A method for synthesizing gold nanoparticles based on DNA regulation
By reacting chloroauric acid with sodium citrate solution with DNA, and adding reducing agents and growth reagents, the problem of unfavorable adsorption of DNA and gold nanoseeds is solved, the morphology control of gold nanoparticles is achieved, and the DNA adsorption intensity is enhanced. , simplifies the synthesis process.
Patent Information
- Application Number
- CN202210334046.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-30
AI Technical Summary
In traditional methods, DNA and gold nanoseed adsorption is not favorable, making it difficult to control the growth morphology of gold nanomaterials, and additional reagents and changes in the properties of the solution are often required.
By mixing the chloroauric acid solution with sodium citrate solution, then reacting with the DNA solution, and adding reducing agents and growth reagents, the adsorption amount and intensity of DNA on the gold surface are controlled, and the growth morphology of gold nanoparticles is regulated.
It realizes the simple and convenient synthesis of gold nanoparticles with different morphology without additional reagents and changing the properties of the solution, which enhances the adsorption intensity of DNA on the surface of gold nanoparticles and controls the growth direction and morphology of gold nanoparticles.
Smart Images

Figure CN115232859B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of nanomaterial synthesis, and in particular, to a method for synthesizing gold nanoparticles based on DNA regulation. Background Art
[0002] The use of DNA to regulate the growth of precious metal nanoparticles has been widely studied. DNA with different sequences and lengths can regulate the growth of single metal or bimetallic nanoparticles into different morphologies. The changes in the plasma properties of these nanoparticles during growth combined with the molecular recognition properties of DNA can be used in the field of biosensors. In addition, this DNA-bound nanomaterial has been used in research such as drug and DNA delivery. In general, most studies only discuss the effect of DNA sequence on nanoparticle growth.
[0003] In the traditional method, DNA is mixed with gold seeds, and then chloroauric acid and a reducing agent are added to initiate subsequent growth. The DNA will adsorb on the seeds and exert its effect. However, since both DNA and gold nanoseeds are negatively charged, this simple mixing is not conducive to the adsorption of DNA.
[0004] Based on the above problems, there is an urgent need to provide a convenient and rapid method that can regulate the adsorption effect of DNA and gold nanomaterials, thereby controlling the growth morphology of gold nanomaterials. Summary of the invention
[0005] The purpose of the present disclosure is to provide a method for synthesizing gold nanoparticles based on DNA regulation, which method does not require the addition of additional reagents or the change of the properties of the solution, and can simply and conveniently synthesize gold nanoparticles of different morphologies.
[0006] In order to achieve the above object, the present disclosure provides a method for synthesizing gold nanoparticles based on DNA regulation in a first aspect, the method comprising the following steps:
[0007] S1, mixing the chloroauric acid solution and the sodium citrate solution to perform a first reaction to obtain a first mixed solution;
[0008] S2, performing a second reaction on the first mixed solution and the DNA solution to obtain a second mixed solution;
[0009] S3, adding a reducing agent and a growth reagent to the second mixed solution to carry out a third reaction to obtain a solution containing the gold nanoparticles.
[0010] According to the present disclosure, in step S1, the molar ratio of the chloroauric acid solution to the sodium citrate solution is 1:(1-20), preferably 1:(1-10);
[0011] The concentration of the chloroauric acid solution is 0.1-10 mmol / L, preferably 0.5-5 mmol / L;
[0012] The concentration of the sodium citrate solution is 1-100 mmol / L, preferably 2-50 mmol / L.
[0013] According to the present disclosure, in step S2, the molar ratio of the first mixed solution to the DNA solution is 1:(20-2000), preferably 1:(100-500); the concentration of the DNA solution is 10-1000nmol / L, preferably 100-500nmol / L.
[0014] According to the present disclosure, the DNA sequence in the DNA solution includes 5 to 60 bases, preferably 10 to 40 bases; each base is independently selected from any one of A, G, C, and T.
[0015] According to the present disclosure, the mass ratio of the second mixed liquid, the reducing agent and the growth reagent is 100:(1-20):(1-20), preferably 100:(1-10):(1-10).
[0016] According to the present disclosure, the reducing agent includes at least one of hydroxylamine hydrochloride, ascorbic acid and sodium citrate; and the growth reagent includes at least one of chloroauric acid, silver nitrate, chloroplatinic acid and chloropalladic acid.
[0017] According to the present disclosure, among the reducing agents, the concentration of the ascorbic acid solution is 50-100 mmol / L, the concentration of the hydroxylamine hydrochloride solution is 0.1-1 mol / L, and the concentration of the sodium citrate solution is 10-100 mmol / L.
