A layered Na3M2XO6 oxide-coated modified sodium manganate positive electrode material and a preparation method thereof
By coating the sodium manganate cathode material with layered Na3M2XO6 oxide, the problems of structural stability and low conductivity of manganese-based sodium electrical materials in sodium-ion batteries are solved, achieving high stability and high specific capacity of the material. , extending cycle life.
Patent Information
- Application Number
- CN202210928414.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-08-03
AI Technical Summary
Manganese-based sodium electrical materials have poor structural stability and low conductivity in sodium-ion batteries, resulting in poor cycle stability and short cycle life of electrode materials.
The sodium manganate cathode material modified by layered Na3M2XO6 oxide coating is used to improve the structural stability and specific capacity of the material by combining the sodium manganate matrix with the layered Na3M2XO6 oxide coating layer. The preparation method of the material includes the complexation reaction of metal salts and organic ligands, followed by mixing with sodium salts and sodium sintering to form a Na3M2XO6 oxide coating layer with a high sodium content.
It improves the structural stability and specific capacity of the sodium manganate cathode material, protects the material from being eroded by the electrolyte, reduces the surface embedding energy barrier of sodium manganate, enhances the ionic conductivity, and extends the cycle life of the material.
Smart Images

Figure CN115241435B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of battery materials, and in particular relates to a coated modified sodium manganate positive electrode material and a preparation method thereof. Background Art
[0002] Sodium-ion batteries have the characteristics of low cost, abundant reserves of raw materials, and energy storage mechanisms similar to lithium-ion batteries. In lithium-ion batteries, lithium manganese oxide materials have good stability, high safety and low cost, and have been successfully used in commercial production. Based on this, manganese-based sodium electric materials have also become the main research object of current sodium electric positive electrode materials. However, due to the large ionic radius of sodium ions themselves, the volume strain of manganese-based materials is large during ion transfer. Therefore, they have poor structural stability and low conductivity in the application of sodium-ion batteries, which leads to poor cycle stability of electrode materials and short cycle life. In order to solve these problems, we usually use coating and doping for modification.
[0003] The coating materials selected in the prior art have limited improvement effects on manganese-based sodium electrical materials, which still limits their application. Therefore, selecting a coating material with high stability and capable of providing a certain amount of energy can achieve dual improvements in structure and performance at the same time, which is conducive to the promotion and application of manganese-based sodium electrical materials. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a layered Na 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material and preparation method thereof. To solve the above technical problems, the technical solution proposed by the present invention is:
[0005] A layered Na 3 M 2 XO 6 The oxide-coated modified sodium manganate positive electrode material comprises a sodium manganate matrix and a layered Na 3 M 2 XO 6 Oxide coating layer, the molecular formula of the sodium manganate matrix is Na x MnO 2 , where x is in the range of 0.5≤x≤1; the layered Na 3 M 2 XO 6 The molecular formula of the oxide is Na 3 M 2 XO 6 , wherein M is one of Co, Ni, and Cu; and X is one of Bi and Sb.
[0006] As a general technical concept, the present invention also provides a layered Na 3 M 2 XO 6 The method for preparing an oxide-coated modified sodium manganate positive electrode material comprises the following steps:
[0007] (1) dissolving an M metal salt and an X metal salt in an organic solvent to obtain a metal salt solution; dissolving an organic ligand in an organic solvent to obtain an organic ligand solution; slowly dripping the organic ligand solution into the metal salt solution to carry out a complexation reaction; after the reaction is completed, centrifuging, washing, and drying to obtain a solid phase; and then uniformly mixing the solid phase with a sodium salt or sodium oxide, and then sintering the solid phase to obtain a layered Na 3 M 2 XO 6 Oxides;
[0008] (2) dissolving manganese salt and sodium salt in deionized water, adding a certain amount of citric acid, and stirring the mixture to react until a gel-like mixture is formed;
[0009] (3) The layered Na obtained in step (1) 3 M 2 XO 6 The oxide is added to the gel-like mixture of step (2), stirred continuously, and then dried to obtain a layered Na 3 M 2 XO 6 Oxide composite modified manganese-based sodium electrode precursor;
[0010] (4) Sintering the manganese-based sodium precursor obtained in step (3) to obtain a layered Na 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material.
