Extrusion molding die, plastic manufacturing device and plastic manufacturing method
By optimizing the plastic channel structure and pressure control, the problem of corrugations and creases in foamed plastics has been solved, achieving the production of high expansion ratio and high-quality foamed plastics suitable for various application scenarios.
Patent Information
- Application Number
- CN202210389653.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-16
- Filing Date
- 2022-04-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-04-14
AI Technical Summary
Existing technologies tend to create ripples and creases in foamed plastics, which affects product quality and application performance.
A plastic channel structure is designed, including a first channel, a second channel, and a third channel. The cross-sectional area of the second channel gradually decreases downstream along the flow direction of the plastic composition, and the cross-sectional area of the third channel also gradually decreases along the flow direction. By controlling the ratio and angle of the channel cross-sectional areas, the pressure distribution of the plastic composition is optimized to suppress ripples and creases during the foaming process.
It effectively suppresses ripples and creases in foamed plastics, achieving high expansion ratio and high-quality foamed plastic production, suitable for various application needs.
Smart Images

Figure CN115214105B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an extrusion molding die, a plastic manufacturing device and a plastic manufacturing method. Background Art
[0002] An example of a conventionally known extrusion mold includes an extrusion port and a plastic channel, from which a plastic composition containing at least one plastic is extruded, and in which the supplied plastic composition flows toward the extrusion port.
[0003] In Japanese Patent No. 4573505, the plastic channel includes a first channel, a second channel connected to the first channel, and a third channel connected to the second channel and allowing the plastic composition to flow toward the extrusion port. The second channel is formed in such a way that the channel cross-sectional area gradually decreases downstream along the flow direction of the plastic composition. The third channel is formed in such a way that the plastic composition flows in a direction away from the extrusion center axis. In a cross section including the extrusion center axis and parallel to the extrusion center axis, the ratio (GB) / (GA) of the gap (GB) of the extrusion port to the gap (GA) of the connecting portion of the second channel and the third channel is 5 to 20, and the channel cross-sectional area of the third channel increases toward the extrusion port.
[0004] However, corrugated folds may form in foamed plastics. Summary of the invention
[0005] According to one aspect of the present invention, an extrusion molding die includes an extrusion port and a plastic channel. The extrusion port is configured to extrude a plastic composition containing at least one plastic. The plastic channel is configured to allow the supplied plastic composition to flow toward the extrusion port. The plastic channel includes a first channel, a second channel, and a third channel. The second channel is connected to the first channel and has a channel cross-sectional area that gradually decreases downstream along the flow direction of the plastic composition. The third channel is connected to the second channel and is configured to allow the plastic composition to flow toward the extrusion port. The third channel has a channel cross-sectional area that gradually decreases downstream along the flow direction of the plastic composition.
[0006] According to one aspect of the present invention, the occurrence of corrugated folds in foamed plastic can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 It is a schematic structural diagram of a plastic manufacturing device for manufacturing foamed plastic according to one embodiment.
[0008] Figure 2 It is a schematic diagram of the structure of the kneading equipment for manufacturing the masterbatch.
[0009] Figure 3 is a schematic cross-sectional view of a conventional die.
[0010] Figure 4 This is a cross-sectional view of the die of the embodiment parallel to the extrusion center axis.
[0011] Figure 5 is a cross-sectional view of the die according to Example 2 parallel to the extrusion center axis.
[0012] Figure 6 is a cross-sectional view of the die according to Example 3 parallel to the extrusion center axis.
[0013] Figure 7 is a cross-sectional view parallel to the extrusion center axis of the die according to Example 4; and
[0014] Figure 8 This is a cross-sectional view of the die according to Comparative Example 1, parallel to the extrusion center axis.
[0015] The accompanying drawings are intended to depict exemplary embodiments of the present invention and should not be interpreted as limiting its scope. The same or similar reference numerals represent the same or similar components in the various drawings. DETAILED DESCRIPTION
[0016] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0017] As used herein, the singular forms are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0018] In describing the preferred embodiments shown in the accompanying drawings, specific terms may be used for the sake of clarity. However, the disclosure of this patent specification is not intended to be limited to the specific terms so selected, and it should be understood that each specific element includes all technical equivalents having the same function, operating in a similar manner and achieving similar results.
[0019] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0020] First, a method for manufacturing a plastic foam sheet made of foamed plastic is described.
[0021] The method for producing a plastic foam sheet according to the present invention includes a kneading step, a foaming step, etc., and includes other steps as necessary.
[0022] The kneading step and the foaming step may be performed simultaneously or as separate steps.
[0023] Mixing steps
[0024] The kneading step is a step of kneading plastic and filler as necessary. In the kneading step, a foaming agent may be added to promote more efficient foaming. Depending on the use of the molded product, a cross-linking agent, an antioxidant, a colorant, various light absorbers, an antistatic agent, a conductive material, etc. may also be mixed. The kneading step may be performed in the presence of a compressible fluid for more efficient foaming or more efficient kneading.
[0025] Plastics, fillers and mixtures produced in intermediate steps of the process to obtain the final moulding may also be referred to as plastic compositions or masterbatches.
[0026] plastic
[0027] Examples of plastics include: styrene-based homopolymers, for example, polystyrene and poly-p-methylstyrene; styrene-based copolymers, for example, styrene-maleic anhydride copolymer, styrene-acrylonitrile copolymer, styrene-butadiene copolymer, styrene-acrylonitrile-butadiene copolymer, styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer; styrene-based resins, for example, a mixture of polystyrene and polyphenylene oxide; aliphatic polyester resins, for example, polylactic acid; acid), polyglycol acid, poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-3-hydroxyhexanoate), poly(3-hydroxybutyrate-3-hydroxyvalerate), polycaprolactone, polybutylene succinate, and poly(butylene succinate-adipate).
[0028] Among them, preferably biodegradable resins and aliphatic polyester resins that can be biodegraded by microorganisms are environmentally friendly low environmental burden polymer materials, more preferably polylactic acid, which is a carbon neutral material and relatively cheap. By containing more than 90 mass % (mass%, mass percentage) of polylactic acid, biodegradable foamed plastics can be obtained.
[0029] filler
[0030] The filler (hereinafter also referred to as "foam core material") is used to adjust the foaming state (size, quantity, arrangement) of the foam sheet, to reduce costs, and to improve strength.
[0031] The filler may be an inorganic filler, an organic filler, etc. These fillers may be used alone or in combination of two or more.
[0032] Examples of the inorganic filler include talc, kaolin, calcium carbonate, layered silicate, zinc carbonate, wollastonite, silicon dioxide, aluminum oxide, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, magnesium silicate, glass balls, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, metal fiber, metal whisker, ceramic whisker, potassium titanate, boron nitride, graphite, glass fiber, carbon fiber.
[0033] Examples of organic fillers include polymers occurring in nature such as starch, cellulose particles, wood flour, bean curd residue, rice husk and bran, and modified products thereof, sorbitol compounds, benzoic acid, metal salts of their compounds, phosphate ester metal salts and rosin compounds.
[0034] Among them, silica as an inorganic nucleating agent is preferred because of its high affinity with the compressible fluid, as will be discussed below. If a filler other than silica is used as the matrix, a filler surface-treated with silica is preferred.
