A gradient rigid-flexible interconnection method based on liquid metal doping
By using a gradient interconnection method with doped liquid metal on the interface between rigid chips and flexible circuit systems, Young's modulus mismatch problem is solved, mechanical stability and electrical interconnection under high tensile properties are achieved, and the system is improved durability and applicability.
Patent Information
- Application Number
- CN202210755539.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The Young's modulus mismatch problem at the joint interface between rigid chips and flexible circuit systems leads to a decrease in mechanical stability under severe and repeated deformation conditions, and the prior art metal serpentine traces under high tensile loads It is easy to fall off the attached surface, affecting durability and stability.
Using a gradient rigid-flexible interconnection method based on doped liquid metal, by mixing conductive nanomaterials with liquid metals, liquid metal interconnection conductors with different doping ratios, and immersing rigid chip pins into liquid metals with high doping ratios. , realize electrical interconnection and use the doping gradient distribution of conductive nanomaterials to improve interface binding force and conductivity.
Effectively solve the problem of Young's modulus mismatch, realize reliable electrical interconnection and stability under high tensile properties, and the liquid metal doped with conductive nanomaterials has high conductivity, good repeatability and adhesion, which is suitable for Various substrates reduce system manufacturing costs.
Smart Images

Figure CN115175449B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rigid-flexible interconnection, and relates to a gradient rigid-flexible interconnection method based on doped liquid metal. Background Art
[0002] Stretchable flexible electronic systems are developing rapidly in various cross-fields at an unprecedented speed. In particular, rigid-flexible hybrid electronic systems represented by flexible electronic and communication systems, flexible health monitoring equipment and flexible wearable sensors have been widely used in medical, military and robotics fields, triggering important technological changes. Especially in the field of wearable electronic technology, through the perfect adhesion of flexible substrates to the human body, electronic systems are attached to the human skin, realizing a long-term wearable body surface signal detection system.
[0003] In these flexible electronic systems, the detection of ECG, EEG and EMG signals has outstanding medical and health application value. Although flexible electronic systems have very good biocompatibility, due to the large size of their electronic devices and the low integration of devices, it is difficult to realize complex integrated circuit systems and signal processing and information storage of fully flexible electronics. The use of integrated circuit chips based on silicon-based materials is a necessary means to achieve complex signal processing.
[0004] The present invention relates to electrical interconnection technology between rigid circuit systems and flexible circuit systems. The rigid circuit system refers to hard and non-stretchable circuit hardware, while the flexible circuit system refers to a soft circuit system part with a low Young's modulus and elasticity that can be stretched or bent. The rigid-flexible hybrid electronic system is a system composed of a rigid chip and a flexible substrate. The rigid chip part is responsible for fast and complex signal processing and algorithm recognition, and the flexible system part is responsible for the interconnection between rigid chips and flexible intelligent sensing, which well reflects the functional complementarity of rigid and flexible systems.
[0005] However, the inherent Young's modulus mismatch between the rigid system and the flexible system deteriorates the bonding strength of the rigid-flexible interconnect interface under severe and repeated deformation conditions, resulting in a sharp decrease in the mechanical stability of the system. Therefore, how to improve the contradiction of the Young's modulus mismatch between the rigid chip and the flexible interconnect is the key to realizing a highly stretchable rigid-flexible hybrid electronic system.
[0006] Patent document 1 discloses a flexible system that improves comfort and stretchability. While taking into account the overall package thickness, the system replaces the connecting wires between circuits with multiple thin serpentine wires in parallel to improve the stretchability of the overall system. The system uses two buffer structures, a flexible boss array and an embedded fluid cavity, to reduce the stress of the circuit on the skin, thereby improving the comfort when wearing the packaged circuit.
[0007] Patent document 2 discloses a flexible system-level packaging solution for a wearable device. The embodiment disclosed in patent document 2 is directed to an integrated circuit (IC) package. In an embodiment, the integrated circuit (IC) package may include a flexible substrate. The flexible substrate may have a plurality of dies coupled thereto. The IC package may include a first encapsulation material having a first stiffness and disposed on the flexible substrate to at least partially encapsulate each of the plurality of dies. The IC package may also include a second encapsulation material having a second stiffness and disposed on the flexible substrate. In an embodiment, the second stiffness and the first stiffness are different from each other.
