Optical component manufacturing method and manufacturing device

The powder residues of optical components are removed by impacting dry ice particles, and the dimensional accuracy and pollution problems in the prior art are solved, thereby achieving efficient powder removal and accuracy improvement.

CN115220143BActive Publication Date: 2024-11-05SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210828748.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-19
Filing Date
2018-10-04
Publication Date
2024-11-05
Estimated Expiration
2038-10-04

AI Technical Summary

Technical Problem

The existing optical component manufacturing methods are difficult to meet the requirements of high precision dimensionality, and powder residues are prone to occur during cutting and grinding, resulting in contamination of the final product.

Method used

Dry ice particles are used to impact the end surface of the optical member to remove powder residues. By adjusting the average particle size and atmosphere conditions of the dry ice particles, the powder is efficiently removed and the defects of the adhesive layer are suppressed.

Benefits of technology

Effectively remove powder residues such as cutting, cutting, grinding, etc., improve the accuracy and quality of optical components, reduce the risk of pollution, and shorten the processing time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115220143B_ABST
    Figure CN115220143B_ABST
Patent Text Reader

Abstract

[Subject] Provide a method and apparatus for manufacturing an optical component with less adhesion of powder such as grinding debris. [Solution] The method for manufacturing an optical component includes: a step of preparing a laminate (100) having an optical film (50) and an adhesive layer (80) provided on one surface of the optical film (50), and having powder (f) adhered to its end surface (E); and a step of causing dry ice particles (d) to impact the end surface (E) of the laminate (100) to remove the powder (f) from the end surface (E).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application is a divisional application of an application filed on October 4, 2018, with application number 201880064320.X, and invention name “Manufacturing method and manufacturing device for optical components”. Technical Field

[0002] The present invention relates to a method and an apparatus for manufacturing an optical component. Background Art

[0003] Conventionally, there is known an optical member including an optical film such as a polarizing plate and a pressure-sensitive adhesive layer.

[0004] As a method for obtaining an optical member of a desired size, it is known to cut a raw material laminate having an optical film and a pressure-sensitive adhesive layer with a laser or a blade (see Patent Documents 1 and 2).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: WO2014 / 189078

[0008] Patent Document 2: Japanese Patent Application Publication No. 2009-86675 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, in recent years, the requirements for the dimensional accuracy of optical components using optical films and adhesive layers have become increasingly stringent. Therefore, it is difficult to obtain the desired dimensional accuracy by simply cutting the raw material laminate. Thus, sometimes the end faces of the laminate after cutting are processed by grinding and polishing.

[0011] However, when the end surface of the laminate is processed by grinding or the like, powder such as grinding debris may adhere to the end surface of the laminate. If the powder remains on the laminate, it may cause contamination of the final product including the laminate, which is not preferred.

[0012] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a method and an apparatus for manufacturing an optical member with little adhesion of powder such as grinding scraps.

[0013] Means for solving problems

[0014] The manufacturing method of the optical component described in the present invention includes: a step of preparing a stacked body having an optical film and an adhesive layer provided on one surface of the optical film and having powder attached to its end surface (preparation step); and a step of removing the powder from the end surface by causing dry ice particles to impact the end surface of the stacked body (impact step).

[0015] According to the present invention, powders such as cutting chips, shavings, and grinding chips can be suitably removed from the end surface of a laminate (optical member) using dry ice particles.

[0016] Here, the average particle size of the dry ice particles may be 100 to 1000 μm.

[0017] This makes it possible to appropriately remove powder such as grinding chips and suppress the adhesive on the end surface from being damaged.

[0018] Furthermore, in the impact step, the dry ice particles may be caused to impact an end surface of a stacked structure in which a plurality of stacked bodies are stacked.

[0019] This enables mass processing of laminated bodies.

[0020] Furthermore, the dry ice particles may impact a portion of the end surface, while at the same time, the other portion of the end surface of the stacked body may be subjected to at least one selected from the group consisting of cutting, chipping, and grinding.

[0021] This allows a plurality of processes to be performed simultaneously and in parallel, thereby shortening the process time.

[0022] In the preparation step, the end surface may be subjected to at least one treatment selected from the group consisting of cutting, milling, and grinding, and when the dry ice particles are caused to impact a portion of the end surface, the end surface may not be subjected to any treatment selected from the group.

[0023] This allows the atmosphere (space) for removing powders by the impact of dry ice particles to be separated from the atmosphere (space) for processing where powders are generated, thereby preventing powders generated by processing of the end surface from contaminating the portion impacted by dry ice.

[0024] The optical film may be at least one selected from a polarizing plate, a protective film, a phase difference film, a brightness enhancement film, a window film, and a touch sensor; or may contain two or more laminated films of at least one selected from the group, or may contain at least two laminated films selected from the group.

[0025] The relative humidity of the atmosphere in the impact process may be 30 to 75%.

[0026] The optical component manufacturing device described in the present invention comprises: an end surface processing section for cutting, grinding or grinding the end surface of a stacked body having an optical film and an adhesive layer provided on one surface of the optical film; and a dry ice particle supply section for causing dry ice particles to impact a portion of the stacked body processed into the end surface processing section.

[0027] The optical member manufacturing apparatus may further include a transport unit that moves the stacked body between the end surface processing unit and the dry ice particle supply unit.

[0028] Effects of the Invention

[0029] According to the present invention, it is possible to provide a method and an apparatus for producing an optical member with little adhesion of powder such as grinding scraps. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 (a) and (b) are cross-sectional views of a laminate 100 according to one embodiment of the present invention.

[0031] Figure 2 (a) and (b) are cross-sectional views of another example of the laminate.

[0032] Figure 3 This is a schematic diagram of the dry ice particle supply unit.

[0033] Figure 4 This is a conceptual diagram showing a method of causing dry ice particles to impact the end surface of a stacked structure 120 having a plurality of stacked bodies 100 .

[0034] Figure 5 This is a perspective view of an optical member manufacturing apparatus according to one embodiment of the present invention.

[0035] Figure 6 It is shown Figure 5 A three-dimensional view of another example of the end surface processing portion in FIG.

[0036] Figure 7 This is a conceptual diagram showing a mode in which ice particles are made to collide with the inner end surface of the stacked structure 120 having the through hole H′. DETAILED DESCRIPTION

[0037] A method and an apparatus for manufacturing an optical member according to an embodiment of the present invention will be described with reference to the drawings.

[0038] (Preparation of a laminate with powder attached to the end surface)

[0039] First, if Figure 1 As shown in (a), a laminate 100 having an optical film 50 and an adhesive layer 80 provided on one surface of the optical film 50 and having powder f attached to its end surface E is prepared. It should be noted that the end surface E is not limited to the outer end surface of the laminate 100. For example, Figure 1 As shown in (b) of FIG. 1 , when the stacked body 100 has a hole H penetrating in the stacking direction, powder f such as pore chips may also adhere to the inner wall of the hole H, that is, the inner end surface E of the stacked body 100 .

[0040] (Optical Film)

[0041] The optical film 50 is a film that transmits at least a part of visible light.

[0042] Examples of the optical film 50 include a polarizing plate, a protective film, a phase difference film, a brightness enhancement film, a window film, and a touch sensor. The optical film 50 may have a laminated structure including a single type of a plurality of these films, or may have a laminated structure including a plurality of these films.

[0043] (Polarizing Plate)

[0044] Polaroid refers to a film in which the transmittance of linear polarized light is different from each other in two orthogonal directions in the plane. As the material of polaroid, the known materials used in the manufacture of polaroid can be used, such as polyvinyl alcohol resin, polyvinyl acetate resin, ethylene / vinyl acetate (EVA) resin, polyamide resin, polyester resin, etc. can be cited. Among them, polyvinyl alcohol resin is preferred. After these resin films are stretched, dyeing and boric acid treatment based on iodine or dichroic dye are applied, thus a film-shaped polaroid (film-type polaroid) can be obtained.

[0045] The thickness of the film-type polarizing plate can be, for example, 1 to 75 μm.

