A PMMA / PVDF composite diaphragm and its preparation method and application
By coating PMMA/PVDF composite agglomerates on the lithium battery separator, the problem of insufficient adhesion between the lithium battery separator and the pole pieces and the insufficient shuttle properties of lithium ions is solved. The cycle performance and hardness of the battery are improved, and the battery bulge is avoided and maintained. Increased capacity and breathability.
Patent Information
- Application Number
- CN202211016652.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-08-24
AI Technical Summary
Existing lithium battery separators have deficiencies in pole piece adhesion and lithium ion shuttling, resulting in battery cycle performance and storage space problems. In particular, secondary particle size PVDF hinders lithium ion shuttling, resulting in reduced ion conductivity.
PMMA/PVDF composite agglomerates are used to form composite agglomerates by agglomerating PMMA particles and PVDF particles, and are coated on the heat-resistant layer of the separator to improve the lithium ion shuttle channel and enhance the adhesion between the separator and the pole piece. Cover ensures storage space and breathability.
It improves the cycle performance and hardness of lithium batteries, avoids battery bulging, and maintains high capacity retention and breathability.
Smart Images

Figure CN115207566B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of secondary batteries, and in particular to a PMMA / PVDF composite diaphragm and a preparation method and application thereof. Background Art
[0002] Lithium batteries can be divided into four parts in terms of structure: positive and negative electrodes, electrolyte and diaphragm. As an isolation barrier between the positive and negative electrodes of lithium batteries, the diaphragm plays an important role in the battery. It provides a channel for the shuttle of lithium ions and blocks the passage of electrons. However, due to its poor heat resistance, the industry coats a heat-resistant layer on one or both sides of the diaphragm to improve the overall heat resistance of the diaphragm. Since the heat-resistant layer has no bonding effect with the positive and negative electrodes, the battery end appears soft. In order to give the battery a certain hardness, it is often necessary to coat a layer of glue on the heat-resistant layer to improve the adhesion between the diaphragm and the pole piece. PVDF is widely used as a glue layer in lithium battery diaphragms due to its corrosion resistance, easy adhesion, and liquid retention. This increases the adhesion between the diaphragm and the pole piece and ensures the hardness of the battery. However, as people's requirements for the adhesion between diaphragms and pole pieces become higher and higher, the adhesion between pure PVDF and the pole piece does not meet the requirements.
[0003] PMMA, commonly known as acrylic, has much stronger wettability with electrolyte and adhesion to positive and negative electrodes than PVDF. However, since PMMA is an amorphous polymer, it will swell continuously after being soaked in electrolyte until it dissolves. Therefore, pure PMMA is rarely applied on the market to improve the adhesion between the diaphragm and the pole piece. The shaped area and the amorphous area of PVDF used for the diaphragm each account for half, so the existing technology often combines PMMA and PVDF to improve the adhesion between the diaphragm and the pole piece.
[0004] For example, the Chinese invention patent with announcement number CN108807804B uses nano-level PVDF and nano-level PMMA mixed spraying to obtain a 0.1µm~2µm dot-sprayed diaphragm. Although it improves the adhesion between the diaphragm and the electrode, the nano-level PVDF and PMMA are easy to block the holes, resulting in an increase in the overall air permeability time of the diaphragm. In addition, the maximum height of the nano-level PVDF and PMMA spray points is only 2µm. After the spray layer and the electrode are hot-pressed and bonded, the spray layer is compressed and the lateral space becomes smaller. PVDF and PMMA swell after absorbing electrolyte and can only expand longitudinally, which will inevitably lead to battery bulging. Therefore, the nano-level PVDF and PMMA mixed spraying cannot meet the storage space requirements of the prior art for the spray layer and the electrode.
[0005] The Chinese invention patent with announcement number CN110048057B uses coupling agents to improve the compatibility of PVDF and PMMA, obtaining a 0.1~4µm full-coated PMMA and PVDF mixed coating. Although the adhesion between the diaphragm and the electrode is improved, the introduction of the coupling agent greatly increases the air permeability time of the diaphragm, thereby increasing the internal resistance of the diaphragm. In addition, after PVDF and PMMA absorb electrolyte and swell, it is bound to cause battery bulging.