[0035] Foaming agent
[0036] As the foaming agent, the following physical foaming agents are preferred because a plastic foamed sheet having a high expansion ratio can be obtained: hydrocarbons including lower alkanes such as propane, n-butane, isobutane, n-pentane, isopentane and hexane, ethers such as dimethyl ether, halogenated hydrocarbons such as methyl chloride and ethyl chloride, and compressible gases such as carbon dioxide and nitrogen.
[0037] Among them, compressible gases such as carbon dioxide and nitrogen are preferably used because they have no odor, can be handled safely, and have low impact on the environment.
[0038] Compressible fluid
[0039] For example, substances that can be used as the above-mentioned compressible fluid include carbon monoxide, carbon dioxide, nitrous oxide, nitrogen, methane, ethane, propane, 2,3-dimethylbutane, ethylene and dimethyl ether. Among them, carbon dioxide is preferred because it has a critical pressure of about 7.4 MPa and a critical temperature of about 31°C, is easy to form a supercritical state, and is non-flammable and easy to handle. These compressible fluids can be used alone or in combination of two or more.
[0040] Since the solubility of the compressible fluid varies depending on the combination of plastic and compressible fluid, temperature and pressure, the supply amount of the compressible fluid needs to be adjusted accordingly.
[0041] For example, in the case of a combination of polylactic acid and carbon dioxide, the preferred value is greater than or equal to 2% by mass and less than or equal to 30% by mass. If more than 2% by mass of carbon dioxide is supplied, the problem of limited plasticizing effect can be prevented. If the supply amount of carbon dioxide is less than 30% by mass, the problem of phase separation between carbon dioxide and polylactic acid and failure to obtain a foamed sheet with uniform thickness can be prevented.
[0042] Kneading device
[0043] The kneading apparatus used in the kneading step may be a continuous method in which the kneading step and the foaming step are performed continuously, or a batch method. It is best to select the reaction process in consideration of equipment efficiency, product characteristics, quality, etc.
[0044] As for kneading equipment, single screw extruder, multi-screw extruder, kneading machine, non-screw cage type agitator, Sumitomo Heavy Industries (Sumitomo Heavy Industries, Ltd.) BIVOLAK, Mitsubishi Heavy Industries (MitsubishiHeavy Industries, Ltd.) N-SCR, Hitachi spectacle blades (spectacle blades) or lattice blades (lattice blades), Kenix or Sulzer SMLX type static mixer equipped with tubular polymerization tank etc. can be used, because these devices can handle the viscosity suitable for kneading. In terms of color tone, self-cleaning polymerization equipment such as finishing machine, N-SCR, twin screw extruder is provided. Wherein, from the color tone, stability, heat resistance of resin, preferred finishing machine, N-SCR. In terms of production efficiency, preferred single screw extruder and multi-screw extruder.
[0045] Foaming steps
[0046] In the foaming step, the foaming agent expands to foam the plastic composition. In the case of a compressible fluid, the expansion agent and the foaming agent can be removed by releasing the pressure. As for the temperature during the foaming step, it is preferably set to a temperature that plasticizes the plastic composition to an extent that it can be extruded.
[0047] As a driving force for causing the plastic composition to flow in the foaming step, the pressure from the above-mentioned kneading device may be used, or a separate mechanical device such as a single-screw or multi-screw extruder or a cylinder may be used to carry out the foaming step.
[0048] Additional Steps
[0049] The other steps are not limited to specific steps and may be steps generally used for producing a plastic foam sheet and may be appropriately selected according to the purpose. Examples of the steps include a step of molding into a sheet.
[0050] The molding step may be, for example, vacuum molding, pressure air molding, and compression molding. In this embodiment, a cylindrical masterbatch is molded, and the masterbatch is made into a sheet through the molding step to obtain a plastic foamed sheet.
[0051] Figure 1 It is a schematic structural diagram of a plastic manufacturing device for manufacturing foamed plastic according to one embodiment.
[0052] The plastic manufacturing device 20 connects in series a first extruder 21A as a kneading device for performing a kneading step and a second extruder 21B for performing a foaming step.
[0053] A die 1 as an extrusion molding die is installed at one end (downstream end in the extrusion direction) of the second extruder 21B, and the plastic composition is extruded from the die 1 while foaming to form a foamed plastic.
[0054] The first extruder 21A includes a raw material mixing and melting zone (a), a compressible fluid supply zone (b), and a kneading zone (c), and the second extruder 21B includes an extrusion zone (d).
[0055] The first extruder 21A and the second extruder 21B are twin-screw extruders (manufactured by JSW, screw diameter 42 mm, L / D=48).
[0056] Raw material mixing and melting area
[0057] In the raw material mixing and melting area a, the first quantitative feeder 22A supplies filler, and the second quantitative feeder 22B supplies resin material such as polylactic acid. Figure 2 ) can be supplied from the first quantitative feeder 22A.
[0058] Compressible fluid supply area
[0059] The gas introduction part 23 is connected to the compressible fluid supply area b. The gas introduction part 23 includes a gas tank 231 storing a compressible fluid containing a foaming agent and a metering pump 232 supplying a predetermined amount of the compressible fluid in the gas tank 231 to the compressible fluid supply area b.
[0060] In the raw material mixing and melting area a, the resin particles are melted by heating to wet the filler. A compressible fluid containing a foaming agent is supplied to the raw material mixture in this state by a metering pump 132 to plasticize the molten resin.
[0061] Mixing area
[0062] The plastic composition supplied with the compressible fluid in the compressible fluid supplying area b is extruded to the kneading area c.
[0063] In the kneading area c, the temperature is set to achieve a viscosity suitable for kneading the filler. The set temperature depends on the specifications of the equipment, the type of resin, the structure of the resin, the molecular weight, etc. Therefore, the temperature is not particularly limited, but in the case of commercially available polylactic acid with a weight average molecular weight (Mw) of about 200,000, kneading is generally performed at a set temperature of 10°C to 20°C above the melting point of the polylactic acid. In contrast, kneading with a compressible fluid allows kneading at a temperature below the melting point of the polylactic acid. By setting the temperature below the melting point of the resin, kneading can be performed at a higher viscosity. Specifically, the curing temperature is preferably 20°C to 80°C, more preferably 30°C to 60°C below the melting point of the resin. For simplicity, the temperature can be set, for example, based on the current value of the stirring power of the equipment.
[0064] By kneading the plastic composition at a temperature below the melting point, the kneading efficiency can be improved, and the foaming speed in the mold 1 can be made uniform in the plastic composition. Therefore, the occurrence of local corrugation creases in the molded foamed plastic can be suppressed. Additional effects can be obtained; for example, the occurrence of degradation, carbonization, oxidation, tar, and decomposition of combustion deposits in the extruder 11 can be suppressed.
[0065] By kneading the plastic composition at a temperature below the melting point, the kneading efficiency can be improved, and the foaming speed in the mold 1 can be made uniform in the plastic composition. Therefore, the occurrence of local corrugation creases in the molded foamed plastic can be suppressed. Additional effects can be obtained; for example, the occurrence of degradation, carbonization, oxidation, tar, and decomposition of combustion deposits in the extruder 11 can be suppressed.
