A method for rapidly rejuvenating bulk amorphous alloy without damage and its application

Through the damage-free method of rapid heating and cooling, the problem of degradation of performance of block amorphous alloys after relaxation is solved, and the rapid rejuvenation without damage is achieved, which significantly improves its plasticity and fracture toughness. It is suitable for a wide range of amorphous alloys Material.

CN115198210BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110376211.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-08
Publication Date
2024-11-22
Estimated Expiration
2041-04-08

AI Technical Summary

Technical Problem

The performance of bulk amorphous alloys decreases during the relaxation process, resulting in material embrittlement and short life. Existing rejuvenation methods such as mechanical rejuvenation and low-temperature cycles or damage to samples, limiting their application prospects.

Method used

By rapidly heating the amorphous alloy to the enthalpy relaxation temperature range (Tg-80 K~Tg) and cooling it quickly, a rapid rejuvenation without damage is achieved, and its energy state and structural disorder is improved, thereby improving plasticity and toughness.

Benefits of technology

This method is simple and widely applicable to all kinds of amorphous samples, without destroying the sample shape, significantly improving the mechanical properties, and the plasticity and fracture toughness are much higher than those of cast samples, and are suitable for all bulk amorphous alloy structural materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003011266170000051
    Figure BDA0003011266170000051
  • Figure BDA0003011266170000061
    Figure BDA0003011266170000061
  • Figure BDA0003011266170000071
    Figure BDA0003011266170000071
Patent Text Reader

Abstract

The present invention discloses a method for non-damage-driven rapid rejuvenation of bulk amorphous alloys and its application, belonging to the technical field of improving bulk amorphous alloy structural materials. The method first heats the low-energy amorphous alloy at a rate greater than 2K / s to a temperature below the glass transition temperature T g The present invention rapidly heats the relaxed sample to the enthalpy relaxation temperature range and then rapidly cools it, thereby improving the energy state of the amorphous and making the structure more disordered, thereby solving the problem of deterioration of mechanical properties such as plasticity and toughness of bulk amorphous alloys after relaxation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of improving bulk amorphous alloy structural materials, and in particular to a method for driving rapid rejuvenation of bulk amorphous alloys without damage and application thereof. Background Art

[0002] Amorphous alloy is a new type of metastable material, usually obtained by rapid cooling of molten metal. Amorphous alloy has the characteristics of metal and amorphous, solid and liquid. Since its discovery, due to its unique structure and excellent performance, compared with traditional crystal structure materials, bulk amorphous alloy has excellent properties such as ultra-high strength, high fracture toughness, high hardness, high elasticity, good corrosion resistance, etc. These characteristics make bulk amorphous alloy materials widely used in many fields such as aerospace, military industry, machinery, chemical industry, consumer electronics and medical equipment.

[0003] Since amorphous is a metastable structure obtained by rapid cooling of liquid, this metastable high-energy state structure will spontaneously transform to a lower energy state, and this process is called relaxation. Relaxation has already occurred since the formation of amorphous, or during the formation process, and the energy state of the alloy decreases over time. In addition, the increase in service temperature will also accelerate the relaxation of amorphous materials. This relaxation process will cause atoms to stack more tightly, the energy state will decrease, and its plasticity and toughness will be seriously damaged. A large number of experimental results have shown that this relaxation process will lead to the embrittlement of the material, thus severely limiting the application prospects of amorphous alloys and the service life of amorphous alloys as structural materials.

[0004] Rejuvenation is a means to solve the above problems. It is the reverse process of relaxation. It can make the structure of amorphous materials more disordered, generate more free volume, increase its energy state, and improve its plasticity and toughness. Currently, the commonly used rejuvenation methods are divided into two categories: mechanical rejuvenation (large plastic deformation, elastic loading) and thermal rejuvenation (low temperature cycle). Mechanical rejuvenation has strict requirements on the shape of the sample and will damage the sample. This makes it impossible to use these methods to effectively rejuvenate the formed workpiece, or the sample after rejuvenation is deformed and cannot be used again. However, the low temperature cycle process is cumbersome, usually with more than 30 cycles, which is not conducive to mass industrial production.

