Heat tempered glass ceramics

The aluminum silicate glass ceramics are strengthened through the heat tempering process to form aluminosilicate glass ceramics with high compression stress and high mechanical strength, which solves the problem of the underestimation of the heat tempering process and the contribution of residual glass in the existing technology. , achieving the improvement of the efficient mechanical properties of glass ceramics.

CN115244014BActive Publication Date: 2024-11-01CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180019376.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-06
Filing Date
2021-02-19
Publication Date
2024-11-01
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

In the prior art, when strengthening glass ceramics, the heat tempering process takes a long time and is difficult to effectively improve its mechanical properties, and the contribution of the existing methods to residual glass is underestimated.

Method used

Aluminosilicate glass ceramic composition strengthened by a thermal tempering process is developed, including crystalline phase and residual glass phase, to form a system with high compression stress by heating and rapid cooling within a specific temperature range, and to improve its thermal expansion curve. Differences in the divergence segments of inflection point temperature and mechanical strength.

Benefits of technology

It has achieved significant improvement in the mechanical strength and thermal expansion performance of glass ceramics in a short period of time, with a surface compression stress greater than 60MPa and a Young's modulus between 70GPa and 110GPa. It is suitable for products in the fields of electronics, automobiles and construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115244014B_ABST
    Figure CN115244014B_ABST
Patent Text Reader

Abstract

The thermally tempered aluminosilicate glass-ceramic composition comprises a crystalline phase and a residual glass phase, wherein the two phases form a system in which the thermal expansion curve of the system has two different segments radiating from an inflection point temperature in the range of about 450°C to about 600°C, and wherein the difference in thermal expansion coefficient of the glass-ceramic below and above the inflection point is greater than about 4 ppm / °C.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references to related patent applications

[0002] This application claims priority under 35 USC §119 to U.S. Provisional Serial No. 62 / 986,069, filed on March 6, 2020, the contents of which are relied upon and incorporated herein by reference in their entirety.

[0003] The present disclosure relates to thermally tempered glass-ceramics. Specifically, the present disclosure relates to glass-ceramics and precursor glasses that can be crystallized into glass-ceramics, which can be strengthened by a thermal tempering process, methods of making thermally tempered glass-ceramics, and articles and devices containing thermally tempered glass-ceramics. Background Art

[0004] The following discussion is provided to assist the reader in understanding the present disclosure and is not intended to be an admission that describes or constitutes prior art.

[0005] Various processes can be used to strengthen glass and glass ceramic (GC) products, including chemical strengthening, thermal tempering, and lamination. Lamination strengthening is used to strengthen tableware, for example, to make tableware able to withstand damage from handling and cutting tools. Chemical strengthening by methods such as ion exchange is used, for example, to strengthen cover glass for displays and touch screens used in electronic devices (e.g., smartphones, tablets, and televisions). Thermally tempered glass provides excellent mechanical properties in many applications (e.g., architectural windows and automotive glazing).

[0006] In the case of glass ceramics, the role of residual glass in glass ceramics in terms of what contribution it can bring to the material is often underestimated. For example, by allocating higher boron oxide additions to the residual glass, the residual glass can also be designed to improve the indentation response. In several glass ceramic systems, it is the residual glass that has undergone ion exchange that leads to chemical strengthening. Thermal tempering of glass ceramics can generally have advantages over the stress provided by ion exchange in terms of processing time and the resulting stress distribution. Although ion exchange takes several hours, due to the characteristics of thermal tempering, thermal tempering is a time specification of several minutes. Therefore, it is strongly desired to develop new glass ceramic compositions that can be thermally tempered to enhance their mechanical properties. Summary of the invention

[0007] According to a first aspect, a thermally tempered aluminosilicate glass-ceramic composition comprises a crystalline phase and a residual glass phase, wherein the two phases form a system wherein a thermal expansion curve of the system has two distinct segments emanating from an inflection temperature in the range of about 450° C. to about 600° C. In certain embodiments, the difference between the thermal expansion coefficients of the glass-ceramic below and above the inflection point is greater than about 4 ppm / ° C. In certain embodiments, the difference between the thermal expansion coefficients of the glass-ceramic below and above the inflection point is from about 4 ppm / ° C. to about 10 ppm / ° C.

[0008] In certain embodiments, the coefficient of thermal expansion of the glass-ceramic below the inflection point ranges from 1 ppm / °C to 10 ppm / °C. In certain embodiments, the coefficient of thermal expansion of the glass-ceramic above the inflection point ranges from 6 ppm / °C to 20 ppm / °C. In certain embodiments, the Young's modulus of the thermally tempered aluminosilicate glass-ceramic composition is from 70 GPa to 110 GPa. In certain embodiments, the crystalline phase of the composition comprises a main crystalline phase or a dominant crystalline phase selected from the group consisting of mullite, fluorphlogopite, and β-spodumene solid solution.

[0009] In certain embodiments, the precursor glass of the thermally tempered aluminosilicate glass ceramic composition comprises, in terms of mole percent of oxides: about 65% to about 75% SiO 2 ; about 8% to about 13% Al 2 O 3 ; about 3% to about 13% Li 2 O; about 0.02% to about 5% B 2 O 3 ; about 0.5% to about 2% K 2 O; about 0% to about 2% BaO; and about 2% to about 6% RO 2 , where RO 2 From about 1% to about 4% TiO 2 , about 0% to about 2% ZrO 2 and about 0% to about 1% SnO 2 constitute.

[0010] In certain embodiments, the precursor glass of the thermally tempered aluminosilicate glass ceramic composition comprises, in terms of mole percent of oxides: about 55% to about 65% SiO 2 ; about 13% to about 19% Al 2 O 3 ; about 0% to about 4% Li 2 O; about 12% to about 17% B 2 O 3 ; about 1% to about 4% K 2 O; and about 2% to about 8% MgO.

[0011] In certain embodiments, the precursor glass of the thermally tempered aluminosilicate glass ceramic composition comprises, by weight percent of oxides: about 40% to about 55% SiO 2 ; about 12% to about 20% Al 2 O 3 ; about 10% to about 18% MgO; about 4% to about 8% F; about 5% to about 10% B 2 O 3 ; about 0% to about 2% BaO; about 0% to about 2% ZrO 2 ; and from about 0% to about 16% R 2 O, where R 2 O from about 5% to about 13% K 2 O, about 0% to about 2% Li 2 O and about 0% to about 2% Na 2 O composition.

[0012] According to the second aspect, a method for thermally tempering a glass-ceramic composition comprising a crystalline phase and a residual glass phase comprises: heating the glass-ceramic composition to a temperature between an annealing point and a softening point of the residual glass phase to produce a heated glass-ceramic composition; and rapidly cooling the heated glass-ceramic composition to a temperature of about 250°C to about -40°C by contacting it with a quenching medium to provide a thermally tempered glass-ceramic.

[0013] In certain embodiments, the heated glass-ceramic composition is cooled to produce a temperature difference of at least about 200°C between the outer surface of the glass-ceramic composition and the center of the glass composition. In certain embodiments, the quenching medium is selected from the group consisting of vegetable oil, water, glycols, and liquid nitrogen, or a combination thereof. In certain embodiments, the quenching medium is a vegetable oil selected from the group consisting of peanut oil, high oleic sunflower oil, rapeseed oil, soybean oil, corn oil, olive oil, sunflower oil, safflower oil, cottonseed oil, and a combination thereof. In certain embodiments, the quenching medium is maintained at a temperature of about 10°C to about 50°C before contacting the heated glass-ceramic. In certain embodiments, the glass composition is heated to a temperature of about 750°C to about 950°C for a time range of 6 minutes to about 4 hours to produce a heated glass-ceramic composition. In certain embodiments, the method further comprises performing an ion exchange process on the heat-tempered glass-ceramic, thereby producing a compressive stress layer in addition to the compressive stress produced by heat tempering in the outer surface region of the glass-ceramic.

[0014] According to a third aspect, a method for thermally tempering a glass-ceramic composition comprising a crystalline phase and a residual glass phase comprises: heating the glass-ceramic composition to a temperature of about 700° to about 1000° C. to produce a heated glass-ceramic composition; and rapidly cooling the heated glass-ceramic composition to a temperature of about 250° C. to about −40° C. by contacting it with a quenching medium to provide a thermally tempered glass-ceramic. In certain embodiments, the glass-ceramic composition is a glass plate having a thickness of about 1 mm to 5 mm.

[0015] According to a fourth aspect, an article comprises a thermally tempered aluminosilicate glass-ceramic composition, a crystalline phase and a residual glass phase, wherein the two phases form a system wherein the thermal expansion curve of the system has two distinct segments emanating from an inflection temperature in the range of about 450°C to about 600°C. In certain embodiments, the difference between the coefficient of thermal expansion of the glass-ceramic article below and above the inflection point is greater than about 4 ppm / °C. In certain embodiments, the difference between the coefficient of thermal expansion of the glass-ceramic article below and above the inflection point is about 4 ppm / °C to about 10 ppm / °C. In certain embodiments, the glass-ceramic article comprises a surface and has a compressive stress greater than about 60 MPa at the surface of the glass-ceramic. In certain embodiments, the compressive stress at the surface of the glass-ceramic is about 60 MPa to about 330 MPa. In certain embodiments, the article comprises: an electronic device, an automotive device, a building device, or an electrical device.

[0016] The foregoing summary is merely illustrative and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments, and features described above, further aspects, embodiments, and features will become apparent by reference to the following drawings and detailed descriptions. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A and 1B represent X-ray diffraction of an exemplary glass-ceramic (AX) of the present technology, wherein, Figure 1 A shows β-spodumene solid solution, rutile, ZrTiO 4 and residual glass, and Figure 1 B shows a picture showing, in magnified format, a glassy halo corresponding to the residual glass present in the glass-ceramic.

[0018] Figure 2 X-ray diffraction of another exemplary glass-ceramic (ESS) representing glass-ceramics of the present technology having a mullite solid solution as the primary or dominant crystalline phase.

[0019] Figure 3The bar graph of FIG. 1 shows failure strength values ​​of thermally tempered glass-ceramics versus untempered glass-ceramics of the present technology according to one or more embodiments shown and described herein.

[0020] Figure 4 Represents ring-on-ring results for a mullite glass-ceramic according to one or more embodiments shown and described herein.

[0021] Figure 5 Represents a method according to one or more embodiments shown and described herein. Ring-on-ring results for glass ceramics.

[0022] Figure 6 Thermal expansion curves are represented for a glass-ceramic material containing a β-spodumene solid solution as the primary or predominant crystalline phase according to one or more embodiments shown and described herein.