[0006] In this regard, in order to increase the storage space of the diaphragm and the pole piece, the prior art introduces secondary particle size PVDF, which is formed by agglomeration of primary particle size PVDF, and the particle size can reach the micron level. Mixing and spraying with PMMA can meet the storage space requirements of the diaphragm and the pole piece, and can also improve the adhesion between the diaphragm and the pole piece. For example, the Chinese invention patent application with publication number CN114221088A uses PMMA emulsion and secondary particle size PVDF mixed coating to obtain a composite diaphragm with a coating of 1.0~4.5µm, which effectively improves the adhesion between the diaphragm and the pole piece, and has a certain storage space. However, since the shaped area and the unshaped area of the PVDF used for the diaphragm each account for half, lithium ions cannot pass through the shaped area, so the secondary particle size PVDF will seriously hinder the passage of lithium ions, increase the resistance of ion passage, thereby reducing the ionic conductivity and affecting the cycle performance of the battery end. Summary of the invention
[0007] The purpose of this application is to provide a PMMA / PVDF composite diaphragm and its preparation method and application, which has a certain storage space when the composite diaphragm is bonded to the pole piece, can improve the adhesion between the composite diaphragm and the pole piece, and can also improve the resistance of the secondary particle size PVDF to the shuttle of lithium ions, thereby improving the cycle performance of the battery.
[0008] To achieve the above-mentioned purpose, the embodiment of the present application adopts the following technical scheme: a PMMA / PVDF composite diaphragm, comprising: a base film, the base film is a porous film; a heat-resistant layer, the heat-resistant layer is arranged on at least one side surface of the base film; an organic layer, the organic layer is arranged in dots on the surface of the heat-resistant layer, and the organic layer includes PMMA / PVDF composite agglomerates, a binder and a defoaming agent; the PMMA / PVDF composite agglomerates are formed by the agglomeration of PMMA particles and PVDF particles, and the mass ratio of the PMMA particles to the PVDF particles is between 3:7 and 5:5.
[0009] In the above technical scheme, the embodiment of the present application agglomerates PMMA particles and PVDF particles to form PMMA / PVDF composite agglomerates, which are coated on the heat-resistant layer of the diaphragm. The PMMA in the agglomerates can provide channels for lithium ions to shuttle through the secondary particle size agglomerates, thereby improving the hindrance of the secondary particle size PVDF to the shuttle of lithium ions, thereby improving the cycle performance of the battery; the introduction of PMMA increases the adhesion between the diaphragm and the electrode, and improves the hardness of the battery; the use of point-like coating of PMMA / PVDF composite agglomerates has little effect on the overall air permeability of the diaphragm, and can ensure that the diaphragm and the electrode have a certain storage space, and can also store electrolyte, thereby improving the capacity retention rate of the battery and effectively avoiding the bulging phenomenon at the battery end.
[0010] Further, according to an embodiment of the present application, the thickness of the heat-resistant layer is 1-3µm.
[0011] Further, according to an embodiment of the present application, the heat-resistant layer includes ceramics, a stabilizer, glue and a wetting agent.
[0012] Further, according to an embodiment of the present application, the particle size of the ceramic is 0.5-1.2µm.
[0013] Further, according to an embodiment of the present application, the added amount of the stabilizer is 0.4-2wt% of the ceramic ratio.
[0014] Further, according to an embodiment of the present application, the amount of glue added is 2-8wt% of the ceramic ratio.
[0015] Further, according to an embodiment of the present application, the added amount of the wetting agent is 0.2-2wt% of the ceramic ratio.
[0016] Further, according to an embodiment of the present application, the particle size of the PMMA particles is 250-400 nm.
[0017] Further, according to an embodiment of the present application, the particle size of the PVDF particles is 150-280 nm.
[0018] Further, according to an embodiment of the present application, the particle size of the PMMA / PVDF composite agglomerates is 4-8µm.
[0019] Further, according to an embodiment of the present application, the added amount of the binder is 4-12wt% of the PMMA / PVDF composite agglomerate.
[0020] Further, according to an embodiment of the present application, the added amount of the defoaming agent is 0.5-2wt% of the PMMA / PVDF composite agglomerate.
[0021] Further, according to an embodiment of the present application, the thickness of the base film is 5-20µm.
[0022] In order to achieve the above object, the present application also discloses a method for preparing a PMMA / PVDF composite diaphragm, comprising the following steps:
[0023] Coating the heat-resistant layer: coating the heat-resistant layer slurry on at least one side of the surface of the base film;
[0024] Coating the organic layer: taking the PMMA / PVDF composite aggregate, the binder and water, mixing them, and stirring at high speed; adding a defoaming agent, stirring at a slow speed to obtain an organic layer slurry; using an air gun spraying or a high-speed centrifugal method to spray the organic layer slurry on the heat-resistant layer.
