A method for refining glycolide

Through the spray cooling-continuous crystallization coupling method, the problem of self-polymerization and low purification efficiency of glycolide at high temperatures is solved, the continuous production of high-purity glycolide is achieved, and energy consumption and costs are reduced.

CN115246812BActive Publication Date: 2024-10-11SHANGHAI PUJING CHEM NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110467557.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-28
Publication Date
2024-10-11
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

In the existing polyglycolic acid preparation process, glycolide self-polymerizes at high temperatures, resulting in reduced purity, increased energy consumption and high production costs. Moreover, the purification process efficiency is low, making it difficult to achieve continuous production.

Method used

The spray cooling-continuous crystallization coupling method is used to spray-cool the glycolide vapor or gas phase glycolide generated by cracking into rings. After forming the slurry, it is cooled and crystallized through series crystallization kettles to separate and obtain refined glycolide. And recycle the mother liquor to reduce solvent consumption.

Benefits of technology

It effectively reduces the loss of glycolide, realizes continuous production of refined glycolide, improves product purity and process efficiency, reduces energy consumption and production costs, and avoids the problems of self-polymerization and deterioration and solidification.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a method for refining glycolide, which comprises the following steps: (1) spray cooling glycolide vapor or gas-phase glycolide generated by cracking into rings to obtain slurry 1; (2) treating slurry 1 to obtain a pretreatment solution; (3) introducing the pretreatment solutions into two or more crystallization kettles connected in series one by one to obtain slurry 2; and (4) separating slurry 2 to obtain refined glycolide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer preparation, in particular to a method for purifying glycolide by spray cooling-continuous crystallization coupling. Background Art

[0002] Polyglycolic acid (PGA) is a biodegradable aliphatic polymer that can be hydrolyzed under the catalysis of enzymes or acids and bases in microorganisms or organisms to eventually form carbon dioxide and water. It is a biodegradable material with great development potential. In terms of application, PGA can be used in the field of membrane products in addition to being used in the field of medical and medical device materials. For example, it can be made into agricultural mulch, shopping bags, express bags, packaging bags, fresh-keeping bags, etc. It can also be processed into downhole tool components for hydrocarbon resource recovery (such as bridge plugs, fracturing balls, etc.), temporary plugging agent materials, etc. It can be seen that PGA, as an emerging biodegradable material, has considerable economic benefits and good application prospects.

[0003] Currently, the preparation process of polyglycolic acid includes a route called a two-step process, which is to firstly prepare a polymer with a low molecular weight by condensation of glycolic acid or glycolic acid esters (such as methyl glycolate), then heat the polymer with a low molecular weight and crack it into rings to form glycolide, and then prepare polyglycolic acid by ring-opening polymerization of glycolide.

[0004] In the two-step process, glycolide is an important intermediate product for the synthesis of polyglycolic acid and its copolymers. Glycolide will slowly undergo self-polymerization at room temperature. The higher the temperature and the longer the time, the faster and more obvious the self-polymerization will occur. This uncontrolled self-polymerization will produce low molecular weight polymers and mix them into glycolide, causing the purity of glycolide to decrease. Moreover, since the melting point of low molecular weight polymers is often greater than 180°C, when the content of low molecular weight polymers produced by self-polymerization in glycolide increases, higher temperatures are required to melt glycolide that has undergone a certain degree of self-polymerization, which means greater energy consumption and higher requirements for subsequent separation and purification, which will undoubtedly greatly increase production costs, and there are problems such as reduced glycolide yield and deterioration of quality.

[0005] In the industrial large-scale production process, glycolide is evaporated in the form of gas from the cracking ring reactor under high temperature and high vacuum. If the hot liquid glycolide is collected directly, it will inevitably stay in the heat exchanger, buffer tank, pump, and transmission pipeline of the heating equipment, which further aggravates the deterioration of glycolide. What's more, glycolide staying in the dead zone of the flow of the heating equipment, pipeline, and valve (even if it is only a few millimeters) will also be blocked due to self-polymerization and solidification, which will greatly affect the continuity of production. Although the occurrence of such problems can be minimized by improving, transforming, and modifying the relevant equipment or components, this not only means a significant increase in costs, but also still cannot completely avoid the occurrence of such problems.

[0006] In addition, the current purification process for glycolide usually adopts a recrystallization process. For example, CN110511205A and CN100999516 use organic solvents such as ethyl acetate, acetone, isopropanol, etc. to purify glycolide by recrystallization. However, the glycolide obtained by one recrystallization is not pure enough, and usually 3-5 recrystallizations are required. The solvent consumption is large, the purification cycle is long, the product yield is low, and it is difficult to achieve continuous production.

[0007] Therefore, with respect to the glycolide vapor or gas-phase glycolide generated by the cracking ring reactor, there is an urgent need in the art to provide a process that can effectively reduce glycolide losses and continuously produce refined glycolide. Most of the mother liquor collected after purification can also be recycled to save solvent. Summary of the invention

[0008] The present invention aims to provide a method for refining glycolide by coupling spray cooling and continuous crystallization.

[0009] The present invention provides a method for refining glycolide, which comprises the steps of:

[0010] (1) spray cooling glycolide vapor or gas-phase glycolide generated by cracking into rings to obtain slurry 1;

[0011] (2) treating slurry 1 to obtain a pretreatment solution;

[0012] (3) introducing the pre-treated solutions one by one into two or more crystallization kettles connected in series to obtain slurry 2; and

[0013] (4) Separate slurry 2 to obtain refined glycolide.

[0014] In another embodiment, the solvent used for spray cooling in step (1) comprises at least one of esters, alcohols, ethers, and ketones; the alcohol is selected from C 3-5One or more of saturated monohydric alcohols or polyhydric alcohols; the ester is butyl acetate; the ether is selected from ethylene glycol dimethyl ether and / or n-butyl ether; the ketone is selected from cyclohexanone and / or methyl isobutyl ketone.

