Rotor core and its manufacturing method

By using a thermosetting resin material with a coefficient of linear expansion lower than that of electromagnetic steel plates, and by controlling the filling and curing process of the resin material, the problem of resin material damage due to excessive stress in the rotor core was solved, thereby improving the reliability and lifespan of the rotor core.

CN115244823BActive Publication Date: 2026-11-17AISIN CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180019295.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-03-23
Publication Date
2026-11-17
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

In the prior art, the tensile stress caused by the difference in the coefficient of linear expansion during the curing and cooling process of the resin material in the rotor core is too large, which can easily lead to material damage and affect the reliability and life of the rotor.

Method used

Thermosetting resin material with a coefficient of linear expansion lower than that of electromagnetic steel plate is used. By controlling the filling and curing process of resin material, tensile stress is reduced, ensuring that the shrinkage of resin material during curing and cooling is less than that of electromagnetic steel plate, thereby reducing residual stress.

Benefits of technology

It effectively prevents the resin material from breaking due to excessive stress during rotor operation, thereby improving the reliability and service life of the rotor core.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115244823B_ABST
    Figure CN115244823B_ABST
Patent Text Reader

Abstract

This invention provides a rotor core and a method for manufacturing the rotor core. The rotor core comprises a thermosetting resin material, which is disposed in a magnet housing portion and a permanent magnet is fixed within the magnet housing portion, and has a coefficient of linear expansion that is lower than that of the electromagnetic steel plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to rotor cores and methods for manufacturing rotor cores. Background Technology

[0002] Previously, it was known that rotor cores with permanent magnets fixed in resin materials and methods for manufacturing such rotor cores were also known. For example, such rotor cores and methods for manufacturing such rotor cores were disclosed in Japanese Patent No. 5971176.

[0003] Japanese Patent No. 5971176 discloses a rotor core with multiple holes. Magnets are inserted into each of the holes in the rotor core. A thermosetting fixing member is provided in each hole. The fixing member is used to fix the magnets disposed in the holes. Furthermore, the fixing member is a thermosetting resin containing epoxy resin. The rotor core is heated while the fixing member is filled into the holes, thereby curing the fixing member.

[0004] Patent Document 1: Japanese Patent No. 5971176

[0005] However, although not explicitly described in Japanese Patent No. 5971176, the fixing component shrinks only a certain amount during curing while fixed to the rotor core. Therefore, the fixing component experiences tensile stress from the rotor core during this shrinkage. Furthermore, although not explicitly described in Japanese Patent No. 5971176, a cooling process for the rotor core is performed after the curing process. During this cooling process, both the rotor core and the fixing component shrink due to cooling. Generally, the coefficient of linear expansion of the thermosetting resin containing epoxy resin is greater than that of the electromagnet steel sheet constituting the rotor core; therefore, the fixing component shrinks more than the rotor core during the cooling process. In this case, the fixing component experiences tensile stress from the rotor core. That is, the fixing component experiences tensile stress from the rotor core during both the curing and cooling processes. Therefore, there is an undesirable situation where residual tensile stress remains on the fixing component as residual stress from the curing and cooling processes. In this case, during rotor rotation, there may be problems such as damage to fixed components due to residual stress. Summary of the Invention

[0006] The present invention was made to solve the aforementioned problems. One object of the present invention is to provide a rotor core that can prevent damage to resin materials and a method for manufacturing the rotor core.

[0007] To achieve the above objectives, the rotor core of the first aspect of the present invention comprises: a laminated core, which is constructed by stacking a plurality of electromagnetic steel plates, including a magnet housing portion extending along the stacking direction of the electromagnetic steel plates; a permanent magnet disposed in the magnet housing portion of the laminated core; and a thermosetting resin material, which is filled in the magnet housing portion between the laminated core and the permanent magnet and fixes the permanent magnet in the magnet housing portion, and has a coefficient of linear expansion that is less than the coefficient of linear expansion of the electromagnetic steel plates.

[0008] In the rotor core of the first aspect of the present invention, as described above, a thermosetting resin material is provided, which has a coefficient of linear expansion that is lower than or equal to that of the electromagnet plate. Here, when the thermosetting resin material is cured, the resin material is heated while the molten resin material is injected into the magnet housing. At this time, the resin material shrinks while fixed to the laminated core, thus subjecting the resin material to tensile stress from the laminated core. Furthermore, after the resin material has cured, both the laminated core and the resin material shrink during cooling. Since the coefficient of linear expansion of the resin material is lower than or equal to that of the electromagnet plate, the amount of shrinkage of the resin material in the lamination direction of the electromagnet plate is lower than the amount of shrinkage of the electromagnet plate (laminated core). In this case, the tensile stress on the resin material from the laminated core does not increase, so the residual stress of the resin material after the rotor core manufacturing process can be set to be lower than or equal to the tensile stress generated during the curing process. As a result, compared to situations where the coefficient of linear expansion of the resin material is greater than that of the electromagnetic steel sheet, leading to increased tensile stress on the resin material during the cooling process, the residual stress in the resin material after the rotor core manufacturing process can be reduced. Consequently, damage to the resin material during rotor operation can be prevented.

[0009] Furthermore, since the coefficient of thermal expansion of the resin material is lower than that of the electromagnetic steel sheet, even when the temperature of the resin material changes during rotor operation, the amount of expansion (contraction) of the resin material can be kept below that of the electromagnetic steel sheet. As a result, it is possible to prevent the stress applied to the resin material from increasing during rotor operation, thus more reliably preventing damage to the resin material during rotor operation.

[0010] The second aspect of the present invention is a method for manufacturing a rotor core comprising a stacked core having a magnetic housing portion extending along the stacking direction of the electromagnetic steel plates, and comprising the following steps: a placement step in which a permanent magnet is placed in the magnetic housing portion of the stacked core; a filling step in which, after the placement step, a molten resin material having a coefficient of linear expansion less than that of the electromagnetic steel plates is filled into the magnetic housing portion between the stacked core and the permanent magnet; a curing step in which, after the filling step, the resin material is cured by heating; and a cooling step in which, after the curing step, the stacked core and the resin material are cooled.