[0046] In addition, as another example of the polarizer, it can be a liquid crystal coating polarizer formed by a liquid crystal compound. The liquid crystal coating polarizer can be manufactured, for example, by using a suitable substrate and coating a liquid crystal polarizing light composition on the substrate. Before coating the liquid crystal polarizing light composition on the substrate, an orientation film can also be formed. The liquid crystal polarizing light composition can include a liquid crystal compound and a dichroic pigment compound. As the liquid crystal compound, as long as it has the property of showing a liquid crystal state, it is particularly preferred to have a high-order liquid crystal state such as a smectic phase, because the obtained liquid crystal coating polarizer can exert high polarization performance. In addition, the liquid crystal compound is also preferably provided with a polymerizable functional group. The dichroic pigment compound is a pigment that is oriented together with the liquid crystal compound to show dichroism, and the dichroic pigment itself can also have liquid crystal properties and can also have a polymerizable functional group. Any compound contained in the liquid crystal polarizing light composition preferably has a polymerizable functional group. The liquid crystal polarizing light composition can also include an initiator, a solvent, a dispersant, a leveling agent, a stabilizer, a surfactant, a crosslinking agent, a silane coupling agent, and the like.

[0047] Here, a typical example of a method for producing a liquid crystal coating type polarizing plate by forming an alignment film on a substrate and coating a liquid crystal polarizing composition on the substrate having the alignment film formed thereon is shown.

[0048] The liquid crystal coated light type polarizing plate manufactured by this method can be made thinner than the film type polarizing plate. The thickness of the liquid crystal coated light type polarizing plate is 0.5 to 10 μm, preferably 1 to 5 μm.

[0049] For the alignment film, a coating film is formed by, for example, coating an alignment film-forming composition on a substrate, and the coating film is given orientation by friction, polarized light irradiation, etc., so that an alignment film can be formed on the substrate. The alignment film-forming composition includes an alignment agent, and in addition to the alignment agent, it may also include a solvent, a cross-linking agent, an initiator, a dispersant, a leveling agent, a silane coupling agent, etc. As the alignment agent, for example, polyvinyl alcohols, polyacrylates, polyamic acids, and polyimides can be cited. As a method for imparting the alignment, when light orientation is applied, an alignment agent containing a cinnamate group is preferred.

[0050] The alignment agent may be a polymer. The weight average molecular weight of the polymer alignment agent is about 10,000 to 1,000,000. The thickness of the alignment film formed on the substrate is preferably 5 nm to 10,000 nm, and particularly preferably 10 to 500 nm, because sufficient alignment restriction force can be exhibited.

[0051] A liquid crystal polarizing composition is applied onto a substrate having an alignment film formed thereon and dried as necessary to form a coating film of the liquid crystal polarizing composition. A liquid crystal coating-type polarizing plate is produced from the coating film of the liquid crystal polarizing composition.

[0052] The liquid crystal polarizer thus manufactured can be peeled off from the substrate. As a method for peeling the liquid crystal coated polarizer from the substrate, for example, by using a second substrate to be attached to the surface of the unlaminated substrate of the liquid crystal coated polarizer, and then peeling the substrate, thereby obtaining a method for obtaining a laminate composed of a liquid crystal coated polarizer-a second substrate, the liquid crystal coated polarizer can also be transferred to the second substrate, or it can be kept laminated on the substrate without being transferred to the second substrate. The substrate or the second substrate also preferably functions as a transparent substrate for a protective film, a phase difference plate, or a window film.

[0053] (Protective film)

[0054] The protective film is a transparent film for preventing damage or the like to other optical films such as polarizing plates and / or optical devices (such as liquid crystal cells) to which the laminate 100 is later bonded. The protective film may be any of various transparent resin films.

[0055] Here, the protective film for protecting the polarizing plate is described. Examples of resins forming the protective film are:

[0056] Cellulose resins represented by triacetyl cellulose;

[0057] Polyolefin resins represented by polypropylene resins;

[0058] Cyclic olefin resins represented by norbornene resins;

[0059] Acrylic resins, typified by polymethyl methacrylate resins; and

[0060] Polyethylene terephthalate resins are representative examples of polyester resins. Among these, cellulose resins are representative.

[0061] The thickness of the protective film may be, for example, 5 to 90 μm.

[0062] The protective film may contain a plasticizer, an ultraviolet absorber, an infrared absorber, a colorant such as a pigment or a dye, a fluorescent brightener, a dispersant, a heat stabilizer, a light stabilizer, an antistatic agent, an antioxidant, a lubricant, a solvent, and the like as necessary.

[0063] A hard coating may also be provided on at least one side of the protective film in order to improve the scratch resistance of the protective film surface. The thickness of the hard coating is usually in the range of 2 to 100 μm. When the thickness of the hard coating is less than 2 μm, it is difficult to ensure sufficient scratch resistance. If it exceeds 100 μm, the bending resistance is reduced, and when the protective film is attached to a polarizer, etc., curling may occur due to curing shrinkage.

[0064] The hard coating layer can be formed using a hard coating composition containing a reactive material that forms a cross-linked structure by irradiating active energy rays or thermal energy rays. Among these, a hard coating layer obtained by irradiation with active energy rays is preferred. Active energy rays are defined as energy rays that can decompose compounds that produce active species and produce active species. As active energy rays, visible light, ultraviolet rays, infrared rays, X-rays, α rays, β rays, γ rays and electron beams can be cited. Among these, ultraviolet rays are particularly preferred. The hard coating composition preferably contains at least one of a free radical polymerizable compound and a cationic polymerizable compound. Oligomers obtained by partially polymerizing these free radical polymerizable compounds and cationic polymerizable compounds may also be included in the hard coating composition.

[0065] First, the radical polymerizable compound will be described.

[0066] The radical polymerizable compound refers to a compound having a radical polymerizable group. As the radical polymerizable group, any functional group capable of undergoing a radical polymerization reaction may be a group containing a carbon-carbon unsaturated double bond, and examples thereof include a vinyl group, a (meth)acryloyl group, and the like. It should be noted that when the radical polymerizable compound has two or more radical polymerizable groups in one molecule, these radical polymerizable groups may be the same or different. When the radical polymerizable compound has two or more radical polymerizable groups in one molecule, the hardness of the obtained hard coating layer tends to be improved. As the radical polymerizable compound, from the perspective of high reactivity, a compound having a (meth)acryloyl group is preferred, and examples thereof include a compound called a multifunctional acrylate monomer having 2 to 6 (meth)acryloyl groups in one molecule, epoxy (meth)acrylate, urethane (meth)acrylate, and an oligomer having multiple (meth)acryloyl groups in the molecule and a molecular weight ranging from hundreds to thousands. Among the compounds having a (meth)acryloyl group, at least one selected from epoxy (meth)acrylate, urethane (meth)acrylate, and polyester (meth)acrylate is preferred.

[0067] Next, the cationically polymerizable compound will be described.

[0068] The cationic polymerizable compound refers to a compound having a cationic polymerizable group such as an epoxy group, an oxetane group, a vinyl ether group, etc. With regard to the number of cationic polymerizable groups in one molecule of the cationic polymerizable compound, from the viewpoint of increasing the hardness of the obtained hard coating, it is preferably 2 or more, and more preferably 3 or more. In addition, as the cationic polymerizable compound, a compound having at least one cationic polymerizable group of an epoxy group and an oxetane group is preferred. The cyclic ether group of the epoxy group and the oxetane group has the advantage of small shrinkage associated with the polymerization reaction. In addition, among the compounds having an epoxy group among the cyclic ether groups, compounds of various structures are easily available from the market, and are not likely to have an adverse effect on the durability of the obtained hard coating. When the hard coating composition uses a combination of a free radical polymerizable compound and a cationic polymerizable compound, the compound having an epoxy group has the advantage that the compatibility with the free radical polymerizable compound is also easy to control. In addition, the oxetane group among the cyclic ether groups has the following advantages compared with the epoxy group: the degree of polymerization can be easily increased, the toxicity is low, the network formation rate obtained by the cationic polymerizable compound of the obtained hard coat is accelerated, and the unreacted monomers in the area mixed with the free radical polymerizable compound will not remain in the film but form an independent network.

