3 and the silver plating layer 2, it should be noted that since there is a good bond between the wire bonding and the silver plating layer 2, if the wedge is controlled to lead the wire bonding from the upper surface of the metal solder paste layer 3 to the upper surface of the silver plating layer 2, it is not necessary to pre-plant balls on the silver plating layer 2. Specifically, the wedge is controlled to deliver the second wire bonding 72 to the upper surface area of ​​the metal solder paste layer 3. Through electrical discharge machining, the second wire bonding 72 pre-reserved at the wedge tip is melted on the metal solder paste layer 3 under a certain current to form the second solder ball 62. Under a certain bonding pressure, the wedge is controlled to lead the second wire bonding 72 to the silver plating layer 2. Cutting the wire bonding can form a bonding fishtail structure on the upper surface of the silver plating layer 2, completing the wire bonding connection between the silver plating layer 2 and the metal solder paste layer 3, and realizing the electrical connection between the pin 12 and the bare copper area 13.

[0075] In this embodiment, the length and curvature of the first bonding wire 71 and the second bonding wire 72 can be designed according to actual product requirements and achieved by setting different bonding wire process parameters.

[0076] Example 2

[0077] The difference between this embodiment and the manufacturing method in Embodiment 1 is that the upper surface of pin 12 is not silver-plated. In step S2, a solder layer 2 is formed on the upper surface of pin 12, specifically including:

[0078] Using the same process as fabricating the solder paste layer 3 on the bare copper area 13, solder paste is sprayed onto the surface of the pin 12 using a printing / dot / laser process to form another solder paste layer, creating the structure shown in Figure 2(a). Similarly, the thickness of the other solder paste layer should not be too thick or too thin. Excessive thickness can affect subsequent wire bonding processes, increasing the wire height and thus increasing the risk of product packaging. Insufficient thickness will affect the bonding strength with the subsequent wires. Therefore, the thickness of the other solder paste layer should be controlled between 5 and 25 μm. In other embodiments of the present invention, the other solder paste layer can also be other solderable materials that are in a semi-molten state at the soldering temperature.

[0079] It should be noted that in this embodiment, at the set soldering temperature, the other metal solder paste layer on pin 12 is also in a semi-molten state. For the bonding process between the metal solder paste layer 3 and the other metal solder paste layer on pin 12, balls can be pre-planted on the surface of the metal solder paste layer 3 to make a second solder ball 62. Then, the wedge is controlled to deliver the second bonding wire 72 to melt on the other metal solder paste layer on pin 12 to form a fourth solder ball 64. The wedge is controlled to wire bond the second bonding wire 72 to the second solder ball 62, thus completing the wire bonding connection between the metal solder paste layer 3 and the other metal solder paste layer on pin 12, and realizing the electrical connection between pin 12 and bare copper area 13.

[0080] Specifically, in this embodiment, the bottom surface and part of the side surface of the second solder ball 62 are bonded to the metal solder paste layer 3 to form a eutectic structure, and the upper surface of the second solder ball 62 is higher than the upper surface of the metal solder paste layer 3. The bottom surface and part of the side surface of the fourth solder ball 64 are bonded to another metal solder paste layer on the pin 12 to form a eutectic structure, and the upper surface of the fourth solder ball 64 is higher than the upper surface of the other metal solder paste layer on the pin 12. Of course, the manufacturing method in this embodiment is not limited to pre-planting balls on the metal solder paste layer 3, controlling the cutter to deliver the second bonding wire 72 to create the fourth solder ball 64 from the other metal solder paste layer on the pin 12, and then wire bonding it to the second solder ball 62. Alternatively, balls can be planted on the upper surface of the other metal solder paste layer on the pin 12 first, the fourth solder ball 64 can be created first, the bonding wire can be cut, and then the cutter can be controlled to create the second solder ball 62 from the metal solder paste layer 3 and then wire bonded to the fourth solder ball 64.

[0081] Other methods for achieving electrical connection between chip 4 and bare copper area 13 are the same as the manufacturing method in Embodiment 1, and will not be described in detail here.