[0011] In the rotor core manufacturing method of the second aspect of the present invention, as described above, a filling step is included in which a molten resin material having a coefficient of linear expansion of less than or equal to that of the electromagnet is filled into the magnet housing portion. Here, during the curing step, the resin material shrinks while fixed to the laminated core, thus subjecting the resin material to tensile stress from the laminated core. Furthermore, during the cooling step, both the resin material and each part of the laminated core shrink due to cooling. Since the coefficient of linear expansion of the resin material is less than or equal to that of the electromagnet, the amount of shrinkage of the resin material in the lamination direction of the electromagnet is less than or equal to the amount of shrinkage of the electromagnet (laminated core). In this case, the resin material is not subjected to stress from the laminated core, or it is subjected to compressive stress from the laminated core, so the residual stress of the resin material after the rotor core manufacturing step can be set to be less than or equal to the tensile stress generated during the curing step of the resin material. As a result, compared to the case where the coefficient of linear expansion of the resin material is greater than that of the electromagnet, and the tensile stress acting on the resin material during the cooling step of the resin material increases, the residual stress of the resin material after the rotor core manufacturing step can be reduced. As a result, a method for manufacturing a rotor core is provided that can prevent damage to the resin material during rotor operation.

[0012] According to the present invention, damage to the resin material can be prevented. Attached Figure Description

[0013] Figure 1 This is a top view showing the structure of a rotor (rotary motor) constituting one embodiment.

[0014] Figure 2 This is a cross-sectional view of a rotor core according to one embodiment.

[0015] Figure 3 This is a flowchart illustrating a method for manufacturing a rotor core according to one embodiment.

[0016] Figure 4This is a diagram showing the resin material and stress state of the laminated core during the manufacturing of a rotor core according to one embodiment.

[0017] Figure 5 This is a diagram showing the changes in the axial dimensions of the resin material, the laminated core, the permanent magnet, and the resin molded part (comparative example) during the manufacturing of the rotor core of one embodiment.

[0018] Figure 6 This is a graph showing the variation of the axial dimensional difference between the resin material and the resin molding part (comparative example) relative to the laminated core during the manufacturing of the rotor core of one embodiment.

[0019] Figure 7 This is a graph showing the variation in the axial dimensional difference between the resin material and the resin molded part (comparative example) relative to the permanent magnet during the manufacturing of the rotor core of one embodiment.

[0020] Figure 8 This is a graph showing the changes in the axial dimensions of the resin material, the laminated core, the permanent magnet, and the resin molded part (comparative example) when the rotor core of one embodiment is used.

[0021] Figure 9 This is a graph showing the variation in the axial dimensional difference between the resin material and the resin molding (comparative example) relative to the laminated core when the rotor core of one embodiment is in use.

[0022] Figure 10 This is a graph showing the variation in the axial dimensional difference between the resin material and the resin molded part (comparative example) relative to the permanent magnet when the rotor core of one embodiment is in use. Detailed Implementation

[0023] The embodiments of the present invention will now be described with reference to the accompanying drawings.

[0024] [This implementation method]

[0025] Reference Figures 1-10 The rotor core 4 and the manufacturing method of the rotor core 4 in this embodiment will be described.

[0026] In this application specification, "axial direction" refers to the direction along the rotation axis C1 of the rotor 1 (rotor core 4), which is the Z direction in the figure. Additionally, "stack direction" refers to the direction of the electromagnetic steel plate 4a of the rotor core 4 (see reference). Figure 2 The stacking direction refers to the Z direction in the diagram. In addition, "radial" refers to the radial direction (R1 direction or R2 direction) of rotor 1 (rotor core 4), and "circumferential" refers to the circumferential direction (E1 direction or E2 direction) of rotor 1 (rotor core 4).

[0027] like Figure 1 As shown, the rotary motor 100 includes a rotor 1 and a stator 2. Both the rotor 1 and the stator 2 are formed in annular shapes. Furthermore, the rotor 1 is arranged opposite the stator 2 radially inward. That is, in this embodiment, the rotary motor 100 is configured as an inner rotor type rotary motor. Additionally, a shaft 3 is arranged radially inward of the rotor 1. The shaft 3 is connected to an engine or axle via a rotational force transmission component such as gears. For example, the rotary motor 100 is configured as a motor, generator, or a combination of both, and is configured to be mounted in a vehicle. Furthermore, in Figure 1 For simplicity, the illustration of resin material 6, which will be described later, is omitted.

[0028] In addition, the rotor core 4 includes a laminated core 4d, which is composed of multiple electromagnetic steel plates 4a having multiple surrounding closed holes 4b (see reference). Figure 2 The rotor core 4 is formed by overlapping the holes 4b along the axial direction and has a magnet housing 10 extending along the stacking direction of the electromagnetic steel plate 4a. That is, the magnet housing 10 is a space surrounded by the stacked iron core 4d and extending along the axial direction of the stacked iron core 4d. Furthermore, the rotor core 4 has permanent magnets 5 disposed in the magnet housing 10 of the stacked iron core 4d. Multiple magnet housings 10 are provided in the stacked iron core 4d (32 in this embodiment). That is, the rotary motor 100 is configured as an interior permanent magnet motor (IPM). The magnet housing 10 is disposed on the radially outer portion of the stacked iron core 4d (rotor core 4). Furthermore, two adjacent magnet housings 10 are arranged in a V-shape. However, the arrangement and number of magnet housings 10 are not limited to this.

[0029] Furthermore, the stator 2 includes a stator core 2a and a coil 2b disposed on the stator core 2a. The stator core 2a has, for example, multiple electromagnetic steel plates (silicon steel plates) stacked axially and configured to allow magnetic flux to pass through. The coil 2b is connected to an external power source and is configured to be supplied with electricity (e.g., three-phase alternating current). Moreover, the coil 2b is configured to generate a magnetic field by being supplied with electricity. Additionally, the rotor 1 and shaft 3 are configured to rotate relative to the stator 2 even without power being supplied to the coil 2b, in conjunction with the drive of an engine or the rotation of an axle. Furthermore, in Figure 1 Although a portion of coil 2b is shown in the figure, coil 2b is arranged around the entire circumference of stator core 2a.

[0030] The permanent magnet 5 has a rectangular cross-section orthogonal to the axial direction of the laminated iron core 4d (rotor core 4). Furthermore, the surface of the permanent magnet 5 is covered with an insulating film, on which minute irregularities are formed. Additionally, the axial length of the permanent magnet 5 is less than or equal to the axial length of the magnet housing 10. For example, the permanent magnet 5 is configured such that its magnetization direction is the direction of the shorter side of the cross-section orthogonal to its axial direction. Moreover, the permanent magnet 5 is, for example, a neodymium magnet.