[0025] Further, according to the embodiment of the present application, the PMMA / PVDF composite agglomerate is prepared by the following method:
[0026] Add deionized water and dispersant into the reactor and stir evenly; introduce nitrogen repeatedly to exhaust oxygen, and after the replacement is qualified, introduce VDF into the reactor; increase the temperature and pressure to a constant temperature and pressure, and then inject initiator and emulsifier to carry out polymerization reaction;
[0027] After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain PVDF emulsion;
[0028] Add PMMA emulsion into PVDF emulsion, stir evenly, dry, and air flow grind to obtain PMMA / PVDF composite agglomerates.
[0029] In order to achieve the above-mentioned purpose, the embodiments of the present application also disclose an application of a PMMA / PVDF composite diaphragm in a lithium battery.
[0030] Compared with the prior art, the present application has the following beneficial effects: the present application forms PMMA / PVDF composite agglomerates by agglomerating PMMA particles and PVDF particles, and coats the agglomerates on the heat-resistant layer of the diaphragm; the PMMA in the agglomerates can provide channels for lithium ions to shuttle through the secondary particle size agglomerates, thereby improving the hindrance of the secondary particle size PVDF to the shuttle of lithium ions, thereby improving the cycle performance of the battery; the introduction of PMMA increases the adhesion between the diaphragm and the electrode piece, and improves the hardness of the battery; the use of point-like coating of PMMA / PVDF composite agglomerates has little effect on the overall air permeability of the diaphragm, and can ensure that the diaphragm and the electrode piece have a certain storage space, and can also store electrolyte, thereby improving the capacity retention rate of the battery and effectively avoiding the bulging phenomenon at the battery end. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The present application is further described below in conjunction with the accompanying drawings and embodiments.
[0032] Figure 1 It is a schematic diagram of the structure of the PMMA / PVDF composite agglomerate in this application.
[0033] In the attached drawings: 1. PMMA particles; 2. PVDF particles. DETAILED DESCRIPTION
[0034] In order to make the purpose and technical solution of the present invention clearly and completely described, and the advantages more clearly understood, the embodiments of the present invention are further described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] In the description of the present invention, it should be noted that the terms "center", "middle", "upper", "lower", "left", "right", "inner", "outer", "top", "bottom", "side", "vertical", "horizontal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "one", "first", "second", "third", "fourth", "fifth", "sixth" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0036] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0037] For the purpose of simplicity and illustration, the principles of the embodiments are mainly described by reference to examples. In the following description, many specific details are proposed to provide a thorough understanding of the embodiments. However, it is obvious that for those of ordinary skill in the art, these embodiments may not be limited to these specific details in practice. In some instances, known methods and structures are not described in detail to avoid making these embodiments unnecessarily difficult to understand. In addition, all embodiments can be used in combination with each other.
[0038] The present application discloses a PMMA / PVDF composite diaphragm, comprising a base film and a heat-resistant layer disposed on the surface of the base film, and a dot-shaped organic layer disposed on the heat-resistant layer, wherein the organic layer comprises a PMMA / PVDF composite aggregate, a binder and a defoamer. Figure 1 As shown, PMMA particles 1 and PVDF particles 2 are aggregated. PMMA can provide channels for lithium ions to shuttle through secondary particle aggregates, improving the barrier of secondary particle PVDF to lithium ion shuttle, thereby improving the battery's cycle performance; the introduction of PMMA increases the adhesion between the diaphragm and the pole piece, and improves the hardness of the battery. Furthermore, the use of dot-coating PMMA / PVDF composite aggregates has little effect on the overall air permeability of the diaphragm, and can ensure that the diaphragm and the pole piece have a certain storage space, and can also store electrolyte, thereby improving the battery's capacity retention rate and effectively avoiding the phenomenon of battery terminal bulging.