[0066] Extrusion Area
[0067] The plastic composition is kneaded in the kneading area c of the first extruder 21A and supplied to the extrusion area d of the second extruder 21B. A die 1 as an extrusion molding die is installed at the end of the extrusion area d (the downstream end in the extrusion direction). When the plastic composition is extruded from the die 1, the plastic composition foams, thereby producing a cylindrical foamed plastic.
[0068] As for the set temperature of the extrusion zone d in which the foaming step of foaming the plastic composition is performed, it is preferred to set the temperature of the plastic composition when it is extruded from the die 1 to be lower than the melting point of the plastic composition. By setting the temperature of the plastic composition when it is extruded from the die 1 to be lower than the melting point of the plastic composition, the plastic composition can be thickened, thereby obtaining a foamed plastic with a high expansion ratio.
[0069] Molding processing area
[0070] A mandrel 25 for cooling the tubular foamed plastic extruded from the die 1 is placed in the molding process area e. The tubular foamed plastic extruded from the die 1 is placed along the mandrel 25, and its outer surface is cooled by air blown from the air ring to form the tubular foamed plastic. After that, the cooled tubular foamed plastic is cut by a cutter to form a flat sheet. After the flat sheet passes through the roller 26, the flat sheet is wound by the winding roller 27 to obtain a foamed sheet.
[0071] Next, the production of the masterbatch supplied from the first quantitative supply device 22A to the first extruder 21A will be described.
[0072] Figure 2 Schematic diagram of the structure of a kneading device 10 for manufacturing a masterbatch.
[0073] The kneading device 10 is a twin-screw extruder (manufactured by JSW, screw diameter 42 mm, L / D=48). Figure 1 In the plastic manufacturing apparatus 20 shown, the kneading device 10 includes a raw material mixing and melting area (a), a compressible fluid supply area (b), a kneading area (c), an extrusion area (d), and a molding process area (e).
[0074] In the raw material mixing and melting zone a, the filler is supplied by the first quantitative feeder 12A, and the resin material such as polylactic acid is supplied by the second quantitative feeder 12B. Then, in the compressible fluid supplying area b, a prescribed amount of compressible fluid is supplied from the gas inlet 13. Then, the material is kneaded in the kneading area c and then extruded to the extrusion area d.
[0075] The extrusion area d includes a pressure valve 14. After the pressure valve 14 is opened and the compressible fluid of the plastic composition is discharged to the outside, the plastic composition is extruded into a strand. The extruded strand-shaped plastic composition is cooled and then granulated with a cutter in the molding processing area e to produce a masterbatch in the form of granules.
[0076] Foamed plastics with a higher expansion ratio are more cost-effective. From the perspective of cost, the expansion ratio of the foamed plastic is preferably 5 times or more, more preferably 10 times or more, further preferably 20 times or more, further preferably 30 times or more, and particularly preferably 40 times or more. In addition, foamed plastics with an expansion ratio of 45 times or more have low strength and poor performance as general foamed plastic components, and their use is limited to packaging materials and the like.
[0077] However, high expansion ratios increase the risk of corrugation marks in the foamed plastic. In packaging applications, corrugation marks are acceptable from an aesthetic point of view; however, in order to avoid poor stacking properties, it is best not to have corrugation marks.
[0078] When the formed foamed plastic sheet is subjected to secondary molding of disposable containers, blister packages, etc., the expansion ratio is preferably 1 to 30 times, more preferably 1 to 10 times, and further preferably 1 to 3 times. In such applications, the expansion ratio is low; however, the generation of corrugated creases will reduce the appearance, and the corrugated creases may cause a decrease in strength, thereby causing secondary molding failure. Therefore, the corrugated creases are unacceptable in this application.
[0079] The desired expansion ratio can be obtained by comprehensively controlling one or more of the following factors: kneading temperature, residence time, ambient temperature, foaming agent concentration, foaming agent type, foaming agent uniformity, plastic molecular weight distribution, ejection speed from mold 1, etc.
[0080] It is known that corrugation folds are related to the expansion ratio, and the higher the expansion ratio, the more corrugation folds there are. However, as mentioned above, the optimal expansion ratio depends on the application of the molded foamed plastic, and reducing the expansion ratio to suppress corrugation folds has limitations.
[0081] Figure 3 is a schematic cross-sectional view of a conventional mold 100.
[0082] like Figure 3 As shown, the conventional mold 100 includes an outer mold 101a, the outer mold 101a includes a through hole extending along the extrusion direction of the plastic composition (from right to left in the figure), and an inner mold 101b arranged in the through hole of the outer mold 101a.
[0083] The inner peripheral surface of the through hole of the outer die 101a and the outer peripheral surface of the inner die 101b form a plastic passage 102 having an annular cross-sectional shape orthogonal to the extrusion center axis g. The plastic passage 102, which is a gap between the inner die 101b and the outer die 101a, has an upstream passage 102a and a downstream passage 102b.
[0084] The channel cross-sectional area of the upstream channel 102a (a cross section perpendicular to the flow direction of the plastic composition in the channel) decreases toward the downstream in the flow direction of the plastic composition in the channel.
[0085] The downstream channel 102b is configured to have a diameter that gradually increases downstream along the flow direction of the plastic composition in the channel. The downstream channel 102b is configured such that the channel cross-sectional area gradually increases downstream along the flow direction of the plastic composition.
[0086] Obtaining a foamed plastic sheet with a high expansion ratio results in corrugated folds. In-depth studies by the applicant have clarified that the pressure applied to the plastic composition in the downstream passage 102b becomes less than or equal to the pressure at which the plastic composition starts to foam, and the plastic composition starts to foam in the downstream passage 102b. When the plastic composition foams in the narrow downstream passage 102b and the volume of the plastic composition increases, the generated foam has nowhere to go. As a result, it is thought that the plastic composition foams upstream and downstream of the plastic composition to find an escape location, thereby causing these corrugated folds.
[0087] In view of this, in this embodiment, the shape of the plastic channel in which the plastic composition flows is designed to optimize the pressure applied to the plastic composition in the plastic channel. Therefore, a foamed plastic sheet with a higher expansion ratio and fewer corrugated folds is obtained. The following is a detailed description with reference to the accompanying drawings.
[0088] Figure 4 This is a cross-sectional view of the die of this embodiment parallel to the extrusion center axis.
[0089] Figure 4 It is a cross-sectional view including and parallel to the extrusion center axis g of the die 1 .
[0090] The extrusion center axis g is the center line of the annular plastic channel 111 where the size center of the inner mold 1b coincides with the size center of the outer mold 1a. When the size center line of the inner mold 1b does not coincide with the size center line of the outer mold 1a, the straight line containing the center of gravity of the plastic fluid flowing in the annular plastic channel 111 is used as the extrudate center axis g. In this embodiment, the mold manufactures a circular tubular molded product, but the above description is also applicable to the mold 1 for manufacturing a square tubular molded product.
[0091] The mold 1 includes an outer mold 1a and an inner mold 1b. The outer mold 1a includes a through hole 101 extending along the extrusion direction of the plastic composition (from right to left in the figure), and the inner mold 1b is arranged in the through hole 101 of the outer mold 1a.