[0008] Flexible interconnects use serpentine routing, which can improve the tensile performance of circuit system interconnects to a certain extent. However, serpentine routing will cause the metal wire to warp in three dimensions under a large tensile load, which will cause the following problems:
[0009] On the one hand, the metal serpentine traces are separated from the attached surface or circuit substrate under a large tensile load, which cannot ensure the good bonding performance of the interconnection system. The tensile strain is generally below 100%, which cannot meet the conditions of high tensile properties.
[0010] On the other hand, under a larger tensile load, the metal wire will warp in three dimensions, which will inevitably cause the metal serpentine routing to detach from the attached surface or circuit substrate under a larger tensile load, making it impossible for the interconnection line to maintain good durability and stability under severe and repeated use conditions, thereby increasing the electronic noise of the system.
[0011] Prior art literature
[0012] Patent Document 1 Chinese invention patent application publication number: CN113194601A, publication date: 2021.07.30;
[0013] Patent document 2 Chinese invention patent application publication number: CN105590903A, publication date: 2016.05.18. Summary of the invention
[0014] The purpose of the present invention is to propose a gradient rigid-flexible interconnection method based on doped liquid metal to solve the Young's modulus mismatch problem at the joint interface between the rigid chip and the flexible circuit system, and to achieve electrical interconnection that takes both rigidity and flexibility into consideration.
[0015] In order to achieve the above object, the present invention adopts the following technical scheme:
[0016] A gradient rigid-flexible interconnection method based on liquid metal doping includes the following steps:
[0017] Step 1. Mixing multiple portions of conductive nanomaterials and multiple portions of liquid metal materials in different proportions and stirring them to obtain multiple portions of liquid metals with different conductive nanomaterial doping proportions;
[0018] Step 2. According to the gradient transformation relationship of the conductive nanomaterial doping ratio from high to low or from low to high, the liquid metals with different conductive nanomaterial doping ratios are sequentially connected and combined to form a section of liquid metal interconnection wire.
[0019] Preferably, the gradient rigid-flexible interconnection method based on liquid metal doping also includes:
[0020] Step 3. Immerse the rigid chip pins into the portion of the liquid metal interconnect wire with the highest conductive nanomaterial doping ratio to form electrical interconnections.
[0021] Preferably, in step 1, before doping the conductive nanomaterial, the one-dimensional or two-dimensional conductive nanomaterial is firstly ground, and then the ground conductive nanomaterial is transferred to a sample sieve for screening.
[0022] Preferably, in step 1, the one-dimensional or two-dimensional conductive nanomaterial comprises metal nanoparticles, metal nanowires, carbon-based nanoparticles, carbon-based nanowires, carbon-based nanosheets or transition metal carbides.
[0023] Preferably, in step 1, the liquid metal material includes gallium-indium alloy, gallium-indium-tin alloy, cesium-rubidium-francium alloy or liquid mercury metal.
[0024] Preferably, in step 1, the doping mass ratio concentration of the conductive nanomaterial doped in the liquid metal is in the range of 0 to 30%.
[0025] Preferably, in step 1, the conductivity of the liquid metal after doping with the conductive nanomaterial is in the range of 1×10 5 S / m to 1×10 7 S / m.
[0026] Preferably, the liquid metal interconnect wire formed in step 2 is partitioned according to different doping ratios of the conductive nanomaterial in the liquid metal, and the number of partitions ranges from 2 to 100.
[0027] Preferably, the liquid metal interconnect wire formed in step 2 is divided into zones according to different doping ratios of the conductive nanomaterial in the liquid metal, and the doping ratio of the conductive nanomaterial in each zone changes linearly or nonlinearly.
[0028] Preferably, the liquid metal interconnect wire formed in step 2 is partitioned according to different doping ratios of the conductive nanomaterial in the liquid metal, and the partition with the highest doping ratio appears at one end of the liquid metal interconnect wire.
