Water-soluble high-temperature resistant infrared carbon-based heating slurry and preparation method thereof

Through the design of water-soluble high-temperature resistant infrared carbon-based heating slurry, the problem of poor stability and high cost of graphene heating materials in high temperature environments is solved, and a long-term stable operation and low-cost electric heating materials are realized at high temperatures. Various high-temperature application scenarios.

CN115175385BActive Publication Date: 2024-12-06WUXI CHENHAI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210899979.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-28
Publication Date
2024-12-06
Estimated Expiration
2042-07-28

AI Technical Summary

Technical Problem

The existing graphene heating materials have poor stability and high cost in high temperature environments, especially the low operating temperature and high cost of graphene heating plates.

Method used

Use water-soluble high-temperature resistant infrared carbon-based heating slurry, including phosphate solution, glass powder, carbon-based conductive powder, inorganic filler, tetrabutyl titanate, anti-high-temperature oxidant and other components, and through specific weight ratios and preparation Method, an electric heating material with high temperature stability and low cost is formed.

Benefits of technology

The electric heating material that has long-term stable working under high temperature environment has excellent resistance to high temperature oxidation and aging, reduces the oxidation risk of the material, improves infrared emissivity, and is low in cost. It is suitable for household appliances and industrial baking. and other high temperature applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115175385B_ABST
    Figure CN115175385B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of material electrothermal technology, and specifically provides a water-soluble high-temperature resistant infrared carbon-based heating slurry and a preparation method thereof, wherein the heating slurry comprises water and a slurry matrix, and the components of the slurry matrix are mixed according to the following weight ratio: 15-20 parts of 40-50wt% phosphate solution or an amount of phosphate equivalent thereto; 2-14 parts of glass powder; 1-40 parts of carbon-based conductive powder; 5-10 parts of inorganic filler powder; 1-3 parts of tetrabutyl titanate; 1-5 parts of high-temperature oxidant; 0.1-5 parts of dispersant; 1-20 parts of film-forming agent; 0.1-3 parts of leveling agent; 0.1-3 parts of anti-settling agent; 0.1-3 parts of defoamer; 0.01-3 parts of thickener; 10-100 parts of water. Through such a composition, it is possible to seek to obtain a water-soluble high-temperature resistant infrared carbon-based heating slurry that is particularly suitable for high-temperature fields such as household appliances, industrial baking, and boiler heating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electric heating materials, and in particular to a water-soluble high-temperature-resistant infrared carbon-based heating slurry and a preparation method thereof. Background Art

[0002] Nanocarbon materials represented by graphene are a new type of material. Due to their excellent performance in conductivity and infrared radiation, they have great application potential in the field of electric heating. One product form using graphene, a new material, is graphene heating film. At present, the more common application of graphene heating film is in the form of floor heating heating film to cope with low temperature scenes within 100°C, and the application field is very limited. In view of the aforementioned excellent properties of graphene, how to develop graphene electric heating slurry with the advantages of high operating temperature, low cost, and convenient construction method is a common demand in the field. Such as:

[0003] Chinese patent application (CN112521796A) discloses a graphene heating ink and its preparation method and application. The graphene heating ink comprises a resin matrix, a conductive filler, an additive and a solvent. The conductive filler comprises graphene. The resin matrix is ​​composed of an organic polymer and polysilazane in a mass ratio of 1:0.08-1.5. The preparation method is as follows: the graphene is in the form of graphene powder, and the polysilazane is in the form of a polysilazane solution. First, the graphene powder and the polysilazane solution are stirred and dispersed to be fully mixed. After the mixture is evenly mixed, the remaining raw materials are added under stirring to prepare the ink.

[0004] However, in this document, the graphene heating ink obtained has the defect of high cost due to the high price of polysilazane therein.