[0092] The outer mold 1a and the inner mold 1b can be made of materials such as S45C, S50C, SS400, SCM440, SUS316, SUS304, etc. In order to improve durability, various coatings such as hard chrome plating can be used, or in order to improve thermal conductivity, C2810, A5052, alumina, etc. can be selected. Quartz glass or other materials can be used for analytical purposes, or mirror polishing can be used for the purpose of improving demoulding properties. Sandblasting or coating with a release agent can be performed. In addition, a mold with a variable mold structure can be used.
[0093] The through hole 101 of the outer die 1a is a perfect circle, having a first inner peripheral surface 4a with a constant inner diameter upstream in the extrusion direction, a second inner peripheral surface 4b with a decreasing inner diameter downstream in the extrusion direction, and a third inner peripheral surface 4c with an increasing inner diameter downstream in the extrusion direction.
[0094] The outer peripheral surface 5 of each position of the inner die 1b in the extrusion direction is a perfect circle, and has a first outer peripheral surface 5a with a constant diameter from upstream in the extrusion direction, and a second outer peripheral surface 5b with an outer diameter increasing toward downstream in the extrusion direction.
[0095] The inner peripheral surface 4 of the through hole of the outer mold 1a becomes the outer inner wall surface of the plastic passage 2 through which the plastic composition flows. The outer peripheral surface of a portion of the inner mold 1b located in the through hole becomes the inner inner wall surface of the plastic passage 2.
[0096] The plastic channel 2, which is a gap between the inner mold 1b and the outer mold 1a, has a first channel 2a, a second channel 2b and a third channel 2c. The first channel 2a has a constant channel cross-sectional area. The second channel 2b is connected to the first channel 2a, and its channel cross-sectional area decreases downstream in the flow direction of the plastic composition. The third channel 2c is connected to the second channel 2b, and the downstream end in the flow direction of the plastic composition is an annular extrusion port 3, from which the plastic composition is extruded.
[0097] The third channel 2c is configured so that its channel cross-sectional area gradually decreases downstream in the flow direction of the plastic composition. By virtue of the structure in which the channel cross-sectional area gradually decreases downstream in the flow direction of the plastic composition, the pressure of the third channel 2c is high upstream in the flow direction of the plastic, and the pressure decreases downstream due to pressure loss, and at the extrusion port 3, the pressure becomes the lowest.
[0098] As a result, when the pressure of the plastic composition at the extrusion port 3 is adjusted to a predetermined pressure (e.g., 7 MPa), the pressure applied to the plastic composition in the third channel 2c can reach 7 MPa or more, and the foaming of the plastic composition in the third channel 2c can be suppressed. Therefore, the generation of corrugated folds can be suppressed.
[0099] In order to obtain a foamed plastic with a high expansion ratio, the plastic composition is supplied from the extruder under high pressure (e.g., 30 MPa). The plastic composition subjected to the high pressure (e.g., 30 MPa) needs to be decompressed to a predetermined pressure (e.g., about 7 MPa) at the extrusion port 3. In view of this, it is necessary to reduce the pressure of the plastic composition extruded from the extrusion port 3 to a predetermined pressure by causing a pressure loss in the plastic channel 2.
[0100] If possible, the pressure loss of the plastic composition preferably occurs on the downstream side of the plastic passage. This is because causing the pressure loss of the plastic composition on the downstream side of the plastic passage makes it easier to control the pressure of the plastic composition at the extrusion port 3 to a predetermined pressure.
[0101] Therefore, in the die 1 according to the present embodiment, the first channel 2a has a wide channel cross-sectional area while the plastic composition flows in the first channel 2a parallel to the extrusion center axis g to suppress pressure loss in the first channel 2a.
[0102] If the flow of the plastic composition is blocked at the third channel 2c connected to the extrusion port 3, resulting in a large pressure loss, the flow of the plastic composition may be interrupted at the third channel 2c. As a result, the plastic composition cannot be smoothly extruded from the extrusion port 3, and corrugated folds may appear.
[0103] Therefore, the third channel 2c is designed to have a gradually narrowing channel cross-sectional area so that the plastic composition does not stagnate in the third channel 2c, and the pressure applied to the plastic composition gradually loses. Therefore, by preventing the plastic composition from stagnating in the third channel 2c, the flow of the plastic composition in the third channel 2c can be prevented from being disturbed, and the plastic composition can be smoothly extruded from the extrusion port 3. Therefore, the generation of corrugation folds can be appropriately suppressed.
[0104] The channel cross-sectional area of the third channel 2c is a cross section orthogonal to the flow direction of the plastic composition in the third channel 2c (channel center line h3 of the third channel 2c). The third channel 2c has an annular shape and is Figure 4 In the cross section, the third channel 2c is separated from the extrusion center axis g as it moves downstream along the flow direction of the plastic composition. Therefore, the channel cross-sectional area of the third channel 2c is a three-dimensional plane where a portion of the cone surface is cut off. The channel cross-sectional area can be obtained by analytical calculation. If analytical calculation is difficult, such as when a hollow mold that is not a perfect circle is used, the cross-sectional area can be determined by actual measurement using methods such as 3D CAD.
[0105] However, the pressure loss in the third channel 2c alone is not enough to reduce the pressure of the plastic composition supplied from the extruder at high pressure to a predetermined pressure (about 7 MPa) before the extrusion port 3. Therefore, the second channel 2b has a large ratio (D1 / D2) of the channel cross-sectional area D1 at the connection part A with the first channel 2a (the inlet of the second channel 2b) and the channel cross-sectional area D2 at the connection part B with the third channel 2c (the outlet of the second channel 2b). By increasing the ratio (D1 / D2), the pressure loss of the plastic composition in the second channel 2b can be increased. Thus, the pressure of the plastic composition extruded from the extrusion port 3 can be reduced to a predetermined pressure (for example, about 7 MPa), and a foamed plastic sheet with a high expansion ratio can be obtained.
[0106] The ratio (D1 / D2) of the channel cross-sectional area D1 at the connection portion A (the inlet of the second channel) to the channel cross-sectional area D2 at the connection portion B with the third channel 2c (the outlet of the second channel) is preferably 3 or more, that is, the channel cross-sectional area D1 is preferably 3 times or more of the channel cross-sectional area D2. By setting this ratio to 3 times or more, the pressure loss of the plastic composition can be appropriately caused in the second channel 2b, and the pressure of the plastic composition extruded from the extrusion port 3 can be reduced to a predetermined pressure. Therefore, a foamed plastic sheet having a high expansion ratio can be obtained.
[0107] The connection part A between the first channel 2a and the second channel 2b is the intersection of the channel center line h1 of the first channel 2a and the channel center line h2 of the second channel 2b. The connection part B between the second channel 2b and the third channel 2c is the intersection of the channel center line h2 of the second channel 2b and the channel center line h3 of the third channel 2c.
[0108] The channel cross-sectional area D1 at the connection portion A (the inlet of the second channel) is a cross section orthogonal to the extrusion center axis g including the intersection point where the channel center line h1 of the first channel 2a and the channel center line h2 of the second channel 2b intersect. The channel cross-sectional area D2 at the connection portion B (the outlet of the second channel) is a cross section orthogonal to the extrusion center axis g including the intersection point where the channel center line h2 of the second channel 2b and the channel center line h3 of the third channel 2c intersect.