[0082] It should be noted that, in this embodiment, the order of steps S2 and S3 is not limited by the present invention. Forming another metal solder paste layer on the pin and forming a metal solder paste layer on the bare copper area can also be performed simultaneously.

[0083] Compared to the manufacturing method in Example 1, the manufacturing method proposed in this embodiment only requires forming a layer of solder paste on pin 12. Compared to the process of forming a silver plating layer by electroplating, it is simpler. Moreover, at a certain soldering temperature, the bottom surface and part of the side surface of the fourth solder ball 64 can form a eutectic structure with the solder paste, which greatly enhances the soldering bond with pin 12.

[0084] This invention provides a packaging structure for bonding wires in bare copper areas, which is fabricated using the method for fabricating a packaging structure for bonding wires in bare copper areas described in any of the above embodiments.

[0085] Example 3

[0086] like Figure 3 and 4 As shown, Embodiment 3 of the present invention provides a packaging structure for bonding wires in the bare copper area, including a lead frame 1 and at least one chip 4.

[0087] The lead frame 1 includes at least one base island 11 and pins 12 distributed around the base island 11. A bare copper area 13 is formed on the surface of the base island 11, and the chip 4 is disposed above the bare copper area 13. Specifically, an adhesive layer 5 is provided between the chip 4 and the bare copper area 13 to connect and fix the chip 4 to the lead frame 1. In some embodiments of the present invention, the adhesive layer 5 can be a composite material of one or more of the following: non-conductive / conductive adhesive, film, or solder paste.

[0088] Furthermore, at least one solder pad 41 is provided on the upper surface of chip 4 to serve as a solder joint for electrical connection with external circuitry.

[0089] A metal solder paste layer 3 is also provided on a portion of the upper surface of the bare copper area 13. At least a first solder ball 61 and a second solder ball 62 are provided on the upper surface of the metal solder paste layer 3. The bottom surface and part of the side surface of the first solder ball 61 and the second solder ball 62 are provided in the metal solder paste layer 3 and form a eutectic structure with the metal solder paste layer 3.

[0090] Specifically, the upper surfaces of the first solder ball 61 and the second solder ball 62 are higher than the upper surface of the metal solder paste layer 3 to prevent the cleaver from touching the metal solder paste layer during the wire bonding process and causing contamination to the cleaver.

[0091] More specifically, the thickness of the metal solder paste layer 3 is 5–25 μm. If the metal solder paste layer 3 is too thick, it can easily affect the subsequent wire bonding process, increasing the wire height and thus increasing the risk of product packaging. If it is too thin, it will affect the bonding strength with the subsequent wires. It can be adjusted according to the actual needs of the product. The size of the metal solder paste layer 3 and its specific location in the bare copper area 13 can also be adjusted according to the actual design requirements of the product.

[0092] In this embodiment, the metal solder paste layer 3 is made of solder paste. Of course, in other embodiments of the present invention, the metal solder paste layer 3 may also be made of other solderable materials that can be in a semi-molten state at the soldering temperature.

[0093] Furthermore, a solder layer 2 is provided on the upper surface of pin 12. The solder layer 2 can be a silver plating layer or another metal solder paste layer formed by solder paste.

[0094] The first solder ball 61 is connected to the solder pad 41 by the first solder wire 71, and the second solder ball 62 is connected to the solder layer 2 by the second solder wire 72. The chip 4 is electrically connected to the pin 12 in sequence through the first solder wire 71, the metal solder paste layer 3, and the second solder wire 72.