[0015] In another embodiment, the amount of solvent used for spray cooling in step (1) is 4-20 times the mass of glycolide vapor or gas-phase glycolide to be treated.

[0016] In another embodiment, the temperature of the solvent used for spray cooling in step (1) is -20°C to 60°C.

[0017] In another embodiment, the treatment in step (2) is to dissolve the solid obtained after solid-liquid separation of slurry 1 to obtain a pretreatment solution; the solvent used to dissolve the solid is at least one of acetates, ketones or methane chloride.

[0018] In another embodiment, the content of glycolic acid dimer is no more than 500 ppm based on the total weight of the pretreatment solution.

[0019] In another embodiment, the temperature of the first crystallization kettle introduced in step (3) is 5-30°C lower than the dissolution temperature of step (2), and the temperature of the last crystallization kettle introduced is not higher than 0°C; for example, the temperature settings from the first to the last crystallization kettle decrease one by one, and the temperature difference between each crystallization kettle and the adjacent crystallization kettle in series is between 5-35°C.

[0020] In another embodiment, the residence time of the introduced pretreatment solution in the crystallization kettle is 5-150 minutes.

[0021] In another embodiment, step (4) separates the slurry 2 into solid and liquid to obtain refined glycolide and mother liquor.

[0022] In another embodiment, the mother liquor of step (4) is returned to step (2) to participate in mixing and adding solvent, and the amount of solvent added is 5-50w / w% of the returned mother liquor; preferably 5-15w / w%.

[0023] Based on this, the present invention provides a process for effectively reducing glycolide loss and continuously producing refined glycolide, and most of the mother liquor collected after purification can be recycled to save solvent. DETAILED DESCRIPTION

[0024] After extensive and in-depth research, the inventors found that the solvent can be directly contacted with the glycolide vapor or gaseous glycolide generated by the cracking ring reactor by spraying, which not only has high cooling efficiency, but also can achieve cooling and capturing of almost 100% glycolide vapor or gaseous glycolide, effectively reducing the loss of glycolide; and using a continuous crystallization kettle, the crystallization mother liquor is recycled to produce refined glycolide. On this basis, the present invention was completed.

[0025] The present invention provides a method for refining glycolide, the method comprising the steps of:

[0026] In the first step, a solvent is used to spray glycolide vapor or gas-phase glycolide to form a slurry 1;

[0027] The second step is to separate the slurry 1 into solid and liquid to obtain a solid material;

[0028] The third step is to mix the solid material with an organic solvent to fully dissolve the solid material to obtain a pretreatment solution;

[0029] The fourth step is to sequentially introduce the pretreated solution into at least two series-connected crystallization kettles with step-wise decreasing temperatures for cooling and crystallization, and obtain slurry 2 from the last crystallization kettle;

[0030] The fifth step is to separate the slurry 2 into solid and liquid to obtain refined glycolide.

[0031] The solvent used in the first step includes at least one of esters, alcohols, ethers and ketones. The ester can be selected from butyl acetate; the alcohol can be selected from one or more of C3-C5 saturated monohydric alcohols or polyhydric alcohols, for example, one or more of n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, ethylene glycol, diethylene glycol, propylene glycol or glycerol; the ether can be selected from one or both of ethylene glycol dimethyl ether or n-butyl ether; the ketone can be selected from one or both of cyclohexanone or methyl isobutyl ketone.

[0032] The inventors have found that in the above-mentioned first step of spraying under high vacuum, if the boiling point of the spray solvent is too low, under the corresponding high vacuum and temperature conditions, the spray solvent will be vaporized and the gas phase glycolide cannot be effectively spray-cooled. However, if the boiling point of the spray solvent is too high, it will be unfavorable for subsequent removal, and more solvent will remain in the liquid phase glycolide, affecting the quality of the liquid phase glycolide.

[0033] In one embodiment of the present invention, the glycolide vapor or gas-phase glycolide in the first step is produced by cracking into a loop reactor.

[0034] In one embodiment of the present invention, the spraying in the first step is performed in a spray cooler.

[0035] In one embodiment of the present invention, the glycolide vapor or gaseous glycolide in the first step is discharged from the side line or top of the cracking loop reactor and directly introduced into the spray cooler from the lower side of the spray cooler.

[0036] As an embodiment, the amount of the spray solvent is 4 to 20 times the mass of glycolide vapor or gas-phase glycolide entering the spray cooler.

[0037] As an embodiment, the spraying temperature of the spraying solvent is set to -20°C to 60°C.

[0038] As an embodiment, the absolute pressure in the spray cooler is not lower than the saturated vapor pressure of the solvent with the largest saturated vapor pressure in the spray solvent. For example, the absolute pressure in the spray cooler is 100-1800Pa.

[0039] As an embodiment, the temperature of the slurry 1 formed by cooling in the spray cooler is not greater than 80°C, preferably not greater than 60°C.

[0040] The solid-liquid separation method in the second step includes, but is not limited to, suction filtration, centrifugation, etc.

[0041] In one embodiment of the present invention, based on the total weight of the solid material obtained in the second step, the content of glycolic acid dimer is no more than 0.25 wt%, preferably no more than 0.23 wt%.

[0042] The organic solvent used in the third step may include at least one of acetates, ketones or methane chlorides. The acetates may be selected from at least one of ethyl acetate or methyl acetate; the ketones may be selected from at least one of acetone, butanone, methyl ethyl ketone or methyl isobutyl ketone; the methane chloride may be selected from at least one of dichloromethane, chloroform or carbon tetrachloride.

[0043] Furthermore, the organic solvent used may also include alcohols, such as one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol or tert-butanol.

[0044] Most preferably, the organic solvent used in the third step is ethyl acetate.

[0045] As an embodiment, the amount of the organic solvent used in the third step is preferably 4-6 times the mass of the solid material.