[0023] Figure 7 Thermal expansion curves are represented for glass-ceramic materials containing a mullite solid solution as the primary or predominant crystalline phase according to one or more embodiments shown and described herein.

[0024] Figure 8 Represents a commercial product according to one or more of the embodiments shown and described herein. Thermal expansion curve of glass ceramics. DETAILED DESCRIPTION

[0025] Various embodiments are described below. It should be noted that the specific embodiments are not intended to be exhaustive descriptions or limitations on the broader aspects discussed herein. An aspect described in conjunction with a specific embodiment is not necessarily limited to that embodiment and can be practiced for any other embodiment.

[0026] Those skilled in the art will appreciate that, as used herein, "about" will vary to some extent depending on the context in which it is used. If the use of the term is not clear to one skilled in the art considering the context in which it is used, "about" will mean up to plus or minus 10% of the term.

[0027] The terms "one" and "a kind of" and similar expressions such as "the" used in describing elements (especially in the content of the claims) should be interpreted as covering both the singular and the plural, unless otherwise stated or clearly indicated to the contrary. The statement of the numerical range herein is intended only as a shorthand method, individually representing each independent value falling within the range, unless otherwise stated, otherwise each independent value is included in the specification as if they were individually stated herein. Unless otherwise stated or clearly indicated to the contrary, all methods described herein can be performed in any suitable order. Unless otherwise stated, any and all embodiments provided herein, or the use of exemplary language (e.g., "for example") are intended only to better illustrate the implementation method, rather than to limit the scope of the claims. All language in the specification should not be understood as requiring any element not in the claims.

[0028] As used herein, the phrase "and / or" used in the specification and claims should be understood to mean "either or both" of the associated elements, i.e., elements that are associated in some cases and unassociated in other cases. With the "and / or" clause, other elements may optionally be present in addition to the specifically specified elements, whether or not they are related or unrelated to those specifically specified. As non-limiting examples, reference to "X and / or Y" may refer to only X (optionally including elements other than Y) in one embodiment; may refer to only Y (optionally including elements other than X) in another embodiment; may refer to both X and Y (optionally including other elements) in another embodiment.

[0029] When the composition herein is given in the range of 0-Z mol %, this range refers to the amount of material added to the batch, and excludes the contamination level of the same material. As will be appreciated by those skilled in the art, for example, metals of contamination magnitude are often found in prepared glass and glass-ceramic products, such as sodium and iron. Therefore, it is to be understood that in those cases where no material is specifically added to the batch, any such material that may be present in the analytical sample of the final glass-ceramic material is a contaminant material. Except that the contaminant level is generally about 0.03 mol % (300ppm) level of iron oxide, the contaminant level is less than 0.005 mol % (50ppm). The term "substantially consisting of ... " is interpreted as the contaminant level that does not include any material.

[0030] As used herein, the term "heat-tempered" is understood to mean heat-treated, for example by heated solutions or hot gases. The term also includes precursor compositions that are capable of being heat-tempered.

[0031] As used herein, the term "inflection point" is understood to be a point in a thermal expansion curve where a change in slope is observed. For example, a glass-ceramic composition or article may exhibit two distinct segments emanating from an inflection point, such that one segment of the curve represents thermal expansion below or before the inflection point, while the other segment represents thermal expansion above or after the inflection point.

[0032] As used herein, the terms "ceramicizing" and "heat treating" are used interchangeably, and the terms "ceramicizing" and "heat treating" are also used interchangeably and include heat treating a precursor glass to form a glass-ceramic.

[0033] As used herein, the term "major or predominant crystalline phase" means that such crystalline phase constitutes the largest weight % of all crystalline phases in the thermally tempered glass-ceramic described herein.

[0034] The present disclosure provides a new class of heat-tempered glass-ceramics (GC). The glass-ceramics include a crystalline phase with a low coefficient of thermal expansion (CTE) and a residual glass composition with a high CTE, which combination results in a useful degree of heat tempering as confirmed by mechanical evaluation. The high mechanical strength of the heat-tempered glass-ceramics of the present technology is achieved in part by engineering the residual glass to have a high CTE. The resulting profile is approximately parabolic, with a compression depth of about 20% or more of the total thickness.

[0035] composition

[0036] Various aspects and / or embodiments of the present disclosure relate to glass-ceramics, precursor glass compositions and / or glass-ceramic articles that are suitable for thermal tempering or that are thermally tempered. Other aspects and / or embodiments relate to articles comprising thermally temperable glass-ceramics and / or precursor glass compositions. Thermally tempered glass-ceramics may include aluminosilicate glass-ceramics. Thermally tempered glass-ceramic materials may include β-spodumene, mullite, fluorphlogopite crystalline phases or combinations thereof as the primary or dominant crystalline phase. Depending on the composition, thermally tempered glass-ceramics, precursor glass compositions and / or glass-ceramic articles may be characterized as transparent, translucent and / or opaque.

[0037] In one aspect, provided herein is a thermally tempered aluminosilicate glass ceramic or glass ceramic composition comprising two phases, i.e., a crystalline phase and a residual glass phase. In various embodiments, the glass ceramic comprises a low CTE crystalline phase and a high CTE residual glass phase. In various embodiments, the system formed by the two phases of the thermally tempered glass ceramic is such that the thermal expansion curve of the system has two different sections radiating from an inflection point temperature in the range of about 450°C to about 600°C. In various embodiments, the difference between the thermal expansion coefficients of the glass ceramic below and above the inflection point is greater than about 4ppm / °C.

[0038] The system formed by these two phases (i.e., crystalline phase and residual glass phase) of heat-tempered glass-ceramics makes the thermal expansion curve of the system have two different sections diverging from the inflection point. The thermal expansion below this inflection point is the thermal expansion of glass-ceramics (i.e., the weighted average between the CTE of the crystalline phase and the CTE of the residual glass according to their corresponding amount). Above the inflection point (corresponding to the Tg of the residual glass), the increase in thermal expansion is caused by the strong increase of the CTE of the residual glass. Glass-ceramics can be heat-tempered to significantly increase the failure strength compared to the just-made material (e.g., almost 2 times). This is by designing the composition and subsequent phase set to obtain a material with a lower CTE and a residual glass with a high CTE higher than Tg. In one aspect, heat-tempered GC is realized in part by designing the residual glass to have a high thermal expansion coefficient higher than Tg. Without wishing to be limited by theory, it is believed that the low CTE of the glass-ceramics below the inflection point and the high CTE of the residual glass phase higher than the inflection point have obtained a useful degree of heat tempering confirmed by mechanical evaluation. It is observed that the high level of B in the residual glass 2 O 3 It is usually advantageous to increase the high temperature CTE (CTE above Tg) of the residual glass. In the examples given here based on the crystallization of β-spodumene, mullite and fluorphlogopite, respectively, the precursor glass composition contains boron. This element does not enter the crystal (or is present only in small amounts), so that the residual glass is strongly enriched in B. 2 O 3 This is especially true for spodumene glass-ceramics with a relatively small amount of residual glass. 2 O 3 One possible reason for the high CTE differences observed below and above the inflection point is that these materials have lower amounts of residual glass.

[0039] In various embodiments, the thermally tempered glass-ceramic composition has a difference in coefficient of thermal expansion above and below the inflection point in the range of about 4 ppm / °C to about 10 ppm / °C, including but not limited to a CTE difference of about 4.5 ppm / °C to about 9.5 ppm / °C, about 5 ppm / °C to about 9 ppm / °C, about 5.5 ppm / °C to about 8.5 ppm / °C, about 6 ppm / °C to about 8 ppm / °C, or about 7 ppm / °C to about 7.5 ppm / °C, or any two of these values ​​and / or a range of any two of these values.

[0040] In various embodiments, the thermally tempered glass-ceramic has a coefficient of thermal expansion of the glass-ceramic from room temperature to the inflection point in a range of about 0.1 ppm / °C to about 10 ppm / °C. In certain embodiments, the CTE of the glass-ceramic below the inflection point is about 0.2 ppm / °C to about 10 ppm / °C, for example: about 0.4 ppm / °C to about 9 ppm / °C, about 0.4 ppm / °C to about 8 ppm / °C, about 0.4 ppm / °C to about 6 ppm / °C, about 0.4 ppm / °C to about 5 ppm / °C, about 0.4 ppm / °C to about 4 ppm / °C, about 0.5 ppm / °C to about 8 ppm / °C, about 0.5 ppm / °C to about 6 ppm / °C, about 0.5 ppm / °C to about 4 ppm / °C, about 0.6 ppm / °C to about 10 ppm / °C, about 0.6 ppm / °C to about 9 ppm / °C, about 0.6 ppm / °C to about 8 ppm / °C, about 0.6 ppm / °C to about 10 ... ppm / ℃ to about 6ppm / ℃, about 0.7ppm / ℃ to about 9ppm / ℃, about 0.7ppm / ℃ to about 8.0ppm / ℃, about 0.7ppm / ℃ to about 6.0ppm / ℃, about 1ppm / ℃ to about 10ppm / ℃, about 1ppm / ℃ to about 9ppm / ℃, about 1ppm / ℃ to about 8ppm / ℃, about 1ppm / ℃ to about 10ppm / ℃, about 3ppm / ℃ to about 9ppm / ℃, about 3ppm / ℃ to about 8ppm / ℃, about 3ppm / ℃ to about 6ppm / ℃, about 3ppm / ℃ to about 4ppm / ℃, about 8ppm / ℃ to about 9ppm / ℃, or a range including any two of these values ​​and / or any two of these values.

[0041] In various embodiments, the thermally tempered glass-ceramic has a coefficient of thermal expansion range of 4 ppm / °C to 20 ppm / °C above the inflection point. In certain embodiments, the CTE of the glass-ceramic above the inflection point is: about 4 ppm / °C to about 19 ppm / °C, about 4 ppm / °C to about 18 ppm / °C, about 4 ppm / °C to about 15 ppm / °C, about 4 ppm / °C to about 12 ppm / °C, about 4 ppm / °C to about 10 ppm / °C, about 5 ppm / °C to about 20 ppm / °C, for example: about 5 ppm / °C to about 19 ppm / °C, about 5 ppm / °C to about 18 ppm / °C, about 5 ppm / °C to about 17.5 ppm / °C, about 5 ppm / °C to about 12 ppm / °C, about 5 ppm / °C to about 10 ppm / °C, about 6 ppm / °C to about 15 ppm / °C About 20ppm / °C, about 6ppm / °C to about 18ppm / °C, about 6ppm / °C to about 15ppm / °C, about 6ppm / °C to about 10ppm / °C, about 9.5ppm / °C to about 20ppm / °C, about 9.5ppm / °C to about 18.0ppm / °C, about 9.5ppm / °C to about 15.0ppm / °C, about 9.5ppm / °C to about 10ppm / °C, about 16ppm / °C to about 20ppm / °C, about 16ppm / °C to about 19ppm / °C, about 16ppm / °C to about 18ppm / °C, or a range including any two of these values ​​and / or any two of these values.