[0018] According to the present disclosure, in the growth reagent, the concentration of the chloroauric acid solution is 10-100mmol / L, the concentration of the silver nitrate is 10-100mmol / L, the concentration of the chloroplatinic acid is 10-100mmol / L, and the concentration of the chloropalladic acid solution is 10-100mmol / L.
[0019] According to the present disclosure, the gold nanoparticles include at least one of gold nanorods, gold nanoflowers and gold nanosheets.
[0020] According to the present disclosure, the reaction conditions of the first reaction include: reaction temperature of 80-140°C, preferably 80-100°C; reaction time of 1-30min, preferably 5-20min;
[0021] The reaction conditions of the second reaction include: reaction temperature of 4-100°C, preferably 60-100°C; reaction time of 2-720min, preferably 3-60min;
[0022] The reaction conditions of the third reaction include: reaction temperature of 4-37° C., preferably 25-27° C., and reaction time of 1-60 min, preferably 10-20 min.
[0023] According to the present disclosure, the gold nanoparticles include at least one of single metal gold, gold-silver alloy, gold-palladium alloy and gold-platinum alloy.
[0024] Through the above technical scheme, the present disclosure provides a method for synthesizing gold nanoparticles based on DNA regulation, which can control the growth of gold nanoparticles into different morphologies by changing the amount and adsorption strength of DNA on the gold surface.
[0025] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0027] Figure 1 TEM image of the gold nanoparticles prepared in Example 1.
[0028] Figure 2 This is the TEM image of the gold nanoparticles prepared in Comparative Example 1.
[0029] Figure 3 It is the UV image of the gold nanoparticle solution prepared in Example 1 and Comparative Example 1.
[0030] Figure 4 The DNA adsorption strength on the surface of the gold nanoparticles prepared in Example 2 and Comparative Example 2 was measured.
[0031] Figure 5 It is the adsorption state of DNA on the surface of gold nanoparticles under different conditions.
[0032] Figure 6 The amount of DNA adsorbed on the surface of the gold nanoparticles prepared in Example 2 and Comparative Example 2 was determined.
[0033] Figure 7 This is a TEM image of the gold nanoparticles prepared in Example 3.
[0034] Figure 8 This is the TEM image of the gold nanoparticles prepared in Comparative Example 3.
[0035] Fig. 9 It is the UV image of the gold nanoparticle solution prepared in Example 3 and Comparative Example 3. DETAILED DESCRIPTION
[0036] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0037] The present invention provides a method for synthesizing gold nanoparticles based on DNA regulation, the method comprising the following steps:
[0038] S1, mixing the chloroauric acid solution and the sodium citrate solution to perform a first reaction to obtain a first mixed solution;
[0039] S2, performing a second reaction on the first mixed solution and the DNA solution to obtain a second mixed solution;
[0040] S3, adding a reducing agent and a growth reagent to the second mixed solution to carry out a third reaction to obtain a solution containing the gold nanoparticles.
[0041] Optionally, in step S1, the molar ratio of the chloroauric acid solution to the sodium citrate solution is 1:(1-20), preferably 1:(1-10); the concentration of the chloroauric acid solution is 0.1-10 mmol / L, preferably 0.5-10 mmol / L; the concentration of the sodium citrate solution is 1-100 mmol / L, preferably 2-50 mmol / L.
[0042] Optionally, in step S2, the molar ratio of the first mixed solution to the DNA solution is 1:(20-2000), preferably 1:(100-500); the concentration of the DNA solution is 10-1000nmol / L, preferably 100-500nmol / L.
[0043] Optionally, the DNA sequence in the DNA solution includes 5 to 60 bases, preferably 10 to 40 bases; each base is independently selected from any one of A, G, C, and T.
[0044] Optionally, the mass ratio of the second mixed solution, the reducing agent and the growth reagent is 100:(1-20):(1-20), preferably 100:(1-10):(1-10).
[0045] Optionally, the reducing agent includes at least one of hydroxylamine hydrochloride, ascorbic acid and sodium citrate; and the growth reagent includes at least one of chloroauric acid, silver nitrate, chloroplatinic acid and chloropalladic acid.
[0046] Optionally, in the reducing agent, the concentration of the ascorbic acid solution is 50-100 mmol / L, the concentration of the hydroxylamine hydrochloride solution is 0.1-1 mol / L, and the concentration of the sodium citrate is 10-100 mmol / L;
[0047] In the growth reagent, the concentration of the chloroauric acid is 10-100mmol / L, the concentration of the silver nitrate is 10-100mmol / L, the concentration of the chloroplatinic acid is 10-100mmol / L, and the concentration of the chloropalladic acid solution is 10-100mmol / L.