[0029] The present invention has the following advantages:
[0030] As described above, the present invention relates to a gradient rigid-flexible interconnection method based on doped liquid metal. The rigid-flexible interconnection method proposed in the present invention, the solid-liquid composite interconnection method, can effectively realize the functional complementarity of liquid metal. Through the interconnection interface design of the method, the present invention solves the Young's modulus mismatch problem of the rigid chip and the flexible circuit system at the joint interface, and realizes the electrical interconnection that takes both rigidity and flexibility into account, so that the rigid-flexible hybrid electronic system can still maintain reliable rigid-flexible interface connection and stable electrical properties under high stretchability. In addition, the conductive nanomaterial-doped liquid metal prepared by the method of the present invention has high electrical conductivity, good repeatability and strong adhesion, has good wettability to different metals, can be patterned onto various flexible or rough substrates, and has a wide range of applications. In addition, the liquid metal is recyclable, and the liquid metal can be recycled using alcohol cotton, further reducing the cost of system manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a flow chart for preparing liquid metal doped with conductive nanomaterials in an embodiment of the present invention.
[0032] Figure 2 Schematic diagram of liquid metal after material doping and corresponding physical photograph in an embodiment of the present invention.
[0033] Figure 3 This is an electron microscope photograph of the liquid metal surface after being doped with conductive nanomaterials in an embodiment of the present invention.
[0034] Figure 4 Schematic diagram of the gradient distribution of doping amount in an embodiment of the present invention.
[0035] Figure 5 This is a test diagram of the electrical interconnection performance of liquid metal doped with conductive nanomaterials in an embodiment of the present invention.
[0036] Figure 6 It is a flow chart of a gradient rigid-flexible interconnection method for doping liquid metal in an embodiment of the present invention. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0038] This embodiment describes a gradient rigid-flexible interconnection method based on doped liquid metal to solve the Young's modulus mismatch problem at the joint interface between the rigid chip and the flexible circuit system, and to achieve electrical interconnection that takes both rigidity and flexibility into consideration.
[0039] like Figure 6 As shown, the gradient rigid-flexible interconnection method based on doped liquid metal includes the following steps:
[0040] Step 1. Mix multiple portions of conductive nanomaterials and multiple portions of liquid metal materials in a one-to-one correspondence according to different proportions and stir to obtain multiple portions of liquid metals with different conductive nanomaterial doping proportions.
[0041] Before doping the conductive nanomaterial, the one-dimensional or two-dimensional conductive nanomaterial is fully ground, and then the ground conductive nanomaterial is transferred to a sample sieve for sieving to obtain conductive nanomaterials of a certain particle size and size.
[0042] The one-dimensional or two-dimensional conductive nanomaterials used in this embodiment include, but are not limited to, metal nanoparticles, metal nanowires, carbon-based nanoparticles, carbon-based nanowires, carbon-based nanosheets, or transition metal carbides (MXene), etc.
[0043] Among them, the transition metal carbide (MXene) is a multi-layer clay-like transition metal carbide (MXene).
[0044] The liquid metal used in this embodiment is an amorphous, flowable liquid metal, such as gallium-indium alloy (EGaIn), wherein the electrical conductivity of the gallium-indium alloy can reach 3×10 6 S / m and above.
[0045] Of course, liquid metal is not limited to EGaIn, but also includes gallium indium tin alloy, cesium rubidium francium alloy or liquid mercury metal.
[0046] In this embodiment, the doping mass ratio concentration range of the conductive nanomaterial in the liquid metal is 0 to 30%, for example, forming a doping gradient distribution with a doping mass ratio concentration of 0%, 5%, 10%, 15% and 20% respectively.
[0047] The doping mass ratio concentration is 0%, that is, no doping.
[0048] Take liquid metal doped with conductive nanomaterials at a doping ratio of 5% by mass as an example:
[0049] Pour 5g of conductive nanomaterial into a beaker containing 100g of liquid metal in small amounts over and over again, stirring rapidly with a stirring rod or other stirring equipment;
[0050] When the liquid metal completely wraps the conductive nanomaterial, the entire doping process is completed.
[0051] According to the above method, this embodiment can respectively dope liquid metals in a certain gradient, for example, liquid metals with doping mass ratios of conductive nanomaterials of 5%, 10%, 15%, and 20% respectively.