[0011] In the above preparation method, preferably, the M metal salt and the X metal salt are one or more of acetate, oxalate, nitrate or sulfate; the organic solvent is one or more of methanol, ethanol or ethylene glycol; and the organic ligand is one or more of 2-methylimidazole, trimesic acid, terephthalic acid or imidazole.
[0012] In the above preparation method, preferably, the total concentration of the metal salt in the metal salt solution is 0.01-0.1 mol / L, which can ensure the uniformity and continuity of the metal ions. If the concentration is too low, the continuity of the metal ions will be poor, affecting the reaction progress. If the concentration is too high, the reaction will be too fast locally, affecting the particle size of the product; the concentration of the organic ligand solution is 0.5-2 mol / L, which can ensure the uniformity and continuity of the organic ligand. If the concentration is too low, the complexation reaction rate will be slow and it will not be easy to form a precipitate. If the concentration is too high, the precipitation rate will be too fast, which will make the size of the generated precipitate uneven; the molar ratio of the metal salt to the organic ligand is 1: (100-300), which can ensure that the metal salt and the organic ligand are fully reacted. If the metal salt is too little, the product yield will be affected, resulting in excessive waste of the organic ligand. If the organic ligand is too little, the complexation reaction will not react fully, which will also affect the yield.
[0013] In the above preparation method, preferably, the reaction time of the complex reaction is 0.5-6h, and the reaction temperature is room temperature. The above complex reaction time and temperature can ensure that the complex reaction is fully carried out.
[0014] In the above preparation method, preferably, the sodiumization atmosphere is controlled to be oxygen or air atmosphere during the sodiumization sintering; the sintering temperature of the sodiumization sintering is 800-1000°C, and the sintering time is 6-24h. At the above temperature, the sodiumization reaction can be carried out well. If the temperature is too low, the sodiumization will be incomplete. If the temperature is too high, the metallic sodium will partially volatilize, so that the prepared active material will have a reduced sodium content, which directly affects the specific capacity of the material. Under the above sintering time, the sodiumization reaction can occur completely. If the time is too short, the reaction cannot be sufficient. If the time is too long, it will affect the crystal form and morphology of the material, and ultimately affect the performance of the material.
[0015] In the above preparation method, preferably, the sodium salt is one or more of sodium carbonate, sodium acetate or sodium oxalate.
[0016] In the above preparation method, preferably, in the step (2), the molar ratio of the sum of the molar amounts of the manganese salt and the sodium salt to the citric acid is (0.5-2):1, and this molar ratio can ensure that the reaction can be carried out completely. If the proportion of manganese sodium salt is reduced, it will affect the final sodium manganate yield; if the proportion of citric acid is too small, the sol will be thinner and difficult to form a gel; during the stirring reaction, the reaction temperature is controlled to be 60-100°C, at which temperature a gel can be formed. If the temperature is too low, the sol rate will be affected. If the temperature is too high, the water solvent will evaporate, which will ultimately affect the completeness of the reaction.
[0017] In the above preparation method, preferably, the layered Na 3 M 2 XO 6The molar ratio of the oxide to the manganese-based sodium electric precursor core is (0.01-0.05): 1. The above ratio can ensure the uniformity of the coating layer. If the coating layer content is too high, the coating layer is too thick or the thickness is uneven locally, or the coating layer content is too low, the coating effect is not obvious. More preferably, the layered Na 3 M 2 XO 6 The molar ratio of the oxide to the manganese-based sodium electric precursor core is (0.01-0.015):1.