[0005] Chinese patent application (CN112996153A) discloses a graphene heating plate and its preparation method and application. The preparation method of the graphene heating plate is as follows: S1. Graphene is coated on the surface of glass powder to generate graphene-coated glass powder; S2. The graphene-coated glass powder is mixed with glass powder, organic carrier, and silane coupling agent in a preset weight ratio (1 part of graphene-coated glass powder, 0.2-0.5 parts of glass powder, 10 parts of organic carrier, and 0.5-1.5 parts of silane coupling agent) to obtain graphene conductive slurry; S3. The graphene conductive slurry is spread on a substrate and then baked and cured to form a graphene conductive heating layer; S4. The graphene conductive heating layer is wired and insulated to generate a graphene heating plate.

[0006] However, in this document, since the working temperature of the glass powder is relatively low, the graphene heating plate produced has the defect of having a relatively low stable working temperature.

[0007] Accordingly, the art needs a new technical solution to solve the above problems. Summary of the invention

[0008] Technical issues

[0009] The present invention is proposed to solve the above technical problems at least to a certain extent.

[0010] Technical Solution

[0011] In view of this, the first aspect of the present invention provides a water-soluble, high-temperature resistant infrared carbon-based heating slurry, which comprises water and a slurry matrix, and the components of the slurry matrix are mixed according to the following weight ratio: 15-20 parts of 40-50wt% phosphate solution or an amount of phosphate equivalent thereto; 2-14 parts of glass powder; 1-40 parts of carbon-based conductive powder; 5-10 parts of inorganic filler powder; 1-3 parts of tetrabutyl titanate; 1-5 parts of high-temperature oxidant; 0.1-5 parts of dispersant; 1-20 parts of film-forming agent; 0.1-3 parts of leveling agent; 0.1-3 parts of anti-settling agent; 0.01-3 parts of defoaming agent; and 0.01-3 parts of thickener.

[0012] Through such a composition, a composition method of a water-soluble high-temperature resistant infrared carbon-based heating slurry is provided.

[0013] Specifically, the phosphate solution is used as a binder. Compared with organic binders, it has better heat resistance and weather resistance, that is, the phosphate solution mainly plays a bonding role, and it can resist high temperature while playing a bonding role. The carbon-based conductive powder plays a conductive role, generates heat when powered on, and can have an infrared radiation effect. The inorganic filler can be selected according to the corresponding functional materials to enhance radiation, adjust the temperature coefficient of resistance, enhance thermal conductivity and enhance insulation. The tetrabutyl titanate is a coupling agent that can make the phosphates more tightly bonded. The glass powder can achieve high-temperature secondary film formation and play a sealing protection effect at high temperature, so that the prepared heating film can work stably for a long time under high temperature environment. The addition of the high-temperature oxidant has a good antioxidant protection effect on the carbon-based powder in a temperature environment of less than 750°C.

[0014] It should be noted that the amount equivalent to 15-20 parts of phosphate content in a 40-50wt% phosphate solution should be interpreted as: assuming that the mass percentage of the phosphate solution in the commercially available phosphate solution is adjusted or the phosphate solution can be obtained by homemade means, the net content of phosphate should be roughly the same.

[0015] For the above-mentioned water-soluble high-temperature resistant infrared carbon-based heating slurry, in a possible implementation, the slurry matrix also includes the following components mixed in the following weight ratio: 8-12 parts of inorganic sol; and / or 0.1-10 parts of oxygen absorbent.

[0016] Through such a composition, a preferred composition mode of the water-soluble high-temperature resistant infrared carbon-based heating slurry is provided.

[0017] For the above-mentioned water-soluble high-temperature resistant infrared carbon-based heating slurry, in a possible implementation manner, the inorganic sol includes aluminum-based sol; and / or the oxygen absorber is elemental boron powder and / or metal boride.

[0018] The aluminum-based sol can greatly improve the bonding properties of adhesives such as aluminum dihydrogen phosphate and participate in film formation, and has a great promoting effect on the adhesion strength and thermal shock resistance at high temperatures. Therefore, by combining aluminum dihydrogen phosphate and aluminum-based sol as adhesives, the effect of complementary performance advantages can be achieved.

[0019] For the above-mentioned water-soluble high-temperature resistant infrared carbon-based heating slurry, in a possible implementation manner, the aluminum-based sol has the following properties: pH is 5-7; and the particle size of the sol particles is 20-80 nm.