[0046] As an embodiment, based on the total weight of the pretreatment solution obtained in the third step, the content of glycolic acid dimer does not exceed 500 ppm.

[0047] The third step can be carried out by mixing and dissolving in a container commonly used in the art, such as but not limited to, a stirring kettle, a dissolving agitator, and the like.

[0048] In one embodiment of the present invention, the third step is to add the solid material into a container containing an organic solvent, and heat the container while stirring to fully dissolve the solid material.

[0049] The dissolution temperature in the third step depends on the organic solvent used, as long as the solid material can be completely dissolved, but it should be lower than the boiling point of the organic solvent to avoid unnecessary loss of the solvent.

[0050] In one embodiment of the present invention, the third step is filtered after the solid material is fully dissolved to remove insoluble matter (such as glycolic acid tetramers, pentamers, hexamers and other glycolic acid polymers) in the crude glycolide product, thereby obtaining a pretreated solution.

[0051] As an embodiment, a dissolving agitator is provided between the spray cooler and the at least two crystallization kettles connected in series, and the solid material obtained after solid-liquid separation of the slurry 1 formed by spray cooling is transferred to the dissolving agitator, and the solid material is stirred and dissolved with an organic solvent to obtain a pretreatment solution.

[0052] As an embodiment, the solid material in the dissolving agitator in the third step is stirred and dissolved under normal pressure, and the dissolving agitator can be heated by conventional heating methods. The temperature of the pretreated solution obtained by dissolution is 50-60°C, preferably 60°C.

[0053] The pretreatment solution in the fourth step is sequentially introduced into two or more series-connected crystallization kettles whose temperatures are gradually reduced. The temperature difference between two adjacent series-connected crystallization kettles needs to be conducive to recrystallization, that is, the degree of temperature reduction is conducive to the reduction of the solubility of glycolide in the pretreatment solution, and the solution is saturated and refined glycolide is precipitated. The inventors found that the temperature difference between two adjacent crystallization kettles is too large, which makes the material quenching speed too fast or the degree of quenching too strong. During the process, a large amount of glycolide will be rapidly precipitated and accumulated sharply, so that the glycolide precipitated earlier is pressed by the large amount of glycolide precipitated relatively later, and it is easy to adhere to and be retained on the inner wall of the crystallization kettle, so that when the next batch of materials flows through the crystallization kettle, it is also difficult to carry out the retained materials of the previous batch, thereby causing waste of materials and greatly reducing the final glycolide yield.

[0054] By using multiple crystallization kettles, before the material reaches the last crystallization kettle, the appropriate temperature difference between the two adjacent crystallization kettles can be used to appropriately reduce the quenching speed or degree of the material, so that the glycolide in the material can be precipitated more gently, which is beneficial to minimize or eliminate the retention of the precipitated glycolide in the crystallization kettle. Even if a small amount of retention occurs, the retained glycolide can be easily carried out by the next batch of materials.

[0055] The term "crystallization kettle" in the present invention has the common meaning in the art, that is, refers to a container capable of controlling the temperature within a certain range.

[0056] As an embodiment, the at least two crystallization kettles connected in series both adopt side line feeding, and the side line of the next crystallization kettle is connected to the bottom discharge port of the previous crystallization kettle.

[0057] In one embodiment of the present invention, the side line of the first crystallization kettle in the at least two crystallization kettles connected in series in the fourth step is connected to the bottom liquid outlet of the dissolving agitator used in the third step.

[0058] In one embodiment of the present invention, the temperature difference between each crystallization kettle and its adjacent crystallization kettle connected in series is between 5-35°C.

[0059] The temperature of the first crystallization kettle into which the pretreatment solution is introduced in the fourth step is 5-30°C lower than the dissolution temperature in the third step, and the temperature of the last crystallization kettle into which the pretreatment solution is introduced generally does not exceed 0°C.

[0060] As an embodiment, in the at least two crystallization kettles connected in series and arranged with the temperature decreasing in a stepwise manner, the temperature of the first crystallization kettle is lower than the temperature of the pretreatment solution.

[0061] In one embodiment of the present invention, the crystallization kettle described in the fourth step is 5 series crystallization kettles with the temperature decreasing in a step-by-step manner, wherein the temperature of the first crystallization kettle is set to 42°C, the temperature of the second crystallization kettle is set to 30°C, the temperature of the third crystallization kettle is set to 18°C, the temperature of the fourth crystallization kettle is set to 10°C, and the temperature of the fifth crystallization kettle is set to -5°C.

[0062] In one embodiment of the present invention, the crystallization kettle in the fourth step is 4 crystallization kettles connected in series with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 35°C, the temperature of the second crystallization kettle is set to 18°C, the temperature of the third crystallization kettle is set to 5°C, and the temperature of the fourth crystallization kettle is set to -5°C.

[0063] In one embodiment of the present invention, the crystallization kettle in the fourth step is three crystallization kettles connected in series with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 40°C, the temperature of the second crystallization kettle is set to 12°C, and the temperature of the third crystallization kettle is set to -5°C.

[0064] In one embodiment of the present invention, the crystallization kettle in the fourth step is two crystallization kettles connected in series with the temperature decreasing in a stepwise manner, wherein the temperature of the first crystallization kettle is set to 32°C, and the temperature of the second crystallization kettle is set to -2°C.

[0065] The pretreatment solution introduced into the crystallization kettle in the fourth step needs to stay in the crystallization kettle for a period of time, such as 5-150 minutes; in one embodiment of the present invention, the higher the temperature of the crystallization kettle, the longer the stay time is generally.

[0066] The solid-liquid separation in the fifth step can be carried out by a method commonly used in the art, such as but not limited to centrifugation.

[0067] In one embodiment of the present invention, the solid material obtained by centrifuging the slurry 2 in the fifth step can be dried to obtain refined glycolide. The drying can be carried out by conventional methods in the art, such as but not limited to vacuum drying at 40-60°C and absolute pressure ≤500Pa for 1-2 hours.

