Lithium ion battery electrolyte and lithium ion battery containing the electrolyte

By using silicon nitrogen compounds and anicyclic-boron trifluoride coordination compounds in lithium-ion battery electrolytes, the cycle performance and life problems of liquid lithium-ion batteries at high voltage and high temperatures are solved, and a higher degree of Battery stability and efficiency.

CN115172879BActive Publication Date: 2024-12-06ZHANGJIAGANG GUOTAI HUARONG NEW CHEM MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210903898.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-12-06
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

Liquid lithium-ion batteries have cycling performance and life problems under high voltage and high temperature conditions. Conventional electrolytes are easily oxidized and decomposed at high temperatures, resulting in attenuation of battery capacity, and existing additives are costly and difficult to control internal resistance.

Method used

Using lithium-ion battery electrolyte containing silicon nitrogen compounds and a nitrogen-borotrifluoride coordination compound, silicon nitrogen compounds block moisture reaction by introducing silane groups to form SEI films, reducing battery internal resistance and nitrogen Ring-boron trifluoride forms a dense film on the surface of the positive electrode to reduce the dissolution of transition metal ions.

Benefits of technology

It significantly reduces the generation of HF, extends the battery life, improves high-temperature cycle and shelving performance, reduces the internal resistance of the battery, and enhances the high-temperature and high-voltage stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention relates to a lithium ion battery electrolyte and a lithium ion battery containing the electrolyte. In order to solve the problem that the existing lithium ion battery electrolyte cannot take into account both the cycle performance and high temperature performance under high voltage conditions, the present invention provides a lithium ion battery electrolyte, including a non-aqueous organic solvent, a lithium salt and an additive, the additive including a silicon nitrogen compound and selectively including a nitrogen heterocycle-boron trifluoride coordination compound, the silicon nitrogen compound used in the present invention can improve the generation of HF in the electrolyte during storage, and can improve the oxidation resistance of the electrolyte under high voltage conditions, while the nitrogen heterocycle-boron trifluoride coordination compound can increase the solubility of LiF in the positive electrode solid surface film and reduce the impedance of the solid interface film, and the synergistic effect of the two can improve the cycle performance and high temperature performance of the battery under high voltage conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium ion battery electrolyte and a lithium ion battery containing the electrolyte. Background Art

[0002] Lithium-ion batteries have developed rapidly in the fields of mobile devices, electric vehicles and energy storage due to their high capacity, high energy density and environmental friendliness. Lithium-ion batteries can be divided into liquid lithium-ion batteries, solid lithium-ion batteries and solid-liquid hybrids, i.e., so-called semi-solid lithium-ion batteries, according to the state of the electrolyte. The technology of solid-state lithium-ion batteries is still not perfect. The low ion conductivity and interface contact problems of solid-state membranes cause solid-state lithium-ion batteries to have low cycle efficiency and serious capacity attenuation. Although adding a small amount of electrolyte to the solid-state membrane can alleviate the above problems, it still cannot meet the needs of modern life. Therefore, in the short term, liquid lithium-ion batteries will still dominate.

[0003] Liquid electrolytes are composed of non-aqueous organic solvents, lithium salts and additives. Among them, the commonly used lithium salt is lithium hexafluorophosphate, which is very unstable in the electrolyte and will react with a small amount of water to generate hydrofluoric acid. On the one hand, it consumes the effective lithium ions in the electrolyte. On the other hand, HF will dissolve the transition metal oxide material in the positive electrode in the electrolyte, destroy the structure of the positive electrode material, and cause the battery capacity to decay. This phenomenon is more obvious under high temperature conditions. Increasing the voltage has become an important means to obtain high-capacity batteries, but the oxidation potential of conventional carbonate electrolytes is around 4.5V. Further increase in material voltage will cause oxidative decomposition of the electrolyte, greatly affecting the effective life of the battery. In addition to replacing battery materials and modifying and coating materials, additives are widely used as a simple and effective method to improve electrolyte stability and battery cycle performance, because additives can form a layer of solid interface film on the surface of the positive and negative electrodes during the pre-charging process of the battery, preventing the electrode material from directly contacting the electrolyte and avoiding more invalid side reactions in the battery. However, in order to solve the many problems faced in batteries, the synergistic effect of multiple additives is usually required, which not only brings higher costs, but also makes the internal resistance of the battery difficult to control. Therefore, there is an urgent need to find a multi-faceted additive to solve the problems encountered in the above batteries. Summary of the invention

[0004] The object of the present invention is to provide a lithium ion battery electrolyte that can simultaneously take into account the cycle performance under high voltage conditions and the high temperature performance.