[0020] For the above-mentioned water-soluble high-temperature resistant infrared carbon-based heating slurry, in a possible implementation manner, the solute of the phosphate solution includes aluminum dihydrogen phosphate and aluminum chromium phosphate; and / or the glass powder is one or more of silicate, borate, silicon boron and phosphate glass; and / or the carbon-based conductive powder is one or more of graphene, nanographite sheets, conductive carbon black, carbon fiber, and carbon nanotubes; and / or the inorganic filler includes thermal conductive powder, insulating powder and TCR (temperature coefficient of resistance) regulator; and / or the high-temperature oxidant is one or more of phosphoric acid, zinc phosphate, triammonium phosphate and boric acid.

[0021] For the above-mentioned water-soluble high temperature resistant infrared carbon-based heating slurry, in a possible implementation manner, the phosphate solution contains a curing agent.

[0022] Aluminum dihydrogen phosphate, aluminum chromium phosphate, etc. combined with a curing agent can have more excellent temperature resistance, bonding properties and low-temperature film-forming properties.

[0023] For the above-mentioned water-soluble high-temperature resistant infrared carbon-based heating slurry, in a possible embodiment, the curing agent includes oxides and / or hydroxides of magnesium, copper, zinc, zirconium and / or aluminum; and / or the content of the curing agent is 2-10wt% of the solute of the phosphate solution.

[0024] Through such a composition, possible forms and specific contents of the curing agent are given.

[0025] For the above-mentioned water-soluble, high-temperature resistant infrared carbon-based heating slurry, in a possible implementation manner, the thermally conductive powder is one or more of inert ceramic powder, cordierite-based infrared radiation powder, transition metal oxide infrared radiation powder and boron nitride; and / or the insulating powder is mica and / or kaolin; and / or the TCR regulator is one or more of ruthenium oxide, modified barium titanate, eucryptite and zirconium phosphate.

[0026] For the above-mentioned water-soluble high temperature resistant infrared carbon-based heating slurry, in a possible implementation manner, the oxygen absorber is elemental boron powder and / or metal boride.

[0027] In summary, the water-soluble high-temperature graphene heating slurry with the above-mentioned components / weight ratio has excellent resistance to high-temperature oxidation and aging after film formation, so it can work stably and reliably for a long time in a high-temperature environment. In addition, it has extremely high infrared emissivity at high temperatures, which can achieve a large energy-saving effect. In addition, due to the low cost of the raw materials used, the heating slurry also has the advantage of low cost. In this way, it can be widely used in high-temperature application fields such as household appliances, industrial baking, boiler heating, etc.

[0028] In the water-soluble high-temperature infrared carbon-based heating slurry of the present invention, the carbon material without glass powder and high-temperature oxidant begins to oxidize in the air above 400°C, which is the fundamental reason for the power attenuation of the carbon-based electric heating slurry. Usually, the highest electric heating working temperature requires that its construction temperature is higher than 200°C, and the carbon-based material will undergo rapid oxidation at a high temperature of 600-800°C. Therefore, inhibiting the oxidation of the material is the core way to improve its high-temperature working performance. Coating, encapsulation, plugging and other treatments can effectively alleviate the oxidation of the carbon material during construction and working at high temperatures, thereby extending the service life of the electric heating film. The phosphates and borates contained in the heating slurry of the present invention can be coated on the surface of the carbon material at low temperatures to block the air; and the elemental boron powder and boride have the function of absorbing oxygen in the air, thereby effectively protecting the carbon material during the construction process and reducing its oxidation degree. Finally, through the combined action of glass powder and high-temperature oxygen absorber, the pores between the materials of the heating slurry are filled, further ensuring the stability of the heating slurry working at high temperatures.

[0029] The second aspect of the present invention provides a method for preparing a water-soluble, high-temperature resistant infrared carbon-based heating slurry, the preparation method comprising: S101, at a temperature of 40-80°C, uniformly mixing at least a phosphate solution, an anti-high-temperature oxidant and water to obtain a first mixed solution; S103, adding at least glass powder, carbon-based conductive powder and inorganic filler powder to the first mixed solution, and dispersing for 0.5-1h, cooling, to obtain a second mixed solution; S105, adding tetrabutyl titanate to the second mixed solution, stirring at a speed of 500-2000r / min for 1-4h, to obtain a third mixed solution; S107, rolling the third mixed solution to a set thickness to obtain the water-soluble, high-temperature resistant infrared carbon-based heating slurry.