[0005] CN1009972065A discloses a method for improving the plasticity of an amorphous alloy by low temperature cycling, wherein an amorphous alloy sample is cycled between liquid nitrogen temperature and room temperature for 30-50 cycles. The method is cumbersome to operate, and the invention simply increases the plasticity of the sample, and the change trend of the hardness and fracture toughness of the alloy is not reported. Summary of the invention

[0006] In response to the problems existing in the above-mentioned methods for rejuvenation of amorphous alloys, the present invention provides a method for non-destructively driving the rapid rejuvenation of bulk amorphous alloys and its application, by rapidly heating the relaxed sample to the enthalpy relaxation temperature range and then rapidly cooling it, thereby improving the energy state of the amorphous material and making the structure more disordered, thereby solving the problem of deterioration in mechanical properties such as plasticity and toughness of bulk amorphous alloys after relaxation.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A method for rapidly rejuvenating a bulk amorphous alloy without damage, comprising the following steps:

[0009] (1) The low-energy amorphous alloy is heated at a rate greater than 2K / s to a temperature below the glass transition temperature (T g ) and hold for 60-1000s;

[0010] (2) Cooling at a cooling rate greater than 100 K / s.

[0011] The reasons causing the amorphous alloy to be in a low energy state include aging factors, stress and heat, mechanical treatment, heat treatment and other methods that can reduce the energy state of the amorphous alloy.

[0012] In step (1), the heating method is resistance furnace heating, induction heating or tubular furnace heating.

[0013] In step (1), the heating temperature is (T g -80 K)~T g between.

[0014] In step (2), the cooling method is rapid quenching such as water quenching, oil quenching, air quenching, brine quenching or other methods that can quickly cool the sample.

[0015] The method for non-damage driven rapid rejuvenation of bulk amorphous alloys is applied to restore the mechanical properties of amorphous alloy structural materials.

[0016] The method of the present invention is used to drive the rapid rejuvenation of bulk amorphous alloys, which has the following advantages compared with the prior art:

[0017] (1) The process of the present invention is simple, widely applicable to various types of amorphous samples, and is non-destructive to the shape and structure of the samples, and has high industrial application value.

[0018] (2) The amorphous alloy sample treated by the method of the present invention still maintains an amorphous structure.

[0019] (3) The mechanical properties of the samples obtained by this rejuvenation method are greatly improved. The plasticity and fracture toughness values ​​of the samples after rejuvenation are much higher than those of the cast samples. The plasticity and fracture toughness of the rejuvenated amorphous samples obtained by the method of the present invention are improved to varying degrees.

[0020] (4) This rejuvenation method is applicable to all bulk amorphous alloy structural materials. As long as the amorphous alloy produces enthalpy relaxation during the relaxation process, it can be rejuvenated according to this method. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The calculation diagram of relaxation enthalpy and enthalpy relaxation based on the design concept of the present invention; wherein: (a) the sample is heated to 823K (higher than the crystallization temperature) and then cooled to room temperature, and the second heating is carried out under the same conditions, and the relaxation enthalpy ΔH rel is the area between the two heating curves; (b) Enthalpy relaxation endothermic enthalpy ΔH endo It is the area between the DSC curve of the sample and the DSC curve of the standard sample, where the standard sample is obtained by first heating the sample to the supercooled liquid region (710K) and then cooling it to room temperature.

[0022] Figure 2 DSC curves of as-cast, relaxed and rejuvenated samples of bulk amorphous alloy; (a) DSC curves of as-cast and relaxed samples. Both samples exhibit the same crystallization behavior. The as-cast sample (dashed line) exhibits an exothermic signal before the glass transition temperature, while the relaxed sample exhibits an endothermic peak in the same temperature range; (b) After rejuvenation of the relaxed amorphous alloy, an exothermic signal peak appears on the DSC curve of the sample, while the endothermic peak almost disappears.

[0023] Figure 3 These are the XRD curves of the as-cast (As-cast), relaxed (Relaxed) and rejuvenated samples of bulk amorphous alloy.

[0024] Figure 4 Hardness and stress-strain curves of the as-cast, relaxed and rejuvenated samples of bulk amorphous alloy; (a) shows the change trend of hardness with rejuvenation temperature after rejuvenation treatment; (b) shows the change trend of compressive plasticity with rejuvenation temperature after rejuvenation treatment.

[0025] Figure 5 Fracture toughness diagram of the as-cast (As-cast), relaxed (Relaxed) and rejuvenated samples of bulk amorphous alloy. DETAILED DESCRIPTION

[0026] The document [Enthalpy relaxation and recovery in amorphous materials. J. Non-Cryst. Solids 169, 211-266 (1994)] points out that enthalpy relaxation is commonly present in low-energy state amorphous materials that undergo relaxation (hereinafter referred to as relaxed samples). The low-energy state amorphous material refers to an amorphous material in a low-energy state. From the classification of alloys, it is mainly applicable to amorphous structural materials such as zirconium-based amorphous alloy systems, lanthanum-based amorphous alloy systems, cerium-based amorphous alloy systems, magnesium-based amorphous alloy systems, and gold-based amorphous alloy systems.