[0109] exist Figure 4 In the cross section shown, the angle α between the channel centerline h2 of the second channel 2b and the extrusion center axis g is preferably greater than or equal to 10° and less than or equal to 45°, more preferably greater than or equal to 15° and less than or equal to 40°, and even more preferably greater than or equal to 20° and less than or equal to 35°. If the angle α is less than 10°, the pressure loss of the plastic composition in the second channel 2b may be insufficient, and the pressure of the plastic composition may not be reduced to the pressure at which the plastic composition foams before the plastic composition reaches the extrusion port 3. On the other hand, if the angle α exceeds 45°, the flow direction of the plastic composition changes greatly at the connection portion B with the third channel, wherein the plastic composition flows in a direction away from the extrusion center axis g, as shown in FIG. Figure 4 As a result, the flow of the plastic composition may be disturbed on the upstream side of the third channel 2c at the outlet of the connection portion B. Therefore, the plastic composition cannot be smoothly extruded from the extrusion port 3, which may cause corrugation folds. In addition, since the flow of the plastic composition is disturbed and causes a large pressure loss, there is a risk that the plastic composition will foam in the channel.
[0110] By setting the angle α between the channel center line h2 of the second channel 2b and the extrusion center axis g to be greater than or equal to 10° and less than or equal to 45°, the flow disturbance of the plastic composition in the third channel 2c can be suppressed, and the pressure of the plastic composition at the extrusion port 3 can be reduced to a specified level. Therefore, the generation of corrugation folds can be suppressed, and a foamed plastic sheet with a high expansion ratio can be obtained.
[0111] The length of the second channel 2b in the direction of the extrusion center axis is preferably 10 mm or more. If the length is less than 10 mm, the angle between the extrusion center axis g and the second inner peripheral surface 4b constituting the outer inner wall surface of the second channel 2b on the inner peripheral surface of the outer mold 1a becomes too large. Therefore, the plastic composition flowing out of the first channel quickly changes its direction through the second inner peripheral surface 4b after flowing parallel to the extrusion center axis g, thereby flowing in the direction toward the extrusion center axis g. Therefore, the flow of the plastic composition is disturbed in the second channel 2b. If the flow in the channel is disturbed in this way, a large pressure loss will occur at the point where the flow is disturbed, which may cause the plastic composition to foam in the channel. If the flow is disturbed, for example, vortices appear and disappear, the pressure of the plastic composition in the channel becomes unstable.
[0112] On the other hand, the length of the second channel 2b in the extrusion central axis direction is 10 mm or more, so the inclination of the second inner peripheral surface 4b is gentle. In addition, the disturbance of the flow of the plastic composition in the second channel 2b can be suppressed, and the pressure of the plastic composition in the channel can be appropriately controlled.
[0113] In this embodiment, if Figure 4 As shown, the inner inner wall surface of the first channel 2a and the first outer peripheral surface 5a of the inner mold 1b constituting the inner inner wall surface of the second channel 2b are parallel to the extrusion center axis g. Therefore, the plastic composition flowing in the first channel 2a directly flows in the second channel 2b parallel to the extrusion center axis g without changing the flow direction. Therefore, the disturbance of the flow of the plastic composition in the second channel 2b can be suppressed, and the pressure of the plastic composition in the channel can be appropriately controlled.
[0114] The diameter of the first outer peripheral surface 5a of the inner mold 1b is preferably 20 mm or less. Figure 4 If the diameter of the first outer peripheral surface 5a of the similar plastic channel 2 exceeds 20 mm, the mold will become larger. By setting the diameter of the first outer peripheral surface 5a of the inner mold 1b to 20 mm or less, the enlargement of the mold 1 can be suppressed, and the channel cross-sectional area of the first channel 2a can be increased, and the pressure loss of the plastic composition in the first channel 2a can be successfully suppressed.
[0115] exist Figure 4In the cross section shown, the angle β between the extrusion direction (the channel center line h3 of the third channel 2c) of the plastic composition extruded from the extrusion port 3 and the extrusion center axis g is preferably greater than or equal to 50° and less than or equal to 90°. If the angle β is less than 50°, the pressure loss of the plastic composition when it flows from the second channel 2b to the third channel 2c may be insufficient, and the pressure of the plastic composition at the extrusion port 3 may not be reduced to a predetermined pressure. As a result, a foamed plastic sheet having a high expansion ratio may not be obtained.
[0116] If the angle β is 90° or less, the flow direction of the plastic composition changes greatly at the connection portion B. As a result, the flow of the plastic composition may be disturbed on the upstream side of the third channel 2c at the outlet of the connection portion B. Therefore, the plastic composition cannot be smoothly extruded from the extrusion port 3, which may cause corrugation folds. In addition, since the flow of the plastic composition is disturbed and a large pressure loss is caused, there is a risk that the plastic composition will foam in the channel.
[0117] By setting the angle β to be equal to or greater than 50° and equal to or less than 90°, the flow disturbance of the plastic composition in the third passage 2c can be suppressed, and the pressure of the plastic composition at the extrusion port 3 can be reduced to a predetermined pressure. Therefore, the generation of corrugation folds can be suppressed, and a foamed plastic sheet having a high expansion ratio can be obtained.
[0118] exist Figure 4 In the example shown, the first channel 2a is parallel to the extrusion center axis g (angle γ between the channel center line h1 of the first channel 2a and the extrusion center axis = 0°), but the first channel 2a may be slightly inclined to the extrusion center axis g. If the angle γ between the channel center line h1 of the first channel 2a and the extrusion center axis is greater than or equal to -10° and less than or equal to 30°, the plastic composition can flow smoothly from the first channel 2a to the second channel 2b. Therefore, the pressure loss of the connection portion A between the first channel and the second channel can be suppressed. A more preferred angle γ is greater than or equal to -10° and less than or equal to 20°, and a further preferred angle γ is greater than or equal to -10° and less than or equal to 10°.
[0119] Regarding the above-mentioned angle γ, at the inclined portion where the downstream side of the first channel 2a in the extrusion direction is closer to the extrusion central axis g than the upstream side thereof, the angle between the channel center line of the first channel 2a and the extrusion central axis g is positive. On the other hand, at the inclined portion where the upstream side of the first channel 2a in the extrusion direction is closer to the extrusion central axis g than the downstream side thereof, the angle between the channel center line of the first channel 2a and the extrusion central axis g is negative.
[0120] Next, the evaluation test conducted by the applicant will be described.
[0121] First, the preparation of the plastic foam sheet used for evaluation is described.
[0122] Preparation of plastic foam sheets
[0123] use Figure 1 The plastic manufacturing device 20 shown prepares a plastic foam sheet. A twin-screw extruder (manufactured by JSW, screw diameter 42 mm, L / D=48) is used as the first extruder 21A and the second extruder 21B in the plastic manufacturing device 20. The molds of Examples 1 to 3 and Comparative Example 1 described later are attached to the downstream end of the extrusion direction of the second extruder 21B to manufacture sheet-like foamed plastics and evaluate the presence or absence of corrugated creases. The outer diameter of the molds of Examples 1 to 3 and Comparative Example 1 is 70 mm and is made of chrome-plated SCM440.
