Preparation method and application of high-efficiency defoaming agent

Silicone-polymer-silicon triblock polymer prepared by reacting dimeric acid diallyl ethoxy ether ester with single-ended hydrogen-containing polysiloxane in an aqueous two-component PU system, solving The traditional defoaming agent has difficulty in balancing the defoaming efficiency and compatibility, and has achieved efficient defoaming and excellent compatibility, which has improved the leveling effect of the paint film.

CN115253393BActive Publication Date: 2024-11-05POLYONTECH ADVANCED MATERIAL SHANGHAI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210885527.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-26
Publication Date
2024-11-05
Estimated Expiration
2042-07-26

AI Technical Summary

Technical Problem

Traditional silicone defoamers are difficult to balance the defoaming efficiency and compatibility in aqueous two-component PU systems, resulting in the possibility of shrinkage and negative impacts under high addition amounts.

Method used

The silicone-polymer-silicon triblock polymer is prepared by reacting diallyl ethoxy ether ester with a single-ended hydrogen-containing polysiloxane to serve as a high-efficiency defoaming agent. Optimize molecular chain structure to improve defoaming performance and compatibility.

Benefits of technology

It achieves excellent defoaming effect and compatibility in aqueous two-component PU system, avoids shrinkage and negative effects, and significantly improves the leveling effect of the paint film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003765738860000021
    Figure BDA0003765738860000021
  • Figure BDA0003765738860000022
    Figure BDA0003765738860000022
  • Figure BDA0003765738860000031
    Figure BDA0003765738860000031
Patent Text Reader

Abstract

The present invention discloses a high-efficiency defoamer, characterized in that the high-efficiency defoamer is a polymer of organosilicon-polymer-organosilicon triblock as shown in the following formula 3. The present invention also discloses a preparation method and application thereof. The present invention controls the content of oligomers of dimer acid diallyl ethoxy ether ester in the middle of the molecular chain, and has excellent compatibility and defoaming efficiency regardless of high content of silicone oil or low content of silicone oil. Moreover, the defoamer will not produce shrinkage holes and negative effects on the water-based two-component PU system at a high addition amount.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of defoamers, and in particular to a preparation method and application of a high-efficiency defoamer. Background Art

[0002] Foams are two-phase systems consisting of gas bubbles, such as air, dispersed in a liquid. They usually show a cellular structure in which the gas-containing cells are surrounded by a liquid film. (Meta) Stable foams require the presence of surfactants, such as surfactants.

[0003] From a thermodynamic point of view, a large foam interface represents an unstable state, so every foam system tries to achieve a structure that minimizes the diffusion of the film. However, any change in the film structure first requires energy, because surfactants stabilize the foam through different stabilization mechanisms.

[0004] For example, foam stability is determined by the surface elasticity, surface viscosity and steric interaction of the foam. In aqueous foam systems, electrostatic interactions also play an important role. Depending on the proportion of the liquid phase, a distinction can be made between "wet" spherical foams and relatively dry polyhedral foams. When the liquid in the foam layer flows downward due to gravity, spherical foams transform into polyhedral foams.

[0005] A foam only causes problems when it is metastable, i.e. when it does not collapse quickly. This kinetic stability comes from the active species at the air / liquid interface, which on the other hand would combine very quickly in a pure two-phase system, such as air in pure water.

[0006] The kinetic stabilization effect of small molecule surfactants depends on the Gibbs film elasticity and the Marangoni effect. Changes or stretching inside the foam film will cause a decrease in the number of surfactant molecules on the interface, resulting in different surface tensions. Due to the increase in surface tension (Gibbs elastic film), the foam film is stretched together again. The movement of the surfactant from the solution to the interface is a diffusion movement determined by time (Marangoni effect), which further strengthens this effect.

[0007] Therefore, the simple requirements for a defoamer are that it is insoluble in the foam medium, easy to diffuse in the foam medium, and lower than the surface energy / surface tension of the foam medium. If the surface tension of the defoamer is smaller than the foam film, it will dissolve in the film, which will enhance the formation of foam; easy diffusion means that the defoamer can be quickly converted into droplets of appropriate size under stirring. Chemical inertness (defoaming efficiency) and compatibility are very important to ensure that the defoamer will not damage the product performance.