[0039] Preferably, the mass ratio of PMMA particles to PVDF particles is between 3:7 and 5:5, the particle size of PMMA particles is 250-400nm, the particle size of PVDF particles is 150-280nm, the crystal form of PVDF particles is α crystal form, the crystallinity is about 50%, and the particle size of the PMMA / PVDF composite agglomerate formed is 4-8µm. Specifically, the PMMA / PVDF composite agglomerate is prepared by the following method:
[0040] Select a suitable reactor, add deionized water and dispersant and stir evenly;
[0041] Repeatedly introduce nitrogen to exhaust oxygen, and after the replacement is qualified, introduce VDF into the reactor;
[0042] The temperature and pressure are raised to a constant temperature and pressure, and then the initiator and emulsifier are introduced to carry out the polymerization reaction. During this period, VDF can be introduced to control the reaction pressure;
[0043] After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain PVDF emulsion, and the particle size, crystal form and crystallinity of the emulsion PVDF are tested;
[0044] PMMA emulsion was added into the emulsion, stirred evenly, dried, and air flow crushed to obtain PMMA / PVDF composite agglomerates. The particle size change of the agglomerates was tested before and after high-speed shearing and ultrasound.
[0045] Furthermore, the binder in the organic layer is one or more of styrene-butadiene rubber, polystyrene, polyacrylate, acrylic acid, acrylonitrile, etc., and the added amount is 4-12wt% of the PMMA / PDVF composite agglomerate. The defoamer is one or more of polydimethylsiloxane, dimethyl polysiloxane, dimethyl silicone oil, emulsified silicone oil, etc., and the added amount is 0.5-2wt% of the PMMA / PDVF composite agglomerate.
[0046] The heat-resistant layer includes ceramics, stabilizers, glue and wetting agents. The ceramics are one or two of alumina, aluminum hydroxide, boehmite, zirconium oxide, silicon oxide, etc., and the particle size D50 is 0.5-1.2µm. The stabilizer is one or more of gelatin, hydroxyethyl cellulose, methyl cellulose, xanthan gum, sodium carboxymethyl cellulose, etc., and the added amount is 0.4-2wt% of the ceramic ratio. The glue is one or more of acrylic polymer, styrene-butadiene rubber, polystyrene, polyacrylate, epoxy resin, etc., and the added amount is 2-8wt% of the ceramic ratio. The wetting agent is one or more of sodium dodecyl sulfate, fatty alcohol, alkyl naphthalene sulfonate, sodium dodecylbenzene sulfonate, nonylphenol polyoxyethylene ether, etc., and the added amount is 0.2-2wt% of the ceramic ratio.
[0047] The base film is a porous film, specifically one of PP film, PE film, PP film and PE film composite film, etc., with a thickness of 5-20µm.
[0048] In addition, the present application also discloses a method for preparing a PMMA / PVDF composite diaphragm, comprising the following steps:
[0049] Coating the heat-resistant layer: coating the heat-resistant layer slurry on at least one side of the base film, with a coating thickness of 1-3 μm;
[0050] Coating the organic layer: taking the PMMA / PVDF composite agglomerate, the binder and the water, mixing them, and stirring at high speed; adding the defoaming agent, stirring at slow speed, and obtaining the organic layer slurry; spraying the organic layer slurry on the heat-resistant layer by air gun spraying or high-speed centrifugation; the spraying particle size is 80µm~350µm, the coating thickness is 5~10µm, and the coverage is 5%~20%.
[0051] The technical scheme and effects of the present application are further described below by listing embodiments and comparative examples, but the present application is not limited to these embodiments.
[0052] [Example 1]
[0053] Preparation of PMMA / PVDF composite agglomerates: Select a suitable reactor, add 2000 parts of deionized water and 0.9 parts of polyvinyl alcohol and stir evenly; Repeatedly introduce nitrogen to exhaust oxygen, and after the replacement is qualified, introduce 500 parts of VDF into the reactor; Raise the temperature and pressure to 80°C and 3.5MPa, and then inject 2.6 parts of diisopropyl peroxydicarbonate and 0.8 parts of perfluorooctanoic acid agent, and VDF can be introduced during the reaction to control the reaction pressure; After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain a PVDF emulsion with a solid content of 25%, and the particle size of the PVDF emulsion is 220nm; Take 1000 parts of PVDF emulsion, add 470 parts of PMMA emulsion with a solid content of 25% and a particle size of 380nm (PMMA: PVDF = 3.2: 6.8), stir evenly, dry, control the air flow crushing strength, and obtain a PMMA / PVDF composite agglomerate with a particle size of 7.54μm.