[0042] In various embodiments, the residual glassy phase of the GC has a coefficient of thermal expansion that is at least 2 ppm / °C higher than the crystalline phase. In certain embodiments, the residual glassy phase has a CTE that is at least 2.5 ppm / °C, at least 3 ppm / °C, at least 3.5 ppm / °C, at least 4 ppm / °C, at least 4.5 ppm / °C, or at least 5 ppm / °C higher than the crystalline phase.

[0043] Depending on the composition, the inflection temperature range of the glass ceramic is about 400°C to about 700°C, such as the following range: about 450°C to about 600°C, about 465°C to about 550°C, or about 500°C to about 550°C, or a range comprising any two of these values ​​and / or any two of these values. In various embodiments, the inflection temperature of the glass ceramic is about 450°C, about 455°C, about 465°C, about 467°C, about 470°C, about 475°C, about 480°C, about 485°C, about 490°C, about 495°C, about 500°C, about 505°C, about 510°C, about 515°C, about 520°C, about 525°C, about 530°C, about 535°C, about 540°C, about 551°C, about 552°C, about 553°C, about 554°C, about 555°C, about 556°C, about 557°C, about 558°C, about 559°C, about 560°C, about 561°C, about 562°C, about 563°C, about 564°C, about 565°C, about 566°C, about 567°C, about 568°C, about 570°C, about 571°C, about 572°C, about 573°C, about 574°C, about 575°C, about 576°C, about 577°C, about 578°C, about 579°C, about 580°C, about 581°C, The temperature may be as follows: 45°C, about 550°C, about 555°C, about 560°C, about 565°C, about 570°C, about 575°C, about 580°C, about 585°C, about 590°C, about 595°C, about 600°C, about 605°C, about 610°C, about 615°C, about 620°C, about 625°C, about 630°C, about 635°C, about 640°C, about 645°C or about 650°C, but is not limited to these.

[0044] Thermal tempering of the glass-ceramic composition results in compressive stress (CS) at the surface. Mechanical properties depend on the stress level and stress layer depth at the surface. In various embodiments, the compressive stress at the glass-ceramic surface of the thermally tempered glass-ceramic composition is greater than about 60 MPa, including but not limited to: greater than about 65 MPa, greater than about 70 MPa, greater than about 75 MPa, or greater than about 80 MPa. In certain embodiments, the thermally tempered glass-ceramic composition has a compressive stress of about 60 MPa to about 330 MPa at the surface of the glass-ceramic, including but not limited to: about 65 MPa to about 320 MPa, about 70 MPa to about 310 MPa, about 75 MPa to about 300 MPa, about 80 MPa to about 280 MPa, about 90 MPa to about 250 MPa, about 100 MPa to about 220 MPa, about 110 MPa to about 200 MPa, about 120 MPa to about 180 MPa, about 130 MPa to about 160 MPa, or about 140 MPa to about 150 MPa, or any two of these values ​​and / or a range comprising any two of these values.

[0045] In certain embodiments, the stress layer depth of the thermally tempered glass-ceramic article is greater than about 15% or greater than about 20% of the total thickness of the thermally tempered glass-ceramic article. In certain embodiments, the stress layer depth of the thermally tempered glass-ceramic article is about 15% to about 50% of the total thickness of the article, including but not limited to about 17% to about 45%, about 18% to about 40%, about 19% to about 35%, about 20% to about 30%, about 20% to about 28%, or about 22% to about 25% of the total thickness of the thermally tempered glass-ceramic article, or any two of these values ​​and / or a range of any two of these values.

[0046] In certain embodiments, the crystalline phase occupies greater than about 10%, greater than about 20%, greater than about 30%, or greater than about 45% of the total weight of the thermally tempered glass-ceramic article. In certain embodiments, the crystalline phase occupies about 20% to about 90% of the total weight of the thermally tempered glass-ceramic article, including but not limited to about 25% to about 85%, about 30% to about 80%, about 35% to about 75%, about 40% to about 70%, about 45% to about 65%, or about 50% to about 60% of the total weight of the thermally tempered glass-ceramic article, or any two of these values ​​and / or a range of any two of these values.

[0047] In certain embodiments, the residual glass phase occupies greater than about 10%, greater than about 20%, greater than about 30%, or greater than about 45% of the total weight of the thermally tempered glass-ceramic article. In certain embodiments, the residual glass phase occupies about 10% to about 80% of the total weight of the thermally tempered glass-ceramic article, including but not limited to about 15% to about 75%, about 20% to about 70%, about 25% to about 65%, about 30% to about 60%, about 35% to about 55%, or about 40% to about 50% of the total weight of the thermally tempered glass-ceramic article, or any two of these values ​​and / or a range of any two of these values.

[0048] In various embodiments, the thermally tempered glass-ceramic composition has a Young's modulus of at least 65 GPa, which minimizes bending of the GC during processing and prevents breakage of devices attached to the GC. In certain embodiments, the thermally tempered glass-ceramic composition has a Young's modulus greater than 65 GPa, greater than 70 GPa, greater than 75 GPa, greater than 80 GPa, greater than 85 GPa, greater than 90 GPa, greater than 95 GPa, or greater than 100 GPa. In certain embodiments, the thermally tempered glass-ceramic composition has a Young's modulus less than 120 GPa, less than 115 GPa, less than 110 GPa, less than 105 GPa, or less than 100 GPa. In some embodiments, the heat-tempered glass-ceramic composition has a Young's modulus of about 70 GPa to about 110 GPa, for example: about 80 GPa to about 100 GPa, about 80 GPa to about 95 GPa, about 80 GPa to about 90 GPa, about 80 GPa to about 85 GPa, 85 GPa to about 100 GPa, about 85 GPa to about 95 GPa, about 85 GPa to about 90 GPa, 90 GPa to about 100 GPa, about 90 GPa to about 95 GPa, 95 GPa to about 100 GPa, or a range including any two of these values ​​and / or any two of these values. However, it is contemplated that the desired properties (including Young's modulus) will vary depending on the specific embodiment, end use, and processing requirements of the heat-tempered glass-ceramic composition. In some embodiments, the glass-ceramic composition has a Young's modulus of 70 GPa to 110 GPa.

[0049] In another aspect, the present technology relates to precursor or base glass compositions and glasses used to form the thermally tempered glass-ceramics described herein.

[0050] In one embodiment, the precursor glass composition for a heat-tempered glass-ceramic may include, in terms of mole % of oxides: SiO 2 , which ranges from about 65 to about 75; Al 2 O 3 , which ranges from about 8 to about 13; Li 2 O, which ranges from about 3 to about 13; B 2 O 3 , which ranges from about 0.02 to about 5; K 2 O, which ranges from about 0.5 to about 2; BaO, which ranges from about 0 to about 2; and RO 2 , which ranges from about 2 to about 6; wherein RO 2 Including: TiO 2 (ranging from about 1 to about 4), ZrO 2 (which ranges from about 0 to about 2) and SnO 2(Its range is from about 0 to about 1).

[0051] In other embodiments, the precursor glass composition for a heat-tempered glass-ceramic may include, by mole % of oxides: SiO 2 , which ranges from about 55 to about 65; Al 2 O 3 , which ranges from about 13 to about 19; Li 2 O, which ranges from about 0 to about 4; B 2 O 3 , which ranges from about 12 to about 17; K 2 O, which ranges from about 1 to about 4; MgO, which ranges from about 2 to about 8.

[0052] In another embodiment, the precursor glass composition for a heat-tempered glass-ceramic may include, by weight % of oxides: SiO 2 , which ranges from about 40 to about 55; Al 2 O 3 , which ranges from about 12 to about 20; MgO, which ranges from about 10 to about 18; B 2 O 3 , which ranges from about 5 to about 10; F, which ranges from about 4 to about 8; BaO, which ranges from about 0 to about 2; ZrO 2 , which ranges from about 0 to about 2; and, R 2 O, which ranges from about 0 to about 16; wherein R 2 O includes: K 2 O (ranging from about 5 to about 13), Li 2 O (which ranges from about 0 to about 2), and Na 2 O (which ranges from about 0 to about 2). In certain embodiments, the heat-tempered glass-ceramic comprises or consists of, by weight percent of oxides: 25-60% SiO 2 , 15-35% R 2 O 3 (Among them, R 2 O 3 3-15% B 2 O 3 and 5-25% Al 2 O 3 Composition), 4-25MgO+0-7%Li 2 O(MgO+Li 2 O total about 6-25%), 2-20% R 2 O(where R 2 O consists of 0-15% Na 2 O, 0-15% K 2 O, 0-15% Rb2 O and 0-20% Cs 2 O), and 4-20% F. In some embodiments, the heat-tempered glass-ceramic comprises or consists of, in terms of mole % of oxides: SiO 2 42.2%SiO 2 , 6.6% B 2 O 3 , 8.8%Al 2 O 3 , 19.3% MgO, 17.8% F, and 5.4% K 2 O.

[0053] In certain embodiments, the precursor glass for the heat-tempered glass-ceramic comprises or consists of, in terms of mole % of oxides: 65 to 75% SiO 2 , 8 to 13Al 2 O 3 , 3 to 13% Li 2 O, 0.02 to 5% B 2 O 3 , 0.5 to 2% K 2 O, 0 to 2% BaO, 1 to 4% TiO 2 ,0 to 2%ZrO 2 , and 0 to 1% SnO 2 , wherein the main crystalline phase or the dominant crystalline phase of the glass ceramic includes β-spodumene.

[0054] In certain embodiments, the precursor glass for the heat-tempered glass-ceramic comprises or consists of, in terms of mol % of oxides: 55 to 65% SiO 2 , 13 to 19% Al 2 O 3 , 0 to 4% Li 2 O, 12 to 17% B 2 O 3 , 1 to 4% K 2 O, and 2 to 8% MgO, wherein the main crystalline phase or the dominant crystalline phase of the glass-ceramic is mullite.