[0018] In the above preparation method, preferably, the sintering atmosphere is controlled to be oxygen or air during the sintering treatment; the sintering temperature of the sodium sintering is 700-1000°C, and the sintering time is 2-20h. At this sintering temperature, the preparation of sodium manganate can be achieved. If the sintering temperature is too low, sodium manganate cannot form a uniform structure. If the temperature is too high, the structure and morphology of the material will undergo irreversible changes, which will have an adverse effect on the subsequent electrochemical properties. The sintering time is 2-20h, which can ensure the complete synthesis of sodium manganate. If the time is too short, the synthesis is incomplete. If the time is too long, the structure and morphology of the material will be irreversibly changed. More preferably, the sintering treatment is pre-sintering at 300°C for 2h, and then further sintering at 900°C for 10h.
[0019] Our study shows that layered Na 3 M 2 XO 6 The oxide has a high sodium content and good structural stability, and is directly coated on the surface of the sodium manganate positive electrode material with good electrochemical performance, which can improve the structural stability and reversible capacity of the material. 3 M 2 XO 6 Nanomaterials are coated on the surface of sodium manganate, which has low cost and good electrochemical properties, to provide more sodium ions, thereby increasing the specific capacity of the material. At the same time, since the coating layer is coated on the surface of sodium manganate, it will protect and constrain the surface of sodium manganate, which can not only protect the material from being corroded by the electrolyte, but also ensure that the structure of sodium manganate is stable and does not collapse during the continuous ion deintercalation process, and can isolate sodium manganate from the electrolyte, thereby inhibiting the occurrence of side reactions on the surface of sodium manganate. At the same time, since both have common sodium ions, the combination of the two is closer and the synergistic effect is more obvious. In the subsequent long-term cycle process, the two are not easy to separate or peel off. In addition, since the sodium manganate we synthesized is a P2 phase layered structure, because the layered Na 3 M 2 XO 6The structure of the oxide is similar to that of the main material, so the compatibility is strong and the matching is good, which will reduce the structural difference between the main material and the coating layer, thereby improving the structural stability of the main body and surface of sodium manganate. 3 M 2 XO 6 The good ionic conductivity of the oxide can reduce the embedding energy barrier on the surface of sodium manganate and improve the ionic conductivity, thereby achieving the optimized synthesis of high-capacity and high-rate positive electrode materials.
[0020] In the present invention, more preferably, the coating layer is a layered Na 3 Ni 2 SbO 6 Oxide coating, and the molecular formula of the sodium manganate matrix is Na 0.67 MnO 2 The synergistic effect between the two is the best and the comprehensive performance is the best.
[0021] In the preparation method of the present invention, MOF synthesis is a room temperature complexation reaction, which is simpler and easier to achieve. The subsequent coating sintering is also a structural formation process of the main material, which will not cause irreversible structural changes to the main material itself, thereby ensuring the structural stability of the main sodium manganate material. At the same time, the preparation method of the present invention synthesizes bimetallic MOF in one step, and uses it as a substrate and template, and directly prepares Na with uniform particles, porous and perfect morphology through further sodium treatment. 3 M 2 XO 6 Nanomaterials provide high-quality raw materials for subsequent coating, which are more practical, simpler to operate, and have a shorter process. The layered Na prepared by the above process 3 M 2 XO 6 The oxide is more suitable for use as a coating layer, and has a good synergistic relationship with other process steps, and the final product has good stability and high specific capacity. 3 M 2 XO 6 The oxide-coated modified sodium manganate positive electrode material has a better matching degree between the coating layer and the core matrix, and is more tightly combined, which is conducive to the synergistic effect between the coating layer and the core matrix.
[0022] Compared with the prior art, the advantages of the present invention are:
[0023] 1. Layered Na 3 M 2 XO 6 Oxide-coated modified sodium manganate cathode material, layered Na 3 M 2XO 6 The oxide has a high sodium content and good structural stability. Directly coating it on the surface of the sodium manganate positive electrode material with good electrochemical properties can improve the structural stability and specific capacity of the material.