[0005] Another object of the present invention is to provide a lithium ion battery with excellent high temperature performance.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A lithium ion battery electrolyte, comprising a non-aqueous organic solvent, a lithium salt and an additive, wherein the additive comprises a silicon nitrogen compound as shown in formula I, and optionally comprises a nitrogen heterocycle-boron trifluoride coordination compound

[0008]

[0009] Wherein, Z in Formula I is a sulfonyl group or a carbonyl group; R1, R2, and R3 are each independently selected from a halogen atom, a halogen substituted or unsubstituted aryl group, a halogen substituted or unsubstituted alkyl group or an alkenyl group having 1 to 4 carbon atoms; R4, R5, R6, and R7 are each independently selected from a hydrogen atom, a halogen atom, a nitro group, an amino group, a halogen substituted or unsubstituted alkyl group or an alkenyl group having 1 to 4 carbon atoms.

[0010] The silicon-nitrogen compound with a specific structure used in the present invention has the following characteristics: 1) a relatively high HUMO electron orbit, so that its ability to obtain electrons is relatively poor and it is not easily oxidized, thereby widening the potential window of the electrolyte and providing sufficient conditions for the electrolyte to work under high voltage conditions; 2) the introduction of silane groups in the silicon-nitrogen compound can consume the water in the electrolyte, blocking the reaction link of the water and lithium hexafluorophosphate reacting to generate HF, avoiding the corrosion of the positive electrode material by HF and the dissolution of transition metal ions therein, thereby improving the life of the battery; 3) the silicon-nitrogen compound can generate an SEI film by a reduction reaction on the surface of the negative electrode, and since there are lone pairs of electrons in heteroatoms such as S and N, when the two elements participate in the formation of a solid interface film, the transmission rate of electrons in the interface can be increased, so that the battery interface resistance can be reduced and the battery cycle efficiency can be improved. Furthermore, silicon-nitrogen compounds of specific structures are combined with nitrogen heterocycle-boron trifluoride coordination compounds to further improve the high-temperature shelf performance and high-temperature cycle performance of the battery. In addition to the N atom in the nitrogen heterocycle-boron trifluoride coordination compound being able to realize the function in 3), it can itself form a thin and dense solid interface film on the surface of the positive electrode, and the B atom can complex with the transition metal ions in the positive electrode material to reduce the dissolution of the transition metal ions from the material, thereby avoiding the structural collapse of the positive electrode material and affecting the cycle capacity of the battery.

[0011] Preferably, R1, R2, and R3 are each independently a halogen-substituted or unsubstituted alkyl or alkenyl group containing 1 to 4 carbon atoms; R4, R5, R6, and R7 are each independently selected from any one of hydrogen, a halogen atom, and a halogen-substituted or unsubstituted alkyl or alkenyl group containing 1 to 4 carbon atoms.

[0012] More preferably, R1, R2, and R3 are each independently a halogen-substituted or unsubstituted methyl group; and R4, R5, R6, and R7 are each independently any one of hydrogen, an unsubstituted alkyl group or an alkenyl group having 1 to 4 carbon atoms.

[0013] Still further preferably, R1, R2, and R3 in Formula I are the same and are selected from a fluorine atom, a methyl group or a trifluoromethyl group; and at least two of R4, R5, R6, and R7 are hydrogen atoms.

[0014] According to some preferred embodiments, the silicon-nitrogen compound is

[0015] One or more of .

[0016] Specifically, the preparation method of compound 3 is: o-benzoylsulfonyl imide and tris(trifluoromethyl)chlorosilane are reacted in the presence of n-butyl lithium and tetrahydrofuran under a nitrogen atmosphere at -80°C to -65°C to obtain compound 3.

[0017] Further, o-benzoylsulfonyl imide is dissolved in dry tetrahydrofuran, and the solution is cooled to -80°C to -65°C, and then n-butyl lithium with a concentration of 2 to 3 mol / L is added to the above coolant under a nitrogen atmosphere, and the reaction is kept warm for 80 to 100 minutes, and then tris(trifluoromethyl)chlorosilane is added and the reaction is continued for 1.5 to 2.5 hours to obtain product 3.