[0055] In other embodiments, the heat-tempered glass-ceramic comprises or consists of, in weight percent of oxides: 40 to 55% SiO 2 , 12 to 20% Al 2 O 3 , 10 to 18% MgO, 4 to 8% F, 5 to 10% B 2 O 3 , 0 to 2%BaO, 0 to 2%ZrO 2 , 5 to 13% K2 O, 0 to 2% Li 2 O, and 0 to 2% Na 2 O, and wherein the main crystalline phase or the dominant crystalline phase of the glass ceramic is fluorophlogopite.

[0056] In certain embodiments, SiO 2 Thus, in certain embodiments, in the heat-tempered glass-ceramics, precursor glass compositions, and / or glass-ceramic articles comprising such compositions described herein, the SiO present, in mole percent, may be present as the primary glass-forming oxide. 2 Can be in the range of about 35 to about 80, including: about 35 to about 45, about 40 to about 60, about 40 to about 55, about 40 to about 50, about 50 to about 70, about 50 to about 65, about 50 to about 60, about 55 to about 80, about 55 to about 75, about 55 to about 65, about 55 to about 60, about 60 to about 80, about 60 to about 75, about 60 to about 70, about 60 to about 65, about 65 to about 80, about 65 to about 75, about 65 to about 80, about 65 to about 70, about 70 to about 80, about 70 to about 75, or about 75 to about 80, or any range including and / or between any two of these values.

[0057] The heat-tempered glass-ceramic, precursor glass composition and / or glass-ceramic article may or may not contain Al. 2 O 3 Thus, in certain embodiments, in the heat-tempered glass-ceramics, precursor glass compositions, and / or glass-ceramic articles comprising such compositions described herein, the presence of Al is, by mole %. 2 O 3 Can be from about 0 to about 25 range, including: about 5 to about 25, about 8 to about 20, about 8 to about 15, about 8 to about 13, about 8 to about 10, about 10 to about 20, about 10 to about 15, about 12 to about 25, about 12 to about 20, about 12 to about 15, about 13 to about 25, about 13 to about 20, about 13 to about 18, or about 13 to about 15, or any range including any two of these values ​​and / or between any two of these values.

[0058] In certain embodiments, the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article comprises one or more alkali metal oxides or basic oxides (e.g., Li 2 O、Na 2 O or K 2 O, etc.), in mole %, the total amount of their presence (i.e., Na 2 O+K 2 O+Li 2O) is as follows: about 0 to about 20, about 0 to about 16, about 0 to about 5, about 0 to about 2, about 0 to about 1, about 1 to about 15, about 1 to about 10, about 1 to about 5, about 1 to about 4, about 2 to about 15, about 2 to about 10, about 2 to about 6, about 4 to about 12, about 4 to about 10, about 4 to about 6, about 5 to about 20, about 5 to about 15, about 5 to about 13, about 5 to about 10, about 8 to about 20, or about 8 to about 15, or any range including any two of these values ​​and / or between any two of these values. The alkali oxides aid in the melting of the glass composition and lower the softening point of the glass, thereby offsetting the increase in the melting temperature due to the higher SiO in the glass composition. 2 and / or Al 2 O 3 The concentration of the basic oxides also helps to adjust the CTE to the desired value.

[0059] In certain embodiments, the alkaline oxide present in the heat-tempered glass-ceramic, precursor glass composition, and / or glass-ceramic article is Na 2 O, in mole %, can be present in an amount ranging from about 0 to about 20, about 2 to about 20, about 3 to about 20, about 5 to 20, about 1 to about 15, about 2 to about 15, about 3 to about 15, about 5 to about 15, about 8 to about 15, about 1 to about 10, about 2 to about 10, about 3 to about 10, about 5 to about 10, about 8 to about 10, about 1 to about 8, about 2 to about 8, about 3 to about 8, about 4 to about 8, about 5 to about 8, about 6 to about 8, about 7 to about 8, about 1 to about 5, about 2 to about 5, about 2 to about 4, about 0 to about 5, about 0 to about 4, about 0 to about 3, or about 0 to about 2, or any range including and / or between any two of these values.

[0060] In certain embodiments, the alkaline oxide present in the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article is K 2O, in mole %, can be present in an amount ranging from about 0 to about 20, about 1 to about 20, about 2 to about 20, about 3 to about 20, about 5 to 20, about 0 to about 15, about 1 to about 15, about 2 to about 15, about 3 to about 15, about 5 to about 15, about 8 to about 15, about 0 to about 10, about 1 to about 10, about 2 to about 10, about 3 to about 10, about 4 to about 10, about 5 to about 10, about 8 to about 10, about 0 to about 8, about 1 to about 8, about 2 to about 8, about 3 to about 8, about 4 to about 8, about 5 to about 8, about 6 to about 8, about 7 to about 8, about 2 to about 7, about 2 to about 6, about 2 to about 5, about 2 to about 4, about 2 to about 3, about 1 to about 4, about 1 to about 3, about 1 to about 2, about 0 to about 4, about 0 to about 3, or about 0 to about 2, or any range including and / or between any two of these values.

[0061] In certain embodiments, the alkaline oxide present in the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article is Li 2 O, in mole %, can be present in an amount ranging from about 0 to about 20, including: about 1 to about 20, about 2 to about 20, about 3 to about 20, about 5 to 20, about 0 to about 15, about 1 to about 15, about 2 to about 15, about 3 to about 15, about 5 to about 15, about 8 to about 15, about 0 to about 13, about 1 to about 13, about 2 to about 13, about 3 to about 13, about 4 to about 13, about 5 to about 13, about 8 to about 13, about 0 to about 8, about 1 to about 8, about 2 to about 8, about 3 to about 8, about 4 to about 8, about 5 to about 8, about 6 to about 8, about 7 to about 8, about 2 to about 7, about 2 to about 6, about 2 to about 5, about 2 to about 4, about 2 to about 3, about 1 to about 4, about 1 to about 3, about 1 to about 2, about 0 to about 4, about 0 to about 3, or about 0 to about 2, or any range including and / or between any two of these values. In certain embodiments, Li 2 O serves as the main alkaline substance during the thermal tempering process.

[0062] The heat-tempered glass-ceramic, precursor glass composition and / or glass-ceramic article may or may not contain MgO. Thus, in certain embodiments, the heat-tempered glass-ceramic, precursor glass composition and / or glass-ceramic article contains MgO, which may be present in an amount, in mole percent, in the range of about 0 to about 25, about 2 to about 20, about 2 to about 15, about 2 to about 10, about 2 to about 6, about 2 to about 5, about 2 to about 4, about 4 to about 20, about 4 to about 15, about 4 to about 10, about 4 to about 6, about 10 to about 25, about 10 to about 20, about 10 to about 18, about 10 to about 15, about 15 to about 20, or about 15 to about 18, or any range including and / or between any two of these values.

[0063] In certain embodiments, the heat-tempered glass-ceramic, precursor glass composition, and / or glass-ceramic article may optionally include B 2 O 3 For example, in mol%, B 2 O 3 The amount present can be in a range of about 0 to about 20, including: about 0.01 to about 10, about 0.01 to about 5, about 0.02 to about 10, about 0.02 to about 5, about 0.02 to about 4, about 0.02 to about 2, about 0.1 to about 10, about 0.1 to about 5, about 0.1 to about 2, about 1 to about 10, about 1 to about 5, about 5 to about 20, about 5 to about 15, about 5 to about 10, about 10 to about 20, about 10 to about 15, about 10 to about 12, about 12 to about 20, about 12 to about 18, about 12 to about 16, about 12 to about 15, about 15 to about 20, about 15 to about 18, or any range including and / or between any two of these values.

[0064] In certain embodiments, the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article comprises one or more transition metal oxides or post-transition metal oxides R 2 O (e.g., TiO 2 、ZrO 2 SnO 2 ), which are present in an amount, in mole %, in the range of about 0 to about 20, about 0 to about 16, about 0 to about 5, about 0 to about 2, about 0 to about 1, about 1 to about 15, about 1 to about 10, about 1 to about 5, about 1 to about 4, about 2 to about 15, about 2 to about 10, about 2 to about 6, about 4 to about 12, about 4 to about 10, about 4 to about 6, about 5 to about 20, about 5 to about 15, about 5 to about 13, about 5 to about 10, about 8 to about 20, or about 8 to about 15, or any range including and / or between any two of these values.

[0065] In certain embodiments, the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article comprises TiO 2 , which can be present in an amount, in mole %, ranging from about 0 to about 15, about 0 to about 10, about 0 to about 5, about 0 to about 2, about 0 to about 1, about 1 to about 15, about 1 to about 10, about 1 to about 5, about 1 to about 4, about 1 to about 3, about 2 to about 15, about 2 to about 10, about 2 to about 6, about 4 to about 12, about 4 to about 10, about 4 to about 6, about 10 to about 15, about 5 to about 15, about 5 to about 13, or about 5 to about 10, or any range including and / or between any two of these values.

[0066] In certain embodiments, the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article comprises ZrO 2 , in mole %, which can be present in an amount ranging from about 0 to about 10, from about 0 to about 8, from about 0 to about 7, from about 0 to about 6, from about 0 to about 5, from about 0 to about 4, from about 0 to about 3.5, from about 0 to about 3, from about 0 to about 2.5, from about 0 to about 2, from about 0 to about 1.5, from about 0 to about 1, from about 0 to about 0.5, from about 0.1 to about 5, from about 0.1 to about 4, from about 0.1 to about 3.5, from about 0.1 to about 3, from about 0.1 to about 2.5, from about 0.1 to about 2, from about 0.1 to about 1.5, from about 0.1 to about 1, from about 0.5 to about 4.5, from about 1 to about 4, from 1.5 to about 3.5, or from about 2 to about 3, or any range including and / or between any two of these values.

[0067] In certain embodiments, the thermally temperable glass-ceramic, precursor glass composition, and / or glass-ceramic article comprises SnO 2 , which can be present in an amount of about 0 to about 10, including: about 0.01 to about 10, about 0.01 to about 5, including: about 0.01 to about 1, about 0.02 to about 10, about 0.02 to about 5, about 0.02 to about 4, about 0.02 to about 2, about 0.02 to about 1, about 0.1 to about 10, about 0.1 to about 5, about 0.1 to about 2, about 0.1 to about 1, about 0.5 to about 10, about 0.5 to about 5, about 0.5 to about 2, or about 0.5 to about 1, or any range including any two of these values ​​and / or between any two of these values.