[0030] For the preparation method of the above-mentioned water-soluble high-temperature resistant infrared carbon-based heating slurry, in a possible implementation mode, the S101 includes: uniformly mixing a phosphate solution, an anti-high-temperature oxidant, an aluminum-based sol and water to obtain a first mixed solution; and / or the S103 includes: adding glass powder, carbon-based conductive powder, oxygen absorber and inorganic filler powder to the first mixed solution, and dispersing for 0.5-1h, cooling, to obtain a second mixed solution; the S105 includes: adding tetrabutyl titanate to the second mixed solution, and stirring for the first time at a speed of 500-2000r / min under a temperature condition of 40-80°C; after cooling, adding a dispersant, a film-forming agent, a leveling agent, an anti-settling agent, a defoaming agent and a thickener, and stirring for a second time at a speed of 500-2000r / min.

[0031] It can be understood that the preparation method of the water-soluble high-temperature resistant infrared carbon-based heating slurry has at least all the technical effects of any of the water-soluble high-temperature resistant infrared carbon-based heating slurry described above, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The water-soluble high temperature resistant infrared carbon-based heating slurry and its preparation method of the present invention are described below in conjunction with the embodiments.

[0033] Figure 1 A schematic flow chart showing a method for preparing a water-soluble high-temperature resistant infrared carbon-based heating slurry according to an embodiment of the present invention. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0035] In addition, in order to better illustrate the present invention, many specific details are given in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In some examples, the slurry preparation process well known to those skilled in the art is not described in detail in order to highlight the main purpose of the present invention.

[0036] The present invention provides a water-soluble high-temperature resistant infrared carbon-based heating slurry, which can be used as a water-soluble high-temperature carbon-based electric heating coating, etc. In a possible embodiment, the heating slurry includes water and a slurry matrix, and the components of the slurry matrix are mixed according to the following weight ratio: 15-20 parts of a 40-50wt% phosphate solution or an amount of phosphate equivalent thereto (this embodiment is described by taking 15-20 parts of a 40-50wt% phosphate solution as an example); 2-14 parts of glass powder; 1-40 parts of carbon-based conductive powder; 5-10 parts of inorganic filler powder; 1-3 parts of tetrabutyl titanate; 1-5 parts of high-temperature oxidant resistance; 0.1-5 parts of dispersant; 1-20 parts of film-forming agent; 0.1-3 parts of leveling agent; 0.1-3 parts of anti-settling agent; 0.01-3 parts of defoaming agent; 0.01-3 parts of thickener.

[0037] In a possible embodiment, the phosphate solution is selected from commercial aluminum dihydrogen phosphate and aluminum chromium phosphate, and is combined with magnesium, copper, zinc, zirconium, and aluminum oxides or hydroxides as curing agents contained in the phosphate solution, such as the curing agent is usually 2-10wt% of the solid content of the phosphate solution.

[0038] In a possible implementation manner, the glass powder is selected from one or more mixtures of silicate, borate, borosilicate and phosphate glasses having acid resistance and a full melting temperature between 300-1050°C.

[0039] In a possible implementation manner, the carbon-based conductive powder is selected from one or more of graphene, nanographite sheets, conductive carbon black, carbon fiber and carbon nanotubes.

[0040] In one possible implementation, the inorganic filler mainly includes (high) thermal conductive powder, insulating powder and TCR regulator, wherein the (high) thermal conductive powder is selected from one or more of inert ceramic powder, cordierite-based infrared radiation powder, transition metal oxide infrared radiation powder and boron nitride, the insulating powder is selected from one or more of mica and kaolin, and the TCR regulator is selected from one or more of ruthenium oxide, modified barium titanate, eucryptite and zirconium phosphate.