[0052] Liquid metals with different doping ratios have different fluidity, surface tension, and bonding strength with rigid chip pins. The surface morphology changes. As the doping amount of conductive nanomaterials increases, the liquid metal gradually changes from a highly fluid liquid oily state to a semi-solid viscous state with a rough surface morphology. In addition, liquid metals with different doping ratios have different electrical conductivities and adhesions. Generally, the doping of high-conductivity nanomaterials has little effect on the conductivity of liquid metals, and doping significantly improves the adhesion between liquid metals and rigid chip pins.
[0053] Liquid metal doped with conductive nanomaterials has a conductivity range of 1×10 5 S / m to 1×10 7 S / m.
[0054] In the process of manufacturing rigid-flexible hybrid electronic systems, the interconnect wire part is required to have good tensile properties. Therefore, the liquid metal should ensure its fluidity. Therefore, pure liquid metal without nanomaterial doping can be used.
[0055] At the rigid-flexible interface, the interconnected liquid metal and the rigid chip pins need to have better bonding and adhesion to ensure the electrical interconnection stability of the device under stretching. Therefore, liquid metal with a larger doping amount is required.
[0056] Therefore, the present invention proposes a segmented doping method with gradient doping distribution to achieve electrical interconnection reliability and stability under large tensile loads. For example, undoped or 5% low-doping liquid metal is used because it has fluidity and better stretchability, which can ensure the high stretchability of rigid-flexible hybrid electronic systems. Liquid metal with a high doping ratio of 20% is used at the chip pins to make it have better adhesion to the chip pins. This method of achieving functional complementarity between MXene-EGaIn is called solid-liquid composite interconnection method, and a transitional doping liquid metal distribution is used between the above two parts.
[0057] Step 2. According to the gradient transformation relationship of the conductive nanomaterial doping ratio from high to low or from low to high, the liquid metals with different conductive nanomaterial doping ratios are sequentially connected and combined to form a section of liquid metal interconnection wire.
[0058] According to different doping ratios of the conductive nanomaterial in the liquid metal, the liquid metal interconnect wire formed in step 2 is partitioned, and the number of partitions ranges from 2 to 100, such as 5, 10, 20, 50, etc.
[0059] The specific number of partitions can be determined according to the actual application scenario.
[0060] According to the different doping ratios of the conductive nanomaterials in the liquid metal, the liquid metal interconnection wires formed in step 2 are divided into zones, and the doping ratios of the conductive nanomaterials in each zone change linearly.
[0061] For example, after division, the formed liquid metal interconnect wire has five doping zones, the doping ratio of the conductive nanomaterial in the first doping zone is 0%, and the doping ratios of the second to fifth doping zones are 5%, 10%, 15% and 20% respectively.
[0062] Of course, the change of the doping ratio in each doping subarea may also be nonlinear, which will not be described in detail here.
[0063] According to the different doping ratios of the conductive nanomaterial in the liquid metal, the liquid metal interconnection wire formed in step 2 is partitioned, and the partition with the highest doping ratio appears at the end of the interconnection wire.
[0064] Step 3. Immerse the rigid chip pins in the liquid metal interconnect wire at the location with the highest conductive nanomaterial doping ratio to form electrical interconnection, and package the liquid metal interconnect wire to form a rigid-flexible hybrid electronic system.
[0065] In this embodiment, the gradient-doped liquid metal interconnect wire can form a corresponding circuit pattern by using a microchannel method, and of course, can also form the corresponding circuit pattern by directly using a mask plate brushing method.
[0066] The rigid chip is then installed in the corresponding position, and its rigid pins are immersed in highly doped liquid metal to form a stable electrical interconnection. After the entire system is encapsulated, a complete rigid-flexible hybrid electronic system is obtained.
[0067] In the embodiment of the present invention, the packaging material of the rigid-flexible hybrid electronic system is preferably the flexible material Ecoflex, and the rigid chip used is a chip required for the rigid-flexible hybrid electronic system to realize a certain function.
[0068] Of course, the packaging material can also be PDMS, PDMS or Ecoflex as a flexible substrate, which has low cost and excellent stretchability.
[0069] Taking the mask brushing method as an example, the formation process of the rigid-flexible hybrid electronic system is explained.
[0070] 1. Design a rigid-flexible hybrid electronic system, select the appropriate chip, and design a mask for patterning liquid metal.
[0071] 2. Spin-coat the flexible substrate Ecoflex on the glass sheet at a speed of 200 rpm for 10 seconds. The speed and spin-coating time in this embodiment are only exemplary, and the speed can be selected in the range of 150-250 rpm and the time is 8-15 seconds.