[0068] In certain embodiments, the heat temperable glass-ceramic, precursor glass composition and / or glass-ceramic article comprises F, which may be present in an amount, in mole %, of about 1 to about 12, including: about 1 to about 10, about 1 to about 8, about 1 to about 7, about 1 to about 6, about 1 to about 5, about 1 to about 4, about 2 to about 9, about 2 to about 8, about 3 to about 8, about 3 to about 6, about 3 to about 4, about 4 to about 10, about 4 to about 9, about 4 to about 8, about 4 to about 7, about 4 to about 6, about 4 to about 5, about 5 to about 10, about 5 to about 9, about 5 to about 8, about 5 to about 7, about 5 to about 6, about 6 to about 10, about 6 to about 9, about 6 to about 8, about 6 to about 7, about 7 to about 8, or any range comprising and / or between any two of these values.

[0069] In certain embodiments, the main or dominant crystalline phase may be such that it includes a main crystalline phase selected from the group consisting of mullite, fluorphlogopite and β-spodumene, β-quartz solid solution, or a combination thereof. For example, in certain embodiments, the β-spodumene crystalline phase includes the main or dominant crystalline phase in a heat-tempered glass-ceramic article. In other embodiments, the mullite crystalline phase may include the main or dominant crystalline phase in a heat-tempered glass-ceramic article. In other embodiments, the fluorphlogopite crystalline phase may include the main or dominant crystalline phase in a heat-tempered glass-ceramic article. In other embodiments, the β-quartz crystalline phase may include the main or dominant crystalline phase in a heat-tempered glass-ceramic article. In one or more embodiments, the glass-ceramic composition described herein may be heat-tempered. In one or more embodiments, the glass-ceramic composition described herein is heat-tempered. In one or more embodiments, the glass-ceramic composition includes or is composed of heat-tempered glass-ceramic.

[0070] An example of a commercially available machinable glass is fluorophlogopite. (Corning Incorporated, Corning, NY, USA.) The Macor microstructure consists of 55% fluorophlogopite mica and 45% borosilicate glass. Offers a unique combination of properties in that it is a non-wetting, white, odorless, non-outgassing material that exhibits zero porosity. Provides tight tolerance capabilities, enabling complex geometry designs (best performance dimensions up to + / - 0.013mm, <0.5μm for finished surfaces, and up to 0.013μm for polished surfaces). It remains stable at 800°C, with a peak of 1000°C under no-load conditions, and unlike ductile materials, it does not creep or deform. Its coefficient of thermal expansion is easily matched to most metals and sealing glasses. As an electrical insulator (especially at high temperatures), it is excellent at high voltages and over a wide frequency spectrum. However, the mechanical strength of this material is not outstanding and can be improved by thermal tempering methods as described herein.

[0071] In another aspect, an article is provided comprising the heat-tempered or heat-tempered glass-ceramic disclosed herein. In another aspect, an article is provided comprising a heat-tempered glass-ceramic comprising, in mole percent of oxides: 50 to 70% SiO 2 , 0 to 20% Al 2 O 3 , 12 to 23% MgO, 0 to 4% Li 2 O, 0 to 10% Na 2 O, 0 to 10% K 2 O, 0 to 5% ZrO 2 , and 2 to 12% F, wherein the main crystalline phase or the dominant crystalline phase of the glass-ceramic is β-spodumene.

[0072] In another aspect, an article provided herein comprises the thermally tempered glass-ceramic described herein.

[0073] method

[0074] Another aspect of the technology herein relates to methods for producing the thermally tempered glass-ceramics, precursor glass compositions, and / or thermally tempered glass-ceramic articles as described herein.

[0075] Aspects of the technology herein relate to methods for making thermally tempered glass-ceramics. In various embodiments, a method for thermally tempering a glass-ceramic article comprising a crystalline phase and a residual glass phase comprises heating the glass-ceramic article to a temperature between an annealing point and a softening point of the residual glass phase to produce a heated glass-ceramic article, and rapidly cooling the heated glass-ceramic article to provide a thermally tempered glass-ceramic article. In various embodiments, thermal tempering is performed on a fully ceramized glass material, i.e., after ceramization and cooling of the ceramized glass material.

[0076] In various embodiments, the heated glass-ceramic product can be rapidly cooled by contacting the heated glass-ceramic with a quenching or cooling medium. Suitable quenching medium is a substance that provides a higher average heat transfer coefficient over the entire temperature range used in the annealing process. The quenching medium can be a liquid, a solid or a gas. Suitable gaseous quenching medium can include cooling air or carbon dioxide gas. Suitable liquid quenching media include, but are not limited to: oils, water, glycols and liquid nitrogen, etc., or a combination thereof. In certain embodiments, the liquid quenching medium includes vegetable oil. In certain embodiments, the vegetable oil is selected from the group consisting of peanut oil, high oleic sunflower oil, rapeseed oil, soybean oil, corn oil, olive oil, sunflower oil, safflower oil and cottonseed oil, etc., or a combination thereof. In certain embodiments, the quenching medium includes peanut oil. In certain embodiments, the heated glass-ceramic product can be contacted with a quenching medium by immersing or submerging the GC product in a bath of a liquid quenching medium or by spraying or atomizing the quenching medium onto the GC product.

[0077] In various embodiments of the thermal tempering method of glass ceramics, the glass ceramics are first heated to a high temperature (usually between the annealing point and the softening point of the residual glass phase), for example, close to the softening point of the residual glass in the specific GC of the annealing. The softening point temperature of the glass will vary depending on the specific composition of the glass phase of the GC. For example, in a borosilicate glass composition, the softening temperature will be about 815°C (1500°F). Therefore, the glass ceramics can be heated to a suitable temperature, for example, from about 600° to about 1100°C to produce a heated glass ceramic article. In certain embodiments, the GC is heated to a temperature range of about 700 to about 1000°C as follows, for example: from about 730°C to about 960°C, from about 750 to about 950°C, or from about 800°C to about 900°C, or any range comprising any two of these values ​​and / or between any two of these values. In certain embodiments, the GC is heated to a temperature of about 700°C, about 710°C, about 720°C, about 730°C, about 740°C, about 750°C, about 760°C, about 770°C, about 780°C, about 790°C, about 800°C, about 810°C, about 820°C, about 830°C, about 840°C, about 850°C, about 860°C, about 870°C, about 880°C, about 890°C, about 900°C, about 910°C, about 920°C, about 930°C, about 940°C, about 950°C, about 960°C, about 970°C, about 980°C, about 990°C, or about 1000°C.

[0078] In various embodiments, the glass ceramic is heated to a temperature range of about 750° C. to about 950° C. for a suitable time to produce a heated glass ceramic article. Suitable heating time ranges are about 5 minutes to about 4 hours, for example: about 10 minutes to about 3.5 hours, about 15 minutes to about 3 hours, about 30 minutes to about 2.5 hours, about 45 minutes to about 2 hours, or about 1 hour to about 1.5 hours, or any range comprising any two of these values ​​and / or between any two of these values.

[0079] After the GC is heated to an elevated temperature, it is rapidly cooled by immediate contact with a quenching medium, where heat is exchanged between the surface of the GC and the quenching medium to provide a thermally tempered glass-ceramic. In certain embodiments, the heated glass-ceramic is rapidly cooled to a temperature of about 250°C to about -40°C by contacting it with the quenching contact. In certain embodiments, the heated glass-ceramic is rapidly cooled to a temperature in the range of about 250°C to about -40°C, for example: about 225°C to about -30°C, about 200°C to about -20°C, about 150°C to about -10°C, about 100°C to about 0°C, for example: about 80°C to about 10°C, about 60°C to about 15°C, or about 50°C to about 25°C, or any range comprising any two of these values ​​and / or between any two of these values.

[0080] The quenching medium is maintained at a temperature range of about 10°C to about 50°C before it contacts the heated glass-ceramic. In certain embodiments, the quenching medium is maintained at a temperature range of about 10°C to about 50°C before it contacts the heated glass-ceramic, for example: about 15°C to about 45°C, about 20°C to about 40°C, about 25°C to about 35°C, or about 28°C to about 30°C, or any range comprising any two of these values ​​and / or between any two of these values. In certain embodiments, the quenching medium is maintained at room temperature before it contacts the heated glass-ceramic. In certain embodiments, the quenching medium is maintained at a temperature of about 25°C before it contacts the heated glass-ceramic.

[0081] The temperature range used in the annealing process is defined based on the GC surface temperature from an upper limit temperature near its softening point to a lower limit surface temperature that reaches down to the interior of the glass and has cooled through the glass strain point. As used herein, the glass strain point is the state when the glass has a viscosity of 10^14.5 poise. When the glass has cooled through the strain point throughout its thickness, the glass has achieved the final annealing degree. Where σ = surface compression, E = Emod (GPa), ν is Poisson's ratio, and ΔL / L is the average temperature from T 0 and T q The CTE curve at T 0is the heating temperature for annealing, and T q Taken from the point in the CTE curve where the slope changes.

[0082] The rapid quenching rate results in a temperature gradient across the GC article. The article surface cools faster than the interior, causing the surface to shrink while the interior remains hot. Eventually, the core cools, but its shrinkage is resisted by the solid outer surface. These temperature differences and the accompanying shrinkage differences then lead to compressive stresses at the surface and balanced tensile stresses in the center. The stress profile replicates the quenching heat profile, which is a good approximation to a parabola. The degree of annealing depends on: article thickness (t), heating temperature T 0 The temperature difference between the quench temperature (ΔT = T 0 -T q ), quench rate, thermal conductivity of the material, and thermal expansion (CTE) and Young's modulus (Emod) and Poisson's ratio of the glass in the GC composition.

[0083] In various embodiments, the glass-ceramic has a thickness of about 1 to about 5 millimeters (mm), including: about 1.2 mm to about 4.8 mm, about 1.5 mm to about 4.5 mm, about 1.8 mm to about 4.0 mm, about 2 mm to about 3.8 mm, about 2.5 mm to about 3.5 mm, or about 2.8 mm to about 3.0 mm, or any range comprising any two of these values ​​and / or between any two of these values. In some embodiments, the glass-ceramic has a thickness of about 3 mm.

[0084] In the present technology, residual glass in GC is advantageously used to induce annealing stresses in GC. Cooling stresses are arranged in multiphase materials (e.g., glass-ceramics) when they are cooled from high temperature. These stresses come from the CTE mismatch between different phases and manifest as local stress fields in the material near and at the phase interfaces. Both microscopic and macroscopic annealing stresses are introduced during the tempering process, resulting in compression at the surface and equilibrium tension inside.