[0008] At present, traditional silicone defoamers are prepared by polyether modification of end-hydrogenated silicone oil or side-hydrogenated silicone oil. Some are linear and some are branched. However, these prepared defoamers have poor defoaming efficiency while having excellent compatibility; or have high defoaming efficiency but poor compatibility, especially in the use of water-based two-component PU systems.

[0009] These problems are mainly caused by different proportions of silicon segments and organic segments. When the silicon segment increases, the defoaming efficiency is high, the compatibility is poor and the leveling effect is poor; when the silicon segment is low, the compatibility is good, the defoaming efficiency is low and the leveling effect is good, which is more difficult to balance. Summary of the invention

[0010] In order to overcome the above-mentioned defects of the prior art, the purpose of the present invention is to provide a preparation method and application of a high-efficiency defoamer, and to improve the problem that the defoaming efficiency and compatibility of the traditional silicone defoamer are difficult to balance and have a leveling effect at the same time.

[0011] In order to achieve the purpose of the present invention, the technical solution adopted is:

[0012] A high-efficiency defoamer, wherein the high-efficiency defoamer is a polymer of organosilicon-polymer-organosilicon triblock as shown in Formula 3:

[0013]

[0014] A method for preparing a high-efficiency defoamer comprises:

[0015] A silicone-polymer-silicone triblock polymer as shown in Formula 3 is prepared by reacting an oligomer of dimer acid diallyl ethoxy ether ester as shown in Formula 1 with a single-terminal hydrogen-containing polysiloxane as shown in Formula 2;

[0016]

[0017]

[0018] The R group in Formula 1 is shown in Formula 4 below:

[0019]

[0020] In a preferred embodiment of the present invention, the oligomer of dimer acid diallyl ethoxy ether ester as shown in Formula 1 and the single-terminal hydrogen-containing polysiloxane as shown in Formula 2 react specifically as follows:

[0021] The oligomer of dimer acid diallyl ethoxy ether ester as shown in Formula 1 is added dropwise to the single-terminal hydrogen-containing polysiloxane as shown in Formula 2 at 100-150° C. for 2-3 hours, wherein the molar ratio of the oligomer of dimer acid diallyl ethoxy ether ester (Formula 1) and the single-terminal hydrogen-containing polysiloxane (Formula 2) added in the reaction is 1.1:2-1.3:2, and 0.01-0.03% of chloroplatinic acid catalyst is added at the same time, and the reaction is carried out at 100-150° C. for 4 hours after the addition is completed;

[0022] The specific reaction is shown in the following reaction formula 1:

[0023]

[0024] In a preferred embodiment of the present invention, the dimer acid diallyl ethoxy ether ester is prepared by esterification reaction of dimer acid and ethylene glycol monoallyl ether in the presence of 98% concentrated sulfuric acid as a catalyst.

[0025] In a preferred embodiment of the present invention, the reaction formula of the esterification reaction is shown in the following reaction formula 2:

[0026]

[0027] In a preferred embodiment of the present invention, the oligomer of dimer acid diallyl ethoxy ether ester represented by Formula 1 is prepared by the following method, as shown in the following reaction formula 3:

[0028]

[0029] An application of a high-efficiency defoamer, wherein the application is used as a defoamer in a water-based two-component PU system.

[0030] In a preferred embodiment of the present invention, the water-based two-component PU system is a water-based two-component hydroxy acrylic acid / isocyanate curing agent system.

[0031] The beneficial effects of the present invention are:

[0032] The present invention controls the content of the oligomer of dimer acid diallyl ethoxy ether ester in the molecular chain, and has excellent compatibility and defoaming efficiency regardless of whether the content of silicone oil is high or low. Moreover, the defoamer will not produce shrinkage holes or negative effects on the water-based two-component PU system at a high addition amount. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the 1H-NMR structure diagram of dimer acid diallyl ethoxy ether ester of Example 1. DETAILED DESCRIPTION

[0034] The inventors of the present invention have found in their long-term research work that if a long-chain diacid diallyl ethoxy ether ester oligomer, such as a dodecanedioic acid diallyl ethoxy ether ester oligomer, is used to react with a single-terminal hydrogen-containing polysiloxane to prepare a defoaming agent, the defoaming agent does not have a leveling effect, and it is difficult to balance the defoaming property and compatibility.