[0069] Examples of the compound having an epoxy group include

[0070] Polyglycidyl ethers of polyols having alicyclic rings;

[0071] Alicyclic epoxy resins obtained by epoxidizing compounds containing cyclohexene rings or cyclopentene rings with a suitable oxidant such as hydrogen peroxide or peracid;

[0072] Polyglycidyl ethers of aliphatic polyols or their alkylene oxide adducts;

[0073] Polyglycidyl esters of aliphatic long-chain polyacids;

[0074] Aliphatic epoxy resins such as homopolymers and copolymers of glycidyl (meth)acrylate;

[0075] Glycidyl ethers produced by the reaction of bisphenols such as bisphenol A, bisphenol F, hydrogenated bisphenol A, or derivatives thereof such as alkylene oxide adducts and caprolactone adducts with epichlorohydrin; and

[0076] Glycidyl ether epoxy resins derived from bisphenols and the like are phenolic epoxy resins.

[0077] The hard coating composition may further include a polymerization initiator. As the polymerization initiator, a suitable substance (free radical polymerization initiator, cationic polymerization initiator) can be selected and used according to the type of polymerizable compound contained in the hard coating composition. These polymerization initiators are decomposed by at least one of active energy ray irradiation and heating to generate free radicals or cations, and perform free radical polymerization or cationic polymerization.

[0078] The radical polymerization initiator may be any one that can release a substance that initiates radical polymerization by at least one of irradiation with active energy rays and heating. For example, examples of thermal radical polymerization initiators include organic peroxides such as hydrogen peroxide and perbenzoic acid, and azo compounds such as azobisbutyronitrile.

[0079] As the active energy ray radical polymerization initiator, there are Type 1 radical polymerization initiators that generate radicals by decomposition of molecules and Type 2 radical polymerization initiators that generate radicals by hydrogen abstraction reaction in the presence of tertiary amines. These can be used alone or in combination.

[0080] The cationic polymerization initiator can be used as long as it can release a substance that initiates cationic polymerization by at least any one of active energy ray irradiation and heating. As the cationic polymerization initiator, aromatic iodonium salts, aromatic sulfonium salts, cyclopentadienyl iron (II) complexes, etc. can be used. They can initiate cationic polymerization by any one or any of active energy ray irradiation or heating depending on their structure.

[0081] The polymerization initiator may contain 0.1 to 10% by weight relative to the total weight of the hard coating composition. When the content of the polymerization initiator is less than 0.1% by weight, sufficient curing cannot be performed, and the mechanical properties of the hard coating obtained in the end are likely to be reduced, or the adhesion between the hard coating and the protective film cannot be achieved. When the content exceeds 10% by weight, poor adhesion, cracking and curling may occur due to the curing shrinkage during the formation of the hard coating.

[0082] The hard coating composition may further include one or more selected from solvents and additives.

[0083] The solvent can dissolve or disperse the polymerizable compound and the polymerization initiator, and any solvent known as a solvent for a hard coating composition in the art can be used without limitation.

[0084] The additives include inorganic particles, leveling agents, stabilizers, surfactants, antistatic agents, lubricants, antifouling agents, and the like.

[0085] Next, a method for bonding the protective film to the polarizing plate will be described.

[0086] The protective film of the polarizer is preferably attached to the polarizer by means of an adhesive. Examples of the adhesive include:

[0087] Water-based adhesives such as polyvinyl alcohol resin aqueous solutions and water-based two-component polyurethane emulsion adhesives are used;

[0088] Active energy ray-curable adhesives such as curable compositions containing a polymerizable compound and a photopolymerization initiator, curable compositions containing a photoreactive resin, and curable compositions containing a binder resin and a photoreactive crosslinking agent are used.

[0089] The polyvinyl alcohol resin contained in the aqueous solution of the polyvinyl alcohol resin used as the adhesive includes a vinyl alcohol homopolymer obtained by saponifying polyvinyl acetate, which is a homopolymer of vinyl acetate, a vinyl alcohol copolymer obtained by saponifying a copolymer of vinyl acetate and other monomers copolymerizable therewith, and a modified polyvinyl alcohol polymer obtained by partially modifying the hydroxyl groups thereof, etc. In such an aqueous adhesive, polyaldehydes, water-soluble epoxy compounds, melamine compounds, zirconium oxide compounds, zinc compounds, etc. may be further added as additives.

[0090] Examples of the active energy ray-curable adhesive used as the adhesive include the same adhesive as exemplified as one of the hard coating compositions described above, which contains a reactive material that forms a crosslinked structure upon irradiation with active energy rays.

[0091] In the above, a method of using a resin film as a protective film (or a protective film having a hard coat layer) and bonding it to a polarizing plate is described. However, a thinner protective layer may be directly laminated on a polarizing plate instead of the resin film to form a protective film.

[0092] As a method for directly laminating a thinner protective layer on a polarizer, for example, a coating film containing an active energy ray-curable resin is formed on the surface of the polarizer, and when the coating film is cured by irradiation with active energy rays (UV, etc.), a protective film thinner than the existing protective film can be directly formed on the surface of the polarizer. As the active energy ray-curable resin, a resin containing a reactive material that forms a cross-linked structure by irradiation with active energy rays, which is exemplified as one of the above-mentioned hard coating compositions, can be cited.

[0093] (Window Film)

[0094] On the other hand, a transparent protective film that prevents damage to an optical device (liquid crystal unit, etc.) to which the laminate 100 is subsequently attached is called a window film. For example, when the optical film 50 has a laminated structure including a plurality of films, the window film is disposed on the outermost surface of the plurality of films on the side opposite to the surface on which the adhesive layer 80 is disposed.

[0095] The window film is arranged on the observation side of the flexible image display device, and plays the function of protecting other components from external impact or environmental changes such as temperature and humidity. In the past, glass was used as such a protective layer, but the window film in the flexible image display device is not rigid and hard like glass, but has flexible characteristics. The window film includes a flexible transparent substrate and may also include a hard coating on at least one side.

[0096] (Transparent substrate)

[0097] A transparent substrate that can be used as a window film will be described.

[0098] The visible light transmittance of the transparent substrate is 70% or more, preferably 80% or more. The transparent substrate may be any material as long as it is a transparent polymer film. Specifically, it may be a film formed of the following polymers, or a film formed by these polymers alone or by mixing two or more of them:

[0099] Polyolefins such as cycloolefin derivatives having units containing monomers of polyethylene, polypropylene, polymethylpentene, norbornene or cycloolefin;

[0100] (Modified) celluloses such as diacetyl cellulose, triacetyl cellulose, propionyl cellulose, etc.;

[0101] Acrylic acids such as methyl methacrylate (co)polymers;

[0102] Polystyrenes such as styrene (co)polymers;

[0103] Acrylonitrile-butadiene-styrene copolymers, acrylonitrile-styrene copolymers;

[0104] Ethylene-vinyl acetate copolymers;

[0105] Polyvinyl chloride, polyvinylidene chloride;

[0106] Polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyarylate, etc.

[0107] Nylon and other polyamides;

[0108] Polyimides, polyamide-imides, polyetherimides;

[0109] Polyethersulfones, polysulfones;

[0110] Polyvinyl alcohols, polyvinyl acetals;

[0111] Polyurethane;

[0112] Epoxy resins.

[0113] In addition, the film may also be an unstretched film, a uniaxially stretched film or a biaxially stretched film. It is preferably a polyamide film, a polyamide-imide film or a polyimide film, a polyester film, an olefin film, an acrylic film, or a cellulose film having excellent transparency and heat resistance among the transparent substrates of the polymers exemplified. In addition, inorganic particles such as silicon dioxide, organic microparticles, rubber particles, etc. are also preferably dispersed in the transparent substrate. Furthermore, it may also contain colorants such as pigments and dyes, fluorescent whitening agents, dispersants, plasticizers, heat stabilizers, light stabilizers, infrared absorbers, ultraviolet absorbers, antistatic agents, antioxidants, lubricants, solvents and other compounding agents. The thickness of the transparent substrate is 5 to 200 μm, preferably 20 to 100 μm.

[0114] (Hard Coating)

[0115] A material having a hard coating layer provided on at least one side of the transparent substrate may also be used as a window film. As the hard coating layer, the same hard coating layer as the hard coating layer of the protective film may be used.

[0116] (Phase difference film)

[0117] The phase difference film is a transparent film whose refractive index is different from each other in two orthogonal directions within a plane, and provides a phase difference to light passing therethrough.

[0118] Examples of the material of the phase difference film include a polycarbonate resin film, a polysulfone resin film, a polyethersulfone resin film, a polyarylate resin film, and a norbornene resin film.