[0031] Additionally, the rotor core 4 has a thermosetting resin material 6 filled into the magnet housing 10 (see reference). Figure 2 The resin material 6 is configured to fix the permanent magnet 5 disposed in the magnet housing 10 within the magnet housing 10. Specifically, the permanent magnet 5 is fixed to the laminated iron core 4d by filling the space between the hole 4b of the laminated iron core 4d forming the magnet housing 10 and the permanent magnet 5 with the resin material 6. The resin material 6 is melted by heating to a first temperature T1 (e.g., 80°C) or higher. Furthermore, the resin material 6 is cured by heating to a second temperature T2 (e.g., 110°C) or higher than the first temperature T1. In detail, the resin material 6 is solid (sheet, granules, or powder, etc.) at room temperature lower than the first temperature T1, and melts when heated from room temperature to a temperature above the first temperature T1. Moreover, the resin material 6 is configured to remain in a molten state (not cured) while at a temperature above the first temperature T1 and below the second temperature T2. Furthermore, the resin material 6 is configured to cure by heating to a second temperature T2 or higher while in a molten state. Figure 1 For simplicity, the illustration of resin material 6 has been omitted.

[0032] For example, the synthetic resin material 6 described in Japanese Patent Application Publication No. 2018-145280 can be used. Furthermore, by adding inorganic fillers (fillers) to the synthetic resin material, the coefficient of linear expansion can be reduced. The coefficient of linear expansion of a synthetic resin material without inorganic fillers is tens of μm / ℃, while the coefficient of linear expansion of the inorganic filler monomer is tens of μm / ℃. By adding inorganic fillers to the resin material, the coefficient of linear expansion is reduced according to the composite principle. Furthermore, the composite principle is a general technical term and will not be elaborated here. That is, the resin material 6 used in this invention contains inorganic fillers. The coefficient of linear expansion of the resin material 6 is reduced by increasing the weight ratio of the inorganic filler. The weight ratio of the inorganic filler relative to the total amount of the resin material 6 is in the range of 50 to 95% by weight. In particular, to reduce the coefficient of linear expansion, the weight ratio of amorphous silicon dioxide (coefficient of linear expansion: 0.5 μm / ℃) in the resin material 6 is maximized. Furthermore, the structure of resin material 6 is not limited to the above-mentioned cases; it can also be a resin material with other structures, as long as it is a thermosetting resin material.

[0033] In this embodiment, the resin material 6 has a coefficient of linear expansion smaller than that of the electromagnetic steel plate 4a (laminated core 4d). Specifically, the coefficient of linear expansion of the electromagnetic steel plate 4a is approximately 13 μm / °C. Furthermore, the coefficient of linear expansion of the resin material 6 is approximately 11 μm / °C. As the rotor core of a rotary motor for a vehicle drive system, the coefficient of linear expansion of the electromagnetic steel plate 4a can be in the range of 11.5 μm / °C or higher and 13 μm / °C or lower, while the coefficient of linear expansion of the resin material 6 can be in the range of 9 μm / °C or higher and 11.5 μm / °C or lower. However, if the coefficient of linear expansion of the resin material 6 is less than 9 μm / °C, the weight ratio of the inorganic filler material in the resin material 6 further increases, resulting in reduced fluidity of the resin material 6 during the filling process of the rotor core 4 manufacturing process (described later). That is, the productivity of the rotor core 4 decreases. Therefore, it is preferable that the coefficient of linear expansion of the resin material 6 is 9 μm / °C or higher.

[0034] Furthermore, in this embodiment, the coefficient of linear expansion of the resin material 6 is less than that of the electromagnet steel plate 4a, but greater than that of the permanent magnet 5. Specifically, the coefficient of linear expansion of the permanent magnet 5 is approximately 2 μm / ℃ before magnetization (during the manufacture of the rotor core 4) and approximately -2.3 μm / ℃ after magnetization (during the use of the rotor core 4 (during the operation of the rotor 1)). Furthermore, the magnetized state refers to the state in which the orientation of the magnetic force within the permanent magnet 5 is adjusted. The magnetization direction, as described above, is the direction of the short side of a cross-section orthogonal to the axial direction of the permanent magnet 5. As is common technical knowledge, it is known that the coefficient of linear expansion of neodymium magnets takes different values ​​in the magnetization direction and in the direction perpendicular to the magnetization direction. The coefficient of linear expansion of the permanent magnet 5 referred to here is the coefficient of linear expansion in the direction perpendicular to the magnetization direction, i.e., the axial direction. Additionally, the coefficient of linear expansion of the permanent magnet 5 can also take a negative value (e.g., -1.5 μm / ℃) before magnetization (during the manufacture of the rotor core 4). Therefore, the linear expansion coefficient of the permanent magnet 5, which is the rotor core of the rotary motor used as a drive device for vehicles, can be in the range of -1.5 μm / ℃ or less and -2.3 μm / ℃ or more, regardless of whether it is before or after magnetization.

[0035] That is, the coefficient of linear expansion of resin material 6 is close to that of electromagnetic steel plate 4a compared to the median of the coefficients of linear expansion of electromagnetic steel plate 4a and permanent magnet 5. Furthermore, the coefficient of linear expansion of resin material 6 is close to that of electromagnetic steel plate 4a compared to the median of the aforementioned medians.

[0036] Furthermore, in this embodiment, the resin material 6 has a glass transition temperature T3 that is higher than the second temperature T2. For example, the glass transition temperature T3 is approximately 210°C. That is, the glass transition temperature T3 is a temperature higher than the upper limit temperature (180°C) at which the resin material 6 is heated during the operation of the rotor 1 and during the manufacture of the rotor core 4.

[0037] (Manufacturing method of rotor core, stress generated between resin material and laminated core)

[0038] Next, refer to Figures 3-7 The manufacturing method of the rotor core 4 in this embodiment will be described.

[0039] First, such as Figure 3 As shown, in step S1, the process of placing the permanent magnet 5 in the magnet storage section 10 of the stacked iron core 4d is performed (see reference). Figure 2 ).