[0124] use Figure 2 The kneading device 10 shown in the figure prepared a filler masterbatch containing 3% by mass of filler. Figure 1 The first quantitative feeder 22A of the plastic manufacturing device 20 shown in FIG. The masterbatch is supplied from the first quantitative feeder 22A to the raw material mixing and melting area a of the first extruder 21A at 1.67 kg / hr per unit time. In addition, polylactic acid resin (Revode 110, manufactured by HISUN, melting point 160° C.) is supplied from the second quantitative feeder 22B to the raw material mixing and melting area a at 8.33 kg / hr per unit time. Thus, a plastic composition containing more than 90% by mass of polylactic acid is obtained.
[0125] In the compressible fluid supply region b, carbon dioxide is supplied as the compressible fluid. The expansion ratio is adjusted by changing the amount of the supplied compressible fluid.
[0126] The plastic composition supplied with the compressible fluid was kneaded in the kneading area c of the first extruder 21A and supplied to the extrusion area d of the second extruder 21B. The compressible fluid was removed from the kneaded plastic composition in the extrusion area d at the extrusion channel portion 111b of the die 1; thus, an extruded foam was obtained. The discharge speed of the plastic composition from the die 1 was set to 10 kg / h, and the temperature of the plastic composition extruded from the die 1 was set to 150°C.
[0127] The temperature of the raw material mixing and melting area a and the compressible fluid supply area b in the first extruder 21A is set to 190°. The temperature of the kneading area c in the first extruder 21A is set to 150°C, which is 10°C lower than the melting point temperature (160°C) of polylactic acid. The temperature of the extrusion area d of the second extruder 21B is set so that the temperature of the plastic composition extruded from the die 1 becomes about 150°C or lower. The pressure of the kneading area c and the extrusion area d from the compressible fluid supply area b to the second extruder 21B (more specifically, the supply channel portion 111a of the die 1) is set to 7.0 MPa or higher.
[0128] Evaluation method of foam
[0129] Expansion ratio
[0130] The expansion ratio of the foamed plastic can be obtained by dividing the density of the composition constituting the foamed plastic (true density ρ0) by the bulk density (ρ1), as shown in the following equation (*). Expansion ratio = true density (ρ0) / bulk density (ρ1) ... (*)
[0131] The true density here is the density of the plastic composition retained as the final plastic composition, which can be a literature value or determined by actual measurement of non-foamed composite particles. In the case of polylactic acid, the true density is about 1.25 g / cm 3 .
[0132] The bulk density is obtained by measurement. The method for measuring the bulk density is not limited to a specific method, and any bulk density measuring method can be appropriately adopted. For example, the bulk density can be measured using the following method. The outer dimensions of a foamed sheet placed in an environment at a temperature of 23° C. and a relative humidity of 50% for more than 24 hours are measured to determine the gross volume. Then, the weight of the foamed sheet is measured. The bulk density of the foamed sheet is obtained by dividing the weight of the foamed sheet by the gross volume.
[0133] Evaluation of corrugation creases
[0134] To evaluate the corrugation creases, the presence or absence of the corrugation creases was checked by visual inspection of the surface and the cross section. The evaluation items included the expansion ratio range in which the corrugations appeared when the expansion ratio was changed by any of the above methods.
[0135] Example 1
[0136] The module in Example 1 is Figure 4 In the mold 1 shown, the channel cross-sectional area of the first channel 2a is constant, and the channel cross-sectional areas of the second channel 2b and the third channel 2c decrease toward the downstream in the flow direction of the plastic composition. The angle β is 60°, the angle α is 30°, and the angle γ is 0°.
[0137] The die of Example 1 was attached to the front end of the second extruder 21B, and the amount of the compressible fluid supplied was intentionally changed, thereby obtaining a foam having an expansion ratio of 1 to 50 times.
[0138] As a result, a suitable foamed body having an expansion ratio of 1 to 50 times and having no corrugation folds was obtained. In addition, the corrugated portion was not damaged or transparent.
[0139] Example 2
[0140] Figure 5 is a cross-sectional view of the die 1 according to Example 2, parallel to the extrusion center axis g.
[0141] The mold according to Example 2 has the same construction as the mold in Example 1, except that the angle β is set to 45°, as shown in FIG. Figure 5 The die according to Example 2 was attached to the end of the second extruder 21B, and a foamed body was obtained in a manner similar to that of Example 1.
[0142] As a result, no corrugation creases were observed in the foams with expansion ratios of 1 to 30 times, but corrugation creases were observed in the foams with expansion ratios of 30 to 50 times, and tearing and transparency phenomena occurred in the sheets with expansion ratios of 40 times or more.
[0143] Example 3
[0144] Figure 6 is a cross-sectional view of the die 1 according to Example 3, parallel to the extrusion center axis g.
[0145] The die 1 according to Example 3 had the same configuration as that of Example 1 except that the angle α was set to 10°. The die according to Example 3 was attached to the end of the second extruder 21B, and a foamed body was obtained in a manner similar to Example 1.
[0146] As a result, no corrugation creases were observed in the foams with expansion ratios of 1 to 30 times, but corrugation creases were observed in the foams with expansion ratios of 30 to 50 times, and tearing and transparency phenomena occurred in the sheets with expansion ratios of 40 times or more.
[0147] Example 4
[0148] Figure 7 is a cross-sectional view parallel to the extrusion center axis g of the die 1 according to Example 4.
[0149] The die 1 according to Example 4 had the same configuration as that of Example 1 except that the angle γ was set to 30°. The die according to Example 4 was attached to the end of the second extruder 21B, and a foamed body was obtained in a manner similar to Example 1.
[0150] As a result, no corrugation creases were observed in the foams with expansion ratios of 1 to 30 times, but corrugation creases were observed in the foams with expansion ratios of 30 to 50 times, and tearing and transparency phenomena occurred in the sheets with expansion ratios of 40 times or more.
[0151] Comparative Example 1
[0152] Figure 8 This is a cross-sectional view of die 1 according to Comparative Example 1, parallel to the extrusion central axis g.
[0153] The mold of Comparative Example 1 has the same structure as that of Example 1, except that the third channel 2c has a structure in which the channel cross-sectional area gradually increases downstream along the flow direction of the plastic composition, such as Figure 8 The die according to Comparative Example 1 was attached to the end of the second extruder 21B, and a foamed body was obtained in a manner similar to that of Example 1.
[0154] As a result, corrugation creases were observed in foams with expansion ratios of 1.5 to 50 times. In particular, periodic ripples in the direction orthogonal to the extrusion direction were conspicuous, and the foams could not be used for practical purposes. Most importantly, corrugation wrinkles at a high expansion ratio of 5 times or more not only caused thickness deviation, but also caused transparency of the foam and rupture due to the corrugations as defects.
[0155] Comparative Example 1 has a structure in which the cross-sectional area of the third channel 2c gradually increases toward the downstream along the flow direction of the plastic composition. It is believed that, accordingly, the plastic composition foams in the third channel 2c. In the case of a high expansion ratio, the volume increase is large, and if foaming occurs in the narrow third channel 2c, the foam will have nowhere to escape. As a result, at an expansion ratio of 1.5 times or more, the plastic composition foams upstream and downstream of the plastic composition to find an escape location, resulting in these corrugated folds.