[0072] 3. The glass sheet with the Ecoflex spin-coated bottom layer was placed in an oven for curing at 70° C. for 3 minutes. The temperature and curing time in this embodiment are only exemplary, and the temperature range is 60-80° C. and the curing time is 2-4 minutes.
[0073] 4. Cover the designed mask plate on the flexible substrate Ecoflex, use a roller brush or scraper, and apply liquid metal with different doping concentrations by screen printing to form a concentration gradient distribution.
[0074] 5. Use tweezers to gently peel off the mask to obtain the patterned liquid metal and make sure that every part is conductive.
[0075] 6. Use tweezers to place the chip in the corresponding position and insert the chip pins into the highly doped liquid metal.
[0076] 7. Spin-coat a layer of Ecoflex on the top layer to encapsulate the system and obtain a functional rigid-flexible hybrid electronic system.
[0077] Of course, if the circuit structure has multiple layers, the other layers can be processed in turn according to the above processing method. Among them, the parameters used for packaging, spin coating and curing are the same as steps 1 to 7 above, and finally a rigid-flexible hybrid electronic system is obtained.
[0078] The following is a production example of a flexible simple digital tube to demonstrate the effectiveness of the method of the present invention. Figures 1 to 6 shown.
[0079] The production process of the flexible simple digital tube is as follows:
[0080] a. Prepare the glass substrate and clean and dry it.
[0081] b. Spin coat the first layer of Ecoflex on the glass slide at a speed of 200 rpm for 10 s.
[0082] c. The glass sheet with the Ecoflex spin-coated bottom layer was placed in an oven for curing at 70°C for 3 minutes.
[0083] d. A first mask plate with a conductor pattern is covered on top of the cured Ecoflex. Since the first layer does not involve the interconnection between the flexible material and the rigid chip, MXene-EGaIn with a doping concentration of 0% is printed in sequence with the help of the first mask plate.
[0084] e. Use tweezers to gently peel off the first layer of mask to obtain the patterned liquid metal and make sure that every part is conductive.
[0085] f. Spin coat the second layer of Ecoflex and cure it. The parameters for spin coating and curing are the same as above.
[0086] g. Place a second mask on top of the second Ecoflex layer, and then print the second layer of MXene-EGaIn. The key is to print a 250-micron transition interconnect wire where the LED rigid electronic device is to be placed.
[0087] According to the different doping concentrations, the doping partitions 1-5 are printed in sequence with the help of a mask plate to form MXene-EGaIn whose doping concentration gradually transitions from 20% to 0%, such as Figure 4 As shown, the rest of the interconnects were printed with 0% or 5% MXene-EGaIn.
[0088] The length of each partition is 50um and the width of the interconnect wire is 800 microns.
[0089] h. After all the liquid metal lines are printed, use tweezers to pick up the LED electronic device and place it in the corresponding 20% MXene-EGaIn position, i.e. Figure 4 The partition 1 location is shown in .
[0090] i. Spin-coat the third layer of Ecoflex and cure it for encapsulation. The parameters for spin coating and curing are the same as above.
[0091] Through the above steps a to i, a flexible simple digital tube is finally obtained.
[0092] like Figure 1 Shown is the doping process of Mxene-EGaIn:
[0093] First, put Mxene into a mortar and grind it thoroughly. Figure 1 (a), and then put it into a sample sieve with a smaller aperture for sieving, as shown in Figure 1 As shown in (b), Mxene with a certain particle size and diameter is obtained.
[0094] A certain amount of liquid metal EGaIn and Mxene are poured into a beaker for mixing and doping, such as Figure 1 (c) as shown.
[0095] Due to the high surface tension of liquid metal and the obstruction of the surface oxide film, the Mxene initially poured all floated on the surface of the liquid metal and could not enter the interior of the liquid metal. A stirring rod was then used for rapid mechanical stirring.
[0096] During the stirring process, Mxene is gradually wrapped by a layer of oxide film. This oxide film is formed by oxidation of EGaIn after contact with air. Its main component is gallium oxide (Ga 2 O 3 ), which is conducive to the adhesion of liquid metal to the surface of other materials.