[0035] Therefore, the inventors of the present invention have found through a large number of experiments that a silicone-polymer-silicone triblock polymer (Formula 3) is generated by reacting a dimer acid diallyl ethoxy ether ester oligomer (Formula 1) with a single-terminal hydrogen-containing polysiloxane (Formula 2). This synthetic triblock polymer has excellent defoaming effect and compatibility when used in a water-based two-component PU system, and can greatly improve the leveling effect of the paint film.

[0036] The advantages of the present invention are further described below in conjunction with embodiments and comparative examples:

[0037] Example 1: Preparation of Dimer Acid Diallyl Ethoxy Ether Ester

[0038] In a 1L four-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel, add 560g of dimer acid and 2g of concentrated sulfuric acid catalyst, stir, and heat to 130°C; then add 220g of ethylene glycol monoallyl ether dropwise into the reaction flask within 3 hours, control the temperature to 130-150°C, perform infrared detection until the reaction is complete, and stop heating to obtain dimer acid diallyl ethoxy ether ester.

[0039] Example 2: Preparation of oligomers of dimer acid diallyl ethoxy ether ester (n=1)

[0040] In a 1L three-necked flask equipped with a stirrer and a thermometer, 728g of the dimer acid diallyl ethoxy ether ester prepared in Example 1 and 1.3g of antimony trioxide catalyst were added, stirred, and heated to 90°C; then the temperature was controlled to 85-95°C for reaction for 4 hours, heating was stopped, and the molecular weight was tested by GPC to obtain a dimer acid diallyl ethoxy ether ester oligomer with a molecular weight of 2184 (n=1).

[0041] Example 3: Preparation of oligomers of dimer acid diallyl ethoxy ether ester (n=3)

[0042] The other preparation methods and parameters were the same as those in Example 2, except that the reaction time was controlled to be 6 hours, and the parameters of the dimer acid diallyl ethoxy ether ester oligomer with a GPC test molecular weight of 3640 (n=3) were changed.

[0043] Example 4: Preparation of oligomers of dimer acid diallyl ethoxy ether ester (n=5)

[0044] The other preparation methods and parameters were the same as those in Example 2, except that the reaction time was controlled to be 8 hours, and the parameters of the dimer acid diallyl ethoxy ether ester oligomer with a GPC test molecular weight of 5096 (n=5) were changed.

[0045] Example 5: Preparation of high efficiency defoamer A1

[0046] In a 2L three-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel, 440g of the dimer acid diallyl ethoxy ether ester oligomer (molecular weight 2184, n=1) prepared in Example 2 and 0.15g of chloroplatinic acid catalyst were added, stirred, and heated to 120°C; then 201.6g of a single-terminal hydrogen-containing polysiloxane (molecular weight 504, m=4) was added dropwise for 3 hours, and the reaction was controlled at 120-140°C after the addition was completed. Infrared detection was performed until the reaction was completed, and heating was stopped. Defoamer A1 was obtained.

[0047] Example 6: Preparation of high efficiency defoamer A2

[0048] The other preparation methods and parameters were the same as those in Example 5, except that 734 g of the dimer acid diallyl ethoxy ether ester oligomer (molecular weight 3640, n=3) prepared in Example 3 and 0.19 g of chloroplatinic acid catalyst were added, infrared detection was performed until the reaction was completed, and heating was stopped to obtain defoamer A2.

[0049] Example 7: Preparation of high efficiency defoamer A3

[0050] The other preparation methods and parameters were the same as those in Example 5, except that 1027 g of the dimer acid diallyl ethoxy ether ester oligomer (molecular weight 5096, n=5) prepared in Example 4 and 0.25 g of chloroplatinic acid catalyst were added, infrared detection was performed until the reaction was completed, and heating was stopped to obtain defoamer A3.

[0051] Example 8: Preparation of high efficiency defoamer A4

[0052] In a 2L three-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel, 440g of the dimer acid diallyl ethoxy ether ester oligomer (molecular weight 2184, n=1) prepared in Example 2 and 0.16g of chloroplatinic acid catalyst were added, stirred, and heated to 120°C; then 344g of a single-terminal hydrogen-containing polysiloxane (molecular weight 860, m=8) was added dropwise for 3 hours, and the reaction was controlled at 120-140°C after the addition was completed. Infrared detection was performed until the reaction was completed, and heating was stopped. Defoamer A4 was obtained.

