Nanocomposite materials, preparation methods and applications

By generating Fe2O3 nanowire arrays in situ on stainless steel, nanocomposite materials are prepared, which solves the problems of high energy consumption and unstable sterilization effect in electroporation sterilization technology, and realizes low voltage input, high voltage output and long-term high-efficiency water sterilization Effect.

CN115181966BActive Publication Date: 2024-11-01OCEAN UNIV OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210838480.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-18
Publication Date
2024-11-01
Estimated Expiration
2042-07-18

AI Technical Summary

Technical Problem

Although the existing electroporation sterilization technology is fast in water disinfection and has no by-products, it requires extremely high external voltage, resulting in high energy consumption and safety hazards. At the same time, the sterilization effect of the obtained electrode or device is unstable.

Method used

Using stainless steel as the substrate, Fe2O3 nanowire array is generated through oxalic acid replacement and heating reaction, nanocomposite materials are prepared, and tip discharge electrodes or filter devices are formed to realize low voltage input and high voltage output, and obtained through cleaning, acid etching and sintering treatment. Nanocomposites.

Benefits of technology

The water sterilization effect is achieved by more than 99%, and the sterilization effect can last for 5 to 6 hours, improving the stability and safety of the material, and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003749807000000061
    Figure BDA0003749807000000061
  • Figure BDA0003749807000000071
    Figure BDA0003749807000000071
  • Figure BDA0003749807000000081
    Figure BDA0003749807000000081
Patent Text Reader

Abstract

The present application relates to a nanocomposite material, a preparation method and an application thereof. Specifically, the preparation method of the nanocomposite material comprises using stainless steel as a substrate, replacing the Fe element on the surface of the stainless steel with oxalic acid, and heating the stainless steel to generate a Fe2O3 nanowire array to obtain a nanocomposite material. When the nanocomposite material obtained by the preparation method of the present application is prepared into a tip discharge electrode or a tip discharge filter device and applied to water sterilization, in addition to low voltage input and high voltage output, its sterilization effect can reach more than 99%, and the sterilization effect can last for 5 to 6 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to nanocomposite materials, preparation methods and applications, and specifically to nanocomposite materials that can be used to prepare tip discharge electrodes, tip discharge filter devices, etc., preparation methods and applications in the field of water sterilization. Background Art

[0002] Traditional water treatment technologies mainly include chemical methods such as chlorine disinfection and ozone treatment, as well as physical methods such as ultraviolet disinfection and activated carbon adsorption. Due to the limited processing capacity and high cost of physical methods, and the problem that ozone treatment will produce strong oxidative free radicals that are harmful to the human body, chlorine disinfection is currently the most widely used method. However, chlorine disinfection will produce more by-products during water treatment, and these by-products may increase people's risk of disease.

[0003] With the continuous development of nanomaterials, electroporation sterilization technology has emerged in the field of water disinfection. Its disinfection speed is fast, irreversible, and has no by-products. However, ordinary electroporation sterilization technology requires the application of an extremely high external voltage (10 3 V-10 5 V), which also brings about high energy consumption and potential safety hazards.

[0004] The electroporation sterilization technology currently under research uses nanomaterials different from nanorods, such as nanowires, which are needle-shaped and have sharp tips. Nanodischarge materials made of metals, metal oxides or metal non-oxides can achieve the effect of lower voltage input and higher voltage output, thereby using the tip discharge of nanomaterials to achieve water sterilization. For example, the patents CN109665599B, ​​CN110407302B, and CN113321234A that the applicant has applied for. These patents all disclose the sterilization effect of water after a tip discharge electrode or a tip discharge filter device made of a material with a metal as a substrate and a metal oxide or metal sulfide as a nanowire is made, which can achieve low voltage input and high voltage output.

[0005] However, in the above patents, the sterilization effect of the obtained electrode or device is not ideal in terms of stability. Summary of the invention

[0006] The purpose of the present application is to provide a nano-composite material, a preparation method and an application. When the nano-composite material obtained by the preparation method is prepared into a tip discharge electrode or a tip discharge filter device and applied to water sterilization, in addition to low voltage input and high voltage output, its sterilization effect can reach more than 99%, and the sterilization effect can last for 5 to 6 hours.

[0007] The first solution provided in this application is:

[0008] The preparation method of the nano composite material comprises the following steps: using stainless steel as a substrate, replacing Fe elements on the surface of the stainless steel with oxalic acid, and heating the stainless steel to generate Fe2O3 nanowire arrays, thereby obtaining the nano composite material.

[0009] Optionally, the nanowire is needle-shaped, with the bottom end close to the stainless steel substrate and the tip end away from the stainless steel substrate, the nanowire length is 500nm-600nm, the bottom diameter is 150nm-200nm, the tip diameter is 50-150nm, and the bottom diameter: tip diameter is 3:1-4:3.

[0010] Optionally, the stainless steel includes any one of a stainless steel mesh, a non-porous stainless steel plate, and a perforated stainless steel plate.