[0097] As the doping ratio Φ increases, more and more EGaIn is oxidized, and the surface morphology changes significantly, and finally a newly doped liquid metal Mxene-EGaIn is obtained, such as Figure 1 (d) as shown.
[0098] Where Φ = m Mxene / m EGaIn , m Mxene is the mass of Mxene, m EGaIn is the mass of EGaIn.
[0099] The microscopic schematic diagram and physical appearance of Mxene-EGaIn with different doping ratios are shown in the figure below. Figure 2 As shown in Figures 2(a) to 2(d), it can be clearly seen that as the doping ratio increases, the fluidity of the liquid metal becomes lower and lower, and the surface tension becomes weaker and weaker.
[0100] Figure 3 (a) is the scanning electron microscope image of Mxene after grinding.
[0101] from Figure 3 (a) to Figure 3 (b) It can be seen that the surface of Mxene is covered with an oxide film, which is Ga 2 O 3 , Figure 3 (c) shows that there are tiny Mxene particles on the surface of Mxene-EGaIn, indicating that most of the Mxene particles are covered by EGaIn.
[0102] Figure 4 A gradient doping diagram shows how liquid metal interconnects are connected.
[0103] In this embodiment, the wires of the interconnection part are composed of Mxene-EGaIn liquid metal with different doping amounts.
[0104] According to the different doping concentrations of Mxene in the liquid metal, the single line of the interconnection part between the flexible system and the rigid system is divided into five doping partitions. In this embodiment, the doping concentrations of the conductive nanomaterials in the five partitions are linearly distributed.
[0105] The concentration of doping partition 1 is 20%, the concentration of doping partition 2 is 15%, the concentration of doping partition 3 is 10%, the concentration of doping partition 4 is 5%, the concentration of doping partition 5 is 0%, and doping partition 1 is connected to the rigid chip pin.
[0106] In this embodiment, the length of each partition is 50 microns, and the width of the interconnection wire is 800 microns.
[0107] Figure 5 The conductivity and adhesion test results of (a) show that the conductivity of Mxene-EGaIn decreases slightly with the increase of doping ratio. This is because the increase of oxidized EGaIn leads to the decrease of fluidity and conductivity of liquid metal.
[0108] Nevertheless, Mxene-EGaIn still has good conductivity and the conductivity meets the requirements for being a stretchable conductor.
[0109] In addition, the surface tension of the oxidized EGaIn is significantly reduced, which enhances the adhesion between the liquid metal and the flexible substrate and is also beneficial to the connection between the liquid metal and the chip pins. This embodiment manufactures liquid metals with different line widths. By comparison, it is found that the resistance gradually increases with the decrease of the line width. Figure 5 (b) as shown.
[0110] The Mxene-EGaIn interconnect wire has good electromechanical properties. This embodiment also tests the resistance change of liquid metals with different line widths under 200% strain, such as Figure 5 (c) is shown. Figure 5 (c) It can be seen that with the increase of tensile strain, the resistance value of the liquid metal increases slightly. This change is much smaller than that of the serpentine electrode. Therefore, when Mxene-EGaIn is used as an interconnect in a rigid-flexible hybrid electronic system, it will not affect the performance of the system under tension.
[0111] in, Figure 5 In (c), the vertical axis R-R0 represents the resistance change of the interconnect wire under stretching, and M-EGaIn is the abbreviation of Mxene-EGaIn. It can be seen from the figure that the interconnection method proposed by the present invention has a smaller resistance change under stretching than the metal serpentine interconnection line, and has a more stable interconnection resistance characteristic.
[0112] In order to evaluate the long-term stability of the liquid metal, the embodiment of the present invention stretched the liquid metal (length 2 cm) to 100% strain for 2000 cycles and still showed good repeatability, such as Figure 5 (d) as shown.
[0113] In addition, the present invention also tests the influence of temperature change on the reliability of Mxene-EGaIn and the IV curve. The results show that within the temperature range of 20°C-100°C, the resistance change of the liquid metal is less than 5%, proving that the conductivity is less affected by temperature changes. Figure 5 (e) In addition, Figure 5 The IV curve of Mxene-EGaIn shown in (f) shows that under the strain condition of 0%-300%, the M-EGaIn interconnect has good electromechanical stability and does not affect the normal operation of the circuit.