[0018] Specifically, the preparation method of compound 4 is: o-phenylenedisulfonyl imide and tris(trifluoromethyl)chlorosilane are reacted in the presence of n-butyl lithium and tetrahydrofuran under a nitrogen atmosphere at -80°C to -65°C to obtain compound 3.

[0019] Further, o-benzenedisulfonyl imide is dissolved in dry tetrahydrofuran, and the solution is cooled to -80°C to -65°C, and then n-butyl lithium with a concentration of 2 to 3 mol / L is added to the above coolant under a nitrogen atmosphere, and the reaction is kept warm for 80 to 100 minutes, and then tris(trifluoromethyl)chlorosilane is added and kept warm for 1.5 to 2.5 hours to obtain product 4.

[0020] Preferably, the nitrogen heterocycle in the nitrogen heterocycle-boron trifluoride compound is one or more of a pyridyl-containing heterocycle, a pyridazine-containing heterocycle, a pyrimidine-containing heterocycle, a pyrazine-containing heterocycle, a pyrrol-containing heterocycle, a pyrazol-containing heterocycle and an imidazole-containing heterocycle.

[0021] According to some preferred embodiments, the nitrogen heterocycle-boron trifluoride coordination compound is pyridine-boron trifluoride.

[0022] Preferably, the nitrogen heterocycle-boron trifluoride coordination compound accounts for 0.05%-2% of the total mass of the lithium ion battery electrolyte, for example 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%.

[0023] Preferably, the silicon-nitrogen compound accounts for 0.05%-5% of the total mass of the lithium-ion battery electrolyte, for example 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.

[0024] Preferably, the additives further include other additives accounting for 0.05%-5% of the total mass of the lithium-ion battery electrolyte, such as 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.

[0025] Preferably, the other additives are one or more of succinonitrile, adiponitrile, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, methylene disulfonate, propylene sulfate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphite, tris(trimethylsilyl)phosphate, vinyl ethylene carbonate, maleic anhydride, and glutaric anhydride.

[0026] More preferably, the other additives are fluoroethylene carbonate and adiponitrile.

[0027] Preferably, the lithium salt is selected from one or more of lithium perchlorate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium hexafluorophosphate, lithium carbonate, lithium sulfate, lithium sulfite, lithium nitrate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorophosphate, and lithium difluorobis(oxalatophosphate).

[0028] Preferably, the concentration of the lithium salt is 0.5-5 mol / L, for example 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L.

[0029] Preferably, the non-aqueous organic solvent is one or more of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethylene carbonate, methyl formate, ethyl acetate, methyl butyrate, methyl acrylate, N-methylpyrrolidone, N-methylformamide, N-methylacetamide, acetonitrile, N,N-dimethylformamide, sulfolane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, and tetrahydrofuran.

[0030] More preferably, the non-aqueous organic solvent is a mixture of diethyl carbonate, ethylene carbonate and ethyl methyl carbonate.

[0031] The present invention also provides a lithium ion battery, which comprises a positive electrode sheet, a negative electrode sheet, a separator arranged between the positive electrode sheet and the negative electrode sheet, and an electrolyte, wherein the electrolyte is the lithium ion battery electrolyte.

[0032] Preferably, the positive electrode material is a lithium transition metal composite oxide, and the lithium transition metal composite oxide comprises one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, or compounds obtained by adding other transition metals or non-transition metals to the above lithium transition metal composite oxides.

[0033] Preferably, the negative electrode material is selected from one or more of soft carbon, hard carbon, artificial graphite, natural graphite, silicon, silicon oxides, silicon-carbon composites, lithium titanate, and metals that can form alloys with lithium.

[0034] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0035] The silicon-nitrogen compound additive in the lithium-ion battery electrolyte of the present invention can greatly reduce the generation of HF in the electrolyte, avoid the structural collapse of the positive electrode material during the storage process, and the heteroatom N introduced contains lone pairs of electrons, which can reduce the resistance of electrons passing through the negative electrode interface film, thereby reducing the internal resistance of the battery, so that the lithium-ion battery electrolyte can take into account both high-temperature storage performance and high-temperature cycle performance. Further, pyridine-boron trifluoride can form a positive electrode interface film on the surface of the positive electrode material, and the silicon-nitrogen compound additive is used in combination with the nitrogen heterocycle-boron trifluoride coordination compound additive, which can further reduce the oxidation of the electrolyte by the positive electrode under high voltage and high temperature conditions, reduce the gas production of the battery during the high-temperature storage process, and thus make the electrolyte show better high-temperature performance. DETAILED DESCRIPTION

[0036] The technical solution, its implementation process and principle will be further explained below. It should be understood that the embodiments described in this specification are only for explaining the present invention, not for limiting the present invention. The implementation conditions adopted in the embodiments can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0037] In the following examples and comparative examples, unless otherwise specified, the raw materials used were commercially available.