[0024] 2. The preparation method of the present invention first prepares Na 3 M 2 XO 6 Nanomaterials are then mixed with a gel-like mixture and finally sintered to treat the layered Na 3 M 2 XO 6 The oxide-coated modified sodium manganate positive electrode material, the coating process is conducive to the preparation of a product with better synergy between the coating layer and the core matrix, and the subsequent coating sintering is also a structural formation process of the main material, which will not cause irreversible structural changes to the main material itself.
[0025] 3. The preparation method of the present invention has a simple process, a short flow, readily available raw materials, no toxic or harmful substances are produced during the preparation process, and is easy to implement large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The layered Na prepared in Example 1 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 SEM image of the positive electrode material. DETAILED DESCRIPTION
[0028] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0029] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0031] Embodiment 1:
[0032] A layered Na 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The positive electrode material comprises a sodium manganate matrix and a layered Na 3 Co 2 SbO 6 Oxide coating, the molecular formula of sodium manganate matrix is Na 0.67 MnO 2 .
[0033] A layered Na 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The method for preparing a positive electrode material comprises the following steps:
[0034] (1) 1 mmol Co(NO 3 ) 2 6H 2 O and 0.5mmol Sb(NO 3 ) 3 Dissolve in 50mL methanol solution; separately, dissolve 0.25mol 2-methylimidazole in 350mL methanol solution, slowly drip the 2-methylimidazole solution into the metal salt solution, and carry out complexation reaction at room temperature. After reacting for 1h, centrifuge, wash, dry, and then mix with 0.78mmol Na 2 CO 3 After uniform mixing, the layered Na 3 Co 2 SbO 6 Oxide.
[0035] (2) 0.04 mol Mn(CH 3 COO 2 ·4H 2 O, 0.04 mol CH 3 COONa was dissolved in 100 ml of deionized water, 0.1 mol of citric acid was added, and the mixture was stirred at 80°C until a gel-like mixture was formed. After the gel was formed, the Na 3 Co2 SbO 6 All (0.5 mmol) was added to the gel-like substance, and the reaction was continued with stirring for 1 h. After drying at 120 °C for 12 h, it was placed in a muffle furnace for high-temperature sintering. After pre-sintering at 300 °C for 2 h, it was further sintered at 900 °C for 10 h to obtain the final layered Na 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 Positive electrode material.
[0036] The layered Na 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 SEM images of the positive electrode materials are shown in Figure 1 As shown by Figure 1 It can be seen that Na 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The positive electrode material is a micron block of 3.5μm long × 2μm wide × 0.5μm thick. The material after coating has uniform morphology and smooth surface, which fully proves the uniformity of coating.
[0037] Take Na 3 Co 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 It is the active material of the positive electrode material, and is mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) is used as the solvent, and the mixture is placed in a small beaker and stirred at a speed of 800r / min for 2h to obtain a slurry. The slurry is coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85℃ for 4h, punched into a pole piece with a diameter of 12mm, and then dried at 105℃ in a vacuum drying oven for 4h. It is placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1ppm for 4h to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The metallic sodium is rolled into a thin sheet and punched into a 14mm round sodium sheet as the negative electrode, and 1mol / L NaClO 4 The solution is used as the electrolyte, and the glass fiber membrane with a diameter of 16 mm is used as the diaphragm.
[0038] After the battery was assembled and aged for 12 hours, the charge and discharge tests were carried out at different potentials. The discharge capacity of the calcined sample after 100 cycles at a voltage of 2-4V and a current density of 1C was 114.2mAh g -1 , the capacity retention rate is 83.9%.
[0039] Comparative Example 1:
[0040] A Na 0.67 MnO 2 The method for preparing a positive electrode material comprises the following steps:
[0041] 0.04 mol Mn(CH 3 COO 2 ·4H 2 O, 0.04 mol CH 3 COONa was dissolved in 100 ml of deionized water, and 0.1 mol of citric acid was added. The mixture was stirred at 80 °C until a gel-like mixture was formed. After the gel was formed, it was dried at 120 °C for 12 h, and then placed in a muffle furnace for high-temperature sintering. After pre-sintering at 300 °C for 2 h, it was further sintered at 900 °C for 10 h to obtain the final Na 0.67 MnO 2 Positive electrode material.