[0095] Specifically, a third solder ball 63 is formed at the end of the first bonding wire 71 that connects to the bonding pad 41. The third solder ball 63 is disposed above the bonding pad 41, and the other end of the first bonding wire 71 is connected to the first solder ball 61, thereby achieving an electrical connection between the chip 4 and the bare copper area 13. Of course, in another embodiment of the present invention, the third solder ball 63 can be disposed on the chip bonding pad 41, and the first bonding wire 71 can form a first solder ball 61 at the end that connects to the metal solder paste layer 3, and the other end can be connected to the third solder ball 63. This can also achieve an electrical connection between the chip 4 and the bare copper area 13. Similarly, in this embodiment, the bottom surface and part of the side surface of the first solder ball 61 formed at the end of the first bonding wire 71 that connects to the metal solder paste layer 3 are disposed within the metal solder paste layer 3 and form a eutectic structure with the metal solder paste layer 3.

[0096] When the solder layer 2 is a silver-plated layer, a second solder ball 62 is formed at the end where the second solder wire 72 connects to the metal solder paste layer 3. The connection between the second solder wire 72 and the solder layer 2 has a fishtail structure (not shown in the figure), realizing the electrical connection between the pin 12 and the bare copper area 13. Of course, in other embodiments of the present invention, a fourth solder ball 64 can also be formed at the end where the second solder wire 72 connects to the solder layer 2, such as... Figure 3 As shown, the other end of the second solder wire 72 is then connected to the second solder ball 62, which can also achieve the electrical connection between the pin 12 and the bare copper area 13.

[0097] When solder layer 2 is another metal solder paste layer formed using solder paste, a fourth solder ball 64 is formed at the end of the second solder line 72 that is connected to the other metal solder paste layer (solder layer 2). It should be noted that when solder layer 2 is another metal solder paste layer formed using solder paste, the bottom surface and part of the side surface of the fourth solder ball 64 are disposed in the other metal solder paste layer and form a eutectic structure with the other metal solder paste layer. The upper surface of the fourth solder ball 64 is higher than the upper surface of the other metal solder paste layer. The other end of the second solder line 72 is then connected to the second solder ball 62, which can also realize the electrical connection between the pin 12 and the bare copper area 13. Compared with the solution of solder layer 2 being a silver-plated layer, the soldering bond between the other metal solder paste layer formed using solder paste and the fourth solder ball 64 is greatly improved. Of course, in other embodiments of the present invention, a fourth solder ball 64 is provided on the upper surface of another metal solder paste layer (soldering layer 2), and the second solder line 72 forms a second solder ball 62 at one end connected to the metal solder paste layer 3, and the other end is connected to the fourth solder ball 64, which can also realize the electrical connection between the pin 12 and the bare copper area 13.

[0098] The specific packaging structure can be fabricated according to different wire bonding processes, and this invention does not limit it.

[0099] Example 4

[0100] like Figure 5 and 6 As shown, this is a packaging structure for implementing bare copper bonding wires provided in Embodiment 4 of the present invention. Unlike the packaging structure in Embodiment 3, in this embodiment, a first metal solder paste layer 31 and a second metal solder paste layer 32 are respectively provided in the area near the solder pad 41 and the area near the pin 12 on the upper surface of the bare copper area 13.

[0101] Specifically, a first solder ball 61 is provided on the upper surface of the first metal solder paste layer 31, and a third solder ball 63 is formed at one end of the first bonding wire 71 that is connected to the bonding pad 41, and the other end is connected to the first solder ball 61 to realize the electrical connection between the chip 4 and the bare copper area 13. Of course, in other embodiments, a third solder ball 63 can also be provided on the bonding pad 41, and the first solder ball 61 is formed at one end of the first bonding wire 71 that is connected to the first metal solder paste layer 31, and the other end is connected to the third solder ball 63, which can also realize the electrical connection between the chip 4 and the bare copper area 13.

[0102] Furthermore, a second solder ball 62 is provided on the upper surface of the second metal solder paste layer 32, and a fourth solder ball 64 is formed at one end of the second solder line 72 that is connected to the solder layer 2, and the other end is connected to the second solder ball 62 to realize the electrical connection between the pin 12 and the bare copper area 13. Of course, in other embodiments, a fourth solder ball 64 can also be provided on the solder layer 2, and the second solder line 72 can form a second solder ball 62 at one end that is connected to the second metal solder paste layer 32, and the other end can be connected to the fourth solder ball 64, which can also realize the electrical connection between the pin 12 and the bare copper area 13.