[0085] After the heat tempering treatment, the glass ceramic can be further processed by any conventional method known in the present invention, such as removing the quenching medium, cleaning, drying, and forming the heat tempered GC material into a desired shape. In some embodiments, the heat tempered GC can be ion exchanged to achieve a higher compression amount at the surface of the component. In some embodiments, the ion exchange process of the heat tempered glass ceramic can produce a compressive stress layer in the outer surface area of ​​the glass ceramic in addition to the compressive stress generated by the heat tempering. Ion exchange is usually carried out in a molten salt bath. For example, any nitrate bath, sulfate bath and halide bath (pure or mixed) can be used in a sodium and / or potassium bath to ion exchange the heat tempered glass ceramic material. The typical temperature of ion exchange is 390°C to 500°C, but in some embodiments, a temperature higher than 500°C can also be used. The duration of ion exchange can be a short time (e.g., about 10 minutes) to a longer time (about 20 hours).

[0086] In certain embodiments, the thermally tempered GC may be ion exchanged to impart a higher level of compressive stress on the surface. In certain embodiments, the thermally tempered GC may be ion exchanged to impart a compressive stress of about 80 to about 800 MPa, including but not limited to about 100 to about 750 MPa, about 150 to about 700 MPa, about 200 to about 650 MPa, about 250 to about 600 MPa, about 300 to about 550 MPa, about 350 to about 500 MPa, about 400 to about 450 MPa, or any range comprising any two of these values ​​and / or between any two of these values. In certain embodiments, the thermally tempered GC may be ion exchanged to impart a high compressive stress having a layer depth of about 1 to about 40 microns, including but not limited to about 2 to about 38 microns, about 5 to about 35 microns, about 10 to about 30 microns, about 15 to about 25 microns, about 10 to about 20 microns, or any range comprising any two of these values ​​and / or between any two of these values.

[0087] Glass-ceramics for a thermal tempering process can be produced by a method comprising: melting a batch of precursor glass at a suitable temperature in a suitable melting apparatus for a period of time sufficient to melt the batch of precursor glass; annealing and ceramicizing the molten glass at a suitable growth temperature; and optionally cooling the glass-ceramic to room temperature.

[0088] The precursor or base glass is as disclosed herein and may comprise, in mole % of oxides: 65 to 75% SiO 2 , 8 to 13Al 2 O 3 , 3 to 13% Li 2O, 0.02 to 5% B 2 O 3 , 0.5 to 2% K 2 O, 0 to 2% BaO, 1 to 4% TiO 2 ,0 to 2%ZrO 2 and 0 to 1% SnO 2 ; or 55 to 65% SiO 2 , 13 to 19% Al 2 O 3 , 1 to 4% Li 2 O, 12 to 17% B 2 O 3 , 1 to 4% K 2 O, and 2 to 7% MgO; or 40 to 55% SiO 2 , 12 to 20% Al 2 O 3 , 10 to 18% MgO, 4 to 8% F, 5 to 10% B 2 O 3 , 0 to 2%BaO, 0 to 2%ZrO 2 , 5 to 13% K 2 O, 0 to 2% Li 2 O, and 0 to 2% Na 2 O.

[0089] Depending on the composition, the precursor glass can be melted in a suitable apparatus (e.g., a covered platinum crucible) at a temperature range of about 800 to about 2000° C. (preferably, a temperature range of 1200-1600° C., or a temperature range of about 1400° C. to about 1500° C.) for a time sufficient to melt the glass, e.g., about 30 minutes to about 20 hours (including about 2 hours to about 10 hours, about 3 hours to about 6 hours). After melting and clarification, the glass is poured and annealed at a temperature of about 500° C. to about 700° C. The annealed glass is ceramized and maintained at a suitable growth temperature, e.g., about 700° C. to about 1100° C., after which the resulting material is naturally cooled at a furnace rate.

[0090] The ceramization step may include, for example, a nucleation step and a growth step. The nucleation step may include: heating the furnace from room temperature to a first temperature of about 700°C to about 850°C (e.g., about 750°C to about 800°C) at a heating rate of about 1 to about 15°C / minute (e.g., about 5°C / minute or about 10°C / minute), and keeping the furnace at the first temperature for a time of about 0.5 to about 5 hours (e.g., about 2 to about 4 hours), or any range of any two of these values ​​and / or between any two of these values. In certain embodiments, the growth step may include: heating the furnace to a second temperature of about 700°C to about 1100°C (e.g., about 820°C to about 1050°C) at a heating rate of about 1 to about 15°C / minute (e.g., about 5°C / minute or about 10°C / minute), and keeping the furnace at the second temperature for a time of about 1 to about 16 hours (e.g., about 2 to about 10 hours), or any range of any two of these values ​​and / or between any two of these values. Other ceramicization schemes are known in the art and can be used according to the present disclosure to convert the precursor glass into glass ceramics. For example, glass can be ceramicized at a lower temperature to result in a transparent glass ceramic having β-quartz SS as the main crystalline phase or the dominant crystalline phase, which can present a thermal expansion curve showing a low expansion below an inflection point of about 500° C. and a high expansion above an inflection point of about 500° C.

[0091] The glass ceramic may be further processed by any conventional method known in the art, such as cooling to room temperature, polishing, grinding, etc. In certain embodiments, the glass ceramic article may be quenched directly from a high ceramizing temperature by contacting it with a liquid or gas, by rapidly cooling the heated glass ceramic article to a temperature of about 250° C. to about −40° C., thereby providing a thermally tempered glass ceramic. The glass ceramic article is thermally tempered separately after it is fully ceramized and cooled.

[0092] In some embodiments, the method may further include subjecting the heat-tempered glass-ceramic to a chemical strengthening process, thereby providing, for example, a chemically strengthened glass-ceramic having a superimposed compressive layer on the surface. In some embodiments, the chemical strengthening method includes: after the glass article is ceramized or even without ceramizing the glass article, subjecting the glass-ceramic article to an ion exchange treatment to provide an ion-exchanged glass-ceramic article. In some embodiments, the precursor glass may also be subjected to an ion exchange treatment to provide an ion-exchanged glass. The ion exchange process may be a single-step process or a multi-step process, and a single alkaline ion bath or a bath having a combination of two or more alkaline ions may be used.

[0093] In some embodiments, a method of forming a thermally tempered glass-ceramic is provided, wherein the method includes melting a batch and forming a glass comprising a precursor glass material as described herein; casting, annealing, ceramicizing, optionally cooling, and thermally tempering the glass-ceramic by contacting it with a quenching medium.

[0094] The heat-tempered glass-ceramics described herein can be used in a variety of applications, including articles such as electronic devices, automotive devices, appliances, and architectural devices (e.g., walls, tiles, stoves, floors, ceilings, etc.). In certain embodiments, the heat-tempered glass-ceramics can be used to make architectural windows and automotive glazing.

[0095] The heat tempered glass ceramics as described herein have improved properties, such as increased mechanical strength compared to non-tempered glass ceramics. The mechanical properties of the strengthened glass are directly related to the shape of the stress distribution (e.g., the layer depth and the magnitude of the compressive stress present at a particular depth). The greater the depth of the compressive layer in the glass and the greater the compressive stress, the higher the glass strength and the more resistant to shattering and shatter propagation. For example, high compressive stresses in the surface region of a heat tempered glass product or article inhibit shatter formation in the surface, provide scratch resistance, and inhibit shatter propagation from any shattering defects present or generated in the surface.

[0096] Glass-ceramics through heat tempering described herein have several advantages compared to chemically strengthened glass-ceramics (e.g., glass-ceramics through ion exchange). For example, heat tempering advantageously provides improved mechanical properties for materials in a shorter time than the required situation of ion exchange, without the need for expensive ion exchange baths and materials. The stress arrangement provided by heat tempering can be carried out on the ceramization of glass material or the cooling of ceramized glass material. The resulting stress distribution is a parabola, and the compression depth is roughly 20% of the thickness of the component. For practical applications, there is no obvious thickness restriction for heat tempering. The process described in US9296638 can be adopted to carry out heat tempering to thin parts (less than 1mm). The stress provided by ion exchange has limitations for thermal stability, and the thermal stability is related to the ion diffusion that reduces stress at higher temperatures. Compared to the stress induced by ion exchange, the stress provided by heat tempering material is more solid for thermal excursion, because there is no ion diffusion at higher temperatures. Depends on the composition of glass-ceramics, if necessary, ion exchange can also be carried out after heat tempering to introduce higher surface stress.

[0097] It will be apparent to those skilled in the art that various modifications and variations may be made without departing from the spirit or scope of the claimed subject matter. Therefore, the claimed subject matter is not to be restricted except by the appended claims and their equivalents.

[0098] Example

[0099] Various embodiments will be further illustrated by the following examples, which are not intended to limit the present disclosure in any way.

[0100] Example 1: Preparation of thermally tempered glass-ceramics

[0101] Table 1 provides examples of representative compositions according to the present technology. Exemplary glass-ceramics described herein exhibit a base composition comprising the constituent components listed in Table 1, measured in mole % or weight % of oxides.

[0102] Table 1

[0103]

[0104] *No secondary phases were recorded. ** In the glass, F is distributed among the various cations, ie, some of the oxygen in the oxide is replaced by fluorine, so the oxygen equivalent of fluorine (16 / 38 x amount of F) is subtracted from the sample to give 100%.

[0105] Precursor glasses were made in platinum crucibles using the raw material batches listed in Table 1. Each crucible containing the formulated raw material batches was placed in a preheated furnace and melted at a suitable temperature for a suitable period of time. The glass was clarified to produce a molten precursor glass, which was then cast and annealed at a suitable annealing temperature. β-spodumene precursor glasses (AV, AW, AX, AY, AZ, and BA) were melted at 1600°C for 16 hours. After melting, the glass was poured onto a cold steel table and annealed at 575°C for 3 hours. The precursor glass ESS composition was melted at 1600°C for 4 hours. After melting, the glass was poured and rolled to a thickness of 4 mm. It was then annealed at 650°C for 1 hour.

[0106] Ceramic

[0107] Precursor glasses of β-spodumene and mullite materials were ceramized according to the protocol given below. After the growth temperature was maintained, the resulting material was cooled naturally at the furnace rate.

[0108] Glass ceramics based on β-crystals

[0109] A sheet of each of the formed β-spodumene glass samples was ceramized in the following scheme:

[0110] Heating from 25°C to 750°C at 10°C / min

[0111] Keep at 750℃ for 2 hours

[0112] Heating from 750°C to 950°C at 10°C / min

[0113] Keep at 950℃ for 4 hours

[0114] Cooling is carried out at furnace rate.