[0042] Take Na 0.67 MnO 2 The material is the active material of the positive electrode material, and is mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) is used as the solvent, and the mixture is placed in a small beaker and stirred at a speed of 800r / min for 2h to obtain a slurry. The slurry is coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85°C for 4h, punched into a pole piece with a diameter of 12mm, and then dried at 105°C in a vacuum drying oven for 4h. It is placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1ppm for 4h to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The metallic sodium is rolled into a thin sheet and punched into a 14mm round sodium sheet as the negative electrode, and 1mol / L NaClO 4 The solution is used as the electrolyte, and the glass fiber membrane with a diameter of 16 mm is used as the diaphragm.
[0043] After the battery was assembled and aged for 12 hours, the charge and discharge tests were carried out at different potentials. The discharge capacity of the calcined sample after 100 cycles at a voltage of 2-4V and a current density of 1C was 56.7mAh g -1 , the capacity retention rate is 51.3%.
[0044] Embodiment 2:
[0045] A layered Na 3 Ni 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The positive electrode material comprises a sodium manganate matrix and a layered Na 3 Ni 2 SbO 6 Oxide coating, the molecular formula of sodium manganate matrix is Na 0.67 MnO 2 .
[0046] A layered Na 3 Ni 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The method for preparing a positive electrode material comprises the following steps:
[0047] (1) 1mmol Ni(NO 3 ) 2 6H 2 O and 0.5mmol Sb(NO 3 ) 3 Dissolve in 50mL methanol solution; separately, dissolve 0.25mol 2-methylimidazole in 350mL methanol solution, slowly drip the 2-methylimidazole solution into the metal salt solution, and carry out complexation reaction at room temperature. After 1h of reaction, centrifuge, wash, dry, and then mix with 0.78mmol Na 2 CO 3 After uniform mixing, the layered Na 3 Ni 2 SbO 6 Oxide.
[0048] (2) 0.04 mol Mn(CH 3 COO 2 ·4H 2 O, 0.04 mol CH 3 COONa was dissolved in 100 ml of deionized water, 0.1 mol of citric acid was added, and the mixture was stirred at 80°C until a gel-like mixture was formed. After the gel was formed, the Na 3 Ni 2 SbO 6All (0.5 mmol) was added to the gel-like substance, and the reaction was continued with stirring for 1 h. After drying at 120 °C for 12 h, it was placed in a muffle furnace for high-temperature sintering. After pre-sintering at 300 °C for 2 h, it was further sintered at 900 °C for 10 h to obtain the final layered Na 3 Ni 2 SbO 6 Oxide complexed Na 0.67 MnO 2 Positive electrode material.
[0049] Take Na 3 Ni 2 SbO 6 Oxide complexed Na 0.67 MnO 2 It is the active material of the positive electrode material, and is mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) is used as the solvent, and the mixture is placed in a small beaker and stirred at a speed of 800r / min for 2h to obtain a slurry. The slurry is coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85℃ for 4h, punched into a pole piece with a diameter of 12mm, and then dried at 105℃ in a vacuum drying oven for 4h. It is placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1ppm for 4h to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The metallic sodium is rolled into a thin sheet and punched into a 14mm round sodium sheet as the negative electrode, and 1mol / L NaClO 4 The solution is used as the electrolyte, and the glass fiber membrane with a diameter of 16 mm is used as the diaphragm.
[0050] After the battery was assembled and aged for 12 hours, the charge and discharge tests were carried out at different potentials. The discharge capacity of the calcined sample after 100 cycles at 2-4V voltage and 1C current density was 125.7mAh g -1 , the capacity retention rate is 88.3%.
[0051] Embodiment 3:
[0052] A layered Na 3 Ni 2 BiO 6 Oxide-coated modified Na 0.67 MnO 2 The positive electrode material comprises a sodium manganate matrix and a layered Na 3 Ni 2 BiO 6 Oxide coating, the molecular formula of sodium manganate matrix is Na 0.67 MnO2 .