[0156] In contrast, Examples 1 to 4 all have a structure in which the cross-sectional area of the third channel 2c gradually decreases toward the downstream along the flow direction of the plastic composition. It is considered that, therefore, the foaming of the plastic composition in the third channel 2c is suppressed, and a suitable foamed body without corrugated folds at an expansion ratio of at least 1 to 30 times is obtained. In particular, in Example 1, a suitable foamed body without corrugated folds at an expansion ratio of at least 1 to 50 times is obtained, and a suitable foamed body with a high expansion ratio without corrugated folds is obtained.
[0157] The above are only examples, and each of the following aspects has its specific effects.
[0158] Aspect 1
[0159] An extrusion molding die, for example, a die 1 includes an extrusion port 3, from which a plastic composition containing at least one plastic is extruded, and a plastic channel 2, in which the supplied plastic composition flows toward the extrusion port 3, wherein the plastic channel 2 includes a first channel 2a, a second channel 2b connected to the first channel 2a and having a channel cross-sectional area that gradually decreases downstream along the flow direction of the plastic composition, and a third channel 2c connected to the second channel 2b and allowing the plastic composition to flow toward the extrusion port 3, and the third channel 2c has a channel cross-sectional area that gradually decreases downstream along the flow direction of the plastic composition.
[0160] In the evaluation test, by forming a third channel with a gradually decreasing channel cross-sectional area on the downstream side of the flow direction of the plastic composition as described above, the corrugated folds can be suppressed, so that the foamed plastic can obtain a high expansion ratio.
[0161] Aspect 2
[0162] In aspect 1, the channel cross-sectional area of the connecting portion A between the first channel 2a and the second channel 2b is 3 times or more the channel cross-sectional area of the connecting portion B between the second channel 2b and the third channel 2c.
[0163] According to this aspect, the pressure loss in the second passage 2b can be increased as described in the embodiment, and the pressure of the plastic composition at the extrusion port 3 can be reduced to a predetermined pressure. Therefore, a foamed body having a high expansion ratio can be obtained.
[0164] Aspect 3
[0165] In aspect 1 or 2, the extrusion molding die includes: an outer die 1a having a through hole; and an inner die 1b, which is arranged in the through hole and has a gap with the inner peripheral surface 4 of the through hole, wherein a plastic channel 2 having an annular cross-sectional shape orthogonal to the extrusion center axis g is formed by the inner peripheral surface 4 of the through hole of the outer die 1a and the outer peripheral surface 5 of the inner die 1b, and the inner peripheral surface forms a second channel 2b. For example, the second inner peripheral surface 4b of the through hole of the outer die 1a has an inner diameter that gradually decreases toward the downstream along the flow direction of the plastic composition. The inner circumferential surface forms the third channel 2c, for example, the third inner circumferential surface 4c of the through hole of the outer mold 1a has a shape in which the inner diameter gradually increases downstream along the flow direction of the plastic composition, and the outer circumferential surface forms the third channel 2c, for example, the second outer circumferential surface 5b of the inner mold has a shape in which the inner diameter gradually increases downstream along the flow direction of the plastic composition, and the gap between the outer circumferential surface of the inner mold forming the third channel 2c and the inner circumferential surface of the through hole of the outer mold 1a forming the third channel 2c gradually decreases downstream along the flow direction of the plastic composition.
[0166] According to this aspect, as described in the embodiment, the first channel 2a having an annular shape, the second channel 2b having an annular shape with a channel cross-sectional area decreasing toward the downstream along the flow direction of the plastic composition, and the third channel 2c having an annular shape with a diameter increasing toward the downstream along the flow direction can be formed. In addition, the third channel 2c having a channel cross-sectional area decreasing toward the downstream side along the flow direction of the plastic composition can be formed.
[0167] Aspect 4
[0168] In Aspect 3, the outer peripheral surface of the inner die 1b forming the first passage 2a and the outer peripheral surface forming the second passage 2b are parallel to the extrusion central axis g.
[0169] According to this aspect, as described in the embodiment, the plastic composition flowing in the first channel 2a (close to the extrusion center axis g) keeps flowing in the second channel 2b parallel to the extrusion center axis g without changing the flow direction. Therefore, the disturbance of the flow of the plastic composition in the second channel 2b can be suppressed, and the pressure of the plastic composition in the channel can be appropriately controlled.
[0170] Aspect 5
[0171] In aspect 4, the outer diameters of the outer peripheral surface of the inner mold 1b forming the first passage 2a and the outer peripheral surface forming the second passage 2b are 20 mm or less.
[0172] According to this aspect, as described in the embodiment, the channel cross-sectional area of the first channel 2a can be increased while suppressing the size of the extrusion molding die such as the die 1, and the pressure loss in the first channel 2a can be appropriately suppressed.
[0173] Aspect 6
[0174] In any one of aspects 1 to 5, in a cross section including the extrusion central axis g and parallel to the extrusion central axis g, an angle β between the extrusion direction of the plastic composition extruded from the extrusion port and the extrusion central axis g is greater than or equal to 50° and less than or equal to 90°.
[0175] According to this aspect, as described in the embodiment, the disturbance of the flow of the plastic composition in the third passage 2c can be suppressed, and the pressure of the plastic composition at the extrusion port 3 can be reduced to a predetermined pressure. Therefore, the generation of corrugated folds can be suppressed, and a foamed plastic sheet with a high expansion ratio can be obtained.
[0176] Aspect 7
[0177] In any one of aspects 1 to 6, in a cross section including and parallel to the extrusion central axis g, an angle α between a channel center line h2 of the second channel 2b and the extrusion central axis g is 10° or more and 45° or less.
[0178] According to this aspect, as described in the embodiment, the disturbance of the flow of the plastic composition in the third passage 2c can be suppressed, and the pressure of the plastic composition at the extrusion port 3 can be reduced to a predetermined pressure. Therefore, the generation of corrugated folds can be suppressed, and a foamed plastic sheet with a high expansion ratio can be obtained.
[0179] Aspect 8
[0180] In any one of aspects 1 to 7, in a cross section containing the extrusion center axis g and parallel to the extrusion center axis g, an angle γ between the extrusion center axis g and the channel center line h1 of the first channel 2a is greater than or equal to -10° and less than or equal to 30°, wherein the angle at which the channel center line h1 of the first channel 2a intersects the extrusion center axis g on the upstream side in the flow direction of the plastic composition is negative, and the angle at which the channel center line h1 of the first channel 2a intersects the extrusion center axis g on the downstream side in the flow direction of the plastic composition is positive.
[0181] According to this aspect, as described in the embodiment, the plastic composition can smoothly flow from the first channel 2a to the second channel 2b, and the pressure loss at the connection portion A between the first channel and the second channel can be suppressed.
[0182] Aspect 9
[0183] In any one of aspects 1 to 8, the length of the second channel 2b in the extrusion center axis direction is 10 mm or more.
[0184] According to this aspect, as explained in the embodiment, the disturbance of the flow of the plastic composition in the second channel 2b can be suppressed, and the pressure of the plastic composition in the channel can be appropriately controlled.
[0185] Aspect 10
[0186] The plastic manufacturing equipment 20 includes a mold, such as mold 1, to which a plastic composition containing at least one plastic is supplied, and the plastic composition is extruded from the extrusion port 3 of the mold to produce foamed plastic, wherein the extrusion molding mold described in any one of aspects 1 to 9 above is used as the mold.