[0119] These resin films can be given a desired phase difference by stretching.

[0120] Alternatively, a retardation film that is easily available on the market may be used.

[0121] The thickness of the retardation film may be, for example, 0.5 to 80 μm.

[0122] (Brightness enhancement film)

[0123] The brightness enhancement film is a film that transmits polarized light in a first direction in the plane and reflects polarized light in a second direction in the plane orthogonal to the first direction. When the optical film used in the present invention has a polarizer, the first direction is preferably aligned with the transmission axis of the polarizer.

[0124] The brightness enhancement film may be a multilayer laminate in which a layer having birefringence and a layer having substantially no birefringence are alternately laminated. Examples of materials for the layer having birefringence are naphthalene dicarboxylic acid polyesters (e.g., polyethylene naphthalate), polycarbonate, and acrylic resins (e.g., polymethyl methacrylate), and examples of the layer having substantially no birefringence are copolyesters of naphthalene dicarboxylic acid and terephthalic acid.

[0125] The thickness of the brightness enhancement film may be, for example, 10 to 50 μm.

[0126] Each film constituting the optical film exemplified above may have multiple functions. For example, the protective film may also be a film having optical functions such as a retardation film and a brightness enhancement film.

[0127] (Adhesion in optical film)

[0128] When the optical film 50 has a laminated structure including a plurality of films, the films may be bonded to each other via an adhesive. The adhesive is not particularly limited, and may be any of the above-mentioned water-based adhesives and active energy ray-curable adhesives.

[0129] In addition, a binder may be used as the adhesive. The binder will be described later.

[0130] The thickness of the adhesive can be set to 1 to 200 μm.

[0131] (Thickness of optical film in laminated body)

[0132] When the optical film 50 has a laminated structure including a plurality of films, the total thickness of the optical film 50 can be set to 10 to 1200 μm.

[0133] (Adhesive layer)

[0134] As described above, the laminate used in the present invention has an optical film and a pressure-sensitive adhesive layer provided on one surface thereof. The pressure-sensitive adhesive layer refers to a layer formed using a pressure-sensitive adhesive. Here, the pressure-sensitive adhesive is described.

[0135] The adhesive is a pressure-sensitive adhesive, which is a material that is in a soft solid (viscoelastic) state in a temperature range near room temperature (e.g., 25°C) and has the property of being easily bonded to an adherend by pressure. The adhesive described here is defined by "CADahlquist, Adhesion: Fundamental and Practice", McLaren & Sons, (1966), p.143", and generally speaking, it can be a material having a tensile modulus of elasticity E * (1Hz)<10 7 dyne / cm 2 The adhesive in the technology disclosed herein can also be understood as a solid component (non-volatile component) of an adhesive composition or a constituent component of an adhesive layer.

[0136] Examples of adhesives are compositions in which acrylic resins, styrene resins, silicone resins, etc. are used as base polymers, and crosslinking agents such as isocyanate compounds, epoxy compounds, and aziridine compounds are added thereto. In this specification, the "base polymer" of an adhesive refers to the main component of the rubbery polymer contained in the adhesive. The rubbery polymer refers to a polymer that exhibits rubber elasticity in a temperature range near room temperature. In addition, in this specification, the "main component" refers to a component that contains more than 50% by weight unless otherwise specified.

[0137] The thickness of the adhesive can be set to 1 to 40 μm.

[0138] (Thickness of optical film in laminated body)

[0139] When the optical film 50 has a laminated structure including a plurality of films, the total thickness of the optical film 50 can be set to 10 to 1200 μm.

[0140] The adhesive layer 80 is provided on at least one surface of the optical film (single layer structure or laminated structure) 50 .

[0141] As the adhesive, the above-mentioned adhesives can be used.

[0142] (Isolation film)

[0143] The laminated body 100 may include a separator 90 on the surface of the pressure-sensitive adhesive layer 80 opposite to the surface in contact with the optical film 50 .

[0144] The separator 90 is a film having weaker adhesion to the adhesive layer 80 than the optical film 50. During transportation and storage of the laminate 100 before the optical film 50 is attached to other components such as an optical device (liquid crystal cell) via the adhesive layer 80, the separator 90 protects the surface of the adhesive layer 80. When the adhesive layer 80 is attached to other components, the separator 90 can be easily peeled off from the adhesive layer 80.

[0145] The separator is not necessarily transparent, but is preferably transparent. An example of a material of the separator is polyethylene terephthalate. The thickness of the separator can be set to 1 to 40 μm.

[0146] (Protective film)

[0147] In addition, the laminated body 100 may include a protective film 70 disposed on the outer surface of the optical film 50 on the side opposite to the surface on which the pressure-sensitive adhesive layer 80 is provided.

[0148] Protective film 70 has the function of preventing damage to the optical device and / or optical film 50 during processing of laminate 100, when laminate 100 is attached to an optical device (such as a liquid crystal cell), or when an optical device to which laminate 100 is attached is transported.

[0149] Examples of materials for such a pellicle include polyethylene terephthalate, polyethylene, polypropylene, etc. The pellicle 70 is not necessarily transparent, but is preferably transparent. The thickness of the pellicle can be set to 1 to 40 μm.

[0150] The protective film 70 may be a film that protects the optical film 50 until a product using the optical film 50 is used. In this case, the protective film 70 will not be peeled off from the optical film 50 even after the optical film 50 is attached to an optical device (such as a liquid crystal cell) via the adhesive layer 80 .

[0151] The protective film 70 may be attached to the optical film 50 via an adhesive layer or by utilizing self-adhesion based on electrostatic adsorption.

[0152] A specific example of the stacked structure of the stacked body 100 is shown in Figure 2 (a) and (b) of the present invention.

[0153] Figure 2 In the laminated body 100 of (a), the protective film 70, the protective film 2, the polarizer 3, the protective film 2 and the adhesive layer 80, and the separator 90 are laminated in this order. The protective film 2, the polarizer 3, and the protective film 2 constitute the optical film 50.

[0154] Figure 2In the laminated body 100 of (b), the protective film 70, the protective film 2 and the polarizer 3, the adhesive layer 80 and the separator 90 are sequentially laminated. The protective film 2 and the polarizer 3 constitute the optical film 50. In addition, although not shown in the figure, in any example, the films in each optical film 50 can be bonded by an adhesive or a pressure-sensitive adhesive.

[0155] (Laminate for flexible image display device)

[0156] The optical film 50 used in the present invention may be a laminate for a flexible image display device used in a flexible image display device that is bendable or the like.

[0157] Regarding the flexible image display device, an image display device having a laminate for a flexible image display device and an organic EL display panel is a typical example. In this typical example, usually, a laminate for a flexible image display device is arranged on the observation side relative to the organic EL display panel, and the flexible image display device is configured in a bendable form. As a laminate for a flexible image display device, a window film, a circular polarizing plate, and a touch sensor may also be contained, and their stacking order is arbitrary, but it is preferably composed of a stacking order of a window film, a circular polarizing plate, and a touch sensor or a stacking order of a window film, a touch sensor, and a circular polarizing plate from the observation side. If there is a circular polarizing plate on the observation side of the touch sensor, the pattern of the touch sensor is difficult to be visually recognized, and the visual recognition of the displayed image becomes better, so it is preferred. Each component can be stacked using an adhesive, an adhesive, etc. In addition, it can be provided with a shading pattern formed on at least one side of any layer of the window film, the circular polarizing plate, and the touch sensor.

[0158] (Circular polarizing plate)

[0159] The circular polarizing plate is a functional film having the function of transmitting only the right or left circularly polarized light component by stacking a λ / 4 phase difference plate as a phase difference film on a linear polarizing plate. When the external light entering the display device passes through the circular polarizing plate arranged on the observation side, it is converted into right circularly polarized light and emitted to the organic EL panel side. When the right circularly polarized light is reflected by the metal electrode of the organic EL panel (reflected light), the reflected light becomes left circularly polarized light. Since the left circularly polarized light cannot transmit the circular polarizing plate, as a result, the reflected light is not emitted to the outside of the display device. Through such a function, only the luminous component of the organic EL is observed in the display panel of the display device. By transmitting only the luminous component, the influence of the reflected light can be prevented, and the image can be easily observed.