[0115] Glass-ceramics based on mullite crystals

[0116] The formed sheets of ESS glass were ceramized with the following protocol:

[0117] Heating from 25°C to 750°C at 10°C / min

[0118] Keep at 750℃ for 4 hours

[0119] Heating from 750°C to 830°C at 10°C / min

[0120] Keep at 830℃ for 2 hours

[0121] Cooling is carried out at furnace rate.

[0122] After ceramization, the thermal expansion of the obtained glass-ceramics was measured and for one of the representative β-spodumene GCs (AX) ( Figure 1 a and 1b) and one of the mullite GCs (ESS) ( Figure 2 ) was subjected to X-ray diffraction (XRD) analysis. For β-spodumene, the crystallinity was estimated to be about 80-90 wt%. Figure 1 a shows β-spodumene solid solution, rutile, ZrTiO 4 and residual glass, and Figure 1 b A magnified version is provided to show the glassy halo corresponding to the presence of residual glass. Figure 2 It shows that the main or dominant crystalline phase in ESS is Al 4 B 2-x Si x O 9 The solid solution of polyaluminum quartz is shown in Figure 2, and it shows that the material contains a high level of residual glass. There is also a small amount of boralsilite (Al 16 B 6 Si 2 O 37 ).

[0123] Example 2: Thermal Tempering of Glass Ceramics

[0124] The following process was used to prepare the exemplary glass ceramics according to the process of Example 1 and the commercial (Corning Incorporated, Corning, NY, USA) for thermal tempering.

[0125] Polished plates (50 x 50 x 3 mm thick) of β-spodumene glass-ceramic were prepared and subjected to a tempering process. To achieve tempering, heat must be extracted quickly from the part so that the surface cools faster than the interior. This is accomplished by heating the glass-ceramic samples close to their annealing point (i.e., temperatures above and below it) and holding for 20 minutes to achieve thermal equilibrium across the part. At this point, the plates were removed from the furnace and rapidly quenched in a commercially available, continuously stirred peanut oil bath at 25°C. After approximately 3 minutes, the samples were removed from the oil and then thoroughly cleaned with dishwashing detergent to remove excess oil. In the case of mullite and In the case of glass ceramics, the same process was used except that the sample size was different (cylinders of 32 mm diameter and 3 mm thickness) and sunflower oil was used instead of peanut oil for annealing.

[0126] Example 3: Characteristics

[0127] In the following examples, various properties of the materials listed in Table 1 are described. Exemplary methods for the properties are provided below.

[0128] The annealing point and strain point of the glass-ceramics and glasses described herein can be measured using methods known to those skilled in the art, for example, ASTM C598 (and its successors, the entirety of which is incorporated herein by reference), "Standard Test Method for Annealing Point and Strain Point of Glass by Beam Bending", ASTM International, Conshohocken, PA, US.

[0129] The characteristics of the crystalline phases of the crystalline phase assembly and / or the crystal size of the crystalline phases are determined by X-ray diffraction (XRD) analysis techniques known to those skilled in the art, using commercially available equipment such as a model PW1830 (Cu Ka radiation) diffractometer manufactured by Philips, Netherlands. The spectrum is usually obtained from 5 to 80 degrees 2θ.

[0130] Table 2 provides comparative properties of exemplary compositions of thermally tempered glass-ceramics described herein.

[0131] Table 2

[0132]

[0133]

[0134] Ring-on-ring test

[0135] Ring-on-ring testing was used to determine the effect of the tempering process on strength, which is expected to be increasing for materials with compressive surface stresses. Ring-on-ring testing was performed according to the test method described in ASTM C1499-08 (Standard Test Method for Monotonic Equibiaxial Flexural Strength of Advanced Ceramics at Ambient Temperature).

[0136] Generally speaking, the ring-on-ring load test method is used to determine the biaxial strength of advanced brittle materials at ambient temperature by means of a concentric ring configuration under monotonic coaxial loading, and it is widely accepted as a method for evaluating the surface strength of glass products.

[0137] The tests were completed on abraded and unabraded samples. The abraded samples were prepared by abrading the outer surface of the glass article with 1 mL of 90 mesh SiC particles at an abrasion pressure of 5 psi for 5 seconds. Abrasion imparts a consistent number of flaws in the material and reduces the effects of the finishing and handling of the flaws on the measurement. The spodumene glass-ceramic samples were abraded, but the mullite and Macor glass-ceramic samples were not. For example, experiments were conducted on mullite glass-ceramic and Macor glass-ceramic on polished samples with a diameter of 32 mm and a thickness of 3 mm (10 samples under each condition), using a 15 mm diameter support ring, a 5 mm diameter load ring, a 1.5 mm ring contact radius, and a 0.5 mm / min head speed and a 50 mm x 5 mm x 3 mm thick β-spodumene sample component to perform a ring-on-ring test.

[0138] Table 3 below reports the average strength values ​​at failure for various tempered glass-ceramics from the ring-on-ring results.

[0139] Table 3:

[0140]

[0141] MV = mean; SD = standard deviation.

[0142] Figure 3 The wear ring on ring results are shown, showing the failure strength values ​​of the heat-tempered β-spodumene glass-ceramic at different quench temperatures (700°C and 900°C) compared to the corresponding untempered samples. The values ​​in the bar graph correspond to the estimated compressive stress values. The failure strength increases with the degree of annealing due to the increase in the estimated compressive stress. It is clear from the graph that the glass-ceramic is heat-temperable. Figure 4Unworn ring-on-ring results are shown, showing failure strength values ​​for heat tempered mullite glass-ceramic at different quench temperatures (750°C and 830°C) versus untempered samples. These results show that this glass-ceramic is heat temperable. As expected, the unworn sample has a high standard deviation. Figure 5 Results for unworn rings are shown, and results for heat tempered Glass ceramics quenched at 960℃ compared to untempered The results show that when When cooled from 960℃, the failure strength increases significantly.

[0143] Stress distribution

[0144] Since direct measurements of the stress distribution in the tempered part are not possible, an idealized equation is used to estimate the magnitude of the surface compression as shown below. Note that the actual stress distribution is expected to be a parabola, where the surface compression is exactly twice the magnitude of the central tension. The equation used here is probably an upper limit of what can be achieved.

[0145] σ=E / (1-ν)*((ΔL / L) T0 )–((ΔL / L) Tq )

[0146] Where σ = surface compression, E = Emod (GPa), ν is Poisson's ratio, and ΔL / L is the ratio from T 0 and T q The CTE curve at T 0 is the heating temperature for tempering, and T q Taken from the point in the CTE curve where the slope changes. Below this point, the thermal expansion is that of the glass-ceramic (i.e., the average between the CTE of the crystalline phase and the CTE of the residual glass). Above this point (corresponding to the Tg of the residual glass), the increase in thermal expansion is due to a strong increase in the CTE of the residual glass.

[0147] Depends on composition and T 0 , the surface compression value is estimated to be 60 to 330 MPa. 0 The experimental compression values ​​are lower, probably because the thermal gradients in the part are likely smaller, the Δppm is smaller, and the T 0 The temperature is below the strain point of the material.

[0148] By checking Figure 6The thermal expansion curve of the β-spodumene glass-ceramic shown, annealing is more obvious relative to the origin of the thermal expansion coefficient. The cooling curve is reproduced, showing a slope change at a temperature of about 500°C. Above this point, the higher expansion in the borosilicate glass-like phase dominates, and quenching from 800°C or higher leads to annealing stress. In the curve, the lower CTE below 500°C attributed to the presence of β-spodumene as the main or dominant crystalline phase has the advantage of being able to maintain the thermal shock resistance of the glass-ceramic. The stress estimated using the above equation is for T below the slope change. q The estimated surface stress is presented as a result of mechanical testing. Tempering starting from 700°C leads to a negligible stress increase at failure compared to the untempered glass-ceramic. However, tempering starting from 900°C shows an increase in both the measured failure stress and the estimated surface compression compared to the 700°C heat treatment. It is expected that a larger ΔT starting from 900°C leads to a larger ΔL / L. In addition, the 900°C heat treatment can be more effective in providing compressive stresses because it is above the annealing point measured for the glass-ceramic. Among the compositions tested, composition AX shows the largest tempering effect, which may be due to the high content of B in the residual glass. 2 O 3 The result is a higher CTE.

[0149] Figure 7 The thermal expansion of ESS glass-ceramics containing a solid solution of polyaluminous spodumene as the main or dominant crystalline phase is shown, showing a slope change corresponding to the difference in expansion associated with the residual glass (temperature above the inflection point) and the crystalline phase (temperature below the inflection point). The length variable of the glass-ceramics as a function of temperature shows the same behavior, with the β-spodumene glass-ceramics described above having a slope change at about 550°C. The stress that can be induced by tempering from 720°C is estimated using the equation given above. This value (187PMa) suggests that thermal tempering of these glass-ceramics can lead to a significant increase in failure stress. In the composition ESS, Li 2 O.K 2 O and part B 2 O 3 and MgO may remain mainly in the residual glass and contribute to the increase in thermal expansion. 2 O helps to lower the temperature at which the slope change is observed. Figure 8 Showing 55% fluorphlogopite and 45% borosilicate glass The thermal expansion of glass ceramics shows a slope change at about 470°C.

[0150] In the case of mullite glass-ceramics, it has been demonstrated that thermal tempering is associated with an increase in the KST (Knoop Scratch Threshold) value. For untempered ESS glass-ceramics, KST ranges from 3 to 6 N, compared to 5 to 7 N for ESS glass-ceramics tempered from 830°C. KST is a measure of the load required to produce a median crack and / or radial crack using a Knoop diamond indenter. Below this load, mainly micro-ductile failure is observed.

[0151] Unless otherwise expressly stated, any method described herein should not be construed as requiring that its steps be performed in a specific order, or requiring that any device have a particular orientation. Therefore, if a method claim does not actually recite the order in which its steps are to be followed, or if any device claim does not actually recite the order or orientation of the components, or if there is no other specific statement in the claims or specification that the steps are limited to a specific order, or if a specific order or orientation of the device components is not recited, then no order or orientation should be inferred in any respect. The same applies to any possible non-expressly stated basis for interpretation, including: logic regarding the setting of steps, operational flow, component order, or component orientation; general meaning derived from grammatical structure or punctuation; and the number or type of embodiments described in the specification.