[0040] Next, in step S2, a filling process is performed in which molten resin material 6, having a coefficient of linear expansion smaller than that of the electromagnet plate 4a, is filled between the laminated iron core 4d and the permanent magnet 5 within the magnet housing 10. Specifically, the resin material 6 is heated to a first temperature T1 or higher and a second temperature T2, becoming a molten state (fluid), and is filled in such a way that it fills the space between the magnet housing 10 and the permanent magnet 5. More preferably, the resin material 6 is injected such that the axially oriented sides of the permanent magnet 5 are surrounded by the resin material 6. Furthermore, at the moment the resin material 6 is injected, the laminated iron core 4d is preheated at a predetermined temperature (e.g., 140°C).

[0041] In the filling process, such as Figure 4 As shown, resin material 6 is a fluid and is not fixed to the laminated iron core 4d, so it follows the thermal expansion of the laminated iron core 4d (refer to...). Figure 5 Therefore, during the filling process, the axial dimensional difference (size of resin material 6 - size of stacked iron core 4d) between resin material 6 and stacked iron core 4d caused by thermal expansion is zero, so stress does not play a role. Here, unless otherwise specified, the axial dimension of stacked iron core 4d can be replaced with the axial dimension of magnet housing 10. Furthermore, unless otherwise specified, the axial dimension of resin material 6 refers to the axial dimension of resin material 6 after injection into magnet housing 10. Additionally, the stress mentioned here refers to the stress generated by the axial dimensional difference between resin material 6 and stacked iron core 4d when resin material 6 and stacked iron core 4d are fixed; it is the tensile or compressive stress acting on resin material 6 along the axial direction of stacked iron core 4d.

[0042] Next, as Figure 3 As shown, in step S3, a curing process is performed whereby the resin material 6 is cured by heating and the resin material 6 is fixed to the laminated iron core 4d. Specifically, as... Figure 5As shown, the resin material 6 and the laminated iron core 4d are heated to a temperature higher than the second temperature T2 (e.g., approximately 180°C). The temperature of the resin material 6 rises mainly through heat conduction from the inner wall surface of the magnet housing 10 of the laminated iron core 4d, so the resin material 6 solidifies and is fixed to the laminated iron core 4d from the part in contact with the inner wall surface of the magnet housing 10. Then, the heating state is maintained at approximately 180°C for a constant time, thereby completing the solidification of the resin material 6 and the fixation of the resin material 6 to the laminated iron core 4d. Specifically, the fixing condition is explained as follows: at the boundary between the holes 4b of the laminated electromagnet plates 4a where the magnet housing 10 is formed, there are recesses (not shown) formed. If the resin material 6 enters the recesses and solidifies, it becomes wedge-shaped. As a result, the resin material 6 is fixed in such a way that it enters the magnet housing 10 of the laminated iron core 4d. During the period when the temperature is maintained at approximately 180°C, no expansion or contraction occurs in the laminated iron core 4d because there is no temperature change. On the other hand, resin material 6 shrinks axially by a certain amount due to curing. In this case, such as Figure 6 As shown, the axial dimensional difference (size of resin material 6 - size of laminated iron core 4d) between the laminated iron core 4d and the resin material 6 is reduced.

[0043] That is, during the curing process, the resin material 6 is fixedly attached to the laminated iron core 4d while curing and shrinking. As a result, tensile stress caused by the dimensional difference between the resin material 6 and the laminated iron core 4d acts on the resin material 6. Therefore, during the curing process, the tensile stress acting on the resin material 6 is related to the amount of shrinkage of the resin material 6.

[0044] Furthermore, during the curing process, the resin material 6, which shrinks while fixed to the laminated iron core 4d, exerts compressive stress on the laminated iron core 4d. Therefore, during the curing process, compressive stress related to the amount of shrinkage of the resin material 6 acts on the laminated iron core 4d.

[0045] Next, as Figure 3 As shown, in step S4, a cooling process is performed to cool the laminated iron core 4d and the resin material 6. Specifically, in this process, the laminated iron core 4d and the resin material 6 are cooled from a high temperature (approximately 180°C) to room temperature (approximately 25°C).

[0046] like Figure 5 As shown, through cooling in the cooling process, the resin material 6 and the laminated iron core 4d each shrink axially. Here, the coefficient of linear expansion of the resin material 6 is smaller than that of the electromagnetic steel plate 4a, so the shrinkage of the laminated iron core 4d is greater than that of the resin material 6. In this case, as... Figure 6As shown, during the cooling process, the axial dimensional difference (dimension of resin material 6 - dimension of laminated iron core 4d) between the laminated iron core 4d and the resin material 6 increases. That is, the aforementioned dimensional difference approaches 0 from the negative side during the cooling process.

[0047] That is, during the cooling process, as the temperature of the laminated iron core 4d and the resin material 6 decreases, the laminated iron core 4d contracts more than the resin material 6. Therefore, the tensile stress acting on the resin material 6 is alleviated by the laminated iron core 4d fixed to the resin material 6. Furthermore, when the coefficient of linear expansion of the resin material 6 is less than that of the electromagnetic steel plate 4a, and the difference in their coefficients of linear expansion is large, after the tensile stress acting on the resin material 6 is alleviated during the cooling process, it can also transition to a compressive stress state. This means... Figure 4 During the cooling process (S4), the inclination of the stress lines of the resin material 6 and the laminated iron core 4d increases. Therefore, during the cooling process, the stress acting on the resin material 6 is related to the difference between the shrinkage of the resin material 6 and the shrinkage of the laminated iron core 4d.

[0048] As described above, during the curing process, the dimensional difference between the resin material 6 and the laminated iron core 4d decreases, while during the cooling process, the dimensional difference between the resin material 6 and the laminated iron core 4d increases. Therefore, as... Figure 4 As shown, the tensile stress accumulated in the resin material 6 during the curing process is relieved during the cooling process.

[0049] Furthermore, during the cooling process, the dimensional difference between the resin material 6 and the laminated iron core 4d increases, thereby mitigating the compressive stress acting on the laminated iron core 4d during the curing process.

[0050] Here, for resins with a coefficient of linear expansion greater than that of electromagnetic steel sheet 4a (hereinafter referred to as resin molded parts: see reference) Figure 5 as well as Figure 6 The case of the dashed line (comparative example) will be explained.