[0054] Coating heat-resistant layer: Mix 500 parts of aluminum oxide and 1000 parts of deionized water, and stir at high speed; add 5 parts of methyl cellulose and 30 parts of polyacrylate, evacuate to -0.7MPa, and stir at high speed; add 5 parts of alkyl naphthalene sulfonate and stir at low speed to obtain finished slurry; use micro-gravure technology to coat the finished slurry on the Enjie diaphragm (thickness 7μm), and after baking and winding, a 2μm heat-resistant layer composite diaphragm is obtained.
[0055] Coating the organic layer: 300 parts of the obtained PMMA / PVDF composite agglomerate, 20 parts of styrene-butadiene rubber, and 1000 parts of deionized water were mixed and stirred at high speed; 5 parts of emulsified silicone oil were added and stirred at low speed to obtain an organic layer slurry; the organic layer slurry was sprayed on the heat-resistant layer by a rotary spraying method, and the spraying surface density was obtained by adjusting the spraying flow rate and rotation speed to 0.6 g / m 2 , spraying PMMA / PVDF composite diaphragm with particle size of 100μm, coverage of 18%, and thickness of 9.0μm.
[0056] [Example 2]
[0057] In the step of preparing PMMA / PVDF composite agglomerates, 1000 parts of PVDF emulsion were taken, 667 parts of PMMA emulsion (PMMA: PVDF = 4.0: 6.0) with a solid content of 25% and a particle size of 260 nm were added, the mixture was stirred evenly, dried, and PMMA / PVDF composite agglomerates with a particle size of 6.05 μm were obtained by adjusting the air flow crushing intensity.
[0058] In the step of coating the organic layer, the spraying flow rate and speed were adjusted to obtain a spraying surface density of 0.6 g / m 2 , spray a PMMA / PVDF composite diaphragm with a particle size of 340 μm, a coverage of 6%, and a thickness of 7.5 μm, and the remaining steps are the same as in Example 1.
[0059] [Example 3]
[0060] In the step of preparing PMMA / PVDF composite agglomerates, 1000 parts of PVDF emulsion were taken, and 923 parts of PMMA emulsion (PMMA: PVDF = 4.8: 5.2) with a solid content of 25% and a particle size of 320 nm were added, stirred evenly, dried, and PMMA / PVDF composite agglomerates with a particle size of 4.26 μm were obtained by adjusting the air flow crushing intensity.
[0061] In the step of coating the organic layer, the spraying flow rate and speed were adjusted to obtain a spraying surface density of 0.6 g / m 2 , spray a PMMA / PVDF composite agglomerate composite diaphragm with a particle size of 200 μm, a coverage of 15%, and a thickness of 5.2 μm, and the remaining steps are the same as Example 1.
[0062] [Example 4]
[0063] In the step of preparing PMMA / PVDF composite agglomerates, 1000 parts of PVDF emulsion were taken, and 818 parts of PMMA emulsion (PMMA: PVDF = 4.5: 5.5) with a solid content of 25% and a particle size of 300 nm were added, stirred evenly, dried, and PMMA / PVDF composite agglomerates with a particle size of 5.54 µm were obtained by adjusting the air flow crushing intensity.
[0064] In the step of coating the organic layer, the spraying flow rate and speed were adjusted to obtain a spraying surface density of 0.6 g / m 2 , spray a PMMA / PVDF composite agglomerate composite diaphragm with a particle size of 240 μm, a coverage of 10%, and a thickness of 6.7 μm, and the remaining steps are the same as in Example 1.
[0065] [Comparative Example 1]
[0066] Coat a 2 μm heat-resistant layer according to the heat-resistant layer coating step in Example 1;
[0067] Coating the organic layer: select 1000 parts of the PVDF emulsion obtained in Example 1, add 450 parts of PMMA emulsion (PMMA: PVDF = 4.5:10) with a solid content of 25% and a particle size of 300 nm, 360 parts of deionized water, and 20 parts of styrene-butadiene rubber, mix and stir at high speed; add 5 parts of emulsified silicone oil, stir at low speed to obtain a mixed slurry of PMMA emulsion and PVDF emulsion; use a rotary spraying method to spray the mixed slurry of PMMA emulsion and PVDF emulsion on the heat-resistant layer, and adjust the spraying flow rate and rotation speed to obtain a spraying surface density of 0.6 g / m 2 , a composite diaphragm with a spray particle size of 380μm, a coverage of 20%, and a thickness of 1.8μm.