[0027] There are many reasons for the reduction of the energy state of amorphous materials (i.e., relaxation), mainly due to the influence of heat, force, and aging, or the reduction of the energy state of the alloy after mechanical or heat treatment. Taking the relaxation caused by annealing as an example, during the DSC heating process, the relaxed sample at the annealing temperature (T a ) and glass transition temperature (T g ) between the two peaks (see Figure 1 ), this endothermic reaction is a process of increasing enthalpy, that is, a process of increasing the energy of the system. This means that rejuvenation can be achieved when the relaxed sample is placed in this temperature range and then quickly cooled. Figure 2 As can be seen from (a), within the same temperature range, the DSC curve of the relaxed sample changes from the exothermic peak of the cast sample to the endothermic peak, and after rejuvenation, the endothermic peak of the relaxed sample disappears and the exothermic peak reappears, indicating that the sample has been rejuvenated.

[0028] When the relaxation sample is heated to a temperature higher than T g The sample will turn into a supercooled liquid when the temperature drops rapidly, and the cast amorphous alloy will be reformed after rapid cooling in this state. The properties of this alloy are usually worse than those of the original cast state.

[0029] Based on the above research, the general idea of ​​the present invention is to rapidly heat the low-energy amorphous sample to (T g -80K)~T g The sample is then rapidly cooled at a rate greater than 100 K / s to obtain a high-energy state sample (hereinafter referred to as a rejuvenation sample). This method improves the plasticity and toughness of the sample without destroying the shape of the sample, thus achieving rejuvenation.

[0030] The present invention is described below in conjunction with specific embodiments and drawings, but the present invention is not limited thereto.

[0031] Examples 1-18 and Comparative Examples 1-3:

[0032] The samples in Examples 1-13 and Comparative Examples 1-3 mainly have the energy state of the amorphous alloy reduced due to heat treatment, Example 14 has the energy state reduced due to aging factors, and Examples 15-18 have the energy state reduced due to stress factors.

[0033] 1. Energy state reduction caused by heat treatment

[0034] By optimizing parameters, a non-destructive rejuvenation method is adopted for the currently widely used zirconium-based amorphous alloys, lanthanum-based, and cerium-based amorphous alloys. By adjusting the process parameters, the rejuvenation of amorphous alloys can be quickly achieved, thereby improving the performance of the materials. Common systems and corresponding composition ranges are shown in the table below. It should be pointed out that the present invention is based on experimental data obtained in the following alloy system, but is not limited to the following system. The idea of ​​our invention is based on the characteristics of bulk amorphous alloys themselves, namely the concept of "enthalpy relaxation", and is applicable to all bulk amorphous materials in a low-energy state.

[0035] Table 1 Alloy system

[0036]

[0037] The insulation time of sample rejuvenation is related to the sample size and the rejuvenation temperature. When the sample size is larger and the rejuvenation temperature is lower, the insulation time is longer. When the size is smaller and the rejuvenation temperature is higher, the insulation time is correspondingly reduced (see Table 2).

[0038] Table 2 Sample size and corresponding holding time and cooling rate

[0039]

[0040] Taking a 2 mm sample as an example, the preparation steps of the cast, relaxed and rejuvenated samples are as follows:

[0041] 1. Preparation and preliminary treatment of cast samples

[0042] (1) Preparation of as-cast samples: The alloys shown in Table 1 were proportioned according to the corresponding atomic percentages, and then smelted in an arc melting furnace under the protection of a high-purity argon atmosphere. The smelting was repeated 8 times to obtain an alloy ingot. An amorphous plate with a thickness of 2 mm, a width of 24 mm, and a length of 50 mm was obtained by a copper mold casting method. The alloy ingot was melted and then sucked into a copper mold by a copper mold suction casting method to prepare an amorphous alloy cast rod sample with a diameter of 2 mm.

[0043] (2) Preliminary treatment of fracture specimens: Use wire cutting to cut the plate sample prepared in step (1) into a 2mm*4mm*16mm plate sample, then use diamond wire cutting to preform a notch with a width of 200μm and a depth of 0.8mm, and then perform fatigue crack preformation after polishing. Preliminary treatment of compression specimens: Use a diamond cutting machine to cut the cast rod sample prepared in step (1) into a 35mm*Ф2mm block sample, use #400-#2000 sandpaper to grind the upper and lower bottom surfaces of the rod sample from coarse to fine to keep them parallel, and then polish them into a mirror surface.

[0044] 2. Preparation of relaxation samples:

[0045] The as-cast samples were annealed at the temperature and time specified in the table. The different annealing conditions are to make the samples reach a lower energy state in a short time. The rejuvenation effect is not affected by the annealing conditions. In order to facilitate the comparison of the rejuvenation effects of samples of the same system, the annealing conditions of the same alloy composition are the same.