[0103] The specific packaging structure can be fabricated according to different wire bonding processes, and this invention does not limit it.

[0104] Other specific structures in this embodiment are the same as the packaging structure in Embodiment 3, and will not be described in detail here. Compared with the packaging structure in Embodiment 3, a metal solder paste layer is respectively provided on the surface of the bare copper area 13 near the chip 4 and pin 12, which can reduce the length of the bonding wire between the chip 4 and pin 12 and the bare copper area 13, improve the stability of the bonding wire structure, and reduce the area of ​​the metal solder paste layer 3, thus saving costs.

[0105] In summary, this invention forms a layer of metal solder paste on the upper surface of a portion of the bare copper area of ​​the leadframe, and fabricates at least two solder balls on the metal solder paste layer. The two solder balls are then wire-bonded to the chip pads and pins, respectively, enabling electrical connection between the chip and the pins through the bare copper area. This significantly reduces the wire length required for direct wire bonding from the chip pads to the pins in existing technologies. Furthermore, the metal solder paste layer is in a semi-molten state when heated, allowing the bottom surface and part of the surface of the solder balls to form a eutectic structure with the metal solder paste layer, enhancing the solder bond strength.

[0106] It should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This way of describing the specification is only for clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

[0107] The detailed descriptions listed above are merely specific descriptions of feasible embodiments of the present invention, and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for fabricating a bare copper area wire bonding package structure, characterized in that, The manufacturing method includes the following steps: A lead frame is provided, the lead frame including at least one base island and pins distributed around the base island, the surface of the base island being a bare copper area; A weld layer is formed on the upper surface of the pin; A metal solder paste layer is formed on a portion of the upper surface of the bare copper area; Provide at least one chip and mount the chip above the bare copper area; Heating causes the metal solder paste layer to be in a semi-molten state. When the metal solder paste layer is in a semi-molten state, at least a first solder ball and a second solder ball are made on the upper surface of the metal solder paste layer, so that the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer. The first solder ball and the pad on the upper surface of the chip are electrically connected by a first bonding wire, and the second solder ball and the solder layer are electrically connected by a second bonding wire. The chip is electrically connected to the pin in sequence through the first bonding wire, the metal solder paste layer and the second bonding wire; the metal solder paste layer is a solder paste layer.

2. The method for fabricating a bare copper area bonding wire package structure according to claim 1, characterized in that, The formation of a metal solder paste layer on a portion of the upper surface of the bare copper area specifically includes: A solder paste layer with a thickness of 5~25μm is formed on a portion of the upper surface of the bare copper area by printing / dot / laser spraying to create the metal solder paste layer.

3. The method for fabricating a bare copper area bonding wire package structure according to claim 2, characterized in that, The heating process brings the metal solder paste layer to a semi-molten state. While the metal solder paste layer is in this semi-molten state, at least a first solder ball and a second solder ball are formed on the upper surface of the metal solder paste layer, such that the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer. Specifically, this includes: Set the welding temperature so that the metal solder paste layer is in a semi-molten state; The reserved solder lines of the wedge are melted in a portion of the upper surface of the metal solder paste layer to form a first solder ball and a second solder ball. At the welding temperature, the bottom surface and part of the side surface of the first solder ball and the second solder ball form a eutectic structure with the metal solder paste layer. The upper surface of the first solder ball and the second solder ball is higher than the upper surface of the metal solder paste layer. The welding wire connecting the first solder ball and the second solder ball is cut using the cutting tool.

4. The method for fabricating a bare copper area bonding wire package structure according to claim 3, characterized in that, The process of forming a weld layer on the surface of the pin specifically includes: A silver plating layer is formed on the upper surface of the pin using an electroplating process.

5. The method for fabricating a bare copper area bonding wire package structure according to claim 3, characterized in that, The process of forming a weld layer on the surface of the pin specifically includes: Using printing / dot / laser processes, solder paste is sprayed onto the upper surface of the pin to form another layer of metal solder paste.