[0041] In a possible implementation, the high temperature oxidation resistance agent is selected from one or more mixtures of phosphoric acid, zinc phosphate, triammonium phosphate or boric acid.

[0042] Preferably, the slurry matrix further comprises the following components mixed in the following weight ratio: 8-12 parts of inorganic sol; 0.1-10 parts of oxygen absorbent.

[0043] Among them, the main function of inorganic sol is to improve the high temperature stability of the slurry. Boron oxygen absorbers can be continuously oxidized in the air at 600-850℃. In addition to the function of taking away oxygen from the surface of the conductive phase to protect the conductive material from oxidation, they can also form a highly viscous, low melting point glass phase, which seals the gaps left by the solidification and shrinkage of phosphates, and fuses with the surrounding glass powder to form borosilicate glass with better performance.

[0044] It is understandable that those skilled in the art can add an appropriate amount of water to form a slurry according to actual needs, such as the slurry containing 10-100 parts of water (excluding water used as a solvent in the phosphate solution).

[0045] In a possible embodiment, the inorganic sol comprises an aluminum-based sol, which is a viscous colloid with a pH of 5-7, a colloidal particle size of 20-80 nm, and good transparency, and produces active alumina or high-purity alumina after high-temperature dehydration. Optionally, the aluminum-based sol may also comprise other inorganic sols such as nano zirconium sol, nano titanium sol, nano yttrium sol, and nano silica sol.

[0046] In a possible implementation, the oxygen absorber may be elemental boron powder, metal boride, or the like.

[0047] Reference Figure 1 , Figure 1 The schematic diagram of the process of preparing a water-soluble high temperature resistant infrared carbon-based heating slurry according to an embodiment of the present invention is shown. Figure 1 As shown, in a possible implementation manner, the preparation method mainly comprises the following steps:

[0048] S101. At a temperature of 40-80° C., uniformly mix aluminum-based sol, phosphate solution, high-temperature oxidant inhibitor and water to prepare a first mixed solution.

[0049] S103, adding glass powder, carbon-based conductive powder, oxygen absorbent and inorganic filler powder to the first mixed solution, and dispersing at high speed for 0.5-1h to obtain a second mixed solution.

[0050] S105. Add tetrabutyl titanate to the second mixed solution, and stir it for the first time at a temperature of 40-80°C and a speed of 500-2000 r / min for 1-4 hours. After cooling (such as cooling to room temperature), add additives (including the aforementioned dispersant, film-forming agent, leveling agent, anti-settling agent, defoaming agent and thickener), and stir it for a second time at a speed of 500-2000 r / min for 1-4 hours at room temperature to obtain a third mixed solution.

[0051] S107. If the third mixed solution is rolled to a corresponding thickness (the thickness is mainly to control the solid content of the slurry, such as 10 μm) using a three-roll rolling mill or other equipment, a water-soluble high-temperature resistant infrared carbon-based heating slurry can be obtained.

[0052] Based on this, the water-soluble high-temperature resistant infrared carbon-based heating slurry and the preparation method thereof of the present invention are further illustrated in combination with four specific embodiments below.

[0053] Embodiment 1:

[0054] In this embodiment, the components of the heated slurry are mixed according to the following weight ratio:

[0055] 8 parts of aluminum-based sol; 20 parts of aluminum dihydrogen phosphate; 8 parts of low-melting-point glass powder; 10 parts of nanographite flakes; 10 parts of alumina powder; 3 parts of tetrabutyl titanate; 3 parts of high-temperature oxidant; 5 parts of oxygen absorber; 5 parts of dispersant; 10 parts of film-forming agent; 2 parts of leveling agent; 0.5 parts of anti-settling agent; 0.5 parts of defoaming agent; 0.1 parts of thickener and 50 parts of water.