[0068] [Comparative Example 2]
[0069] In the step of preparing PMMA / PVDF composite agglomerates, PMMA is not added, and the PVDF emulsion is directly dried and the air flow crushing intensity is adjusted to obtain pure secondary particle size PVDF agglomerates with a particle size of 6.05 μm.
[0070] In the step of coating the organic layer, the spraying flow rate and speed were adjusted to obtain a spraying surface density of 0.6 g / m 2 , spray a pure secondary particle size PVDF agglomerate composite diaphragm with a particle size of 330 μm, a coverage of 7%, and a thickness of 7.2 μm. The remaining steps are the same as in Example 1.
[0071] [Comparative Example 3]
[0072] Coat a 2 μm heat-resistant layer according to the heat-resistant layer coating step in Example 1;
[0073] Coating an organic layer: Select the PVDF emulsion of Example 1, directly dry it, and adjust the air flow crushing strength to obtain a pure secondary particle size PVDF agglomerate with a particle size of 3.00µm; take 250 parts of pure secondary particle size PVDF agglomerate with a particle size of 3.00µm, add 320 parts of PMMA emulsion (PMMA: PVDF = 3.2: 10) with a solid content of 25% and a particle size of 360nm, 1000 parts of deionized water, and 20 parts of styrene-butadiene rubber, mix and stir at high speed; add 5 parts of emulsified silicone oil, stir at low speed to obtain a mixed slurry of PMMA emulsion and pure secondary particle size PVDF agglomerate; use a rotary spraying method to spray the mixed slurry of PMMA emulsion and pure secondary particle size PVDF agglomerate on the heat-resistant layer, and adjust the spraying flow rate and rotation speed to obtain a spraying surface density of 0.6g / m 2 , a composite diaphragm with a spray particle size of 400µm, a coverage of 10%, and a thickness of 4.2µm.
[0074]
Content of PMMA / PVDF composite aggregates
[0075] Since the PMMA crystal region belongs to the amorphous region, there is no obvious melting peak. The PVDF crystal region belongs to the semi-morphous region and has an obvious melting peak at 140℃-150℃. The content of PVDF in the agglomerate can be inferred based on the melting peak of PVDF. The melting peak of the agglomerate powder with a mass of M is tested using a Mettler differential scanning calorimeter DSC. The heat E absorbed by the melting of PVDF is obtained by integrating the melting peak at 140℃~150℃. According to E=M1*Hm*η, M1=E / (Hm*η) can be obtained. From M=M1+M2 (M1 is the mass of PVDF in the test agglomerate, M2 is the mass of PMMA in the test agglomerate, Hm is the melting enthalpy when PVDF is completely crystallized, which is 104.7J / g, and η is the crystallinity of PVDF, which is 49.5%), the mass M2 of PMMA in the test agglomerate powder can be obtained. Finally, the mass ratio of PMMA and PVDF in the agglomerate can be calculated as M2:M1.
[0076] The test and calculation results are summarized in Table 1.
[0077] Table 1
[0078]
[0079] As shown in Table 1, the results of the DSC test of the proportion of PMMA and PVDF in the aggregates are not much different from the proportion of PMMA and PVDF in the synthetic aggregates.
[0080] [Agglomerate particle size]
[0081] The agglomerates obtained in the embodiment and the comparative example were dispersed in ethanol, and ultrasound was used at 1000W and 35KHz for 30 minutes, and then stirred at a high speed of 1500rpm for 60 minutes. The particle size of the agglomerates before and after the test was tested. The particle size change rate (particle size change rate = | (particle size after treatment - particle size before treatment) | / particle size before treatment) was less than 1%. The particle size tester was Battersize2000, and the refractive index was selected as 1.42.
[0082] The calculation results of the test machine are summarized in Table 2.
[0083] Table 2
[0084] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Front / μm 7.54 6.05 4.26 5.54 \ 6.05 3.00 After / μm 7.51 6.04 4.27 5.52 \ 6.04 3.02 Particle size change rate 0.4% 0.2% 0.2% 0.04 \ 0.2% 0.7%
[0085] It can be seen from Table 2 that after ultrasound and high-speed shearing, the particle size change rate of the agglomerates is less than 1%, so it can be seen that the agglomerates exist stably as hard agglomerates.
[0086]
Composite diaphragm performance
[0087] The following performance tests were performed on the composite diaphragms prepared in Examples 1-4 and Comparative Examples 1-3.