[0038] In the following examples and comparative examples, compound 3 and compound 4 are self-made, and the preparation method refers to patent US4181660A. The preparation method of compound 3 is: 0.36 mol o-benzoylsulfonyl imide Dissolve in 600 ml of dry tetrahydrofuran, then cool the solution to -73°C, then add 130 ml of 2.4 mol / L n-butyl lithium to the coolant under nitrogen atmosphere, keep warm for 90 min, then add 0.3 mol of tris(trifluoromethyl)chlorosilane and continue to keep warm for 2 h to obtain product 3.

[0039] The preparation method of compound 4 is as follows: 0.36 mol of o-phenylenedisulfonimide Dissolve in 600 ml of dry tetrahydrofuran, then cool the solution to -73°C, then add 130 ml of 2.4 mol / L n-butyl lithium to the coolant under nitrogen atmosphere, keep warm for 90 min, then add 0.3 mol of tris(trifluoromethyl)chlorosilane and continue to keep warm for 2 h to obtain product 4.

[0040] Example 1

[0041] Preparation of the electrolyte: Diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) are mixed in a weight ratio of 20:30:50, 1M lithium salt LiPF6 is fully dissolved, and then 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, and 0.5% of compound 1 accounting for the total weight of the electrolyte are added.

[0042] Preparation of positive electrode sheet: The positive electrode active material ternary NCM622, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent system at a mass ratio of 95:3:2, and then coated on the positive electrode current collector Al foil, and the positive electrode sheet is obtained by drying and cold pressing.

[0043] Preparation of negative electrode sheet: The negative electrode active material graphite, the conductive agent acetylene black, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC) are fully stirred and mixed in a deionized water solvent system at a mass ratio of 95:2:2:1, and then coated on the negative electrode current collector Cu foil, and dried and cold pressed to obtain the negative electrode sheet.

[0044] Preparation of isolation membrane: PE porous polymer film is used as isolation membrane.

[0045] Preparation of lithium-ion battery: stack the prepared positive electrode sheet, isolation film, and negative electrode sheet in order, so that the isolation film is placed between the positive and negative electrode sheets to play an isolating role, and obtain a bare battery cell after winding; place the bare battery cell in an outer package, inject the above-prepared electrolyte, and obtain a lithium-ion battery after packaging. The obtained lithium-ion battery has a designed capacity of 1800mAh.

[0046] Example 2

[0047] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, and 1% of compound 1 accounting for the total weight of the electrolyte.

[0048] Example 3

[0049] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, 1% of compound 1 accounting for the total weight of the electrolyte, and 0.5% of pyridine-boron trifluoride accounting for the total weight of the electrolyte.

[0050] Example 4

[0051] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, and 2% of compound 1 accounting for the total weight of the electrolyte.

[0052] Example 5

[0053] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, and 5% of compound 1 accounting for the total weight of the electrolyte.

[0054] Example 6

[0055] Basically the same as Example 1, the difference is that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, 1% of compound 2 accounting for the total weight of the electrolyte, and 0.5% of pyridine-boron trifluoride accounting for the total weight of the electrolyte.

[0056] Example 7

[0057] Basically the same as Example 1, the difference is that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, 1% of compound 3 accounting for the total weight of the electrolyte, and 0.5% of pyridine-boron trifluoride accounting for the total weight of the electrolyte.

[0058] Example 8

[0059] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, 1% of compound 4 accounting for the total weight of the electrolyte, and 0.5% of pyridine-boron trifluoride accounting for the total weight of the electrolyte.

[0060] Comparative Example 1

[0061] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate and 0.3% of adiponitrile, which account for 2% of the total weight of the electrolyte.

[0062] Comparative Example 2

[0063] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, and 1% of 2-sulfobenzoic anhydride accounting for the total weight of the electrolyte.

[0064] Comparative Example 3

[0065] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate, 0.3% of adiponitrile, and 0.8% of phthalic anhydride, which account for the total weight of the electrolyte.