[0051] like Figure 5 As shown, the resin molded part has a greater thermal shrinkage rate during heat curing compared to resin material 6, resulting in greater shrinkage during the curing process. Therefore, during the curing process, the resin molded part is subjected to a tensile stress greater than that acting on resin material 6 (refer to...). Figure 4 Furthermore, compared to the case of resin material 6, the compressive stress acting on the laminated iron core 4d is greater (see...). Figure 4 ).

[0052] Furthermore, during the cooling process, the coefficient of linear expansion of the resin molded part is greater than that of the electromagnetic steel plate 4a, so the resin molded part shrinks more than the laminated iron core 4d. In this case, the axial dimensional difference between it and the laminated iron core 4d (the dimension of the resin molded part minus the dimension of the laminated iron core 4d) decreases during the cooling process (see reference). Figure 6 (The dotted line indicates this). That is, the aforementioned dimensional difference increases towards the negative side during the cooling process. Therefore, during the cooling process, tensile stress caused by the aforementioned dimensional difference acts on the resin molded part. Furthermore, during the cooling process, compressive stress caused by the aforementioned dimensional difference acts on the laminated iron core 4d.

[0053] Therefore, as Figure 4 As shown, in the case of using a resin-molded part (comparative example), tensile stress is applied to the resin-molded part and compressive stress is applied to the laminated core 4d during both the curing and cooling processes. Therefore, the stress in both the resin-molded part and the laminated core 4d is not relieved during the curing and cooling processes. Therefore, when using resin material 6, the residual stress in both the resin material 6 and the laminated core 4d after the manufacturing process of the rotor core 4 is smaller compared to the comparative example.

[0054] In addition, such as Figure 6 As shown, during the period from the curing step to the cooling step, if we want to reduce the axial dimensional difference of the resin material 6 (the dimension of the resin material 6 minus the dimension of the laminated iron core 4d) by a value A (increasing towards the negative side), then during the period from the curing step to the cooling step, the axial dimensional difference of the resin molded part (the dimension of the resin molded part minus the dimension of the laminated iron core 4d) must be reduced by a value B (increasing towards the negative side) greater than A. This is because in both the curing and cooling steps, the shrinkage of the resin material 6 is smaller than the shrinkage of the resin molded part.

[0055] (Stress generated between the resin material and the magnet during rotor core manufacturing)

[0056] Next, the dimensions of the permanent magnet 5 and the resin material 6 will be described. During the curing process, the resin material 6 cures and is fixed to the permanent magnet 5. Specifically, the resin material 6 cures into the recesses of the insulating film formed on the surface covering the permanent magnet 5, thereby fixing the resin material 6 to the permanent magnet 5. Figure 7 As shown, the resin material 6 is subjected to tensile stress due to shrinkage during the curing process and the fixing of the resin material 6 to the permanent magnet 5. Furthermore, the tensile stress on the resin material 6 increases because it shrinks more than the permanent magnet 5 during the cooling process. In this case, the axial dimensional difference of the resin material 6 (size of the resin material 6 - size of the permanent magnet 5) decreases by a value C from the curing process to the cooling process.

[0057] Furthermore, the situation is similar for the resin molded part (comparative example). Because the resin molded part shrinks during the curing process and is fixed to the permanent magnet 5, it is subjected to tensile stress. Moreover, because it shrinks more than the permanent magnet 5 during the cooling process, the tensile stress on the resin molded part increases. Here, the resin molded part shrinks more than the resin material 6 in both the curing and cooling processes. Therefore, during the period from the curing to the cooling process, the axial dimensional difference of the resin molded part (the size of the resin molded part minus the size of the permanent magnet 5) decreases by a value greater than C (increasing towards the negative side). Therefore, compared to the comparative example, using resin material 6 reduces the tensile stress acting on the resin material 6.

[0058] (Stress acting between the resin material and the laminated core during the use of the rotor core)

[0059] Next, refer to Figures 8-10 The state of the rotor core 4 when it is used (when the rotor core 4 is assembled in the motor mounted on a vehicle) will be explained.

[0060] like Figure 8 As shown, the laminated iron core 4d, the resin material 6, and the resin molded part (comparative example) each expand as the temperature rises and contract as the temperature falls. Additionally, the permanent magnet 5 contracts as the temperature rises and expands as the temperature falls. Figure 8 The axial dimensions at room temperature (25°C) are shown. Figure 5 The axial dimension after the cooling process.

[0061] like Figure 9 As shown, since the coefficient of linear expansion of resin material 6 is smaller than that of electromagnetic steel plate 4a, the expansion of resin material 6 with increasing temperature is smaller than that of laminated iron core 4d. That is, the axial dimensional difference between resin material 6 and laminated iron core 4d (dimensionality of resin material 6 - dimension of laminated iron core 4d) decreases with increasing temperature. In other words, the aforementioned dimensional difference increases towards the negative side with increasing temperature. Therefore, when the residual stress of resin material 6 at room temperature is zero or tensile stress, tensile stress is generated in resin material 6 with increasing temperature, or the residual tensile stress increases. Furthermore, when the residual stress of resin material 6 at room temperature is compressive stress, the compressive stress of resin material 6 is alleviated with increasing temperature, and the stress acting on resin material 6 can migrate towards tensile stress.

[0062] Furthermore, since the coefficient of linear expansion of resin material 6 is smaller than that of electromagnetic steel plate 4a, the shrinkage of resin material 6 with decreasing temperature is smaller than that of laminated iron core 4d. That is, the axial dimensional difference between resin material 6 and laminated iron core 4d (dimensionality of resin material 6 minus dimensionality of laminated iron core 4d) increases with decreasing temperature. In other words, the aforementioned dimensional difference approaches zero from the negative side with decreasing temperature. Therefore, at high temperatures (e.g., around 180°C), when the stress acting on resin material 6 is tensile stress, the tensile stress acting on resin material 6 is alleviated with decreasing temperature. Moreover, if the tensile stress acting on resin material 6 is alleviated with decreasing temperature, the stress acting on resin material 6 can move from zero to compressive stress.

[0063] Furthermore, since the coefficient of linear expansion of the resin molded part (comparative example) is larger than that of the electromagnetic steel plate 4a, the expansion amount of the resin molded part is greater than that of the laminated iron core 4d as the temperature rises. That is, the axial dimensional difference between the resin molded part and the laminated iron core 4d (size of the resin molded part - size of the laminated iron core 4d) increases with increasing temperature. On the other hand, the axial dimensional difference of the resin molded part decreases as the temperature decreases.