[0048] Optionally, the gold nanoparticles include at least one of gold nanorods, gold nanoflowers and gold nanosheets.
[0049] Optionally, the reaction conditions of the first reaction include: reaction temperature of 80-140°C, preferably 80-100°C; reaction time of 1-30min, preferably 5-20min;
[0050] The reaction conditions of the second reaction include: reaction temperature of 4-100°C, preferably 60-100°C; reaction time of 2-720min, preferably 3-60min;
[0051] Mixing the first mixed solution with the DNA solution and performing a second reaction under the heating condition can change the amount and strength of DNA adsorption on the surface of the gold nanoparticles, control the growth direction of the gold nanoparticles, and regulate the morphology of the gold nanoparticles.
[0052] The reaction conditions of the third reaction include: reaction temperature of 4-37° C., preferably 25-27° C., and reaction time of 1-60 min, preferably 10-20 min.
[0053] Optionally, the gold nanoparticles include at least one of single metal gold, gold-silver alloy, gold-palladium alloy and gold-platinum alloy.
[0054] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0055] The synthesized nanoparticles were detected by electron microscopy using a HT-7700 TEM electron microscope produced by Hitachi. The detection conditions were: instrument resolution 0.204nm, temperature 25°C; the detection method was: drop the reaction liquid on the carbon support film, and observe it under a TEM electron microscope after drying.
[0056] The synthesized nanoparticles were subjected to UV detection using a UV-1750 UV-visible spectrophotometer produced by Shimadzu. The detection conditions were: detection wavelength 300-1000nm, temperature 25°C; the detection method was: use a pipette to take 80 μL of the test solution into a colorimetric dish, and place it in the instrument to detect the UV spectrum.
[0057] The amount of DNA adsorbed on the surface of gold nanoparticles was tested using a Spark fluorescence spectrometer produced by Tecan. The detection conditions were: excitation wavelength 490 nm, emission wavelength 530 nm, temperature 25°C; the detection method was: use a pipette to take 100 μL of the test solution and put it in a fluorescent dish, and then put it in the instrument to detect the fluorescence spectrum.
[0058] Example 1
[0059] (1) Synthesize gold nanomaterials according to the following steps:
[0060] A sodium citrate solution (concentration of 4 mmol / L) was added to a chloroauric acid solution (concentration of 1 mmol / L) for a first reaction, the molar ratio of chloroauric acid to sodium citrate was 1:4, and the reaction was carried out at 100°C for 20 min to obtain a first mixed solution. The first mixed solution was mixed with 100 nM DNA (C30) for a second reaction, DNA (C30) indicated that the DNA sequence consisted of 30 cytosines, the molar ratio of the first mixed solution to the DNA solution was 1:200, and the reaction was carried out at 100°C for 3 min to obtain a second mixed solution.
[0061] To the second mixed solution, hydroxylamine hydrochloride solution (concentration of 0.4 mol / L) and chloroauric acid solution (concentration of 50 mmol / L) were added in sequence to carry out the third reaction. The volume ratio of the second mixed solution, hydroxylamine hydrochloride solution and chloroauric acid solution was 150:7.5:1. The reaction was carried out at 25°C for 15 minutes to obtain a gold nano solution.
[0062] (2) The prepared gold nanoparticle solution is subjected to UV and TEM tests to determine the ultraviolet spectrum and morphology of the gold nanoparticles in the solution.
[0063] TEM test results are as follows Figure 1 Shown: Gold nanoparticles present a nanoflower morphology.
[0064] The prepared gold nanoparticle solution is blue, and the UV detection results are as follows Figure 3 As shown, the gold nanoparticle solution has an absorption peak at 622 nm.
[0065] Comparative Example 1
[0066] Gold nanomaterials were prepared according to the method of Example 1, which differed from Example 1 in that: in this comparative example, the reaction conditions of the second reaction were: temperature 25° C., reaction time 15 min.
[0067] The synthesized gold nanoparticle solution was characterized and tested. The gold nanoparticle solution prepared in this comparative example was purple. Figure 3 As shown, UV detection shows that the gold nanoparticle solution has an absorption peak at 536 nm.
[0068] TEM test results: The electron microscope image of the solution is nano-spherical nanoparticles, such as Figure 2 shown.
[0069] Example 2
[0070] This example is used to measure the adsorption amount and adsorption strength of DNA on the surface of gold nanoparticles in the second mixed solution.