[0053] A layered Na 3 Ni 2 BiO 6 Oxide-coated modified Na 0.67 MnO 2 The method for preparing a positive electrode material comprises the following steps:
[0054] (1) 1mmol Ni(NO 3 ) 2 6H 2 O and 0.5mmol Bi(NO 3 ) 3 Dissolve in 50mL methanol solution; separately, dissolve 0.25mol 2-methylimidazole in 350mL methanol solution, slowly drip the 2-methylimidazole solution into the metal salt solution, and carry out complexation reaction at room temperature. After 1h of reaction, centrifuge, wash, dry, and then mix with 0.78mmol Na 2 CO 3 After uniform mixing, the layered Na 3 Ni 2 BiO 6 Oxide.
[0055] (2) 0.04 mol Mn(CH 3 COO 2 ·4H 2 O, 0.04 mol CH 3 COONa was dissolved in 100 ml of deionized water, 0.1 mol of citric acid was added, and the mixture was stirred at 80°C until a gel-like mixture was formed. After the gel was formed, the Na 3 Ni 2 BiO 6 All (0.5 mmol) was added to the gel-like substance, and the reaction was continued with stirring for 1 h. After drying at 120 °C for 12 h, it was placed in a muffle furnace for high-temperature sintering. After pre-sintering at 300 °C for 2 h, it was further sintered at 900 °C for 10 h to obtain the final layered Na 3 Ni 2 BiO 6 Oxide complexed Na 0.67 MnO 2 Positive electrode material.
[0056] Take Na 3 Ni 2 BiO 6 Oxide complexed Na 0.67 MnO 2It is the active material of the positive electrode material, and is mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) is used as the solvent, and the mixture is placed in a small beaker and stirred at a speed of 800r / min for 2h to obtain a slurry. The slurry is coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85℃ for 4h, punched into a pole piece with a diameter of 12mm, and then dried at 105℃ in a vacuum drying oven for 4h. It is placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1ppm for 4h to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The metallic sodium is rolled into a thin sheet and punched into a 14mm round sodium sheet as the negative electrode, and 1mol / L NaClO 4 The solution is used as the electrolyte, and the glass fiber membrane with a diameter of 16 mm is used as the diaphragm.
[0057] After the battery was assembled and aged for 12 hours, the charge and discharge tests were carried out at different potentials. The discharge capacity of the calcined sample after 100 cycles at a voltage of 2-4V and a current density of 1C was 107.2mAh g -1 , the capacity retention rate is 75.8%.
[0058] Embodiment 4:
[0059] A layered Na 3 Ni 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The positive electrode material comprises a sodium manganate matrix and a layered Na 3 Ni 2 SbO 6 Oxide coating, the molecular formula of sodium manganate matrix is Na 0.67 MnO 2 .
[0060] A layered Na 3 Ni 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The method for preparing a positive electrode material comprises the following steps:
[0061] (1) 0.8 mmol Ni(NO 3 ) 2 6H 2 O and 0.4mmol Sb(NO 3 ) 3Dissolve in 40mL methanol solution; separately, dissolve 0.2mol 2-methylimidazole in 280mL methanol solution, slowly drip the 2-methylimidazole solution into the metal salt solution, and carry out complexation reaction at room temperature. After 1h of reaction, centrifuge, wash, dry, and then mix with 0.62mmol Na 2 CO 3 After uniform mixing, the layered Na 3 Ni 2 SbO 6 Oxide.
[0062] (2) 0.04 mol Mn(CH 3 COO 2 ·4H 2 O, 0.04 mol CH 3 COONa was dissolved in 100 ml of deionized water, 0.1 mol of citric acid was added, and the mixture was stirred at 80°C until a gel-like mixture was formed. After the gel was formed, the Na 3 Ni 2 SbO 6 All of them were added to the gel-like material, and the reaction was continued with stirring for 1 hour. After that, it was dried at 120°C for 12 hours, and then placed in a muffle furnace for high-temperature sintering. After pre-sintering at 300°C for 2 hours, it was further sintered at 900°C for 10 hours to obtain the final layered Na 3 Ni 2 SbO 6 Oxide complexed Na 0.67 MnO 2 Positive electrode material.