[0088] Air permeability: the time required for 100 ml of gas to pass through a diaphragm of a fixed area;
[0089] Liquid storage performance: Take a 10cm*10cm diaphragm and immerse it in a lithium salt electrolyte (EC:EMC:DEC=3:5:2, LiPF6, 1Mol / L) at 60℃ for 24h. Weigh the mass of the diaphragm before and after immersion. Liquid storage rate = mass after immersion / mass before immersion*100%;
[0090] Adhesion performance: Adhesion between the composite diaphragm and the positive electrode sheet at 3MPa, 5min, 90℃. The positive electrode sheet is composed of 200 parts of lithium manganese oxide + 150 parts of lithium iron phosphate + 10 parts of conductive carbon black + 16 parts of PVDF.
[0091] Ionic conductivity performance: In an argon glove box, the diaphragm was made into a 2016 button battery, and an appropriate amount of electrolyte (EC:EMC:DEC=3:5:2, LiPF6, 1Mol / L) was added. The AC impedance test in the electrochemical workstation showed that σ=L / (Rb*A), where σ is the ionic conductivity (S cm -1 ); L is the thickness of the diaphragm (cm); Rb is the intrinsic resistance of the diaphragm (Ω); A is the effective area (cm 2 );
[0092] Capacity retention rate: The battery is cycled 150 times at 0.2C charge and discharge, and the capacity before and after the test cycle is measured. Capacity retention rate = capacity after cycle / capacity before cycle;
[0093] Expansion coefficient: After the diaphragm and the pole piece are hot-pressed and wound and the electrolyte is injected, the temperature is 60°C and the seal is maintained for 10 days. The battery thickness expansion coefficient is tested. Expansion coefficient = thickness after 10 days of sealing / thickness when sealed.
[0094] The test and calculation results are summarized in Table 3.
[0095] Table 3
[0096]
[0097] It can be seen from Table 3 that the overall air permeability of the coatings in Examples 1-4 and Comparative Examples 2 and 3 is relatively small. In Comparative Example 1, nano-level PVDF and PMMA are selected for spraying, so the pore blockage is serious and the air permeability increases greatly. In Examples 1-4 and Comparative Examples 1 and 3, since PMMA has a stronger ability to absorb electrolyte than PVDF, the overall liquid storage performance is better than that of Comparative Example 2. In Examples 1-4 and Comparative Examples 1 and 3, since the adhesion between PMMA and the electrode is much stronger than that between PMMA and PVDF, the adhesion between PMMA and the electrode is stronger than that between PMMA and PVDF.
[0098] In addition, in Examples 1-4, the composite diaphragm PMMA is mixed with PVDF to form secondary particle size PMMA / PVDF composite agglomerates. Since the PMMA crystal region is an amorphous region, it is mixed with PVDF to form secondary particle size composite agglomerates, which can provide more amorphous regions for lithium ions to shuttle through the secondary particle size PVDF agglomerates, thereby solving the congestion phenomenon when lithium ions shuttle through the secondary particle size PVDF agglomerates. Therefore, the ion conductivity of the embodiments is significantly higher; although Comparative Example 1 is also a mixed coating of PVDF and PMMA, the small particle size PVDF and PMMA have more serious pore blocking phenomena on the coating, so its ion conductivity is relatively poor compared with Examples 1-4; Comparative Examples 2 and Comparative Examples 3 did not fundamentally solve the problem of secondary particle size PVDF agglomerates hindering the shuttling of lithium ions, so their ion conductivity is relatively small.
[0099] The coating thickness of the composite diaphragm of Examples 1-4 is relatively large, and there is still a certain space for storing electrolyte after hot pressing and bonding with the pole piece. In addition, due to the presence of PMMA, the electrolyte absorption is stronger than PVDF, and the electrolyte storage capacity is also relatively strong. Therefore, the capacity retention rate of the embodiments is relatively high; since the coating thickness of Comparative Example 1 is relatively low, there is basically no extra space for storing electrolyte after hot pressing with the pole piece, so the capacity retention rate is relatively low; although the coating thickness of Comparative Example 2 is relatively thick and can store electrolyte after hot pressing with the pole piece, the electrolyte storage capacity of pure secondary particle size PVDF is lower than that of PMMA, so its capacity retention rate is worse than that of Examples 1-4; the thickness of the composite diaphragm of Comparative Example 3 is smaller than that of Examples 1-4, and there is a certain space for storing electrolyte after hot pressing with the pole piece, but it is worse than the embodiments, so the capacity retention rate is worse than that of Examples 1-4.