[0064] Furthermore, across the entire temperature range, the axial dimensional difference of the resin material 6 (size of resin material 6 minus size of the laminated iron core 4d) is greater than the axial dimensional difference of the resin molded part (size of the resin molded part minus size of the laminated iron core 4d). That is, across the entire temperature range, the axial dimensional difference of the resin material 6 is close to zero compared to the axial dimensional difference of the resin molded part. Moreover, the difference between the axial dimensional difference of the resin material 6 and the axial dimensional difference of the resin molded part increases as the temperature decreases.

[0065] (Stress acting between the resin material and the magnet during the use of the rotor core)

[0066] In addition, such as Figure 10 As shown, since the coefficient of linear expansion of resin material 6 is larger than that of permanent magnet 5, the expansion amount of resin material 6 is greater than that of permanent magnet 5 with increasing temperature. That is, the axial dimensional difference between resin material 6 and permanent magnet 5 (size of resin material 6 - size of permanent magnet 5) increases with increasing temperature. Therefore, when the residual stress on resin material 6 from permanent magnet 5 at room temperature is tensile stress, the tensile stress on resin material 6 from permanent magnet 5 is alleviated with increasing temperature. Furthermore, as the temperature further increases, the tensile stress on resin material 6 from permanent magnet 5 can migrate from zero to compressive stress.

[0067] Furthermore, as the temperature decreases, the shrinkage of the resin material 6 is greater than that of the permanent magnet 5. That is, the axial dimensional difference between the resin material 6 and the permanent magnet 5 (size of the resin material 6 minus size of the permanent magnet 5) decreases as the temperature decreases. Consequently, the tensile stress on the resin material 6 from the permanent magnet 5 increases as the temperature decreases.

[0068] Furthermore, the coefficient of linear expansion of the resin molded part (comparative example) is the same as that of the resin material 6, but larger than that of the permanent magnet 5. Therefore, as the temperature rises, the tensile stress on the resin molded part from the permanent magnet 5 is reduced, while as the temperature decreases, the tensile stress on the permanent magnet 5 increases.

[0069] Furthermore, across the entire temperature range, the axial dimensional difference of the resin material 6 (size of resin material 6 minus size of permanent magnet 5) is greater than the axial dimensional difference of the resin molded part (comparative example) (size of resin molded part minus size of permanent magnet 5). Additionally, since the coefficient of linear expansion of the resin material 6 is smaller than that of the resin molded part, the difference between the axial dimensional differences of the resin material 6 and the resin molded part increases as the temperature decreases.

[0070] [Effects of this implementation method]

[0071] In this embodiment, the following effect can be obtained.

[0072] In this embodiment, as described above, the rotor core (4) includes a thermosetting resin material (6) that is filled in the magnet housing (10) between the laminated core (4d) and the permanent magnet (5), and that fixes the permanent magnet (5) within the magnet housing (10), and has a coefficient of linear expansion that is less than that of the electromagnetic steel plate (4a). Here, when the thermosetting resin material (6) is cured, the resin material (6) is heated while the molten resin material (6) is injected into the magnet housing (10). At this time, the resin material (6) shrinks while fixed to the laminated core (4d), so the resin material (6) is subjected to tensile stress from the laminated core (4d). In addition, after the resin material (6) is cured, when the laminated core (4d) and the resin material (6) are cooled, the resin material (6) and the laminated core (4d) shrink respectively. At this time, since the coefficient of linear expansion of the resin material (6) is lower than that of the electromagnetic steel plate (4a), the shrinkage of the resin material (6) in the stacking direction of the electromagnetic steel plate (4a) is lower than that of the electromagnetic steel plate (4a) (stacked iron core (4d)). In this case, the tensile stress on the resin material (6) from the stacked iron core (4d) does not increase, so the residual stress of the resin material (6) after the manufacturing process of the rotor iron core (4) can be set to be lower than the tensile stress generated in the curing process of the resin material (6). As a result, compared with the case where the coefficient of linear expansion of the resin material (6) is larger than that of the electromagnetic steel plate (4a), and the tensile stress acting on the resin material (6) during the cooling process of the resin material (6) increases, the residual stress of the resin material (6) after the manufacturing process of the rotor iron core (4) can be reduced. As a result, it is possible to prevent the resin material (6) from breaking during the operation of the rotor (1).

[0073] Furthermore, the coefficient of thermal expansion of the resin material (6) is lower than that of the electromagnetic steel plate (4a). Therefore, even when the temperature of the resin material (6) changes during the operation of the rotor (1), the amount of expansion (contraction) of the resin material (6) can be set to be lower than that of the electromagnetic steel plate (4a). As a result, it is possible to prevent the stress acting on the resin material (6) from increasing during the operation of the rotor (1), and thus it is possible to more reliably prevent the resin material (6) from breaking during the operation of the rotor (1).

[0074] Furthermore, in this embodiment, as described above, the coefficient of linear expansion of the resin material (6) is smaller than that of the electromagnetic steel plate (4a). With this configuration, during the cooling process, the shrinkage of the resin material (6) is less than that of the electromagnetic steel plate (4a) (laminated core (4d)). Therefore, the tensile stress on the resin material (6) from the laminated core (4d) during the cooling process is alleviated. As a result, the residual stress in the resin material (6) after the manufacturing process of the rotor core (4) can be further reduced. Therefore, damage to the resin material (6) during the operation of the rotor (1) can be reliably prevented.

[0075] Furthermore, in this embodiment, as described above, the coefficient of linear expansion of the electromagnetic steel plate (4a) is in the range of 11.5 μm / ℃ or higher and 13 μm / ℃ or lower, and the coefficient of linear expansion of the resin material (6) is in the range of 9 μm / ℃ or higher and 11.5 μm / ℃ or lower. With this configuration, it is easy to make the coefficient of linear expansion of the resin material (6) smaller than that of the electromagnetic steel plate (4a).

[0076] Furthermore, in this embodiment, as described above, the coefficient of linear expansion of the resin material (6) is less than that of the electromagnet plate (4a) but greater than that of the permanent magnet (5). With this configuration, compared to the case where the coefficient of linear expansion of the resin material (6) is greater than that of the electromagnet plate (4a), the coefficient of linear expansion of the resin material (6) can be set to a value close to that of the permanent magnet (5). As a result, the difference in thermal expansion between the resin material (6) and the permanent magnet (5) can be reduced, thus more reliably preventing the resin material (6) from breaking due to the thermal expansion of the permanent magnet (5).