[0063] Take Na 3 Ni 2 SbO 6 Oxide complexed Na 0.67 MnO 2It is the active material of the positive electrode material, and is mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) is used as the solvent, and the mixture is placed in a small beaker and stirred at a speed of 800r / min for 2h to obtain a slurry. The slurry is coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85℃ for 4h, punched into a pole piece with a diameter of 12mm, and then dried at 105℃ in a vacuum drying oven for 4h. It is placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1ppm for 4h to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The metallic sodium is rolled into a thin sheet and punched into a 14mm round sodium sheet as the negative electrode, and 1mol / L NaClO 4 The solution is used as the electrolyte, and the glass fiber membrane with a diameter of 16 mm is used as the diaphragm.
[0064] After the battery was assembled and aged for 12 hours, the charge and discharge tests were carried out at different potentials. The discharge capacity of the calcined sample after 100 cycles at a voltage of 2-4V and a current density of 1C was 114.5mAh g -1 , the capacity retention rate is 78.3%.
[0065] Embodiment 5:
[0066] A layered Na 3 Ni 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The positive electrode material comprises a sodium manganate matrix and a layered Na 3 Ni 2 SbO 6 Oxide coating, the molecular formula of sodium manganate matrix is Na 0.67 MnO 2 .
[0067] A layered Na 3 Ni 2 SbO 6 Oxide-coated modified Na 0.67 MnO 2 The method for preparing a positive electrode material comprises the following steps:
[0068] (1) 1.2 mmol Ni(NO 3 ) 2 6H 2 O and 0.6mmol Sb(NO 3 ) 3Dissolve in 60mL methanol solution; separately, dissolve 0.2mol 2-methylimidazole in 280mL methanol solution, slowly drip the 2-methylimidazole solution into the metal salt solution, and carry out complexation reaction at room temperature. After 1h of reaction, centrifuge, wash, dry, and then mix with 0.62mmol Na 2 CO 3 After uniform mixing, the layered Na 3 Ni 2 SbO 6 Oxide.
[0069] (2) 0.04 molMn(CH 3 COO 2 ·4H 2 O, 0.04 mol CH 3 COONa was dissolved in 100 ml of deionized water, 0.1 mol of citric acid was added, and the mixture was stirred at 80°C until a gel-like mixture was formed. After the gel was formed, the Na 3 Ni 2 SbO 6 All of them were added to the gel-like material, and the reaction was continued with stirring for 1 hour. After that, it was dried at 120°C for 12 hours, and then placed in a muffle furnace for high-temperature sintering. After pre-sintering at 300°C for 2 hours, it was further sintered at 900°C for 10 hours to obtain the final layered Na 3 Ni 2 SbO 6 Oxide complexed Na 0.67 MnO 2 Positive electrode material.
[0070] Take Na 3 Ni 2 SbO 6 Oxide complexed Na 0.67 MnO 2It is the active material of the positive electrode material, and is mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1. N-methylpyrrolidone (NMP) is used as the solvent, and the mixture is placed in a small beaker and stirred at a speed of 800r / min for 2h to obtain a slurry. The slurry is coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85℃ for 4h, punched into a pole piece with a diameter of 12mm, and then dried at 105℃ in a vacuum drying oven for 4h. It is placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1ppm for 4h to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The metallic sodium is rolled into a thin sheet and punched into a 14mm round sodium sheet as the negative electrode, and 1mol / L NaClO 4 The solution is used as the electrolyte, and the glass fiber membrane with a diameter of 16 mm is used as the diaphragm.
[0071] After the battery was assembled and aged for 12 hours, the charge and discharge tests at different potentials were carried out. The discharge capacity of the calcined sample after 100 cycles at 2-4V voltage and 1C current density was 120.2mAh g -1 , the capacity retention rate is 82.1%.