[0011] Optionally, include the following steps:

[0012] 1) Using stainless steel as the substrate, its surface is cleaned and acid-etched;

[0013] 2) Soaking the acid-etched stainless steel in an ethanol solution of oxalic acid to form a layer of iron oxalate film on the surface of the stainless steel;

[0014] 3) Sintering the stainless steel obtained in step 2) to obtain a nanocomposite material.

[0015] Optionally, the cleaning treatment in step 1) includes ultrasonically cleaning the stainless steel in acetone, ethanol or deionized water for 5 minutes and then drying it.

[0016] Optionally, the acid etching treatment in step 1) includes etching the stainless steel with a hydrofluoric acid solution having a mass concentration of 35% to 37% for 13 minutes to 15 minutes.

[0017] Optionally, the density of the oxalic acid ethanol solution in step 2) is 0.188 g / mL to 0.190 g / mL, and the immersion time of the stainless steel is 90 min to 120 min.

[0018] Optionally, the sintering temperature in step 3) is 350° C. to 400° C., and the sintering time is 60 min to 120 min.

[0019] The present application also provides a second solution, namely, a nanocomposite material prepared by any of the aforementioned preparation methods.

[0020] The present application also provides a third solution, namely, application of the nanocomposite material in the field of water sterilization.

[0021] When the nanocomposite material obtained in the present application is prepared into a tip discharge electrode or a tip discharge filter device and applied to water sterilization, in addition to low voltage input and high voltage output, its sterilization effect can reach more than 99%, and the sterilization effect can last for 5 to 6 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 These are macroscopic morphology images of the stainless steel mesh in Example 1 before and after preparation (a, b).

[0023] Figure 2 These are the microscopic morphology pictures of the Fe2O3NWs composite nanomaterials (c, d) grown in situ on the stainless steel mesh in Example 1. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown herein can be arranged and designed in various different configurations.

[0025] The following is a detailed example of this application plan:

[0026] The present application uses stainless steel, for example, a stainless steel mesh, a non-porous stainless steel plate, a perforated stainless steel plate, etc.; the conventional in-situ preparation of Fe oxide nanowires on an iron plate or stainless steel is usually prepared by thermal oxidation, but practice has confirmed that the Fe oxide nanowires prepared by such a preparation method have two structures, FeO and Fe2O3, and the bactericidal effect of such a bactericidal material is usually not stable enough when used.

[0027] The "in situ" mentioned in this application means that the Fe2O3 nanowires are generated by the reaction of the Fe element of the stainless steel itself, rather than by the reaction of an external iron source. This application provides a method for preparing Fe2O3 nanowires in situ on stainless steel, which mainly adopts the method of first generating a layer of iron oxalate film and then heating the reaction to generate Fe2O3 nanowires.

[0028] The "nanowire" described in this application is different from nanorods. Nanorods do not have a tip shape, while nanowires are needle-shaped and have a tip. Such a structure can better achieve low voltage input and high voltage output. For example, the nanocomposite material used in this application can achieve a low voltage input substrate of 1V to 10V, and its nanowire tip can output 10V. 5 V~10 7 The high voltage of V

[0029] In addition, the nanowires of the nanocomposite material provided in the present application are needle-shaped, with the bottom end close to the stainless steel substrate and the tip end away from the stainless steel substrate. The nanowire length is 500nm to 600nm, the bottom diameter is 150nm to 200nm, the tip diameter is 50 to 150nm, and the bottom diameter: tip diameter is 3:1 to 4:3.

[0030] When applied to the field of water sterilization, the nanocomposite material provided in the present application can be made into an electrode to obtain electricity, or it can be made into a filtering device to obtain electricity, and it can adapt to water flow rates of 0.5L / min to 5L / min.

[0031] In the preparation method of the nanocomposite material described in the present application, the stainless steel is firstly cleaned, and the main purpose of the cleaning treatment is to remove the impurities on its surface. The acid etching treatment is to remove the protective film on the surface of the stainless steel, so as to promote the subsequent formation reaction of the iron oxalate film.

[0032] In order to better illustrate the bactericidal effect of the nanocomposite material obtained in the present application in water, a number of examples are provided below for illustration.

[0033] The nanocomposite materials of each embodiment are prepared by the preparation method provided in this application, which is as follows:

[0034] 1) Stainless steel X is used as a substrate, each of which is cut into a size of 10 cm*10 cm, and its surface is cleaned and acid-etched; the cleaning treatment includes ultrasonic cleaning the stainless steel X with acetone, ethanol or deionized water for 5 minutes and then drying; the acid etching treatment includes etching the stainless steel with a hydrofluoric acid solution with a mass concentration of M / % for T1 / min;

[0035] 2) Soaking the stainless steel after acid etching in an ethanol solution of oxalic acid to form a layer of iron oxalate film on the surface of the stainless steel; the density of the ethanol solution of oxalic acid is N / g / mL, and the immersion time of the stainless steel is T2 / min;

[0036] 3) Sintering the stainless steel obtained in step 2) to obtain a nanocomposite material; the sintering temperature is W / °C, and the sintering time is T3 / min.