[0071] (1) synthesizing gold nanoparticles according to the following steps;
[0072] A sodium citrate solution (concentration of 4 mmol / L) was added to a chloroauric acid solution (concentration of 1 mmol / L) for a first reaction, the molar ratio of chloroauric acid to sodium citrate was 1:4, and the reaction was carried out at 100°C for 20 min to obtain a first mixed solution. The first mixed solution was mixed with 1 μM carboxyfluorescein-labeled DNA (FAM-C30) for a second reaction, the molar ratio of the first mixed solution to the DNA solution was 1:200, and the reaction was carried out at 100°C for 3 min to obtain a second mixed solution;
[0073] (2) determining the amount of DNA adsorbed on the surface of the gold nanoparticles in the second mixed solution according to the following steps;
[0074] The fluorescence value of the second mixed solution was measured by fluorescence spectrometer, and the fluorescence value of the solution was measured after adding 20 mM potassium cyanide to dissolve the gold, and the adsorption amount of DNA on the surface of gold nanoparticles was calculated (10%, such as Figure 6 shown).
[0075] (3) Determine the adsorption strength of DNA on the surface of gold nanoparticles according to the following steps;
[0076] The fluorescence value of the second mixed solution was measured by fluorescence spectrometer. After adding 0.5mM and 20mM potassium cyanide to dissolve gold, the fluorescence change of the solution was measured. After adding 0.5mM and 20mM potassium cyanide, the fluorescence value increased. The rate constant of adding 0.5mM potassium cyanide was 0.56±0.01min -1 (like Figure 4As shown in the figure, a small amount of potassium cyanide is first added to desorb the weakly adsorbed DNA from the gold surface, and the fluorescence value increases. Then, an excess of potassium cyanide is added to desorb the strongly adsorbed DNA from the surface, and the fluorescence value increases, thereby determining the adsorption strength of DNA on the surface of gold nanoparticles.
[0077] Comparative Example 2
[0078] In this comparative example, gold nanomaterials were prepared according to the method of Example 2, which differed from Example 2 in that: in this comparative example, the reaction temperature for preparing the second mixed solution was 25° C., and the reaction time was 15 min.
[0079] The adsorption amount of DNA on the surface of gold nanoparticles in the second solution was determined according to the method of Example 2 and was 12%. Figure 6 As shown: After adding 0.5mM and 20mM potassium cyanide, the fluorescence value increased, and the rate constant of adding 0.5mM potassium cyanide was 2.4±0.2min -1 ,like Figure 4 As shown, it is greater than the rate constant under heating conditions measured in Example 2. The larger the rate constant, the easier it is for DNA to be desorbed from the gold surface, and the smaller the DNA adsorption strength on the gold nanoparticle surface.
[0080] It can be seen that Example 2 can change the adsorption amount and adsorption strength of DNA on the surface of gold nanoparticles under heating conditions. The adsorption of DNA on the gold surface is a dynamic process. Under heating conditions, DNA tends to be adsorbed longitudinally, such as Figure 5 As shown, the number of contact points with the surface of gold nanoparticles increased, which changed the adsorption amount of DNA on the surface of gold nanoparticles and increased the adsorption strength of DNA on the surface of gold nanoparticles.
[0081] Example 3
[0082] (1) Synthesize gold nanomaterials according to the following steps:
[0083] A sodium citrate solution (concentration of 4 mmol / L) was added to a chloroauric acid solution (concentration of 1 mmol / L) for a first reaction, the molar ratio of chloroauric acid to sodium citrate was 1:4, and the reaction was carried out at 100°C for 15 min to obtain a first mixed solution. The first mixed solution was mixed with 1 μM DNA (T30) for a second reaction, DNA (T30) indicated that the DNA sequence consisted of 30 thymines, the molar ratio of the first mixed solution to the DNA solution was 1:2000, and the reaction was carried out at 95°C for 5 min to obtain a second mixed solution.
[0084] To the second mixed solution, hydroxylamine hydrochloride solution (concentration of 0.1 mol / L) and chloroauric acid solution (concentration of 25 mmol / L) were added in sequence to carry out the third reaction. The volume ratio of the second mixed solution, hydroxylamine hydrochloride solution and chloroauric acid solution was 150:30:2. The reaction was carried out at 27°C for 20 minutes to obtain a gold nano solution.
[0085] (2) Perform UV and TEM tests on the gold nanoparticle solution prepared in the above steps to determine the ultraviolet spectrum and morphology of the gold nanoparticles in the solution:
[0086] TEM test results: The electron microscope image of the solution is irregular quadrilateral nanoparticles, such as Figure 7 As shown;
[0087] The gold nanoparticle solution prepared above is light blue. Fig. 9 As shown, UV detection shows that the gold nanoparticle solution has an absorption peak at 576 nm.