[0053] Example 9: Preparation of high efficiency defoamer A5

[0054] The other preparation methods and parameters were the same as those in Example 8, except that 734 g of the dimer acid diallyl ethoxy ether ester oligomer (molecular weight 3640, n=3) prepared in Example 3 and 0.22 g of chloroplatinic acid catalyst were added, infrared detection was performed until the reaction was completed, and heating was stopped to obtain defoamer A5.

[0055] Example 10: Preparation of high efficiency defoamer A6

[0056] The other preparation methods and parameters were the same as those in Example 8, except that 1027 g of the dimer acid diallyl ethoxy ether ester oligomer (molecular weight 5096, n=5) prepared in Example 4 and 0.28 g of chloroplatinic acid catalyst were added, and infrared detection was performed until the reaction was completed, and heating was stopped to obtain defoamer A6.

[0057] Comparative Example 1: Preparation of dodecanedioic acid diallyl ethoxy ether ester

[0058] The other preparation methods and parameters were the same as those in Example 1, except that 230 g of dodecanedioic acid was added to obtain dodecanedioic acid diallyl ethoxy ether ester.

[0059] Comparative Example 2: Preparation of oligomers of dodecanedioic acid diallyl ethoxy ether ester (n=1)

[0060] In a 1L three-necked flask equipped with a stirrer and a thermometer, 597g of dodecanedioic acid diallyl ethoxy ether ester prepared in the above Comparative Example 1 and 1.1g of antimony trioxide catalyst were added, stirred, and heated to 90°C; then the temperature was controlled to 85-95°C for reaction for 4 hours, and the heating was stopped. The molecular weight was tested by GPC to obtain a dodecanedioic acid diallyl ethoxy ether ester oligomer with a molecular weight of 1194 (n=1).

[0061] Comparative Example 3: Preparation of oligomers of dodecanedioic acid diallyl ethoxy ether ester (n=5)

[0062] The other preparation methods and parameters were the same as those in Comparative Example 2, except that the reaction time was controlled to be 8 hours, and the molecular weight of the dodecanedioic acid diallyl ethoxy ether ester oligomer tested by GPC was 2786 (n=5).

[0063] Comparative Example 4: Preparation of Comparative Defoamer B1

[0064] In a 2L three-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel, 245g of the oligomer of dodecanedioic acid diallyl ethoxy ether ester (molecular weight 1194, n=1) prepared in the above Comparative Example 2 and 0.09g of chloroplatinic acid catalyst were added, stirred, and heated to 120°C; then 201.6g of a single-terminal hydrogen-containing polysiloxane (molecular weight 504, m=4) was added dropwise for 3 hours, and the reaction was controlled at 120-140°C after the addition was completed. Infrared detection was performed until the reaction was completed, and heating was stopped. Defoamer B1 was obtained.

[0065] Comparative Example 5: Preparation of comparative defoamer B2

[0066] The other preparation methods and parameters were the same as those of Comparative Example 4, except that 572 g of the oligomer of dodecanedioic acid diallyl ethoxy ether ester (molecular weight 2786, n=5) prepared in Comparative Example 3 and 0.16 g of chloroplatinic acid catalyst were added, and infrared detection was performed until the reaction was completed, and heating was stopped to obtain defoamer B2.

[0067] Comparative Example 6: Preparation of comparative defoamer B3

[0068] In a 2L three-necked flask equipped with a stirrer, a reflux condenser, a thermometer and a dropping funnel, 245g of the oligomer of dodecanedioic acid diallyl ethoxy ether ester (molecular weight 1194, n=1) prepared in the above Comparative Example 2 and 0.12g of chloroplatinic acid catalyst were added, stirred, and heated to 120°C; then 344g of a single-terminal hydrogen-containing polysiloxane (molecular weight 860, m=8) was added dropwise for 3 hours, and the reaction was controlled at 120-140°C after the addition was completed. Infrared detection was performed until the reaction was completed, and heating was stopped. Defoamer B3 was obtained.