[0068] The glycolide purity of the refined glycolide or the refined glycolide product obtained by the present invention can reach more than 99.5%, the residual solvent rate is ≤0.3%, the glycolic acid content is less than 0.03wt%, the glycolic acid dimer content is less than 0.03wt%, and the water content is less than 0.03wt%. The contents of glycolide, residual solvent and glycolic acid dimer in the present invention are all measured by gas chromatography analysis method known in the art, the water content is measured by Karl Fischer moisture meter, and the glycolic acid content is measured by potentiometric titration method known in the art (for example, automatic potentiometric titrator).

[0069] In one embodiment of the present invention, the fifth step is to separate the solid and liquid of slurry 2 to obtain refined glycolide and mother liquor; then the mother liquor is returned to the third step to be mixed with the solid material newly obtained from the second step, and then the third to fifth steps are carried out in a continuous cycle, thereby continuously obtaining refined glycolide.

[0070] In one embodiment of the present invention, the solvent lost after drying in the fifth step is collected (for example but not limited to, collected by a heat exchanger) and mixed with the mother liquor. A very small amount of solvent will exist in the dried refined glycolide, which can be ignored if measured in kg.

[0071] In the fifth step, the mother liquor is returned to the container for mixing in the third step, and the container contains the second batch of solid materials from the second step, the mother liquor returned from the fifth step, and the supplemented organic solvent. Then, the pre-treated solution obtained by sufficient dissolution is subjected to the fourth step of the second batch and the following steps, thereby carrying out the second batch of production of refined glycolide. Similarly, the third batch, the fourth batch, and other batches are carried out to achieve continuous circulation / production. Based on the consideration of material balance in industrial production, the next batch cycle will bring out the residual or accumulated materials in the previous batch cycle. From the appearance point of view, the amount of refined glycolide obtained in the next batch is basically the same as that in the previous batch.

[0072] The determination of how many batches of such circulation / production are to be carried out generally depends on the accumulated glycolic acid dimer content in the mother liquor to be returned to the third step in the fifth step or the glycolic acid and / or glycolic acid dimer content in the obtained refined glycolide product.

[0073] In one embodiment of the present invention, the supplemented organic solvent is about 5-50 w / w% of the returned mother liquor, for example but not limited to, about 5-15 w / w%, about 8-12 w / w%, about 9-11 w / w%, etc.

[0074] In one embodiment of the present invention, if the accumulated glycolic acid dimer content in the mother liquor to be returned to the third step exceeds 1000 ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03 wt%, the fifth step is stopped.

[0075] Once a round of continuous production process of multiple batches of purified glycolide of the present invention is completed, a new round of such continuous production process can be started, in which all newly added organic solvent is used in the above third step (instead of the mother liquor returned in the above fifth step and the supplementary organic solvent).

[0076] The various solvents used in the present invention are all of reagent grade and do not require further treatment.

[0077] The inventors found that the crude glycolide product obtained by the cracking ring reactor was stored at about 85°C, and its purity decreased from about 95.7% to about 88.2% after about 5 hours, and its purity decreased from about 95.7% to about 77.5% after about 12 hours, which caused the melting point of the product to increase from about 79°C to about 135°C; while the crude glycolide product obtained by the cracking ring reactor was stored at about 25°C, and its purity decreased from about 95.7% to about 95.3% after about 5 hours, and its purity decreased from about 95.7% to about 92.3% after about 48 hours, and the melting point of the product did not change much (melting point was about 82°C). It can be seen that for the crude glycolide product obtained by the cracking ring reactor, the higher the temperature, the easier it is to deteriorate, and the lower the purity, and the decrease in purity means that more purification costs will be required later.

[0078] Based on the above findings, the inventors of the present technology use a process of coupling spray cooling with continuous crystallization to purify glycolide, that is, the glycolide vapor or gaseous glycolide generated by the cracking ring reactor is first directly introduced into a spray cooler for spray cooling, so that the glycolide vapor or gaseous glycolide and the spray solvent undergo sufficient heat exchange to obtain a glycolide-containing slurry at a lower temperature. This completely avoids the retention of conventionally directly collected hot liquid glycolide in a high temperature state, which not only effectively inhibits or reduces the degree of self-polymerization of glycolide, but also avoids the deterioration of hot liquid glycolide during pipeline transportation. The phenomenon of solidification and clogging of the pipeline occurs, and the large amount of solvent in the slurry can play a good role in promoting the flow of glycolide, and can clean the flow dead zone of the conveying pipeline, valves, etc., which is beneficial to ensure the continuity of the entire glycolide production process; the slurry obtained by spray cooling is then separated into solid and liquid, and the obtained solid material is dissolved and then continuously cooled and crystallized to obtain refined glycolide. Compared with the existing conventional recrystallization method, it can significantly save the use of solvent, there is no need to carry out the residual solvent removal process, there is no waste liquid treatment problem, and there is no pollution to the environment.

[0079] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0080] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0081] In this document, all features defined in the form of numerical ranges or percentage ranges, such as values, quantities, contents and concentrations, are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values ​​within the range (including integers and fractions).

[0082] The above-mentioned features mentioned in the present invention or the features mentioned in the embodiments can be combined in any way. All the features disclosed in the specification of this case can be used in combination with any combination form. As long as there is no contradiction in the combination of these features, all possible combinations should be considered to be within the scope of this specification. Each feature disclosed in the specification can be replaced by any alternative feature that can provide the same, equal or similar purpose. Therefore, unless otherwise specified, the disclosed features are only general examples of equal or similar features.