[0088] Comparative Example 3
[0089] Gold nanomaterials were prepared according to the method of Example 3, which differed from Example 3 in that: in this comparative example, the reaction temperature for preparing the second mixed solution was 25° C., and the reaction time was 15 min.
[0090] The gold nanoparticles prepared in this comparative example are purple-red in color, and the TEM test results show that the gold nanoparticles are nanospheres. Figure 8 As shown; UV measurement results are as follows Fig. 9 As shown, the gold nanoparticles have an absorption peak at 538 nm.
[0091] It can be seen from Examples 1-3 and Comparative Examples 1-3 that the synthesis method provided by the present disclosure can enhance the adsorption strength of DNA on the surface of gold nanoparticles and reduce the amount of DNA adsorbed on the surface of gold nanoparticles. The wavelength of the gold nanoparticle solution measured by UV shifts from 540nm to 632nm, indicating that the gold nanoparticles gradually form nanoparticles of different morphologies from the morphology of gold nanospheres.
[0092] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0093] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0094] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for synthesizing gold nanoparticles based on DNA regulation, It is characterized in that The method comprises the following steps: S1, mixing the chloroauric acid solution and the sodium citrate solution to perform a first reaction to obtain a first mixed solution; S2, performing a second reaction on the first mixed solution and the DNA solution to obtain a second mixed solution; S3, adding a reducing agent and a growth reagent to the second mixed solution to carry out a third reaction to obtain a solution containing the gold nanoparticles; The molar ratio of the chloroauric acid solution to the sodium citrate solution is 1:(1-20); the concentration of the chloroauric acid solution is 0.1-10 mmol / L; the concentration of the sodium citrate solution is 1-100 mmol / L; In step S2, the molar ratio of the first mixed solution to the DNA solution is 1:(20-2000); the concentration of the DNA solution is 10-1000nmol / L; The reaction conditions of the first reaction include: reaction temperature of 80-140°C, reaction time of 1-30min; The reaction conditions of the second reaction include: reaction temperature of 95-100°C, reaction time of 3-5min; The reaction conditions of the third reaction include: reaction temperature of 4-37° C., and reaction time of 1-60 min.
2. The method according to claim 1, in, In step S1, the molar ratio of the chloroauric acid solution to the sodium citrate solution is 1:(1-10); The concentration of the chloroauric acid solution is 0.5-5mmol / L; The concentration of the sodium citrate solution is 2-50 mmol / L.
3. The method according to claim 1, in, In step S2, the molar ratio of the first mixed solution to the DNA solution is 1:(100-500); the concentration of the DNA solution is 100-500nmol / L.
4. The method according to claim 1, in, The DNA sequence in the DNA solution includes 10-40 bases; each base is independently selected from any one of A, G, C, and T.
5. The method according to claim 1, in, The mass ratio of the second mixed solution, the reducing agent and the growth reagent is 100:(1-20):(1-20).
6. The method according to claim 5, in, The mass ratio of the second mixed solution, the reducing agent and the growth reagent is 100:(1-10):(1-10).
7. The method according to claim 1, in, The reducing agent includes at least one of hydroxylamine hydrochloride, ascorbic acid and sodium citrate; the growth reagent includes at least one of chloroauric acid, silver nitrate, chloroplatinic acid and chloropalladic acid.
8. The method according to claim 7, in, In the reducing agent, the concentration of the ascorbic acid solution is 50-100 mmol / L, the concentration of the hydroxylamine hydrochloride solution is 0.1-1 mol / L, and the concentration of the sodium citrate solution is 10-100 mmol / L; In the growth reagent, the concentration of the chloroauric acid solution is 10-100mmol / L, the concentration of the silver nitrate is 10-100mmol / L, the concentration of the chloroplatinic acid is 10-100mmol / L, and the concentration of the chloropalladic acid solution is 10-100mmol / L.
9. The method according to claim 1, in, The gold nanoparticles include at least one of gold nanorods, gold nanoflowers and gold nanosheets.
10. The method according to claim 1, in, The reaction conditions of the first reaction include: reaction temperature of 80-100°C; reaction time of 5-20min; The reaction conditions of the third reaction include: reaction temperature of 25-27° C., and reaction time of 10-20 min.
11. The method according to claim 1, in, The gold nanoparticles include at least one of single metal gold, gold-silver alloy, gold-palladium alloy and gold-platinum alloy.