[0077] Furthermore, in this embodiment, as described above, the coefficient of linear expansion of the permanent magnet (5) is in the range of -1.5 μm / ℃ or less and -2.3 μm / ℃ or more. With this configuration, it is easy to make the coefficient of linear expansion of the resin material (6) greater than that of the permanent magnet (5).

[0078] Furthermore, in this embodiment, as described above, the coefficient of linear expansion of the resin material (6) is closer to the value of the coefficient of linear expansion of the electromagnetic steel plate (4a) than the median of the coefficients of linear expansion of the electromagnetic steel plate (4a) and the permanent magnet (5). Here, the larger the coefficient of linear expansion, the higher the mechanical strength of the resin material (6). Therefore, the coefficient of linear expansion of the resin material (6) is closer to the value of the coefficient of linear expansion of the electromagnetic steel plate (4a) than the aforementioned median, thereby preventing the resin material (6) from breaking due to the thermal expansion of the permanent magnet (5) and ensuring the mechanical strength of the resin material (6).

[0079] Furthermore, in this embodiment, as described above, the magnet housing (10) is formed by overlapping the holes (4b) provided in the electromagnetic steel plate (4a) in the axial direction, and is a space that is enclosed around itself. With this configuration, in the stacked iron core (4d) formed by stacking electromagnetic steel plates (4a), a space filled with resin material (6) can be easily formed through the holes (4b).

[0080] Furthermore, in this embodiment, as described above, the resin material (6) is configured to melt by being heated to a first temperature (T1) or higher, and to solidify in the molten state by being heated to a second temperature (T2) or higher than the first temperature (T1). With this configuration, the first temperature (T1) at which the melting of the resin material (6) begins is lower than the second temperature (T2) at which the solidification of the resin material (6) begins, thus preventing the resin material (6) from solidifying before it is injected into the magnet receiving portion (10).

[0081] Furthermore, in this embodiment, as described above, the resin material (6) has a glass transition temperature (T3) that is higher than the second temperature (T2). It is known that the thermosetting resin material (6) has a relatively large coefficient of linear expansion in the range above the glass transition temperature (T3). Therefore, by curing the resin material (6) at a second temperature (T2) that is lower than the glass transition temperature (T3), the coefficient of linear expansion of the resin material (6) can be made relatively low. As a result, it is possible to prevent the coefficient of linear expansion of the resin material (6) from being greater than that of the electromagnetic steel plate (4a).

[0082] In this embodiment, as described above, the method for manufacturing the rotor core (4) includes: after the arrangement step of the permanent magnet (5), a filling step in which molten resin material (6) having a coefficient of linear expansion of less than that of the electromagnetic steel plate (4a) is filled into the space between the laminated core (4d) and the permanent magnet (5) in the magnet housing (10); a curing step after the filling step, in which the resin material (6) is cured by heating; and a cooling step after the curing step, in which the laminated core (4d) and the resin material (6) are cooled. Here, in the curing step, the resin material (6) shrinks while fixed to the laminated core (4d), so the resin material (6) is subjected to tensile stress from the laminated core (4d). In addition, in the cooling step, both the resin material (6) and the laminated core (4d) shrink due to cooling. At this time, since the coefficient of linear expansion of the resin material (6) is lower than that of the electromagnetic steel plate (4a), the shrinkage of the resin material (6) in the stacking direction of the electromagnetic steel plate (4a) is lower than that of the electromagnetic steel plate (4a) (stacked iron core (4d)). In this case, the tensile stress on the resin material (6) from the stacked iron core (4d) does not increase, so the residual stress of the resin material (6) after the manufacturing process of the rotor iron core (4) can be set to be lower than the tensile stress generated in the curing process of the resin material (6). As a result, compared with the case where the coefficient of linear expansion of the resin material (6) is larger than that of the electromagnetic steel plate (4a), and the tensile stress acting on the resin material (6) during the cooling process of the resin material (6) increases, the residual stress of the resin material (6) after the manufacturing process of the rotor iron core (4) can be reduced. As a result, a method for manufacturing a rotor iron core (4) that can prevent the resin material (6) from breaking during the operation of the rotor (1) can be provided.

[0083] Furthermore, in this embodiment, as described above, the filling process involves injecting molten resin material (6) with a coefficient of linear expansion smaller than that of the electromagnetic steel plate (4a) into the magnet housing (10). With this configuration, during the cooling process, the amount of shrinkage of the resin material (6) is less than that of the electromagnetic steel plate (4a) (laminated core (4d)). Consequently, the tensile stress on the resin material (6) from the laminated core (4d) during the cooling process is alleviated. As a result, the residual stress in the resin material (6) after the manufacturing process of the rotor core (4) can be further reduced. Therefore, a method for manufacturing a rotor core (4) that can reliably prevent damage to the resin material (6) during the operation of the rotor (1) can be provided.

[0084] Furthermore, in this embodiment, as described above, the curing process involves the resin material (6) shrinking during curing, thereby causing the resin material (6) to cure while the tensile stress from the laminated iron core (4d) fixed to the resin material (6) acts on the resin material (6). Additionally, the cooling process involves the laminated iron core (4d) shrinking more than the resin material (6), thereby alleviating the tensile stress acting on the resin material (6) during the curing process and cooling both the laminated iron core (4d) and the resin material (6). With this configuration, compared to the case where the laminated iron core (4d) shrinks less than the resin material (6) during the cooling process, thus increasing the tensile stress acting on the resin material (6), the residual stress in the resin material (6) after the rotor core (4) manufacturing process can be easily reduced.

[0085] [Variation Example]

[0086] Furthermore, the embodiments disclosed herein should be considered illustrative rather than restrictive in all respects. The scope of the invention is not limited to the description of the above embodiments but is shown by the technical solutions, and includes all modifications (variations) within the same meaning and scope as the technical solutions.

[0087] For example, in the above embodiment, although an example has been shown where the coefficient of linear expansion of the resin material 6 is smaller than that of the electromagnetic steel plate 4a, the present invention is not limited thereto. The coefficient of linear expansion of the resin material 6 may also be equal to that of the electromagnetic steel plate 4a.