[0100] The thickness of the coated diaphragm in Examples 1-4 and Comparative Example 2 is relatively large, and after hot pressing with the pole piece, there is still enough space for PVDF and PMMA to swell, so the battery will not bulge; the thickness of the coated diaphragm in Comparative Example 1 is relatively low, and there is no space for PVDF and PMMA to swell after hot pressing with the pole piece, so the battery will bulge; the thickness of the coated diaphragm in Comparative Example 3 is lower than that in Examples 1-4, and although there is a certain space after hot pressing with the pole piece, it is not enough to provide enough space for PVDF and PMMA to swell, so the battery will also bulge, but it is much better than Comparative Example 1.
[0101] Although the above describes the illustrative specific implementation methods of the present application so that technicians in this technical field can understand the present application, the present application is not limited to the scope of the specific implementation methods. For ordinary technicians in this technical field, as long as various changes are within the spirit and scope of the present application defined and determined by the attached claims, all application creations using the concept of the present application are protected.
Claims
1. A PMMA / PVDF composite diaphragm, characterized in that: include: A basement membrane, wherein the basement membrane is a porous film; A heat-resistant layer, the heat-resistant layer being disposed on at least one side surface of the base film; An organic layer, wherein the organic layer is arranged in dots on the surface of the heat-resistant layer, and the organic layer comprises a PMMA / PVDF composite agglomerate, a binder and a defoamer; the PMMA / PVDF composite agglomerate is formed by agglomerating PMMA particles and PVDF particles, and the mass ratio of the PMMA particles to the PVDF particles is 3:7-5:5; The PMMA / PVDF composite agglomerate is prepared by the following method: Add deionized water and dispersant into the reactor and stir evenly; introduce nitrogen repeatedly to exhaust oxygen, and after the replacement is qualified, introduce VDF into the reactor; increase the temperature and pressure to a constant temperature and pressure, and then inject initiator and emulsifier to carry out polymerization reaction; After the reaction is completed, the unreacted VDF is recycled, and the polymer emulsion is condensed, washed, and separated to obtain PVDF emulsion; Add PMMA emulsion into PVDF emulsion, stir evenly, dry, and air flow grind to obtain PMMA / PVDF composite agglomerates.
2. A PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The thickness of the heat-resistant layer is 1-3 μm.
3. A PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The heat-resistant layer comprises ceramics, a stabilizer, glue and a wetting agent.
4. A PMMA / PVDF composite diaphragm according to claim 3, characterized in that: The particle size of the ceramic is 0.5-1.2 μm.
5. The PMMA / PVDF composite diaphragm according to claim 3, characterized in that: The stabilizer accounts for 0.4-2wt% of the ceramic ratio.
6. The PMMA / PVDF composite diaphragm according to claim 3, characterized in that: The glue accounts for 2-8wt% of the ceramic ratio.
7. The PMMA / PVDF composite diaphragm according to claim 3, characterized in that: The wetting agent accounts for 0.2-2wt% of the ceramic ratio.
8. The PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The PMMA particles have a particle size of 250-400 nm.
9. The PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The particle size of the PVDF particles is 150-280 nm.
10. The PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The particle size of the PMMA / PVDF composite agglomerate is 4-8 μm.
11. The PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The binder accounts for 4-12 wt % of the PMMA / PVDF composite agglomerate.
12. The PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The defoamer accounts for 0.5-2 wt % of the PMMA / PVDF composite aggregate.
13. The PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The thickness of the base film is 5-20 μm.
14. A method for preparing the PMMA / PVDF composite diaphragm according to claim 1, characterized in that: The following steps are involved: Coating the heat-resistant layer: coating the heat-resistant layer slurry on at least one side of the surface of the base film; Coating the organic layer: taking the PMMA / PVDF composite aggregate, the binder and water, mixing them, and stirring at high speed; adding a defoaming agent, stirring at a slow speed to obtain an organic layer slurry; using an air gun spraying or a high-speed centrifugal method to spray the organic layer slurry on the heat-resistant layer.
15. Use of a PMMA / PVDF composite diaphragm as claimed in any one of claims 1 to 13 or a PMMA / PVDF composite diaphragm prepared by the method for preparing the PMMA / PVDF composite diaphragm as claimed in any one of claim 14 in a lithium battery.