[0083] The main advantages of the present invention are:

[0084] 1. The present invention creatively couples spray cooling with continuous crystallization, which can not only completely avoid the retention of conventional directly collected hot liquid glycolide in a high temperature state, thereby effectively inhibiting or reducing the degree of self-polymerization of glycolide, and avoiding the phenomenon of hot liquid glycolide blocking the pipeline due to deterioration and solidification during pipeline transportation, but also greatly save the amount of solvent used in the purification process of glycolide, without the need for residual solvent removal process, no waste liquid treatment problem, no pollution to the environment, the whole process flow has good continuity and stability, can effectively avoid unnecessary material loss, reduce process costs, low energy consumption, and facilitate the realization of low-carbon industry to expand production.

[0085] 2. The production method provided by the present invention can realize continuous cycle production.

[0086] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following examples are usually performed under normal conditions or according to the conditions recommended by the manufacturer. Unless otherwise specified, all percentages, ratios, proportions, or parts are by weight. The units in the weight volume percentages in the present invention are well known to those skilled in the art, for example, refer to the weight (grams) of the solute in 100 ml of solution. Unless otherwise defined, all professional and scientific terms used in the text have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar or equivalent to the recorded content can be applied to the method of the present invention. The preferred implementation methods and materials described in the text are for demonstration purposes only.

[0087] In the following embodiments, the contents of glycolide, residual solvent and glycolic acid dimer in the obtained refined glycolide product are measured by gas chromatography analysis method known in the art, the water content is measured by Karl Fischer moisture meter, and the glycolic acid content is measured by potentiometric titration method known in the art (for example, using automatic potentiometric titrator).

[0088] Example 1 (Spray Cooling + Five-Kettle Continuous Crystallization)

[0089] 10kg of glycolide vapor generated by the cracking ring reactor is discharged through the side line and directly introduced into the spray cooler through the lower side of the spray cooler. The spray solvent used in the spray cooler is a mixture of n-propanol and butyl acetate in a mass ratio of 2:1. The total amount of the spray solvent is about 180kg, the spray temperature is about -10°C, and the absolute pressure in the spray cooler is about 100Pa. The spray solvent is sprayed from top to bottom and contacts with the glycolide vapor entering from the lower side of the spray cooler. The slurry (about 190kg, the temperature is about 5°C) formed by spray cooling is collected at the bottom of the spray cooler, and then the slurry is introduced into a centrifuge for centrifugal separation, and the solid material (about 9.6kg) is retained, and then the solid material is transferred The pretreatment solution was introduced into a first crystallization kettle at a temperature of about 42°C for a residence time of about 120 min, and then introduced into a second crystallization kettle at a temperature of about 30°C for a residence time of about 90 min, and then introduced into a third crystallization kettle at a temperature of about 18°C ​​for a residence time of about 50 min, and then introduced into a fourth crystallization kettle at a temperature of about 10°C for a residence time of about 35 min, and then introduced into a fifth crystallization kettle at a temperature of about -5°C for a residence time of about 15 min. Then, about 57.6 kg of the slurry from the fifth crystallization kettle was centrifuged, and the obtained solid was dried at 60° C. and absolute pressure ≤500 Pa for 1 hour to obtain about 7.9 kg of refined glycolide, with a yield of 82.3% (the yield was calculated based on the solid material separated by the centrifuge), and about 80% (i.e., about 39.8 kg) of the obtained mother liquor of about 49.7 kg (the solvent lost after drying will be collected (for example, collected by a heat exchanger) and mixed with the mother liquor. A very small amount of solvent will exist in the refined glycolide after drying, which can be ignored if measured in kg) was returned to the dissolving and stirring device, and about 9.2 kg of ethyl acetate solvent was added to the dissolving and stirring device to mix with the next batch of ethyl acetate solvents entering the dissolving and stirring device. After 8.6 kg of solid materials were mixed, the temperature was raised to about 50° C. while stirring to fully dissolve the solid materials, and a pre-treated solution (about 57.6 kg, wherein the content of glycolic acid dimer was ≤500 ppm) was obtained. The pre-treated solution was then introduced into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, about 57.6 kg of the slurry obtained from the fifth crystallization kettle was centrifuged, and the solid was retained. The mixture was dried at 60° C. and an absolute pressure of ≤500 Pa for 1 hour to obtain about 7.9 kg of refined glycolide (to achieve continuous circulation, the second batch circulation will bring out the residual or accumulated materials in the first batch circulation process. Apparently, the amount of refined glycolide obtained in the first batch and the second batch is the same), with a yield of 91.9% (the yield is calculated based on the solid material put into the dissolving and stirring device), and about 80% (about 39.8kg) of the separated mother liquor of about 49.7kg is returned to the dissolving and stirring device, and so on, the continuous production of refined glycolide is carried out.

[0090] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.88wt%, the content of residual solvent is about 0.07wt%, the content of glycolic acid is about 0.0103wt%, the content of glycolic acid dimer is about 0.0102wt%, and the water content is less than 0.03wt%;

[0091] In the second batch of refined glycolide products, the content of glycolide was about 99.88wt%, the content of residual solvent was about 0.07wt%, the content of glycolic acid was about 0.0107wt%, the content of glycolic acid dimer was about 0.0106wt%, and the water content was less than 0.03wt%;

[0092] In the refined glycolide product produced in the third batch, the glycolide content was about 99.88wt%, the residual solvent content was about 0.07wt%, the glycolic acid content was about 0.0113wt%, the glycolic acid dimer content was about 0.0114wt%, and the water content was <0.03wt%.

[0093] Only three batches of refined glycolide products are listed here, but it should be noted that the pretreated solution formed in the dissolver agitator can be continuously introduced into the first crystallization kettle for continuous cooling and crystallization, so that the fourth batch, the fifth batch, the sixth batch... and even the Nth batch can be continuously produced until the accumulated glycolic acid dimer content in the mother liquor to be returned to the dissolver agitator exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new solvent is replaced in the dissolver agitator, and then new continuous production is restarted.