[0056] Accordingly, the preparation method of the heated slurry is:

[0057] At a temperature of 60-80° C., uniformly mixing aluminum-based sol, aluminum dihydrogen phosphate, a high-temperature oxidant and water to form a first mixed solution;

[0058] Adding glass powder, carbon-based conductive powder, oxygen absorber and aluminum oxide powder to the first mixed solution and dispersing at high speed for 0.5 h to obtain a second mixed solution;

[0059] Tetrabutyl titanate is added to the second mixed solution, and stirred at a temperature of 60-80° C. and a speed of 1500-2000 r / min for about 3 hours (first stirring);

[0060] After cooling to room temperature, an auxiliary agent was added, and the mixture was stirred at a speed of 500-1000 r / min for about 1 hour (second stirring) to obtain a third mixed solution;

[0061] The third mixed liquid is rolled to 10 μm through a three-roll mill to obtain a water-soluble high-temperature graphene heating slurry.

[0062] The prepared heating slurry is used to make an electric heating element by screen printing. The obtained electric heating element has a film thickness of 30 μm, a square resistance of 43 Ωcm, a TCR value of -800 ppm / °C, and can achieve a heating function of 450°C when powered by 220V.

[0063] Embodiment 2:

[0064] In this embodiment, the components of the heated slurry are mixed according to the following weight ratio:

[0065] 12 parts of aluminum-based sol; 20 parts of aluminum dihydrogen phosphate; 8 parts of low-melting-point glass powder; 2 parts of few-layer graphene; 4 parts of modified cordierite powder; 2 parts of ruthenium oxide powder; 3 parts of synthetic mica powder; 3 parts of tetrabutyl titanate; 2 parts of triammonium phosphate; 1 part of boric acid; 3 parts of elemental boron powder; 3 parts of titanium boride; 5 parts of dispersant; 6 parts of amino resin; 2 parts of dipropylene glycol butyl ether DPNB; 2 parts of leveling agent; 0.5 parts of anti-settling agent; 0.5 parts of defoaming agent; 0.1 parts of thickener and 50 parts of water.

[0066] Accordingly, the preparation method of the heated slurry is:

[0067] At a temperature of 80° C., aluminum-based sol, aluminum dihydrogen phosphate, triammonium phosphate, boric acid and water are uniformly mixed to prepare a first mixed solution;

[0068] Adding glass powder, few-layer graphene powder, elemental boron powder, titanium boride powder, ruthenium oxide powder, synthetic mica powder and modified cordierite powder to the first mixed solution, and dispersing at high speed for 1 hour to obtain a second mixed solution;

[0069] Tetrabutyl titanate was added to the second mixed solution, and stirred at 80° C. and 2000 r / min for 3 h;

[0070] After cooling to room temperature, an auxiliary agent was added, and the mixture was stirred at a speed of 1000 r / min for 1 h to obtain a third mixed solution;

[0071] The third mixed liquid was rolled to 10 μm by a three-roll mill to obtain a water-soluble high-temperature graphene heating slurry.

[0072] The prepared slurry is used to make an electric heating element by screen printing. The obtained electric heating element has a film thickness of 15 μm, a square resistance of 100 Ωcm, a TCR value of 120 ppm / °C, and can achieve a heating function of 500°C when powered by 220V.

[0073] Embodiment 3:

[0074] In this embodiment, the components of the heated slurry are mixed according to the following weight ratio:

[0075] 10 parts of aluminum-based sol; 20 parts of aluminum chromium phosphate; 12 parts of low-melting-point glass powder; 15 parts of carbon fiber; 4 parts of synthetic mica powder; 4 parts of bismuth oxide powder; 3 parts of tetrabutyl titanate; 2 parts of triammonium phosphate; 3 parts of boric acid; 5 parts of elemental boron powder; 5 parts of dispersant; 6 parts of amino resin; 2 parts of DPNB; 2 parts of leveling agent; 0.5 parts of anti-settling agent; 0.5 parts of defoamer; 0.1 parts of thickener and 50 parts of water.