[0088] Furthermore, although the above embodiment shows an example where the coefficient of linear expansion of the resin material 6 is closer to the median of the coefficients of linear expansion of the electromagnet 4a and the permanent magnet 5, the present invention is not limited thereto. The coefficient of linear expansion of the resin material 6 may also be a value closer to the coefficient of linear expansion of the permanent magnet 5 than the aforementioned median.

[0089] Furthermore, although the above embodiment shows an example where the second temperature T2 at which the curing of the resin material 6 begins is smaller than the glass transition temperature T3 of the resin material 6, the present invention is not limited thereto. The second temperature T2 may also be a glass transition temperature T3 or higher.

[0090] Furthermore, the temperature and other parameters shown in the above embodiments are merely examples and can be arbitrarily changed. Additionally, the properties of the resin material 6, the laminated iron core 4d, and the permanent magnet 5 shown in the above embodiments are merely examples and can be arbitrarily changed.

[0091] Explanation of reference numerals in the attached figures

[0092] 4… Rotor core

[0093] 4a…Electromagnetic steel plate

[0094] 4b…hole

[0095] 4D…Layered Iron Core

[0096] 5…Permanent magnets

[0097] 6…Resin materials

[0098] 10…Magnetic Storage Section

[0099] T1…First Temperature

[0100] T2…Second Temperature

[0101] T3… Vitrification temperature.

Claims

1. A rotor core comprising: A stacked iron core, which is constructed by stacking multiple electromagnetic steel plates, includes a magnet housing portion that extends along the stacking direction of the electromagnetic steel plates. A permanent magnet, disposed in the magnet housing portion of the aforementioned stacked iron core; and A thermosetting resin material is used to fill the space between the laminated iron core and the permanent magnet within the magnet housing, thereby fixing the permanent magnet within the magnet housing. This material has a coefficient of linear expansion that is less than or equal to that of the electromagnetic steel plate. The coefficient of linear expansion of the aforementioned resin material is less than that of the aforementioned electromagnetic steel plate.

2. The rotor core according to claim 1, wherein, The linear expansion coefficient of the aforementioned electromagnetic steel sheet is in the range of 11.5 μm / ℃ or higher and 13 μm / ℃ or lower, and the linear expansion coefficient of the aforementioned resin material is in the range of 9 μm / ℃ or higher and 11.5 μm / ℃ or lower.

3. The rotor core according to claim 1, wherein, The coefficient of linear expansion of the aforementioned resin material is greater than that of the aforementioned permanent magnet.

4. The rotor core according to claim 2, wherein, The coefficient of linear expansion of the aforementioned resin material is greater than that of the aforementioned permanent magnet.

5. The rotor core according to claim 3, wherein, The linear expansion coefficient of the aforementioned permanent magnet is in the range of -1.5 μm / ℃ to -2.3 μm / ℃.

6. The rotor core according to claim 4, wherein, The linear expansion coefficient of the aforementioned permanent magnet is in the range of -1.5 μm / ℃ to -2.3 μm / ℃.

7. The rotor core according to any one of claims 3 to 6, wherein, The linear expansion coefficient of the resin material is closer to the linear expansion coefficient of the electromagnetic steel plate than the median of the linear expansion coefficients of the electromagnetic steel plate and the permanent magnet.

8. The rotor core according to any one of claims 1 to 6, wherein, The aforementioned magnet storage section is formed by overlapping the holes provided in the aforementioned electromagnetic steel plate in the axial direction, and is a space that is enclosed in all directions.

9. The rotor core according to claim 7, wherein, The aforementioned magnet storage section is formed by overlapping the holes provided in the aforementioned electromagnetic steel plate in the axial direction, and is a space that is enclosed in all directions.

10. The rotor core according to any one of claims 1 to 6 and 9, wherein, The resin material is configured to melt by being heated to a first temperature or higher, and to solidify by being heated in the molten state to a second temperature or higher than the first temperature.

11. The rotor core according to claim 7, wherein, The resin material is configured to melt by being heated to a first temperature or higher, and to solidify by being heated in the molten state to a second temperature or higher than the first temperature.

12. The rotor core according to claim 8, wherein, The resin material is configured to melt by being heated to a first temperature or higher, and to solidify by being heated in the molten state to a second temperature or higher than the first temperature.

13. The rotor core according to claim 10, wherein, The aforementioned resin material has a higher glass transition temperature than the second temperature mentioned above.

14. The rotor core according to claim 11 or 12, wherein, The aforementioned resin material has a higher glass transition temperature than the second temperature mentioned above.

15. A method for manufacturing a rotor core, comprising a stacked core formed by stacking multiple electromagnetic steel plates and including a magnet housing portion extending along the stacking direction of the electromagnetic steel plates, the method comprising the following steps: In the configuration process, a permanent magnet is placed in the magnet storage section of the aforementioned stacked iron core; In the filling process, after the above-mentioned configuration process, a molten resin material having a coefficient of linear expansion lower than that of the electromagnetic steel plate is filled between the laminated iron core and the permanent magnet in the magnet housing section. The coefficient of linear expansion of the resin material is less than that of the electromagnetic steel plate. The curing process, following the filling process, involves heating the resin material to cure it; and The cooling process involves cooling the laminated iron core and the resin material after the curing process described above.

16. The method for manufacturing a rotor core according to claim 15, wherein, The above-mentioned filling process is a process of injecting the above-mentioned resin material, which has a coefficient of linear expansion smaller than that of the above-mentioned electromagnetic steel plate, into the above-mentioned magnet housing.

17. The method for manufacturing a rotor core according to claim 16, wherein, The curing process described above involves the shrinkage of the resin material during curing, thereby causing the resin material to cure while tensile stress from the laminated iron core fixed to the resin material acts on it. The cooling process described above is a process in which the laminated iron core shrinks more than the resin material, thereby easing the tensile stress acting on the resin material during the curing process and cooling both the laminated iron core and the resin material.

Citation Information

Patent Citations

  • Memory and retrieving device of picture information

    JP1984071176A

  • Crystalline radically polymerizable composition for sealing electric / electronic component, sealing body for electric / electronic component using the composition, and method of manufacturing the sealing body

    JP2018145280A

  • Resin composition for fixing, rotor, automobile, and method for manufacturing rotor

    CN103975506A

  • Rotor of permanent magnet-energized electric machine, has cross linked duroplastic material whose second thermal expansion coefficient and cure temperature is higher than maximum operating temperature of electrical machine

    DE102012017329A1