[0094] Example 2 (Spray Cooling + Four-Kettle Continuous Crystallization)

[0095] 10kg of glycolide vapor generated by the cracking ring reactor is discharged through the side line and directly introduced into the spray cooler through the lower side of the spray cooler. The spray solvent used in the spray cooler is a mixture of n-propanol and isopropanol in a mass ratio of 1:1. The total amount of the spray solvent is about 100kg, the spray temperature is about -20°C, and the absolute pressure in the spray cooler is about 200Pa. The spray solvent is sprayed from top to bottom and contacts with the glycolide vapor entering from the lower side of the spray cooler. The slurry (about 110kg, the temperature is about 12°C) formed by spray cooling is collected at the bottom of the spray cooler, and then the slurry is introduced into a centrifuge for centrifugal separation, and the solid material (about 9.1kg) is retained, and then the solid material is transferred to The mixture was placed in a dissolving agitator containing 36.4 kg of solvent (mixed by ethyl acetate and ethanol in a mass ratio of 2:1), and the temperature was raised to about 60°C while stirring to fully dissolve the solid material to obtain a pre-treated solution (about 45.5 kg, wherein the content of glycolic acid dimer is ≤500 ppm), and the pre-treated solution was then introduced into a first crystallization kettle at a temperature of about 35°C for a residence time of about 100 min, and then introduced into a second crystallization kettle at a temperature of about 18°C ​​for a residence time of about 60 min, and then introduced into a third crystallization kettle at a temperature of about 5°C for a residence time of about 30 min, and then introduced into a fourth crystallization kettle at a temperature of about -5°C for a residence time of about 8 min, and then the slurry of the fourth crystallization kettle was about 45 .5kg is centrifuged, and the solid obtained is dried at 52°C and absolute pressure ≤500Pa for 2 hours to obtain about 7.5kg of refined glycolide with a yield of 82.4% (the yield is calculated based on the solid material separated by the centrifuge), and about 90% (i.e., about 34.2kg) of the mother liquor of about 38kg (the solvent lost after drying will be collected (for example, collected by a heat exchanger) and mixed with the mother liquor. A very small amount of solvent will exist in the refined glycolide after drying, which can be ignored if measured in kg) is returned to the dissolving and stirring device, and about 3.2kg of solvent (mixed by ethyl acetate and ethanol in a mass ratio of 2:1) is added to the dissolving and stirring device to mix with the next batch of solvents entering the dissolving and stirring device. After mixing with 8.1 kg of solid materials, the mixture was heated to about 60° C. while stirring to fully dissolve the solid materials, and a pre-treated solution (about 45.5 kg, wherein the content of glycolic acid dimer is ≤500 ppm) was obtained. The pre-treated solution was then introduced into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, about 45.5 kg of slurry obtained from the fourth crystallization kettle was centrifuged, and the solid was retained. The mixture was dried at 52° C. and an absolute pressure of ≤500 Pa for 2 hours to obtain about 7.5 kg of refined glycolide (to achieve continuous circulation, the second batch circulation will bring out the residual or accumulated materials in the first batch circulation process. Apparently, the amount of refined glycolide obtained in the first batch and the second batch is the same), with a yield of 92.6% (the yield is calculated based on the solid material put into the dissolving stirrer), and about 90% (about 34.2kg) of the separated mother liquor of about 38kg is returned to the stirring tank, and so on, the continuous production of refined glycolide is carried out.

[0096] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.85wt%, the content of residual solvent is about 0.1wt%, the content of glycolic acid is about 0.0112wt%, the content of glycolic acid dimer is about 0.0105wt%, and the water content is less than 0.03wt%;

[0097] In the second batch of refined glycolide products, the content of glycolide is about 99.85wt%, the content of residual solvent is about 0.1wt%, the content of glycolic acid is about 0.0115wt%, the content of glycolic acid dimer is about 0.0109wt%, and the water content is less than 0.03wt%;

[0098] In the third batch of refined glycolide products, the glycolide content was about 99.85wt%, the residual solvent content was about 0.1wt%, the glycolic acid content was about 0.0120wt%, the glycolic acid dimer content was about 0.0115wt%, and the water content was <0.03wt%.

[0099] Only three batches of refined glycolide products are listed here, but it should be noted that the pretreated solution formed in the dissolver agitator can be continuously introduced into the first crystallization kettle for continuous cooling and crystallization, so that the fourth batch, the fifth batch, the sixth batch... and even the Nth batch can be continuously produced until the accumulated glycolic acid dimer content in the mother liquor to be returned to the dissolver agitator exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new solvent is replaced in the dissolver agitator, and then new continuous production is restarted.

[0100] Example 3 (Spray Cooling + Three-Kettle Continuous Crystallization)