[0066] Comparative Example 4

[0067] The method is basically the same as Example 1, except that the electrolyte is different. The electrolyte is prepared by mixing diethyl carbonate (DEC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC) in a weight ratio of 20:30:50, fully dissolving 1M lithium salt LiPF6, and then adding 2% of fluoroethylene carbonate accounting for the total weight of the electrolyte, 0.3% of adiponitrile accounting for the total weight of the electrolyte, and 1.5% of lithium bis(trifluoromethylsulfonyl)imide accounting for the total weight of the electrolyte.

[0068] In the above embodiments, compound 1: Compound 2: Compound 3: Compound 4:

[0069] Electrolyte storage test

[0070] The fresh electrolytes prepared in the above Examples 1-8 and Comparative Examples 1-4 were transferred into aluminum-plastic bottles, sealed, and placed at 45° C. for 48 hours. After the placing was completed, the HF content in the electrolytes was tested.

[0071] The HF content in the electrolyte after standing is shown in Table 1.

[0072] Table 1

[0073] Electrolyte HF Example 1 115 Example 2 91 Example 3 83 Example 4 65 Example 5 26 Example 6 78 Example 7 56 Example 8 62 Comparative Example 1 141 Comparative Example 2 228 Comparative Example 3 303 Comparative Example 4 126

[0074] Table 1 shows that compared with Comparative Example 1, after adding the additives 2-sulfobenzoic anhydride and phthalic anhydride, respectively, Comparative Examples 2 and 3, the HF content in the electrolyte after being left at 45°C increased significantly; and Examples 1-8 show that compared with Comparative Example 1, after adding Compounds 1-4, the HF content in the electrolyte after being left at 45°C decreased to varying degrees. This is because the silicon-based groups in the compounds can consume the residual moisture in the electrolyte, prevent the decomposition of LiPF6, and improve the stability of the electrolyte. In addition, Comparative Example 4 shows that compared with Comparative Example 1, the addition of lithium bis(trifluoromethylsulfonyl)imide can also reduce the HF content in the electrolyte after being left at 45°C to a certain extent.

[0075] High temperature cycle test

[0076] At 45°C, the battery was tested for 300 cycles at a charge and discharge rate of 1 / 1C, with a charge and discharge voltage range of 3.0-4.35V, and the discharge capacity of the first week and the 300th week was recorded respectively. The 300th week capacity retention rate (%) = 300th week discharge capacity / first week discharge capacity*100%.

[0077] High temperature storage test

[0078] First, charge and discharge the formed battery three times at 1C at room temperature, with a charge and discharge voltage range of 3.0-4.35V, and record the third discharge capacity as Q1. Then charge the battery to 4.35V at 1C with constant current and constant voltage, with a cut-off current of 0.05C, and then store it at 60℃ for 7 days. Measure the battery thickness before storage and record it as t1. After the high-temperature storage is completed and the battery is completely cooled, measure the battery thickness again and record it as t2. Then perform a discharge test on the removed battery at 1C, and record the discharge capacity of the battery as Q2.

[0079] Thickness change rate = (t2-t1) / t1×100%; storage capacity retention rate = Q2 / Q1×100%.

[0080] The high temperature cycle and high temperature shelf performance results of the battery are shown in Table 2.

[0081] Table 2

[0082]

[0083] Table 2 shows that the high temperature cycle performance and high temperature shelf performance of Examples 1 and 2 are better than those of Comparative Examples 1-4. Although the lithium bis(trifluoromethylsulfonyl)imide of Comparative Example 4 can also reduce the HF content in the electrolyte after being stored at 45°C to a certain extent, its improvement effect on the high temperature performance of the electrolyte is not as good as that of Examples 1-8. It is speculated that the silicon nitrogen compound used in the present invention contains a silicon-based group, which greatly reduces the generation of HF in the electrolyte and avoids the structural collapse of the positive electrode material during the storage process; on the other hand, since the heteroatom N introduced into the system contains a lone pair of electrons, the resistance of electrons passing through the negative electrode interface film can be reduced, thereby reducing the internal resistance of the battery.

[0084] By comparing Examples 1 to 8, it can be found that when the silicon nitrogen compound in the present invention is used in combination with pyridine-boron trifluoride, it can show better high-temperature performance. It is speculated that this is because pyridine-boron trifluoride can form a positive electrode interface film on the surface of the positive electrode material, reducing the oxidation of the electrolyte by the positive electrode under high voltage and high temperature conditions, and reducing the gas production of the battery during high-temperature storage.