[0076] Accordingly, the preparation method of the heated slurry is:

[0077] At a temperature of 80° C., aluminum-based sol, aluminum chromium phosphate, triammonium phosphate, boric acid and water are uniformly mixed to prepare a first mixed solution;

[0078] Adding glass powder, carbon fiber powder, elemental boron powder, synthetic mica powder, bismuth oxide powder and modified cordierite powder to the first mixed solution, and dispersing at high speed for 1 hour to obtain a second mixed solution;

[0079] Tetrabutyl titanate was added to the second mixed solution, and stirred at 1000 r / min for 2 h at 80° C., and after cooling to room temperature, an auxiliary agent was added, and stirred at 800 r / min for 1 h to obtain a third mixed solution;

[0080] The third mixed liquid was rolled to 20 μm by a three-roll mill to obtain a water-soluble high-temperature graphene heating slurry.

[0081] The prepared slurry is used to prepare an electric heating element by screen printing. The obtained electric heating element has a film thickness of 30 μm, a square resistance of 300 Ωcm, a TCR value of -300 ppm / °C, and can achieve a heating function of 400°C when powered by 220V.

[0082] Embodiment 4:

[0083] In this embodiment, the components of the heated slurry are mixed according to the following weight ratio:

[0084] 12 parts of aluminum-based sol; 20 parts of aluminum dihydrogen phosphate; 8 parts of low-melting-point glass powder; 0.5 parts of few-layer graphene; 5 parts of nanographite flakes; 3 parts of synthetic mica powder; 3 parts of tetrabutyl titanate; 4 parts of boric acid; 4 parts of elemental boron powder; 5 parts of dispersant; 6 parts of amino resin; 2 parts of DPNB; 2 parts of leveling agent; 0.5 parts of anti-settling agent; 0.5 parts of defoaming agent; 0.1 parts of thickener and 50 parts of water.

[0085] Accordingly, the preparation method of the heated slurry is:

[0086] At a temperature of 80° C., aluminum-based sol, aluminum dihydrogen phosphate, triammonium phosphate, boric acid and water are uniformly mixed to prepare a first mixed solution;

[0087] Adding glass powder, few-layer graphene powder, nanographite flakes, elemental boron powder and synthetic mica powder to the first mixed solution, and dispersing at high speed for 1 hour to obtain a second mixed solution;

[0088] Tetrabutyl titanate was added to the second mixed solution, and stirred at 2000 r / min for 3 h at 80° C.; after cooling to room temperature, an auxiliary agent was added, and stirred at 1000 r / min for 1 h to obtain a third mixed solution;

[0089] The third mixed liquid was rolled to 10 μm by a three-roll mill to obtain a water-soluble high-temperature graphene heating slurry.

[0090] The prepared heating slurry is used to prepare an electric heating element by screen printing. The obtained electric heating element has a film thickness of 20 μm, a square resistance of 20 Ωcm, a TCR value of -200 ppm / °C, and can achieve a heating function of 500°C when powered by 220V.

[0091] It can be seen that the water-soluble high-temperature graphene heating slurry of the present invention has excellent resistance to high-temperature oxidation and aging after film formation, and can work reliably and stably at high temperatures for a long time. At the same time, the heating slurry has extremely high infrared emissivity at high temperatures, so it can achieve a more obvious energy-saving effect. In addition, the cost of the heating slurry is relatively low, so it is expected to be widely used in high-temperature scenes such as household appliances, industrial baking, boiler heating, etc.

[0092] It should be pointed out that although the various steps in the above embodiments are described in a specific order, those skilled in the art can understand that in order to achieve the effects of the present invention, different steps do not have to be performed in such an order. They can be performed simultaneously or in other orders, and some steps can also be added, replaced or omitted.

[0093] It should be noted that although the preparation method of the water-soluble high temperature resistant infrared carbon-based heating slurry formed in the above specific manner is introduced as an example, those skilled in the art can understand that the present invention should not be limited to this. In fact, the user can flexibly adjust the relevant steps and parameters in the steps according to the actual application scenarios, such as adjusting the stirring time, rolling thickness and other parameters according to actual needs.

[0094] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A water-soluble high temperature resistant infrared carbon-based heating slurry, characterized in that: The heated slurry comprises water and a slurry matrix, and the components of the slurry matrix are mixed according to the following weight ratio: 15-20 parts of 40-50wt% phosphate solution; 2-14 parts of glass powder; 1-40 parts of carbon-based conductive powder; 5-10 parts of inorganic filler powder; 1-3 parts of tetrabutyl titanate; 1-5 parts of high-temperature oxidation inhibitor; 0.1-5 parts of dispersant; 1-20 parts of film-forming agent; 0.1-3 parts of leveling agent; 0.1-3 parts of anti-settling agent; 0.01-3 parts of defoaming agent; 0.01-3 parts of thickener.

2. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 1, characterized in that: The slurry matrix also includes the following components mixed in the following weight ratio: 8-12 parts of inorganic sol; and / or Oxygen absorbent 0.1-10 parts.

3. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 2, characterized in that: The inorganic sol comprises an aluminum-based sol; and / or The oxygen absorbent is elemental boron powder and / or metal boride.

4. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 3, characterized in that: The aluminum-based sol has the following properties: The pH is 5-7; the particle size of the sol is 20-80nm.

5. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 1, characterized in that: The solute of the phosphate solution includes aluminum dihydrogen phosphate, aluminum chromium phosphate; and / or The glass powder is one or more of silicate, borate, borosilicate and phosphate glass; and / or The carbon-based conductive powder is one or more of graphene, nanographite sheets, conductive carbon black, carbon fiber, and carbon nanotubes; and / or The inorganic filler comprises thermal conductive powder, insulating powder and TCR regulator; and / or The high temperature oxidant is one or more of phosphoric acid, zinc phosphate, triammonium phosphate and boric acid.

6. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 5, characterized in that: The phosphate solution contains a curing agent.

7. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 6, characterized in that: The curing agent comprises oxides and / or hydroxides of magnesium, copper, zinc, zirconium and / or aluminum; and / or The content of the curing agent is 2-10wt% of the solute in the phosphate solution.

8. The water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 5, characterized in that: The thermally conductive powder is one or more of inert ceramic powder, cordierite-based infrared radiation powder, transition metal oxide infrared radiation powder and boron nitride; and / or The insulating powder is mica and / or kaolin; and / or The TCR regulator is one or more of ruthenium oxide, modified barium titanate, eucryptite and zirconium phosphate.

9. A method for preparing a water-soluble high temperature resistant infrared carbon-based heating slurry as claimed in any one of claims 1 to 8, characterized in that: The preparation method comprises: S101, uniformly mixing at least a phosphate solution, an anti-high temperature oxidant and water at a temperature of 40-80° C. to prepare a first mixed solution; S103, adding at least glass powder, carbon-based conductive powder and inorganic filler powder to the first mixed solution, dispersing for 0.5-1h, cooling, to obtain a second mixed solution; S105, adding tetrabutyl titanate to the second mixed solution, stirring at a speed of 500-2000 r / min for 1-4 hours to obtain a third mixed solution; S107, rolling the third mixed solution to a set thickness to obtain the water-soluble high-temperature resistant infrared carbon-based heating slurry.

10. The method for preparing the water-soluble high temperature resistant infrared carbon-based heating slurry according to claim 9, characterized in that: The S101 comprises: mixing a phosphate solution, a high temperature oxidant, an aluminum-based sol and water to obtain a first mixed solution; and / or The S103 comprises: adding glass powder, carbon-based conductive powder, oxygen absorbent and inorganic filler powder into the first mixed solution, dispersing for 0.5-1h, cooling, and obtaining a second mixed solution; The S105 includes: Add tetrabutyl titanate to the second mixed solution, and stir for the first time at a temperature of 40-80° C. and a speed of 500-2000 r / min; After cooling, a dispersant, a film-forming agent, a leveling agent, an anti-settling agent, a defoaming agent and a thickener are added, and a second stirring is performed at a speed of 500-2000 r / min to prepare a third mixed solution.

Citation Information

Patent Citations

  • Graphene heating ink, preparation method and application thereof

    CN112521796A

  • Graphene heating plate and preparation method and application thereof

    CN112996153A

  • Water-based slurry for graphene far infrared planar heating element

    CN109688644A

  • Electric heating resistance paste as well as preparation method and application thereof

    CN112670009A

  • Heating element, manufacturing method thereof, composition for forming heating element, and heating apparatus

    KR1020180065886A