[0152] All disclosed ranges are understood to include and provide support for claims stating any and all subranges or any and all individual values ​​contained by each range. For example, the stated range of 1 to 10 should be considered to include and provide support for any and all subranges or individual values ​​between and / or including a minimum value of 1 and a maximum value of 10; that is, all subranges start at a minimum value of 1 or greater and end at a maximum value of 10 or less (e.g., 5.5 to 10, 2.34 to 3.56, etc.), or any value from 1 to 10 (e.g., 3, 5.8, 9.9994, etc.). Any listed range can be easily identified as fully describing and allowing the same range to be decomposed into at least half, one-third, one-quarter, one-fifth, one-tenth, etc. As a non-limiting example, each range discussed herein can be easily decomposed into a lower third, a middle third, and an upper third, etc. It will also be understood by those skilled in the art that all languages, such as "up to", "at least", "greater than", "less than", etc., include the stated numbers and relate to ranges that can be subsequently decomposed into subranges discussed above. Finally, as will be understood by those skilled in the art, a range includes each individual member. Thus, for example, a group having 1-3 layers refers to groups having 1, 2, or 3 layers. Similarly, a group having 1-5 layers refers to groups having 1, 2, 3, 4, or 5 layers, and so on.

[0153] The drawings should be interpreted as showing one or more embodiments drawn to scale and / or one or more embodiments not drawn to scale. This means that the drawings may be interpreted, for example, as showing the following: (a) everything is drawn to scale; (b) nothing is drawn to scale; or (c) one or more features are drawn to scale and one or more features are not drawn to scale. Thus, the drawings may be used to provide support for the size, proportions, and / or other dimensions of any illustrated feature described individually or relative to each other. Furthermore, all such sizes, proportions, and / or other dimensions are understood to vary from 0-100% in either direction, thereby providing support for claims stating such values ​​or any and all ranges or sub-ranges that may be formed from such values.

[0154] Terms stated in the claims should be determined by reference to relevant entries in widely used general dictionaries and / or dictionaries of relevant technology, meanings commonly understood by persons skilled in the art, etc., to determine their ordinary and customary meanings, and it is understood that the terms of the claims have the broadest meaning given by any one or combination of these sources (e.g., two or more relevant dictionary entries should be combined to provide the broadest meaning of the combination of the entries, etc.), subject only to the following exceptions: (a) if a term is used in a manner broader than its ordinary and customary meaning, the term should be given its ordinary and customary meaning plus an additional extended meaning, or (b) if a term is expressly defined as having a different meaning by stating that the term is as used in this document, or similar language (e.g., "this term means," "this term is defined as," "for the purposes of this disclosure, this term should mean," etc.). Reference to specific examples, use of "i.e.," use of the term "technology," etc. is not intended to refer to exception (b) or otherwise limit the scope of the claim terms. Except where exception (b) applies, nothing contained in this document shall be construed as a waiver of a claim or a denial of the scope of a claim.

[0155] Unless otherwise defined, all terms used herein (including technical terms and scientific terms) have the same meanings as commonly understood by those of ordinary skill in the art to which the present technology belongs. It will also be understood that terms (such as those defined in commonly used dictionaries) should be understood to be consistent with their definitions in the present application and related fields, and unless otherwise defined herein, should not be understood as idealized or fully formalized meanings. Although not clearly defined below, such terms should be interpreted according to their common meanings.

[0156] In addition, where features or aspects of the disclosure are described in terms of Markush groups, those skilled in the art will recognize that the disclosure is also thereby described in terms of any individual member or subgroup of members of the Markush group.

[0157] Unless the context clearly states otherwise, it is intended that the various features of the present technology described herein can be used in any combination. In addition, in certain embodiments, the present disclosure also contemplates that any feature or combination of features described herein can be excluded or omitted. Explanatory note, if the specification states that a consortium includes components A, B, and C, it is specifically intended that any or any combination of A, B, or C can be omitted or abandoned individually or in any combination thereof.

[0158] Unless expressly stated otherwise, all specific embodiments, features and terms are intended to include both the stated embodiment, feature or term and its biological equivalents.

[0159] All patents, patent applications, provisional applications, and publications referred to or cited herein are hereby incorporated by reference in their entirety, including all figures and tables, to the extent they are not inconsistent with the teachings of this specification.

Claims

1. A thermally tempered aluminosilicate glass-ceramic composition comprising a crystalline phase and a glass phase, wherein: The two phases form a system in which the thermal expansion curve of the system has two different sections radiating from an inflection point temperature in the range of 450° C. to 600° C.; wherein the difference between the coefficient of thermal expansion of the glass-ceramic below and above the inflection point is 4 ppm / °C to 10 ppm / °C; and Wherein, the precursor glass of the glass-ceramic composition comprises, in terms of mole % of oxides: 1) 65% to 75% SiO2; 8% to 13% Al2O3; 3% to 13% Li2O; 0.02% to 5% B2O3; 0.5% to 2% K2O; 0% to 2% BaO; and 2% to 6% RO2, wherein RO2 consists of 1% to 4% TiO2, 0% to 2% ZrO2 and 0% to 1% SnO2; or 2) 55% to 65% SiO2; 13% to 19% Al2O3; 0% to 4% Li2O; 12% to 17% B2O3; 1% to 4% K2O; and 2% to 8% MgO; or 3) 40% to 55% SiO2; 12% to 20% Al2O3; 10% to 18% MgO; 4% to 8% F; 5% to 10% B2O3; 0% to 2% BaO; 0% to 2% ZrO2; and 0% to 16% R2O, wherein R2O consists of 5% to 13% K2O, 0% to 2% Li2O and 0% to 2% Na2O.

2. The thermally tempered aluminosilicate glass-ceramic composition according to claim 1, wherein: The thermal expansion coefficient of glass ceramics below the inflection point is 1 ppm / °C to 10 ppm / °C.

3. The thermally tempered aluminosilicate glass-ceramic composition of claim 1, wherein: The thermal expansion coefficient of glass ceramics above the inflection point is 6 ppm / °C to 20 ppm / °C.

4. The thermally tempered aluminosilicate glass-ceramic composition of claim 1, having a Young's modulus of 70 GPa to 110 GPa.

5. The thermally tempered aluminosilicate glass-ceramic composition of claim 1, wherein: The crystalline phase of the composition includes a dominant crystalline phase selected from the group consisting of mullite, fluorphlogopite, and β-spodumene solid solution.

6. A method for thermally tempering a glass-ceramic composition comprising a crystalline phase and a residual glass phase, the method comprising: heating the glass-ceramic composition to a temperature between an annealing point and a softening point of the residual glass phase to produce a heated glass-ceramic composition; as well as rapidly cooling the heated glass-ceramic composition to a temperature of 250° C. to −40° C. by contacting it with a quenching medium to provide a thermally tempered glass-ceramic, Wherein, the precursor glass of the glass-ceramic composition comprises, in terms of mole % of oxides: 1) 65% to 75% SiO2; 8% to 13% Al2O3; 3% to 13% Li2O; 0.02% to 5% B2O3; 0.5% to 2% K2O; 0% to 2% BaO; and 2% to 6% RO2, wherein RO2 consists of 1% to 4% TiO2, 0% to 2% ZrO2 and 0% to 1% SnO2; or 2) 55% to 65% SiO2; 13% to 19% Al2O3; 0% to 4% Li2O; 12% to 17% B2O3; 1% to 4% K2O; and 2% to 8% MgO; or 3) 40% to 55% SiO2; 12% to 20% Al2O3; 10% to 18% MgO; 4% to 8% F; 5% to 10% B2O3; 0% to 2% BaO; 0% to 2% ZrO2; and 0% to 16% R2O, wherein R2O consists of 5% to 13% K2O, 0% to 2% Li2O and 0% to 2% Na2O.

7. The method of claim 6, wherein: The heated glass-ceramic composition is cooled to create a temperature difference of at least 200° C. between an outer surface of the glass-ceramic composition and a center of the glass composition.

8. The method of claim 6, wherein: The quenching medium is selected from the group consisting of vegetable oil, water, glycols and liquid nitrogen, or a combination thereof.

9. The method of claim 8, wherein: The vegetable oil is selected from the group consisting of peanut oil, rapeseed oil, soybean oil, corn oil, olive oil, sunflower oil, safflower oil, cottonseed oil, and combinations thereof.

10. The method of claim 9, wherein: Sunflower oil includes high oleic sunflower oil.

11. The method of claim 6, wherein: The quenching medium is maintained at a temperature of 10°C to 50°C before it comes into contact with the heated glass-ceramic.

12. The method of claim 6, wherein: The glass composition is heated to a temperature of 750°C to 950°C for a time ranging from 6 minutes to 4 hours to produce a heated glass-ceramic composition.

13. The method of claim 6, further comprising subjecting the thermally tempered glass-ceramic to an ion exchange process, thereby generating a compressive stress layer in an outer surface region of the glass-ceramic in addition to the compressive stress generated by the thermal tempering.

14. A method for thermally tempering a glass-ceramic composition comprising a crystalline phase and a residual glass phase, the method comprising: heating the glass-ceramic composition to a temperature of 700° to 1000° C. to produce a heated glass-ceramic composition; as well as rapidly cooling the heated glass-ceramic composition to a temperature of 250° C. to −40° C. by contacting it with a quenching medium to provide a thermally tempered glass-ceramic, Wherein, the precursor glass of the glass-ceramic composition comprises, in terms of mole % of oxides: 1) 65% to 75% SiO2; 8% to 13% Al2O3; 3% to 13% Li2O; 0.02% to 5% B2O3; 0.5% to 2% K2O; 0% to 2% BaO; and 2% to 6% RO2, wherein RO2 consists of 1% to 4% TiO2, 0% to 2% ZrO2 and 0% to 1% SnO2; or 2) 55% to 65% SiO2; 13% to 19% Al2O3; 0% to 4% Li2O; 12% to 17% B2O3; 1% to 4% K2O; and 2% to 8% MgO; or 3) 40% to 55% SiO2; 12% to 20% Al2O3; 10% to 18% MgO; 4% to 8% F; 5% to 10% B2O3; 0% to 2% BaO; 0% to 2% ZrO2; and 0% to 16% R2O, wherein R2O consists of 5% to 13% K2O, 0% to 2% Li2O and 0% to 2% Na2O.

15. The method according to any one of claims 6 to 14, wherein: The glass-ceramic composition is a glass plate having a thickness of 1 mm to 5 mm.

16. An article comprising the thermally tempered aluminosilicate glass-ceramic composition of any one of claims 1 to 5.

17. The article of claim 16 comprising a surface and having a compressive stress greater than 60 MPa at the surface of the glass-ceramic.

18. The article of claim 17, wherein the compressive stress at the surface of the glass-ceramic is 60 MPa to 330 MPa.

19. The article of claim 16, comprising: Electronic devices, automotive devices, architectural devices or electrical devices.