[0101] About 10 kg of glycolide vapor generated by the cracking ring reactor is discharged through the side line and directly introduced into the spray cooler through the lower side of the spray cooler. The spray solvent used in the spray cooler is glycerol. The total amount of the spray solvent is about 200 kg. The spray temperature is about 60° C. The absolute pressure in the spray cooler is about 1800 Pa. The spray solvent is sprayed from top to bottom and contacts with the glycolide vapor entering from the lower side of the spray cooler. The slurry (about 210 kg, the temperature is about 68° C.) formed by spray cooling is collected at the bottom of the spray cooler, and then the slurry is introduced into a centrifuge for centrifugal separation, and the solid material (about 9.4 kg) is retained. Then the solid material is transferred to a centrifuge containing 47 kg of solvent (composed of acetone and methyl acetate). The mixture was placed in a dissolving agitator (mixed with glycolide in a mass ratio of 1:4) and heated to about 60°C while stirring to fully dissolve the solid material to obtain a pre-treated solution (about 56.4kg, wherein the content of glycolic acid dimer is ≤500ppm), and then the pre-treated solution was introduced into a first crystallization kettle at a temperature of about 40°C for a residence time of about 95min, then introduced into a second crystallization kettle at a temperature of about 12°C for a residence time of about 30min, and then introduced into a third crystallization kettle at a temperature of about -5°C for a residence time of about 10min, and then about 56.4kg of the slurry in the third crystallization kettle was centrifuged, and the obtained solid was dried at 40°C and an absolute pressure of ≤500Pa for 2 hours to obtain about 7.3kg of refined glycolide. The yield is 77.6%% (the yield is calculated based on the solid material separated by the centrifuge), and about 90% (about 44.2kg) of the obtained mother liquor of about 49.1kg (the solvent lost after drying will be collected (for example, collected by a heat exchanger) and mixed with the mother liquor. There will be a very small amount of solvent in the refined glycolide after drying, which can be ignored if measured in kg) is returned to the dissolving agitator, and then about 4.5kg of solvent (mixed by acetone and methyl acetate in a mass ratio of 1:4) is added to the dissolving agitator. After mixing with the next batch of solid materials entering the dissolving agitator, 7.7kg, the temperature is raised to about 60°C while stirring to fully dissolve the solid materials, and a pre-treated solution (about 56.4kg) is obtained. , wherein the content of glycolic acid dimer is ≤500ppm), then the pretreated solution is introduced into the first crystallization kettle for subsequent continuous cooling crystallization, and finally about 56.4kg of the slurry obtained from the third crystallization kettle is centrifuged, and the solid is retained, and dried at 40°C and absolute pressure ≤500Pa for 2 hours to obtain about 7.3kg of refined glycolide (to achieve continuous circulation, the second batch circulation will bring out the residual or accumulated materials in the first batch circulation process, and the amount of refined glycolide obtained in the first batch and the second batch is the same), with a yield of 94.8% (the yield calculated based on the solid material put into the dissolving stirrer), and about 90% of the separated mother liquor of about 49.1kg (that is, about 44.2kg) is then returned to the stirring tank, and so on, to carry out the continuous production of refined glycolide.

[0102] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.83wt%, the content of residual solvent is about 0.12wt%, the content of glycolic acid is about 0.0122wt%, the content of glycolic acid dimer is about 0.0127wt%, and the water content is less than 0.03wt%;

[0103] In the second batch of refined glycolide products, the content of glycolide was about 99.83wt%, the content of residual solvent was about 0.12wt%, the content of glycolic acid was about 0.0125wt%, the content of glycolic acid dimer was about 0.0131wt%, and the water content was less than 0.03wt%;

[0104] In the refined glycolide product produced in the third batch, the glycolide content was about 99.83wt%, the residual solvent content was about 0.12wt%, the glycolic acid content was about 0.0132wt%, the glycolic acid dimer content was about 0.0139wt%, and the water content was <0.03wt%.

[0105] Only three batches of refined glycolide products are listed here, but it should be noted that the pretreated solution formed in the dissolver agitator can be continuously introduced into the first crystallization kettle for continuous cooling and crystallization, so that the fourth batch, the fifth batch, the sixth batch... and even the Nth batch can be continuously produced until the accumulated glycolic acid dimer content in the mother liquor to be returned to the dissolver agitator exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new solvent is replaced in the dissolver agitator, and then new continuous production is restarted.

[0106] Example 4 (Spray Cooling + Two-Kettle Continuous Crystallization)

[0107] About 10 kg of glycolide vapor generated by the cracking ring reactor is discharged through the side line and directly introduced into the spray cooler through the lower side of the spray cooler. The spray solvent used in the spray cooler is a mixture of n-butyl ether, methyl isopropyl ketone and cyclohexanone in a mass ratio of 3:1:1. The total amount of the spray solvent is about 40 kg, the spray temperature is about 12°C, and the absolute pressure in the spray cooler is about 300 Pa. The spray solvent is sprayed from top to bottom and contacts with the glycolide vapor entering from the lower side of the spray cooler. The slurry (about 50 kg, the temperature is about 53°C) formed by spray cooling is collected at the bottom of the spray cooler, and then the slurry is introduced into a centrifuge for centrifugal separation, and the solid material (about 9.8 kg) is retained, and then the solid material is converted to The mixture was transferred to a dissolving agitator containing 58.8 kg of solvent (mixed by ethyl acetate, isopropanol and butanone in a mass ratio of 7:2:1), and the temperature was raised to about 60°C while stirring to fully dissolve the solid material to obtain a pre-treated solution (about 68.6 kg, wherein the content of glycolic acid dimer is ≤500 ppm), and then the pre-treated solution was introduced into a first crystallization kettle at a temperature of about 32°C, the residence time was about 60 min, and the acidity of the slurry was about 480 ppm, and then introduced into a second crystallization kettle at a temperature of about -2°C, the residence time was about 15 min, and then about 68.6 kg of the slurry in the second crystallization kettle was centrifuged, and the obtained solid was dried at 60°C and an absolute pressure of ≤500 Pa for 2 hours to obtain about 70% of refined glycolide. .4kg, with a yield of 75.5% (the yield is calculated based on the solid material separated by the centrifuge), and about 50% (i.e., about 30.6kg) of the obtained mother liquor of about 61.2kg (the solvent lost after drying will be collected (for example, collected by a heat exchanger) and mixed with the mother liquor. There will be a very small amount of solvent in the refined glycolide after drying, which can be ignored if measured in kg) is returned to the dissolving agitator, and then about 29.4kg of solvent (mixed by ethyl acetate, isopropanol, and butanone in a mass ratio of 7:2:1) is added to the dissolving agitator, mixed with the next batch of solid material 8.6kg entering the dissolving agitator, and heated to about 60°C while stirring to fully dissolve the solid material to obtain a pre-treated solution ( The pre-treated solution was then introduced into the first crystallization kettle for subsequent continuous cooling and crystallization. Finally, the slurry of about 68.6 kg obtained from the second crystallization kettle was centrifuged, and the solid was retained. It was dried at 60°C and an absolute pressure of ≤500 Pa for 2 hours to obtain about 7.4 kg of refined glycolide (to achieve continuous circulation, the second batch circulation will bring out the residual or accumulated materials in the first batch circulation process. Apparently, the amount of refined glycolide obtained in the first batch and the second batch is the same), with a yield of 86% (the yield is calculated based on the solid material put into the dissolving stirrer), and about 50% of the separated mother liquor of about 61.2 kg (that is, about 30.6kg) is then returned to the stirring tank, and so on, to carry out the continuous production of refined glycolide.