[0037] The above parameters are specifically referred to the contents of Table 1, wherein X represents the type of stainless steel, such as stainless steel mesh, non-porous stainless steel plate, and perforated stainless steel plate.

[0038] Table 1

[0039]

[0040]

[0041] the following Figure 1 The following are the macroscopic morphology of the stainless steel mesh used in Example 1 before (a) and after (b) preparation; Figure 2 The microscopic morphology of the Fe2O3NWs nanomaterial (c, d) grown in situ on the stainless steel mesh in Example 1 can be seen from the figure that the surface of the nanocomposite prepared by the preparation method provided in the present application has uniform and dense Fe2O3 nanowires grown, the nanowires are needle-shaped, the bottom is close to the stainless steel substrate, and the tip is far away from the stainless steel substrate. The length of the nanowire is 500nm to 600nm, the bottom diameter is 150nm to 200nm, the tip diameter is 50 to 150nm, and the bottom diameter: tip diameter is 3:1 to 4:3. Such a nanowire structure is conducive to electric field concentration, and the voltage between the internal nanowires can be increased to 10 under a relatively small external voltage (for example, 1V to 10V). 5 V~10 7 V, under this extremely high voltage, the bacteria in the water will be instantly and irreversibly inactivated.

[0042] The nanocomposites prepared above were made into electrodes or filtration pipes, and the electrodes were placed in the same concentration (e.g. 10 4 CFU / mL -1 ) in a flowing bacterial solution and apply an AC voltage of 1 to 10 V, or place an 4 CFU / mL -1 ) is passed into the filter pipe made in different embodiments and an AC voltage of 1V to 10V is applied (the bacterial liquid obtained after bacterial culture is divided into several portions of equal volume. The bacterial species in the embodiment of this application are commercially available Escherichia coli and Staphylococcus aureus as examples, but the method of this application can be applied to all bacterial species, such as bacteria, fungi, etc.; the flow rate of the bacterial liquid can be controlled by a delivery pump, and the flow rate of the bacterial liquid can be controlled to be 0.5L / min to 5L / min), the treated bacterial liquid is collected, and the bacterial liquid tested in different embodiments is diluted with physiological saline, coated on a plate, placed in a constant temperature and humidity chamber for culturing for 15 hours, and then taken out, and observed and counted by plate counting, and the data are counted using the sterilization rate formula. The sterilization rate effect of the water sterilization material obtained in each embodiment at different bacterial liquid flow rates is as shown in the following table.

[0043] Table 2

[0044]

[0045]

[0046] To further illustrate the long-term stability of the nanocomposite materials of the present application in water sterilization technology, the aforementioned embodiments are respectively subjected to 10V electricity in water for 2h, 5h, 6h, and 12h, and then the bacteria solution is passed into the water or the water is placed in the bacteria solution and the electricity is applied to test the sterilization rate according to the experimental method in Table 2 above.

[0047] Table 3

[0048]

[0049]

[0050] It can be seen from the above data that the nanocomposite material provided in the present application can not only effectively improve the sterilization rate, especially the improvement is obvious under high flow rate conditions; and the obtained material also has certain advantages in long-term stability.

[0051] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a nanocomposite material, characterized in that: The following steps are involved: 1) Using stainless steel as the substrate, clean and acid-etch its surface; 2) The stainless steel after acid etching is immersed in an ethanol solution of oxalic acid to form a layer of iron oxalate film on the surface of the stainless steel; 3) Sintering the stainless steel obtained in step 2) at a sintering temperature of 350° C. to 400° C. for a sintering time of 60 min to 120 min to obtain a nanocomposite material; The nanowires of the nanocomposite material are needle-shaped, with the bottom end close to the stainless steel substrate and the tip end away from the stainless steel substrate. The nanowire length is 500nm-600nm, the bottom diameter is 150nm-200nm, the tip diameter is 50-150nm, and the bottom diameter: tip diameter is 3:1-4:

3.

2. The preparation method according to claim 1, characterized in that: The stainless steel includes any one of a stainless steel mesh, a non-porous stainless steel plate, and a perforated stainless steel plate.

3. The preparation method according to claim 1, characterized in that: The cleaning treatment in step 1) includes ultrasonic cleaning the stainless steel in acetone, ethanol or deionized water for 5 minutes and then drying.

4. The preparation method according to claim 1, characterized in that: The acid etching treatment in step 1) includes etching the stainless steel with a hydrofluoric acid solution having a mass concentration of 35% to 37% for 13 minutes to 15 minutes.

5. The preparation method according to claim 1, characterized in that: The density of the oxalic acid ethanol solution in step 2) is 0.188 g / mL to 0.190 g / mL, and the immersion time of the stainless steel is 90 min to 120 min.

6. The nanocomposite material prepared by the preparation method according to claim 1.

7. Use of the nanocomposite material according to claim 6 in the field of water sterilization.