[0160] In order to realize the circular polarization function, the absorption axis of the linear polarizing plate and the slow axis of the λ / 4 phase difference plate must be 45° in theory, but 45±10° in practice. The linear polarizing plate and the λ / 4 phase difference plate do not necessarily have to be stacked adjacent to each other, as long as the relationship between the absorption axis and the slow axis satisfies the above range. Although it is preferred to achieve complete circular polarization at all wavelengths, it is not necessarily necessary in practice, so the circular polarizing plate of the present invention also includes an elliptical polarizing plate. It is preferred to further stack the λ / 4 phase difference plate on the observation side of the linear polarizing plate so that the emitted light becomes circularly polarized light, thereby improving the observability when wearing polarized sunglasses.

[0161] The so-called linear polarizing plate is a functional layer that allows light vibrating in the transmission axis direction to pass through, but shields the polarized light of the vibration component perpendicular to it. The above-mentioned linear polarizing plate is usually composed of a polarizer and a protective film attached to at least one side thereof. The polarizer can be any of the above-mentioned film-type polarizer or liquid crystal coating type polarizer. The protective film can also use the protective film already described. The thickness of the linear polarizing plate constituting the circular polarizing plate is preferably less than 200 μm, and more preferably 0.5 μm to 100 μm. When the thickness exceeds 200 μm, it can sometimes be applied to reduce the softness (flexibility) of the laminate for flexible image display devices. By appropriately adjusting the thickness of the polarizer and the protective film, the thickness of the appropriate linear polarizing plate can be adjusted.

[0162] The λ / 4 phase difference plate as a phase difference film refers to a phase difference plate called a 1 / 4 wavelength plate, which gives a phase difference of π / 2 (=λ / 4) to the polarization plane of the incident light. A phase difference film with such performance is selected from the phase difference film, and a λ / 4 phase difference plate can also be prepared. As another example, a liquid crystal coating phase difference plate formed by coating a liquid crystal composition can also be used as a λ / 4 phase difference plate. As described later, the liquid crystal coating phase difference plate formed by coating the liquid crystal composition can obtain a λ / 4 phase difference plate with an extremely thin thickness. Therefore, the liquid crystal coating phase difference plate is particularly preferred as a λ / 4 phase difference plate of a circularly polarizing plate constituting a laminate for a flexible image display device.

[0163] Here, the liquid crystal composition for forming the λ / 4 phase difference plate will be described.

[0164] The liquid crystal composition includes a liquid crystal compound having the property of showing a liquid crystal state such as a nematic, cholesteric, or smectic state. The liquid crystal compound has a polymerizable functional group. The liquid crystal composition may also include a plurality of liquid crystal compounds, and when it includes a plurality of liquid crystal compounds, at least one of the liquid crystal compounds has a polymerizable functional group. The liquid crystal composition may further include an initiator, a solvent, a dispersant, a leveling agent, a stabilizer, a surfactant, a crosslinking agent, a silane coupling agent, and the like. The liquid crystal coating phase difference plate is similar to that described in the method for manufacturing the liquid crystal polarizer, and is manufactured by coating and curing the liquid crystal composition on the orientation film of the substrate on which the orientation film is preformed, thereby forming a liquid crystal phase difference layer on the orientation film. The liquid crystal coating phase difference plate can be formed with a thinner thickness than the stretched phase difference plate. The thickness of the liquid crystal polarizing layer is 0.5 to 10 μm, preferably 1 to 5 μm. The liquid crystal coating phase difference plate can also be peeled off from the substrate and transferred and stacked, or the substrate can be directly stacked. The substrate also preferably plays the role of a transparent substrate as a protective film or a phase difference plate.

[0165] Most of the common materials constituting the phase difference film have a shorter wavelength and a larger birefringence, and the longer the wavelength, the smaller the birefringence. In this case, the phase difference of λ / 4 cannot be achieved in the entire visible light region, so most of the in-plane phase difference designed to be λ / 4 near 560nm with high visual visibility is 100-180nm, preferably 130-150nm. The use of a reverse dispersion λ / 4 phase difference plate using a material having a birefringence wavelength dispersion characteristic opposite to the usual can improve visual recognition, so it is preferred. As such a material, in the case of a stretched phase difference plate, it is preferred to use a material recorded in Japanese Patent Publication No. 2007-232873, and in the case of a liquid crystal coating phase difference plate, it is preferred to use a material recorded in Japanese Patent Publication No. 2010-30979.

[0166] In addition, as another method for forming a preferred phase difference film constituting a circular polarizing plate, it is also known to obtain a broadband λ / 4 phase difference plate by combining with a λ / 2 phase difference plate (Japanese Patent Publication No. 10-90521). The λ / 2 phase difference plate is also manufactured using the same material method as the λ / 4 phase difference plate. The combination of a stretched phase difference plate and a liquid crystal coated phase difference plate is arbitrary, but the use of a liquid crystal coated phase difference plate can make the thickness of the film thinner, so it is preferred.

[0167] In order to improve the visual recognition of the circular polarizing plate in the tilted direction, a method of stacking positive C plates is also known (Japanese Patent Publication No. 2014-224837). The positive C plate can also be a liquid crystal coating phase difference plate or a stretched phase difference plate. The phase difference in the thickness direction of the positive C plate is -200 to -20nm, preferably -140 to -40nm.

[0168] (Touch sensor)

[0169] The touch sensor is used as an input mechanism. As a touch sensor, various methods such as a resistive film method, a surface acoustic wave method, an infrared method, an electromagnetic induction method, and an electrostatic capacitance method have been proposed, and any method may be used. Among these, the electrostatic capacitance method is preferred.

[0170] The electrostatic capacitance touch sensor is divided into an active area and an inactive area located outside the active area when viewed from the display panel surface. The active area is the area corresponding to the area (display part) where the screen is displayed in the display panel and is the area where the user's touch can be sensed, while the inactive area is the area (non-display part) where the screen is not displayed in the display device.

[0171] The touch sensor may include: a substrate having flexible characteristics; a sensing pattern formed in an active area of ​​the substrate; and sensing lines formed in an inactive area of ​​the substrate and used to connect the sensing pattern to an external driving circuit via a pad. As a substrate having flexible characteristics, a substrate formed of the same material as the transparent substrate of the window film may be used. From the perspective of suppressing cracks in the touch sensor, the toughness of the substrate of the touch sensor is preferably 2000MPa% or more. More preferably, the toughness may also be 2000MPa% to 30000MPa%.

[0172] The sensing pattern may include a first pattern formed in a first direction and a second pattern formed in a second direction. The first pattern and the second pattern are arranged in different directions. The first pattern and the second pattern are formed in the same layer, and in order to sense the touch location, each pattern must be electrically connected. The first pattern is a form in which each unit pattern is connected to each other by means of a joint, and the second pattern becomes a structure in which each unit pattern is separated from each other in an island form, so an additional bridging electrode is required to electrically connect the second pattern. The sensing pattern is formed by a known transparent electrode raw material. As the transparent electrode raw material, for example, indium tin oxide (ITO), indium zinc oxide (IZO), zinc oxide (ZnO), indium zinc tin oxide (IZTO), cadmium tin oxide (CTO), PEDOT (poly (3,4-ethylenedioxythiophene)), carbon nanotubes (CNT), graphene, metal wire (the metal used for the metal wire is not particularly limited, and for example, silver, gold, aluminum, copper, iron, nickel, titanium, tellurium, chromium, etc. can be cited. They can be used alone or mixed with two or more), etc., and they can be used alone or mixed with two or more. ITO is preferred. A bridging electrode may be formed on the upper part of the sensing pattern through an insulating layer, and a bridging electrode may be formed on the substrate, and an insulating layer and a sensing pattern may be formed thereon. The bridging electrode may be formed of the same raw material as the sensing pattern, or may be formed of metals such as molybdenum, silver, aluminum, copper, palladium, gold, platinum, zinc, tin, titanium, or alloys of two or more thereof. The first pattern and the second pattern must be electrically insulated, so an insulating layer is formed between the sensing pattern and the bridging electrode. The insulating layer may be formed only between the junction of the first pattern and the bridging electrode, or may be formed as a structure covering a layer of the sensing pattern. In the latter case, the bridging electrode may be connected to the second pattern by means of a contact hole formed in the insulating layer. The touch sensor may further include an optical adjustment layer between the substrate and the electrode, as a method for appropriately compensating for the difference in transmittance between the pattern area where the pattern is formed and the non-pattern area where the pattern is not formed, specifically, the difference in light transmittance caused by the difference in refractive index in these areas. The optical adjustment layer may contain an inorganic insulating substance or an organic insulating substance. The optical adjustment layer can be formed by coating a photocurable composition containing a photocurable organic binder and a solvent on a substrate. The photocurable composition can further contain inorganic particles. The inorganic particles can be used to increase the refractive index of the optical adjustment layer.