[0069] Comparative Example 7: Preparation of comparative defoamer B4

[0070] The other preparation methods and parameters were the same as those of Comparative Example 6, except that 572 g of the oligomer of dodecanedioic acid diallyl ethoxy ether ester (molecular weight 2786, n=5) prepared in Comparative Example 3 and 0.19 g of chloroplatinic acid catalyst were added, and infrared detection was performed until the reaction was completed, and heating was stopped to obtain defoamer B4.

[0071] Water-based two-component PU system test defoaming performance and test results

[0072] Examples 5-10 and Comparative Examples 4-7 were tested for defoaming, antifoaming, compatibility, and the effect of the defoamer on the gloss and haze value of the paint film in a water-based two-component PU system.

[0073] 1) Test recipe

[0074] Table 1:

[0075]

[0076] 2) Defoaming and foam inhibition test method: Component A prepared according to different defoaming agents according to the above Table 1 was placed in a 200 ml measuring cylinder respectively, and the cylinder was inflated with an air pump for 30 minutes. The height of the foam was recorded. The higher the foam, the worse the foam inhibition. The time for all the foam to disappear was recorded after standing. The shorter the time, the better the defoaming effect.

[0077] 3) Compatibility test method: Component A prepared with different defoamers according to the above Table 1 was mixed evenly with component B, and a 100-micron wire rod was used to apply film on a glass plate, and the presence and number of shrinkage cavities were recorded. The fewer the number of shrinkage cavities, the better the compatibility.

[0078] 4) Gloss and haze test method: Component A prepared with different defoamers according to the above Table 1 was mixed evenly with component B, molded on a glass plate using a 150 micron frame wet film preparation device, placed in an 80°C oven for drying for 2 hours, and then taken out and allowed to cool to room temperature. The gloss and haze values ​​were tested using a haze gloss meter. The higher the gloss, the lower the haze value, indicating that the defoamer has less impact on the paint film.

[0079] Table 2: Defoamer performance test results

[0080]

[0081] From the results recorded in Table 2, it can be seen that the defoamer of the present invention has excellent and balanced defoaming and antifoaming properties, as well as excellent compatibility; and at the same time, it has no negative impact on the paint film.

Claims

1. A high-efficiency defoamer, characterized in that: The high-efficiency defoamer is a polymer of organosilicon-polymer-organosilicon triblock as shown in Formula 3 below: Wherein, n=1, 3 or 5; m=8; The R group is shown in Formula 4 below:

2. The method for preparing a high-efficiency defoamer according to claim 1, characterized in that: include: A silicone-polymer-silicone triblock polymer as shown in Formula 3 is prepared by reacting an oligomer of dimer acid diallyl ethoxy ether ester as shown in Formula 1 with a single-terminal hydrogen-containing polysiloxane as shown in Formula 2; The R group in Formula 1 is shown in Formula 4 below:

3. The method for preparing a high-efficiency defoamer according to claim 2, characterized in that: The oligomer of dimer acid diallyl ethoxy ether ester as shown in Formula 1 and the single-terminal hydrogen-containing polysiloxane as shown in Formula 2 react specifically as follows: The oligomer of dimer acid diallyl ethoxy ether ester as shown in Formula 1 is added dropwise to the single-terminal hydrogen-containing polysiloxane as shown in Formula 2 at 100-150° C. for 2-3 hours, and chloroplatinic acid catalyst is added at the same time. After the addition is complete, the mixture is reacted at 100-150° C. for 4 hours; The specific reaction is shown in the following reaction formula 1:

4. The method for preparing a high-efficiency defoamer according to claim 3, characterized in that: The dimer acid diallyl ethoxy ether ester is prepared by esterification reaction of dimer acid and ethylene glycol monoallyl ether under the action of 98% concentrated sulfuric acid catalyst.

5. The method for preparing a high-efficiency defoamer according to claim 4, characterized in that: The reaction formula of the esterification reaction is shown in the following reaction formula 2:

6. The method for preparing a high-efficiency defoamer according to claim 2, characterized in that: The oligomer of dimer acid diallyl ethoxy ether ester represented by Formula 1 is prepared by the following method, as shown in the following reaction formula 3:

7. The use of a high-efficiency defoamer as claimed in claim 1, characterized in that: The application is to use it as a defoamer in a water-based two-component PU system.

8. The use of a high-efficiency defoamer as claimed in claim 7, characterized in that: The water-based two-component PU system is a water-based two-component hydroxy acrylic acid / isocyanate curing agent system.