6. The method for fabricating a bare copper area bonding wire package structure according to claim 4, characterized in that, The step of electrically connecting the first solder ball and the pad on the upper surface of the chip via a first bonding wire, and electrically connecting the second solder ball and the pin via a second bonding wire, specifically includes: The cutter is controlled to deliver the first bonding wire to the solder pad to melt and form a third solder ball, and the first bonding wire is wire-bonded to the first solder ball; The control cutter delivers the second bonding wire to the silver plating layer to melt and form a fourth solder ball, and then wirebonds the second bonding wire to the second solder ball.

7. The method for fabricating a bare copper area bonding wire package structure according to claim 5, characterized in that, The step of electrically connecting the first solder ball and the pad on the upper surface of the chip via a first bonding wire, and electrically connecting the second solder ball and the pin via a second bonding wire, specifically includes: The cutter is controlled to deliver the first bonding wire to the solder pad to melt and form a third solder ball, and the first bonding wire is wire-bonded to the first solder ball; The cutting tool is controlled to deliver the second welding wire to melt on the other metal solder paste layer to form a fourth solder ball. At the welding temperature, the bottom surface and part of the side surface of the fourth solder ball form a eutectic structure with the other metal solder paste layer, and the upper surface of the fourth solder ball is higher than the upper surface of the other metal solder paste layer. The cutting tool is controlled to bond the second wire lead to the second solder ball.

8. A packaging structure for implementing bare copper area bonding wires, characterized in that, It is manufactured using the method for realizing the bare copper area bonding wire package structure as described in any one of claims 1 to 7.

9. A packaging structure for bonding bare copper areas, comprising a lead frame and at least one chip, wherein the lead frame includes at least one base island and pins distributed around the base island, a bare copper area is disposed on the surface of the base island, the chip is disposed above the bare copper area, at least one solder pad is disposed on the upper surface of the chip, and a solder layer is disposed on the upper surface of the pins, characterized in that, A metal solder paste layer is also provided on a portion of the upper surface of the bare copper area. The metal solder paste layer is a solder paste layer. At least a first solder ball and a second solder ball are provided on the upper surface of the metal solder paste layer. The bottom surface and part of the side surface of the first solder ball and the second solder ball are disposed in the metal solder paste layer and form a eutectic structure with the metal solder paste layer. The first solder ball is connected to the solder pad via a first solder wire, and the second solder ball is connected to the solder layer via a second solder wire. The chip is electrically connected to the pin via the first solder wire, the metal solder paste layer, and the second solder wire in sequence.

10. The packaging structure for implementing bare copper area bonding wires according to claim 9, characterized in that, The upper surfaces of the first solder ball and the second solder ball are higher than the upper surface of the metal solder paste layer.

11. The packaging structure for implementing bare copper area bonding wires according to claim 10, characterized in that, The thickness of the metal solder paste layer is 5~25μm.

12. The packaging structure for implementing bare copper area bonding wires according to claim 11, characterized in that, The first solder wire has a third solder ball at one end connected to the solder pad, and the other end is connected to the first solder ball.

13. The packaging structure for implementing bare copper area bonding wires according to claim 12, characterized in that, The welding layer is a silver-plated layer, and the second solder ball is connected to the silver-plated layer by a second solder wire.

14. The packaging structure for implementing bare copper area bonding wires according to claim 12, characterized in that, The soldering layer is another metal solder paste layer. The second solder wire has a fourth solder ball formed at one end connected to the other metal solder paste layer. The bottom surface and part of the side surface of the fourth solder ball are disposed in the other metal solder paste layer and form a eutectic structure with the other metal solder paste layer. The upper surface of the fourth solder ball is higher than the upper surface of the other metal solder paste layer. The other end of the second solder wire is connected to the second solder ball.

Citation Information

Patent Citations

  • Semiconductor package having copper wire and throwing method

    CN101339931A

  • Wire bonding method, semiconductor chip, and semiconductor package

    US20050054186A1