Claims
1. A layered Na 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that It comprises a sodium manganate matrix and a layered Na coated on the surface of the sodium manganate matrix. 3 M 2 XO 6 Oxide coating layer, the molecular formula of the sodium manganate matrix is Na x MnO 2 , where x is in the range of 0.5≤x≤1; the layered Na 3 M 2 XO 6 The molecular formula of the oxide is Na 3 M 2 XO 6 , wherein M is one of Co, Ni, and Cu; X is one of Bi and Sb; Layered Na 3 M 2 XO 6 The method for preparing an oxide-coated modified sodium manganate positive electrode material comprises the following steps: (1) dissolving metal salt M and metal salt X in an organic solvent to obtain a metal salt solution; dissolving an organic ligand in an organic solvent to obtain an organic ligand solution; slowly dripping the organic ligand solution into the metal salt solution to carry out a complexation reaction; after the reaction is completed, centrifuging, washing, and drying to obtain a solid phase; then uniformly mixing the solid phase with a sodium salt or sodium oxide, and then sintering the solid phase to obtain a layered Na 3 M 2 XO 6 Oxides; (2) dissolving manganese salt and sodium salt in deionized water, adding a certain amount of citric acid, and stirring the mixture to react until a gel-like mixture is formed; (3) The layered Na obtained in step (1) 3 M 2 XO 6 The oxide is added to the gel-like mixture of step (2), stirred continuously, and then dried to obtain layered Na 3 M 2 XO 6 Oxide composite modified manganese-based sodium electrode precursor; (4) Sintering the manganese-based sodium precursor obtained in step (3) to obtain a layered Na 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material.
2. The layered Na according to claim 1 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that The M metal salt and the X metal salt are one or more of acetate, oxalate, nitrate or sulfate; the organic solvent is one or more of methanol, ethanol or ethylene glycol; the organic ligand is one or more of 2-methylimidazole, trimesic acid, terephthalic acid or imidazole.
3. The layered Na according to claim 1 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that The total concentration of the metal salt in the metal salt solution is 0.01-0.1 mol / L; the concentration of the organic ligand solution is 0.5-2 mol / L; and the molar ratio of the metal salt to the organic ligand is 1:(100-300).
4. The layered Na according to claim 1 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that The reaction time of the complex reaction is 0.5-6h, and the reaction temperature is room temperature.
5. The layered Na according to claim 1 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that During the sodium sintering, the sodium sintering atmosphere is controlled to be oxygen or air atmosphere; the sintering temperature of the sodium sintering is 800-1000° C., and the sintering time is 6-24 hours.
6. The layered Na according to any one of claims 1 to 5 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that The sodium salt is one or more of sodium carbonate, sodium acetate or sodium oxalate.
7. The layered Na according to any one of claims 1 to 5 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that In the step (2), the molar ratio of the sum of the molar amounts of the manganese salt and the sodium salt to the citric acid is (0.5-2):1; and the reaction temperature is controlled to be 60-100°C during the stirring reaction.
8. The layered Na according to any one of claims 1 to 5 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that The layered Na 3 M 2 XO 6 The molar ratio of oxide to manganese-based sodium electric precursor core is (0.01-0.05):
1.
9. The layered Na according to any one of claims 1 to 5 3 M 2 XO 6 Oxide-coated modified sodium manganate positive electrode material, It is characterized in that During the sintering treatment, the sintering atmosphere is controlled to be oxygen or air; the sintering temperature of the sodium sintering is 700-1000° C., and the sintering time is 2-20 hours.
Citation Information
Patent Citations
Sodium ion battery anode material and sodium iron battery comprising anode material
CN103985851A
Anode active material for rechargeable battery preparation method thereof and rechargeable battery comprising same
CN110364725A
Positive electrode material for sodium ion battery and sodium ion battery comprising positive electrode material
CN113130896A
Sodium manganate composite modified layered transition metal oxide positive electrode material and preparation method thereof
CN114678501A
NaMnO2-coated NaV2O5 composite material as well as preparation method and application thereof
CN114824191A