[0187] Therefore, the expansion ratio for generating the corrugated folds can be increased.
[0188] Aspect 11
[0189] In aspect 10, the plastic manufacturing apparatus 20 includes a kneading portion, such as a kneading zone c, to obtain a plastic composition by kneading at least one plastic at a temperature below a melting point of the plastic in the presence of a compressible fluid.
[0190] According to this aspect, as described in the examples, the kneading efficiency is improved, and the foaming speed in the mold (e.g., die) in the plastic composition can be made uniform. Therefore, the generation of partial corrugation folds can be suppressed. In addition, the occurrence of degradation, carbonization, oxidation, tar, and decomposition of combustion deposits in the equipment can be suppressed.
[0191] Aspect 12
[0192] In aspect 10 or 11, the plastic manufacturing equipment 20 includes an extrusion molding part, such as extrusion zone d, which extrude the plastic composition from a mold (such as mold 1) in the presence of a compressible fluid at a temperature below the melting point of the plastic (such as polylactic acid) to mold a foamed plastic.
[0193] According to this aspect, the viscosity of the plastic composition can be increased compared to the case where the plastic composition is extruded from a mold (e.g., mold 1) at a temperature higher than the melting point of the plastic to form a foamed plastic. Therefore, the foamed plastic can be molded by extruding the plastic composition in a high viscosity state, and a suitable foamed body can be obtained without any foam rupture.
[0194] Aspect 13
[0195] In any one of Aspects 10 to 12, the plastic composition contains 90% by mass or more of polylactic acid.
[0196] According to this aspect, a device for producing the biodegradable foamed plastic composition as described in the embodiment can be provided.
[0197] Aspect 14
[0198] In a method for manufacturing a foamed plastic for extruding a plastic composition containing at least one plastic from an extrusion port 3 of a mold (eg, die 1 ) to manufacture a foamed plastic, the extrusion molding mold according to any one of aspects 1 to 8 is used as the mold.
[0199] According to this aspect, it is possible to produce a foamed plastic having an expansion ratio of 1 or more and 30 or less and having few corrugation folds.
[0200] The above embodiments are illustrative and do not limit the present invention. Therefore, based on the above teachings, many additional modifications and variations are possible. For example, within the scope of the present disclosure and the appended claims, at least one element of different illustrative and exemplary embodiments herein may be combined with or replaced with each other. In addition, the features of the number, position, shape, etc. of the constituent elements of the embodiments are not limited to the embodiments and may be preferably set. Therefore, it should be understood that within the scope of the appended claims, the disclosure of the present invention may be implemented in a manner different from that specifically described herein.
[0201] The method steps, processes, or operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless specifically specified as an order of performance or clearly indicated by the context. It should also be understood that additional or alternative steps may be employed.
Claims
1. An extrusion molding die, characterized in that: include: an extrusion port, the extrusion port being configured to extrude a plastic composition comprising at least one plastic; and A plastic channel configured to allow the supplied plastic composition to flow toward the extrusion port, wherein The plastic channel includes a first channel, a second channel, and a third channel, the second channel being connected to the first channel and having a channel cross-sectional area gradually decreasing toward downstream along a flow direction of the plastic composition, the third channel being connected to the second channel and configured to allow the plastic composition to flow toward the extrusion port, and The third channel has a channel cross-sectional area that gradually decreases toward the downstream along the flow direction of the plastic composition, and In a cross section including the extrusion central axis and parallel to the extrusion central axis, an angle β between an extrusion direction of the plastic composition extruded from the extrusion port and the extrusion central axis is greater than or equal to 50° and less than or equal to 90°; In a cross section including the extrusion central axis and parallel to the extrusion central axis, an angle γ between the extrusion central axis and a channel centerline of the first channel is greater than or equal to -10° and less than or equal to 30°, wherein an angle at which the channel centerline of the first channel intersects the extrusion central axis on the upstream side in the flow direction of the plastic composition is negative, and an angle at which the channel centerline of the first channel intersects the extrusion central axis on the downstream side in the flow direction of the plastic composition is positive; The length of the second channel in the direction of the extrusion center axis is 10 mm or more; The first outer peripheral surface of the inner die constituting the inner inner wall surface of the second channel is parallel to the extrusion central axis.
2. The extrusion molding die according to claim 1, characterized in that: A channel cross-sectional area of a connection portion between the first channel and the second channel is three times or more than three times a channel cross-sectional area of a connection portion between the second channel and the third channel.
3. The extrusion molding die according to claim 1 or 2, characterized in that: Also includes: an outer mold including a through hole; and The inner mold is arranged in the through hole and has a gap with the inner circumference of the through hole, wherein The plastic channel having an annular cross-sectional shape orthogonal to the extrusion center axis is formed by the inner peripheral surface of the through hole of the outer mold and the outer peripheral surface of the inner mold, The inner peripheral surface of the through hole of the outer mold forming the second channel has an inner diameter that gradually decreases toward the downstream along the flow direction of the plastic composition. The inner peripheral surface of the through hole of the outer mold forming the third channel has an inner diameter that gradually increases toward the downstream along the flow direction of the plastic composition. The outer peripheral surface of the inner mold forming the third channel has an inner diameter that gradually increases toward the downstream along the flow direction of the plastic composition, and The gap between the outer circumferential surface of the inner mold forming the third channel and the inner circumferential surface of the through hole of the outer mold forming the third channel gradually decreases toward the downstream along the flow direction of the plastic composition.
4. The extrusion molding die according to claim 3, characterized in that: The outer peripheral surface of the inner die forming the first channel and the outer peripheral surface forming the second channel are parallel to the extrusion central axis.
5. The extrusion molding die according to claim 4, characterized in that: The outer diameters of the outer peripheral surface of the inner mold forming the first channel and the outer peripheral surface of the inner mold forming the second channel are 20 mm or less.
6. The extrusion molding die according to any one of claims 1, 2, 4 and 5, characterized in that: In a cross section including the extrusion central axis and parallel to the extrusion central axis, an angle α between a channel center line of the second channel and the extrusion central axis is greater than or equal to 10° and less than or equal to 45°.
7. A plastic manufacturing device comprising a mold, characterized in that: The plastic manufacturing device is configured to supply a plastic composition containing at least one plastic to the mold, and extrude the plastic composition from an extrusion port of the mold to manufacture a foamed plastic, wherein As the die, the extrusion-molding die according to any one of claims 1 to 6 is used.
8. The plastic manufacturing device according to claim 7, characterized in that: The invention also includes a kneading section configured to knead the at least one plastic at a temperature lower than a melting point of the at least one plastic in the presence of a compressible fluid to obtain the plastic composition.
9. The plastic manufacturing device according to claim 7 or 8, characterized in that: Also included is an extrusion molding part, which is configured to extrude the plastic composition from the mold at a temperature lower than the melting point of the at least one plastic in the presence of a compressible fluid to mold a foamed plastic.
10. A plastic manufacturing method for extruding a plastic composition comprising at least one plastic from an extrusion port of a mold to manufacture a foamed plastic, characterized in that: As the die, the extrusion-molding die according to any one of claims 1 to 6 is used.