[0173] The photocurable organic binder may include, for example, a copolymer of monomers such as acrylate monomers, styrene monomers, carboxylic acid monomers, etc. The photocurable organic binder may include, for example, a copolymer of different repeating units such as epoxy-containing repeating units, acrylate repeating units, and carboxylic acid repeating units.

[0174] The inorganic particles may include, for example, zirconium oxide particles, titanium oxide particles, aluminum oxide particles, and the like.

[0175] The photocurable composition may further include additives such as a photopolymerization initiator, a polymerizable monomer, and a curing auxiliary agent.

[0176] Each layer (window film, circular polarizing plate, touch sensor) constituting the laminate for the flexible image display device can be formed by an adhesive. As the adhesive, the above-described aqueous adhesive, active energy ray-curable adhesive, or pressure-sensitive adhesive is generally used.

[0177] (Shading pattern)

[0178] The shading pattern can be applied as at least a part of the frame or housing of the flexible image display device. By hiding the wiring arranged at the edge of the flexible image display device with a shading pattern to make it difficult to visually recognize, the visual recognizability of the image can be improved. The shading pattern can be in the form of a single layer or multiple layers. The color of the shading pattern is not particularly limited, and can be various colors such as black, white, and metallic colors. The shading pattern can be formed by a pigment for showing the color, and a polymer such as an acrylic resin, an ester resin, an epoxy resin, a polyurethane, and a silicone resin. They can also be used alone or in a mixture of two or more. The shading pattern can be formed by various methods such as printing, lithography, and inkjet. The thickness of the shading pattern can be 1μm to 100μm, preferably 2μm to 50μm. In addition, the thickness direction of the shading pattern can be given an inclined shape.

[0179] The optical film and the pressure-sensitive adhesive contained in the laminate used in the production method of the present invention have been described above. Next, the production method of the present invention will be described.

[0180] (Powder)

[0181] Refer again Figure 1 (a) and (b) are used to illustrate the production method of the present invention.

[0182] The powder f attached to the end surface E of the optical film 50 is attached to the end surface due to the processing of the end surface of the laminate 100. Generally, in order to obtain the laminate 100 of a desired size from the raw material of the laminate 100, the end surface of the laminate 100 is processed. Examples of processing are cutting, milling, and grinding. Here, cutting refers to a concept including opening holes. Therefore, as described above, the end surface of the laminate 100 includes not only Figure 1 The outer end surface E of the stacked body 100 shown in (a) also includes the inner end surface E of the inner wall forming the hole (opening) H of the stacked body 100.

[0183] Cutting is a process of creating a cut from the front surface to the back surface of the laminate by inserting a blade, removing with a laser, or the like, thereby defining the general shape of the laminate.

[0184] Cutting is a process of cutting a portion of the end portion by bringing a relatively moving cutting blade (blade) into contact with the end portion of the stacked body to form a new end face. As mentioned above, the cutting includes drilling. Drilling refers to, for example, Figure 1 As shown in (b), a hole H is formed at a desired position in the laminate 100 using a drill or the like. In such a hole forming process, powder f (hole forming chips) may adhere to the inner end surface E of the inner wall forming the hole H.

[0185] Grinding is a process of bringing relatively moving abrasive grains (which may be fixed abrasive grains or loose abrasive grains) into contact with the end surface of the stacked body to cut a portion of the end surface. Grinding also includes a process called grinding.

[0186] For example, after the raw material of the stack 100 is cut into a planar shape slightly larger than the desired size by a blade or laser, the planar shape of the stack can be set to a predetermined size by grinding and / or polishing the end face of the cut stack, and the straightness and flatness of the end face can be improved.

[0187] The planar shape (shape viewed from the thickness direction) of the laminate is not particularly limited and may be, for example, square, rectangular, circular or the like.

[0188] Due to these processing on the end surface of the stacked body, powder of the material constituting the stacked body 100 is generated, and part of it adheres to the end surface E of the stacked body 100. Therefore, performing these processing on the stacked body is one embodiment of the preparatory step in the manufacturing method of the present invention. The end surface E may be a surface connecting the two main surfaces of the stacked body 100.

[0189] The average particle size of the powder can be, for example, 10 to 3000 μm. This particle size is D50 of a weight-based particle size distribution based on a laser diffraction method.

[0190] (Impacting process (powder removal process by impact of dry ice particles))

[0191] Next, dry ice particles are made to impact the end surface E of the stacked body 100 to remove the powder f on the end surface from the end surface.

[0192] Specifically, it is appropriate to transport the dry ice particles in a gas and cause them to impact the end surface E of the stacked body 100 .

[0193] The average particle size of the dry ice particles to be impacted is not particularly limited, but is preferably 100 μm or more from the viewpoint of efficiently removing the powder, and is preferably 1000 μm or less from the viewpoint of suppressing the adhesive layer from being damaged by the impact of dry ice.

[0194] The average particle size of dry ice particles can be measured by laser Doppler velocimetry.

[0195] The speed of the dry ice particles to be impacted can be set to 5 m / sec to 100 m / sec.

[0196] The transport gas of dry ice is not particularly limited, and may be, for example, nitrogen, air, or carbon dioxide.

[0197] Specifically, you can use Figure 3 Such a dry ice particle supply unit (device) 300.

[0198] The device includes a liquid carbon dioxide source 310 , a nozzle 320 , a transport gas source 330 , a pipeline L1 connecting the liquid carbon dioxide source 310 and the nozzle 320 , and a pipeline L2 connecting the transport gas source 330 and the nozzle 320 .

[0199] A valve 340 and an orifice 350 are provided in the pipeline L1 , and a valve 360 ​​is provided in the pipeline L2 .

[0200] The valve 340 is opened to adiabatically expand the liquid of the liquid carbon dioxide source 310 at the orifice 350 to generate dry ice particles (dry ice snow), and transport them to the nozzle 320. The valve 360 ​​is opened to supply gas from the transport gas source 330 to the nozzle 320, and the dry ice particles d are ejected from the nozzle 320 by the gas and supplied to the end surface E of the stacked body 100.

[0201] The particle size of the dry ice particles d can be adjusted by the distance from the orifice 350 after adiabatic expansion until being ejected by the nozzle 320 (adiabatic expansion distance), or the distance between the nozzle 320 and the supply target of the dry ice particles (spraying distance). In addition, appropriate preliminary experiments using the dry ice particle supply unit (device) can be performed to confirm the degree of removal of the powder f to adjust the adiabatic expansion distance and the spraying distance.

[0202] The distance (spray distance) between the nozzle 320 and the end surface E of the stacked body 100 is preferably less than 20 mm. In addition, the adiabatic expansion distance can be set to, for example, 10 to 500 mm.

[0203] It is appropriate to move the stacked body 100 and the nozzle 320 relative to each other by the conveying unit 400 so that the portion impacted by the dry ice particles d is scanned on the end surface E. Figure 3 In this process, the transport unit 400 may be used to scan the stacked body 100 in a plane perpendicular to the ejection direction (lateral direction) of the dry ice particles d so that the impact portion of the end surface E with the dry ice particles d is moved.

[0204] The scanning speed of the impact portion of the dry ice particles d on the end surface E can be set to 1 to 100 m / sec.

[0205] (effect)

[0206] According to this embodiment, the dry ice particles d are blown to the end surface E of the stacked body 100, so that powders such as cutting chips, chipping chips, hole processing chips, and grinding chips are appropriately removed from the end surface. This is preferred because it reduces contamination caused by powders in subsequent processes. In addition, compared with methods such as sticking and peeling off tape, the time consumed for removing powders is also short.