[0046] 3. Preparation of rejuvenation samples:

[0047] The relaxed samples were cut into cylinders with a length of 4 mm and a diameter of 2 mm, and placed in a tube furnace set at a specific temperature. The heating temperature and heating time are shown in Table 3. The samples were then quenched in ice water to obtain the rejuvenation samples.

[0048] Table 3 below shows the alloy compositions, annealing conditions and rejuvenation conditions of Examples 1-13 and Comparative Examples 1-3.

[0049] Table 3 Annealing conditions and rejuvenation conditions of each embodiment

[0050]

[0051] 4. Characterization of rejuvenation samples

[0052] (1) Thermal analysis of rejuvenation samples: DSC test of the rejuvenation samples

[0053] from Figure 2 It can be seen that the samples without rejuvenation treatment have a a ) and glass transition temperature (T g ) shows an endothermic peak. After the sample is treated with rejuvenation, the endothermic peak disappears and the glass transition temperature (T g ) The exothermic peak before reappears. This indicates that the energy state of the sample has been improved and rejuvenation has been achieved.

[0054] (2) XRD characterization of the rejuvenated sample 1

[0055] By analyzing the X-ray diffraction patterns of the rejuvenated samples, Figure 3As shown, the diffraction pattern shows the typical bun peaks of amorphous alloys, and no sharp crystal diffraction peaks are found, indicating that the sample has a completely amorphous structure.

[0056] (3) Quasi-static compression test

[0057] Quasi-static compression tests were carried out at room temperature with a strain rate of 5×10 -4 s -1 The compression plasticity of the relaxed samples, cast samples and rejuvenated samples was compared. The experimental results are shown in Table 4 and Figure 4 .

[0058] (4) Fracture toughness test

[0059] The fracture toughness test was carried out on the samples, and the fracture toughness of the relaxed samples, cast samples and samples after rejuvenation were compared. The experimental results are shown in Table 4 and Figure 5 .

[0060] Table 4 Hardness, plasticity and fracture toughness values ​​of cast samples, relaxed samples and rejuvenated samples

[0061]

[0062] 2. Energy state reduction caused by time factors

[0063] Embodiment 14

[0064] (1) A gold-based alloy having a composition of (at.%) Au 50 Cu 22.5 Ag 7.5 Si 17 The alloy strips with a size of 1.5mm*40μm were placed at room temperature and left to stand for 2 years to obtain a low-energy amorphous sample. The strips were heated to 388K at a rate of 2K / s and then rapidly cooled to obtain a rejuvenation sample.

[0065] (2) The bending failure strain of the sample was measured to decrease from 100% of the as-cast sample to 3% of the annealed state, and then recovered to 100% of the as-cast sample.

[0066] 3. Energy state reduction caused by stress factors

[0067] Table 5 Rejuvenation conditions of the embodiment of energy state reduction caused by stress factors

[0068]

[0069] Examples 15-18

[0070] (1) An amorphous alloy, the composition of which is shown in Table 5, is placed on an Instron E3000 fatigue tester within the elastic range (0.2-0.8σ y) was subjected to cyclic loading for 30,000 cycles to obtain a relaxed state sample. The relaxed state sample was then rejuvenated under the conditions in Table 5.

[0071] (2) The measured compressive strain results are shown in Table 6 below.

[0072] Table 6 Hardness and plasticity values ​​of Examples 15-18

[0073]

Claims

1. A method for rapidly rejuvenating bulk amorphous alloy without damage, characterized in that: The method comprises the following steps: (1) Heating the low-energy amorphous alloy to a temperature below the glass transition temperature at a rate greater than 2 K / s T g Then hold for 60-1000 s; (2) Cooling at a cooling rate greater than 100 K / s; In step (1), the heating temperature is ( T g -80 K)~ T g between; The low-energy amorphous alloy refers to an amorphous alloy whose energy state is reduced by one or more of aging factors, force, and mechanical treatment.

2. The method for non-destructively driving rapid rejuvenation of bulk amorphous alloy according to claim 1, characterized in that: The low-energy amorphous alloy can also be heat treated to reduce the energy state of the amorphous alloy; The heat treatment method is high temperature annealing, that is, the bulk amorphous alloy is annealed at an annealing temperature T a Keep warm for 6-9 hours to reduce the energy state of the amorphous alloy, T a =300-570K.

3. The method for non-destructively driving rapid rejuvenation of bulk amorphous alloy according to claim 1, characterized in that: In step (1), the heating method is resistance furnace heating, induction heating or tubular furnace heating.

4. The method for non-destructively driving rapid rejuvenation of bulk amorphous alloy according to claim 1, characterized in that: In step (2), the cooling method is ice water rapid quenching.