[0108] Based on the above steps, in the first batch of refined glycolide products produced by the method of this embodiment, the content of glycolide is about 99.87wt%, the content of residual solvent is about 0.08wt%, the content of glycolic acid is about 0.0138wt%, the content of glycolic acid dimer is about 0.0131wt%, and the water content is less than 0.03wt%;

[0109] In the second batch of refined glycolide products, the content of glycolide was about 99.87wt%, the content of residual solvent was about 0.08wt%, the content of glycolic acid was about 0.0144wt%, the content of glycolic acid dimer was about 0.0139wt%, and the water content was less than 0.03wt%;

[0110] In the refined glycolide product produced in the third batch, the glycolide content was about 99.87wt%, the residual solvent content was about 0.08wt%, the glycolic acid content was about 0.0153wt%, the glycolic acid dimer content was about 0.0150wt%, and the water content was less than 0.03wt%.

[0111] Only three batches of refined glycolide products are listed here, but it should be noted that the pretreated solution formed in the dissolver agitator can be continuously introduced into the first crystallization kettle for continuous cooling and crystallization, so that the fourth batch, the fifth batch, the sixth batch... and even the Nth batch can be continuously produced until the accumulated glycolic acid dimer content in the mother liquor to be returned to the dissolver agitator exceeds 1000ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide product exceeds 0.03wt%, the continuous production is stopped, new solvent is replaced in the dissolver agitator, and then new continuous production is restarted.

[0112] Comparative Example

[0113] In this comparative example, a low boiling point solvent (e.g., methanol) is used as the spray solvent. Under the selected conditions of an absolute pressure of 100-1800 Pa and a temperature of -20°C to 60°C, methanol will quickly turn into gas when entering the spray cooler, making it impossible to spray cool the glycolide vapor from the cracking ring reactor, resulting in the inability to carry out subsequent process operations.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of the substantial technical content of the present invention. The substantial technical content of the present invention is broadly defined in the scope of the claims of the application. Any technical entity or method completed by others, if it is exactly the same as that defined in the scope of the claims of the application or an equivalent variation, will be deemed to be included in the scope of the claims.

Claims

1. A method for refining glycolide, It is characterized in that The method comprises the steps of: (1) spray cooling the glycolide vapor or gas-phase glycolide generated by cleavage to obtain slurry 1, wherein the solvent used for spray cooling comprises at least one of esters, alcohols, ethers, and ketones, and the temperature of the solvent used for spray cooling is -20°C to 60°C; the alcohol is selected from C 3-5 One or more saturated monohydric alcohols or polyhydric alcohols; (2) dissolving the solid material obtained after solid-liquid separation of slurry 1 to obtain a pretreatment solution, wherein the content of glycolic acid dimer is no more than 0.25 wt % based on the total weight of the solid material; (3) introducing the pretreated solutions one by one into two or more crystallization kettles connected in series to obtain slurry 2; (4) The slurry 2 is subjected to solid-liquid separation to obtain refined glycolide and a mother liquor, and the mother liquor is returned to step (2) to participate in dissolution. When the accumulated glycolic acid dimer content in the mother liquor exceeds 1000 ppm or the content of glycolic acid and / or glycolic acid dimer in the obtained refined glycolide exceeds 0.03 wt %, the mother liquor is stopped from being returned to step (2).

2. The method according to claim 1, It is characterized in that The temperature of slurry 1 is not more than 80°C.

3. The method according to claim 1, It is characterized in that The ester is butyl acetate.

4. The method according to claim 1, It is characterized in that The ethers are selected from ethylene glycol dimethyl ether and / or n-butyl ether.

5. The method according to claim 1, It is characterized in that The ketones are selected from cyclohexanone and / or methyl isobutyl ketone.

6. The method according to claim 1, It is characterized in that The amount of solvent used for spray cooling in step (1) is 4-20 times the mass of glycolide vapor or gas-phase glycolide to be treated.

7. The method according to claim 1, It is characterized in that Based on the total weight of the pretreatment solution, the content of glycolic acid dimer is no more than 500 ppm.

8. The method according to claim 1, It is characterized in that The solvent used to dissolve the solid material is at least one of acetates, ketones or methane chloride.

9. The method according to claim 1, It is characterized in that The temperature of the first crystallization kettle introduced in step (3) is 5-30°C lower than the dissolution temperature of step (2), and the temperature of the last crystallization kettle introduced is not higher than 0°C.

10. The method according to claim 9, It is characterized in that The temperature settings of the first to the last crystallization kettles are gradually decreased, and the temperature difference between each crystallization kettle and the adjacent crystallization kettles in series is between 5-35°C.

11. The method according to claim 1, It is characterized in that The introduced pretreatment solution stays in the crystallization kettle for 5-150 minutes.

12. The method of claim 1, It is characterized in that The mother liquor of step (4) is returned to step (2) to participate in mixing and adding solvent, and the amount of solvent added is 5-50w / w% of the returned mother liquor.

13. The method according to claim 12, It is characterized in that The mother liquor of step (4) is returned to step (2) to participate in mixing and adding solvent, and the amount of solvent added is 5-15w / w% of the returned mother liquor.

14. The method of claim 1, It is characterized in that The glycolide purity in the refined glycolide is above 99.5%, the residual solvent rate is ≤0.3%, the glycolic acid content is <0.03wt%, the glycolic acid dimer content is <0.03wt%, and the water content is <0.03wt%.