[0207] Furthermore, the particle size of the dry ice particles to be impacted is preferably 100 to 1000 μm, since the removal rate of the powder can be increased and the defect of the adhesive layer on the end surface can be suppressed. It is more preferably 200 to 700 μm.

[0208] (Powder removal from a laminated structure having a plurality of laminated bodies)

[0209] In the above, dry ice particles are impacted on one stacked body 100, but Figure 4 As shown, it is also suitable to impinge dry ice on the end surface E of the stacked structure 120 in which a plurality of stacked bodies 100 are stacked in the thickness direction. This allows a large number of stacked bodies 100 to be processed.

[0210] (End surface processing and powder removal sequence)

[0211] After processing (cutting, cutting, and grinding) of a portion of the end surface of the stacked body 100 is completed, dry ice particles can be blown to the portion of the end surface where processing is completed to remove powder while processing other portions of the end surface of the stacked body 100. This can shorten the process time.

[0212] On the contrary, after all the processing such as cutting, milling and grinding of the end face of the stacked body is completed, dry ice particles are impacted on the end face of the stacked body 100 to clean the powder on the end face. When the dry ice particles are impacted on the end face, other parts of the end face of the stacked body may not be processed. In this case, the atmosphere (space) where the powder is removed by the impact of dry ice particles and the atmosphere (space) where the end face is processed can be distinguished, so the end face can be prevented from being contaminated by the powder generated by the processing.

[0213] (Atmosphere during the impact process (powder removal process))

[0214] When the powder removal process of the end surface of the stacked body and the stacked structure is performed by ice particles, the surrounding atmosphere of the stacked body and the stacked structure can be an air atmosphere, but can be set to an atmosphere such as nitrogen and carbon dioxide as needed. In addition, the temperature of the atmosphere is usually 20 to 30°C, preferably 20 to 27°C. The relative humidity of the atmosphere is usually less than 80%, preferably 30 to 75%, and more preferably 40 to 70%. When the relative humidity of the atmosphere is 80% or more, condensation will occur due to the cooling of the stacked body and the stacked structure, causing the water-absorbent film (such as a polarizer) in the stack to absorb water and swell, etc., which sometimes causes adverse conditions to the appearance and optical properties of the stacked body and the stacked structure.

[0215] (Optical member manufacturing device)

[0216] Next, refer to Figure 5 Next, an optical member manufacturing apparatus 1000 suitable for carrying out the above-mentioned method will be described.

[0217] The manufacturing device 1000 includes: an end surface processing unit 200 for cutting, cutting or grinding the end surface of the stacked body 100 or the stacked structure 120; a dry ice particle supply unit 300 for impacting dry ice particles on the portion of the stacked body 100 processed into the end surface processing unit 200; and a conveying unit 400 for conveying the stacked body 100.

[0218] exist Figure 5 In the figure, a cutting device is drawn as an end surface processing unit 200. The cutting device includes a rotating shaft 210 extending in the horizontal direction, a disk 220 mounted on the rotating shaft, and a cutting blade 230 mounted on the disk 220. By rotating the cutting blade 230, the end surface of the laminated body or the like can be cut.

[0219] In the dry ice particle supply unit 300 , only the nozzle 320 is described for the sake of convenience.

[0220] The transport unit 400 comprises: a pair of upper clamps 420 and a lower clamp 422 for clamping and supporting the stacked body 100 or the stacked structure 120 in the thickness direction; a cylinder 430 for pressing the upper clamp 420 in the above-mentioned thickness direction (downward direction); a rotating mechanism 410 connected to the lower clamp 422 so as to rotate the upper clamp 420 and the lower clamp 422 around a vertical axis (Z axis); and a moving mechanism 440 for moving the upper clamp 420 and the lower clamp 422 in the horizontal direction (X direction).

[0221] Next, the manufacturing method of the optical component using the device is described. First, the stack 100 or the stacked structure 120 is clamped between the upper clamp 420 and the lower clamp 422. Secondly, the upper clamp 420 is pressed toward the lower clamp 422 by the cylinder 430, thereby fixing the stack 100 or the stacked structure 120. In the present embodiment, the stack 100 or the stacked structure 120 is rectangular when viewed from above and has four end faces. Therefore, the rotation position of the stack 100 or the stacked structure 120 is adjusted by the rotating mechanism 410 so that the two end faces E are parallel to the X-axis.

[0222] Next, the end surface processing unit 200 is started. Specifically, the disk 220 is rotated. Next, the stacked body 100 and the stacked structure 120 are moved in the X direction by the moving mechanism 440 so that the cutting blade 230 of the end surface processing unit 200 contacts the end surface E. Thus, a pair of end surfaces E of the stacked body 100 and the stacked structure 120 facing each other are cut by the cutting blade 230. At this time, cutting chips are attached to the end surface E.

[0223] Next, the stacked body 100 and the stacked structure 120 are moved in the -X direction by the conveyor 400, and dry ice particles are supplied from the nozzle 320 of the dry ice particle supply unit 300. Thus, the dry ice particles impact the cut end surfaces E of the stacked body 100 and the stacked structure 120, and powder on the end surfaces E is removed.

[0224] Next, the stacked body 100 and the stacked structure 120 are further moved in one direction by the conveying unit 400, and the stacked body 100 and the stacked structure 120 are rotated by the rotating mechanism 410 so that the remaining two end faces are parallel to the X direction. Then, the remaining two end faces are processed in sequence and the powder removal using dry ice particles is subsequently performed in the same manner as before.

[0225] The end surface processing portion 200 can be configured in various forms according to the processing method. Figure 6 As shown, cutting can be performed using a CANNA type rotary blade having a cylindrical body 240 rotating around a vertical axis and a long blade 250 provided on the outer peripheral surface of the cylindrical body 240 so as to extend in the axial direction.

[0226] Furthermore, a grinding plate having a large amount of abrasive grains provided on the surface of a disc may be used instead of the cutting blade 230 to perform grinding.

[0227] Furthermore, when cutting and grinding are not required, it can also be set as a cutting device.

[0228] Finally, regarding an example of a method for removing the powder f (drilling processing debris) adhering to the end surface E of the hole H provided in the stacked body 100, refer to Figure 7 Provide explanation.

[0229] First, a plurality of stacked bodies 100 are prepared by subjecting the stacked bodies 100 to hole drilling, and powder (hole drilling chips) f is attached to the end surface E inside the hole H. Figure 1 As shown in (b), each stacked body 100 has a hole H set at a predetermined position by drilling. Next, these stacked bodies 100 are stacked in a manner such that the positions of the holes H of each stacked body 100 are aligned on one axis (axis extending in the thickness direction) to obtain a stacked structure 120. Thus, the holes H of each stacked stacked body 100 are connected to each other, and a through hole H' that penetrates the stacked structure 120 in the thickness direction is formed in the stacked structure 120.

[0230] In a pair of upper jigs 420 and lower jigs 422 for pressing the stacked structure 120 in the thickness direction, a dry ice particle supply port 420a is pre-set on one jig, and a dry ice particle recovery port 422b is pre-set on the other jig. The upper jig 420 and the lower jig 422 are arranged so that the through hole H' is connected to the dry ice particle supply port 420a and the dry ice particle recovery port 422b, and the stacked structure 120 is pressed in the thickness direction. Thus, the preparation process before the dry ice impact process is completed.

[0231] Next, dry ice particles are supplied from the nozzle 320 into the through hole H' via the dry ice particle supply port 420a (impact process). The dry ice particles ejected from the nozzle 320 spread in the width direction as they move forward, impact the end surface E of the through hole H' of the stacked structure 120, and are discharged from the dry ice particle recovery port 422b together with the powder f. If such a device is used, the powder f can be effectively removed from the stacked body 100 on which the powder f is attached to the end surface E of the inner wall of the hole H by the hole drilling process.

[0232] Example

[0233] (Laminate material)

[0234] A raw material stack having the following layer structure was obtained: protective film (made of PET (polyethylene terephthalate): 53 μm) / protective film (made of TAC (triacetyl cellulose): 32 μm) / polarizer (PVA (iodine-adsorbed polyvinyl alcohol): 12 μm) / protective film (made of COP (cyclic olefin resin): 23 μm) / adhesive layer (acrylic adhesive: 20 μm) / isolating film (PET: 38 μm).