[0114] In addition, the present invention also compares the stretching conditions of the pins and liquid metals with different doping ratios. As the stretching length continues to increase, Mxene-EGaIn with different doping ratios show different adhesion capabilities. It is finally concluded that the Mxene-EGaIn with a doping ratio of 20% has the longest stretching length and the best adhesion. Therefore, the present invention selects Mxene-EGaIn with a doping ratio of 20% as the transition interface between the rigid chip pins and the interconnecting wires. The rigid-flexible hybrid electronic system manufactured in this way can better maintain the stability of the rigid-flexible interface during the stretching process, and can thus adapt to large stretching application scenarios.
[0115] In order to prove that the solid-liquid composite interconnection method of the present invention has a significant improvement in stretchability compared to a system not manufactured using this method (manufactured using EGaIn), the present invention also manufactured two LED arrays for stretchability comparison.
[0116] Among them, the production process of the LED array is similar to that of the simple digital tube, which will not be repeated here.
[0117] By comparison, it was found that the LED array manufactured without using this method (ie, manufactured using EGaIn) had unstable contact under a tensile strain of 150%. When the tensile strain reached 200%, EGaIn was directly disconnected from the chip LED and the LED light went out.
[0118] The LED array manufactured by the method of the present invention maintains reliable and stable electrical connection under stretching from 0% to 200%, proving that the method of the present invention has great potential and application prospects in achieving high stretching of rigid-flexible hybrid electronic systems.
[0119] Of course, the above description is only a preferred embodiment of the present invention, and the present invention is not limited to the above embodiments. It should be noted that all equivalent substitutions and obvious deformation forms made by any technician familiar with the field under the guidance of this specification fall within the essential scope of this specification and should be protected by the present invention.
Claims
1. A gradient rigid-flexible interconnection method based on liquid metal doping, characterized in that: The steps include: Step 1. Mixing multiple portions of conductive nanomaterials and multiple portions of liquid metal materials in different proportions and stirring them to obtain multiple portions of liquid metals with different conductive nanomaterial doping proportions; In the step 1, the doping mass ratio concentration of the conductive nanomaterial doped in the liquid metal is in the range of 0 to 30%; Step 2. According to the gradient transformation relationship of the conductive nanomaterial doping ratio from high to low or from low to high, the liquid metals with different conductive nanomaterial doping ratios are sequentially connected and combined to form a section of liquid metal interconnection wire; Step 3. Immerse the rigid chip pins into the portion of the liquid metal interconnect wire with the highest conductive nanomaterial doping ratio to form electrical interconnections.
2. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 1 is characterized in that: In the step 1, before doping the conductive nanomaterial, the one-dimensional or two-dimensional conductive nanomaterial is firstly ground, and then the ground conductive nanomaterial is transferred to a sample sieve for screening.
3. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 2 is characterized in that: In step 1, the one-dimensional or two-dimensional conductive nanomaterial includes metal nanoparticles, metal nanowires, carbon-based nanoparticles, carbon-based nanowires, carbon-based nanosheets or transition metal carbides.
4. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 1, characterized in that: In the step 1, the liquid metal material includes gallium-indium alloy, gallium-indium-tin alloy, cesium-rubidium-francium alloy or liquid mercury metal.
5. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 1, characterized in that: In step 1, the conductivity of the liquid metal after doping with the conductive nanomaterial is in the range of 1×10 5 S / m to 1×10 7 S / m.
6. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 1, characterized in that: According to different doping ratios of the conductive nanomaterial in the liquid metal, the liquid metal interconnection wire formed in step 2 is divided into zones, and the number of the obtained zones ranges from 2 to 100.
7. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 1, characterized in that: According to different doping ratios of the conductive nanomaterial in the liquid metal, the liquid metal interconnection wire formed in step 2 is divided into zones, and the doping ratio of the conductive nanomaterial in each zone changes linearly or nonlinearly.
8. The gradient rigid-flexible interconnection method based on liquid metal doping according to claim 1, characterized in that: According to different doping ratios of the conductive nanomaterial in the liquid metal, the liquid metal interconnection wire formed in step 2 is partitioned, and the partition with the highest doping ratio appears at one end of the liquid metal interconnection wire.