[0085] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A lithium ion battery electrolyte comprising a non-aqueous organic solvent, a lithium salt and an additive, It is characterized in that The additive includes a silicon-nitrogen compound as shown in Formula I, Wherein, Z in Formula I is a sulfonyl group or a carbonyl group; R 1 , R 2 , R 3 Each is independently selected from any one of a halogen atom, a halogen-substituted or unsubstituted aryl group, a halogen-substituted or unsubstituted alkyl group having 1 to 4 carbon atoms, and a halogen-substituted or unsubstituted alkenyl group having 1 to 4 carbon atoms; R 4 , R 5 , R 6 , R 7 Each is independently selected from any one of hydrogen, a halogen atom, a nitro group, an amino group, a halogen-substituted or unsubstituted alkyl group having 1 to 4 carbon atoms, and a halogen-substituted or unsubstituted alkenyl group having 1 to 4 carbon atoms.

2. The lithium ion battery electrolyte according to claim 1, Features: R in the formula I 1 , R 2 , R 3 are the same and are selected from a fluorine atom, a methyl group or a trifluoromethyl group; R 4 , R 5 , R 6 , R 7 At least two of them are hydrogen atoms.

3. The lithium ion battery electrolyte according to claim 2, Features: The silicon-nitrogen compound is , , , One or more of .

4. The lithium ion battery electrolyte according to claim 1, Features: The additive also includes a nitrogen heterocycle-boron trifluoride coordination compound.

5. The lithium ion battery electrolyte according to claim 4, Features: The nitrogen heterocycle in the nitrogen heterocycle-boron trifluoride coordination compound is one or more of a pyridyl-containing heterocycle, a pyridazine-containing heterocycle, a pyrimidine-containing heterocycle, a pyrazine-containing heterocycle, a pyrrol-containing heterocycle, a pyrazol-containing heterocycle and an imidazole-containing heterocycle.

6. The lithium ion battery electrolyte according to claim 5, Features: The nitrogen heterocycle-boron trifluoride coordination compound is pyridine-boron trifluoride.

7. The lithium ion battery electrolyte according to claim 4, Features: The nitrogen heterocycle-boron trifluoride coordination compound accounts for 0.05%-2% of the total mass of the lithium ion battery electrolyte; the silicon nitrogen compound accounts for 0.05%-5% of the total mass of the lithium ion battery electrolyte.

8. The lithium ion battery electrolyte according to claim 1, Features: The additives also include other additives accounting for 0.05%-5% of the total mass of the lithium ion battery electrolyte, and the other additives are one or more of succinonitrile, adiponitrile, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, methylene disulfonate, propylene sulfate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphite, tris(trimethylsilyl)phosphate, vinyl ethylene carbonate, maleic anhydride, and glutaric anhydride.

9. The lithium ion battery electrolyte according to claim 1, Features: The lithium salt is selected from one or more of lithium perchlorate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium hexafluorophosphate, lithium carbonate, lithium sulfate, lithium sulfite, lithium nitrate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorophosphate, and lithium difluorobis(oxalatophosphate); And / or, the non-aqueous organic solvent is one or more of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethylene carbonate, methyl formate, ethyl acetate, methyl butyrate, methyl acrylate, N-methylpyrrolidone, N-methylformamide, N-methylacetamide, acetonitrile, N,N-dimethylformamide, sulfolane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, and tetrahydrofuran.

10. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and an electrolyte, Features: The electrolyte is the lithium ion battery electrolyte according to any one of claims 1 to 9.

11. The lithium ion battery according to claim 10, Features: The positive electrode active material is a lithium transition metal composite oxide, wherein the lithium transition metal composite oxide comprises one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, or a compound obtained by adding other transition metals or non-transition metals to the above lithium transition metal composite oxides; And / or, the negative electrode active material is selected from one or more of soft carbon, hard carbon, artificial graphite, natural graphite, silicon, silicon oxides, silicon-carbon composites, lithium titanate, and metals that can form alloys with lithium.

Citation Information

Patent Citations

  • 3-Substituted benz[d]isothiazole-1,1-dioxides

    US4181660A

  • Preparation methods of 6-O-methylerythromycin A derivative and clarithromycin

    CN102250173A

  • High-temperature high-voltage non-aqueous electrolyte and lithium ion battery containing non-aqueous electrolyte

    CN109818064A

  • New electrolyte and lithium ion battery using the same

    KR1020020085675A