[0235] The protective film and the polarizing plate were bonded together with a water-based adhesive. The thickness of the laminate was 178 μm.

[0236] (Processing of the end surface of the laminate)

[0237] The original laminate was punched out into a rectangular shape having a size of 140×65 mm using a Thomson blade to obtain a laminate.

[0238] Next, 50 sheets of the stacked bodies were stacked to obtain a stacked structure, and each end surface of the stacked structure was cut by a cutting device, and then each end surface of the stacked structure was polished by a polishing device.

[0239] (Removal of powder from the end surface of the laminate)

[0240] In each of the Examples and Comparative Examples, removal of powder from the end surface of the stacked body was performed under the following conditions.

[0241] (Example 1)

[0242] Dry ice particle supply device: CO2 dry ice blasting

[0243] CO2 pressure: 5Mpa (It should be noted that CO2 pressure refers to the supply pressure to the orifice)

[0244] Air pressure: 0.5Mpa

[0245] Distance between the nozzle tip and the end face: about 50mm

[0246] Nozzle scanning speed: 50mm / 5 seconds

[0247] Center position of nozzle and nozzle scanning direction: The nozzle is directed toward the center of the end surface of the stacked structure in the thickness direction, and the nozzle is scanned in a direction perpendicular to the thickness of the end surface of the stacked structure.

[0248] Average particle size of dry ice particles: 1 to 100 μm

[0249] Atmospheric temperature: 24℃~26℃, relative humidity: 45%~65%

[0250] (Example 2)

[0251] Dry ice particle supply device: CO2 dry ice blasting

[0252] CO2 pressure: 7Mpa

[0253] Air pressure: 0.5Mpa

[0254] Distance between the nozzle tip and the end face: about 50mm

[0255] Nozzle scanning speed: 50mm / 5 seconds

[0256] Center position of nozzle and nozzle scanning direction: The nozzle is directed toward the center of the end surface of the stacked structure in the thickness direction, and the nozzle is scanned in a direction perpendicular to the thickness of the end surface of the stacked structure.

[0257] Average particle size of dry ice particles: 200 to 700 μm or less

[0258] Atmospheric temperature: 24℃~26℃, relative humidity: 45%~65%

[0259] (Example 3)

[0260] Dry ice particle supply device: Particle dry ice blasting

[0261] Particle diameter: φ3mm

[0262] Air pressure: 0.5Mpa

[0263] Distance between the nozzle tip and the end face: about 50mm

[0264] Nozzle scanning speed: 50mm / 5 seconds

[0265] Center position of nozzle and nozzle scanning direction: The nozzle is directed toward the center of the end surface of the stacked structure in the thickness direction, and the nozzle is scanned in a direction perpendicular to the thickness of the end surface of the stacked structure.

[0266] Average particle size of dry ice particles: 1000μm or more

[0267] Atmospheric temperature: 24℃~26℃, relative humidity: 45%~65%

[0268] (Example 4)

[0269] The powder on the end surface of the laminate was removed under the same conditions as in Example 2 except that the atmosphere temperature was 26° C. and the relative humidity of the atmosphere was 80 to 90%.

[0270] It should be noted that the stacked body was cooled due to contact with dry ice particles during removal, and condensation occurred on the stacked body. When the condensation occurred, it was found that no grinding debris or defects were generated, but swelling occurred at the end of the stacked body.

[0271] (Comparative Example 1)

[0272] The end surface of the stacked structure was wiped with a clean room wiper (manufactured by KURARAY KURAFLEX) impregnated with ethanol.

[0273] (Comparative Example 2)

[0274] The OLFA cutting blade was moved along the end surface of the stacked structure.

[0275] (Comparative Example 3)

[0276] After an adhesive tape (Cellotape (registered trademark) manufactured by Nichiban Corporation) was attached to the end surface of the laminated structure, the adhesive tape was peeled off from the end surface.

[0277] (Comparative Example 4)

[0278] The air flow was blown to the end surface of the stacked structure in the same manner as in Example 1 except that liquid carbon dioxide was not supplied.

[0279] (evaluate)

[0280] The end surface was observed with a microscope to check the residual state of powder on the end surface and the presence or absence of defects in the adhesive layer on the end surface.

[0281] The results are shown in Table 1.

[0282] [Table 1]

[0283]

[0284] It should be noted that "○" in "powder residue on the end surface" means that no powder was observed in the field of view of 30 mm length (hereinafter referred to as length) in the direction perpendicular to the thickness, "△" means that 1 to 2 powders were observed in the field of view of 30 mm length, and "×" means that 3 or more powders were observed in the field of view of 30 mm length.

[0285] In addition, ○ for "adhesive layer defects on the end face" means that no defects were observed within a field of view of 30 mm in length (hereinafter referred to as length) in a direction perpendicular to the thickness, △ means that 1 to 2 defects were observed within a field of view of 30 mm in length, and × means that defects were observed at 3 or more positions within a field of view of 30 mm in length.

[0286] Description of Reference Numerals

[0287] 50...optical film, 80...adhesive layer, 100...laminated body, 120...laminated structure, 200...end surface processing unit, 300...dry ice particle supply unit, 400...transport unit, 1000...optical component manufacturing device, f...powder, E...end surface.

Claims

1. A method for manufacturing an optical component, comprising: A step of preparing a laminate having an optical film and a pressure-sensitive adhesive layer provided on one surface of the optical film and having a powder attached to an end surface thereof; as well as a step of causing dry ice particles to impact the end surface of the stacked body to remove the powder from the end surface, The laminate has holes penetrating the optical film and the adhesive layer in the thickness direction. The end surface is the inner wall of the hole, In the preparation step, the hole is formed in a laminate having the optical film and the pressure-sensitive adhesive layer using a drill, thereby preparing the laminate having the powder attached to the end surface. In the impact step, the dry ice particles are caused to impact an end surface of a stacked structure formed by stacking a plurality of stacked bodies. In the laminated structure, a plurality of the laminated bodies are laminated so that the positions of the holes of the plurality of the laminated bodies are aligned on one axis extending in the thickness direction of the optical film and the adhesive layer, In the impact step, the dry ice particles are supplied from one end of the hole, and the dry ice particles are discharged together with the powder from the other end of the hole.

2. The method according to claim 1, wherein: The average particle size of the dry ice particles is 100 μm to 1000 μm.

3. The method according to claim 1 or 2, wherein: The dry ice particles are caused to impact a portion of the end surface, while at least one selected from the group consisting of cutting, milling, and grinding is performed on other portions of the end surface of the stacked body.

4. The method according to claim 1 or 2, wherein: In the preparation step, the end surface is subjected to at least one treatment selected from the group consisting of cutting, milling, and grinding, and when the dry ice particles are caused to impact a portion of the end surface, the end surface is not subjected to any treatment selected from the group.

5. The method according to claim 1 or 2, wherein: The optical film is at least one selected from the group consisting of a polarizer, a protective film, a phase difference film, a brightness enhancement film, a window film and a touch sensor; contains two or more laminated films of at least one selected from the group, or contains at least two laminated films selected from the group.

6. The method according to claim 1 or 2, wherein: The relative humidity of the atmosphere in the step of causing the dry ice particles to impact the end surface is 30% to 75%.

7. An optical component manufacturing device comprising: an end surface processing section for cutting, grinding or polishing an end surface of a laminate having an optical film and a pressure-sensitive adhesive layer provided on one surface of the optical film; and a dry ice particle supplying unit causing dry ice particles to impact the portion of the stacked body processed to form the end surface processed portion; The laminate has holes penetrating the optical film and the adhesive layer in the thickness direction. The end surface is the inner wall of the hole, The holes are set by means of a drill, The dry ice particle supply unit causes the dry ice particles to impact an end surface of a stacked structure formed by stacking a plurality of the stacked bodies. In the laminated structure, a plurality of the laminated bodies are laminated so that the positions of the holes of the plurality of the laminated bodies are aligned on one axis extending in the thickness direction of the optical film and the adhesive layer, The dry ice particle supply unit supplies the dry ice particles from one end of the hole and impacts the dry ice particles so that the dry ice particles are discharged together with the powder from the other end of the hole. 8 . The optical member manufacturing apparatus according to claim 7 , further comprising a transport unit that moves the stacked body between the end surface processing unit and the dry ice particle supply unit.