Fischer-Tropsch synthesis catalyst and preparation method and application thereof
By using the impregnation method of raspberry-type oxide microsphere carriers and cobalt additives to prepare Fischer-Tropsch synthesis catalysts, and performing re-reduction and low-temperature passivation in a hydrogen atmosphere, the problems of low catalyst activity and harsh passivation conditions were solved and achieved It has efficient Fischer-Tropsch synthesis performance and simple preparation process.
Patent Information
- Application Number
- CN202110482631.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-04-30
AI Technical Summary
Existing Fischer-Tropsch synthesis catalysts have low catalytic activity and harsh reduction and passivation conditions, making it difficult to effectively apply them to microchannel reactions. In particular, there are difficulties in processing small particle catalysts.
Raspberry-type oxide microspheres are used as carriers, cobalt and additives are introduced through the impregnation method, and re-reduction treatment is carried out in a hydrogen atmosphere, and passivation is performed at low temperature. The passivation temperature is controlled to be no higher than 90°C to improve the efficiency of the process. The number of active centers and selectivity of the catalyst.
It achieves a high number of active centers and excellent CO conversion rate and C5+ hydrocarbon selectivity of the Fischer-Tropsch synthesis catalyst, simplifies the preparation and application process of the catalyst, reduces production costs, and is suitable for large-scale industrial applications.
Smart Images

Figure CN115254113B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a Fischer-Tropsch synthesis catalyst and a preparation method and application thereof. Background Art
[0002] Microchannel reaction technology is one of the new technologies in chemical engineering in the 21st century. It has obvious advantages over conventional reactors: the reaction channel is at the micron level, the surface area is large, and the reactor has a high mass transfer and heat transfer rate; the heat transfer coefficient is high, so that the chemical reaction can occur under isothermal conditions, avoiding the "flying temperature" phenomenon; making the application of high-activity, low-intensity catalysts a reality; the modular form makes engineering amplification simple; the unit volume reactor has a high reaction load, and the miniaturization of large reactors is realized. The FT synthesis reaction is a strong exothermic reaction. Strengthening the heat transfer of the catalyst layer and controlling the temperature of the reaction to be stable are the premise and guarantee for achieving good reaction results. Using microchannel reaction technology, high-activity, particulate Fischer-Tropsch synthesis catalysts can be reacted under isothermal conditions, which not only overcomes the shortcomings of poor heat transfer in fixed beds and the inability to use small-particle catalysts, but also solves the problems of liquid phase mass transfer resistance and catalyst wear and separation in slurry beds. Due to the small particles, the Fischer-Tropsch synthesis catalyst has a large macroscopic surface area, which provides a wide channel and space for the diffusion of reactants and products, greatly promoting the reaction efficiency of the catalyst. The catalyst activity in a microchannel reactor can reach 4 to 8 times that of a fixed bed and a slurry bed. Therefore, it is of great significance to carry out research on efficient FT synthesis microchannel reaction technology.
[0003] The metal components of metal hydrogenation catalysts are usually prepared in the form of oxides. Only by reducing the catalyst can it have catalytic activity. The quality of catalyst reduction directly affects the performance of the catalyst. Reasonable selection of catalyst reduction pretreatment conditions can make the catalyst have higher activity in the reaction.
[0004] The catalyst reduction method can adopt ex situ pre-reduction treatment or in situ reduction treatment technology. The ex situ pre-reduction technology can improve the utilization rate of the reducing agent and reduce the amount of reducing agent. The pre-reduced catalyst can be restored to activity through simple reactivation at a lower temperature, thereby reducing the start-up time, reducing the start-up cost, shortening the start-up cycle, and ultimately increasing the economic benefits of the enterprise.
[0005] For the same catalyst, different reduction and passivation treatment methods have different effects on the activity and selectivity of the reaction. Different catalysts usually use different reduction and passivation treatment methods to achieve better activity and selectivity. The pre-reduction passivation method in the prior art takes a long time and is not suitable for the treatment of microchannel small particle catalysts. It is necessary to develop a pre-reduction method that is simple to operate, safe and reliable for pre-reduction treatment of catalysts. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects of low catalytic activity and harsh reduction passivation conditions of the Fischer-Tropsch synthesis catalyst in the prior art, and to provide a Fischer-Tropsch synthesis catalyst and a preparation method and application thereof. The catalyst provided by the present invention has a high CO conversion rate and C5+ hydrocarbon selectivity when used in the Fischer-Tropsch synthesis process.
[0007] In order to achieve the above object, the first aspect of the present invention provides a Fischer-Tropsch synthesis catalyst, the catalyst comprising a carrier and an active component supported on the carrier, the active component comprising cobalt and an additive, the additive being selected from at least one of Group IA metal elements, Group IIA elements, Group IB elements, Group IIB elements, Group IIIB elements, Group IVB elements, Group VB elements, Group VIB elements, Group VIIB elements and Group VIII elements, based on the total amount of the catalyst, calculated as oxide, the content of cobalt is 20-60% by weight, and the content of the additive is 0.001-25% by weight;
[0008] The carrier is a raspberry-shaped oxide microsphere, which is a hollow microsphere with a large hole on the surface, and a hollow structure inside the hollow microsphere, wherein the large hole and the hollow structure are connected to form a cavity with one end open; wherein the oxide in the raspberry-shaped oxide microsphere is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide;
[0009] Among them, the number of active centers of the catalyst after the re-reduction treatment is 0.06-0.3mmol hydrogen / g catalyst, and the re-reduction treatment conditions include: temperature of 200°C, time of 2 hours, re-reduction atmosphere of an atmosphere containing hydrogen and argon with a hydrogen concentration of 10 volume%, and a gas-to-agent volume ratio of 15000.
[0010] A second aspect of the present invention provides a method for preparing a Fischer-Tropsch synthesis catalyst, the method comprising:
[0011] (1) preparing raspberry-shaped oxide microspheres;
[0012] (2) introducing active components onto the raspberry-shaped oxide microspheres by an impregnation method to obtain an oxidized catalyst; the active components include cobalt and an auxiliary agent, and the auxiliary agent is selected from at least one of Group IA metal elements, Group IIA elements, Group IB elements, Group IIB elements, Group IIIB elements, Group IVB elements, Group VB elements, Group VIB elements, Group VIIB elements, and Group VIII elements;
[0013] (3) reducing the oxidized catalyst under a hydrogen-containing atmosphere;
[0014] (4) after the temperature of the catalyst obtained by reduction in step (3) drops below 60° C., the catalyst obtained by reduction in step (3) is passivated, wherein the passivation comprises: continuously introducing an oxygen-containing gas below 60° C. and controlling the passivation temperature to be no higher than 90° C.; wherein the oxygen concentration of the oxygen-containing gas is continuously increased;
[0015] The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of cobalt in the oxidized catalyst is 20-60% by weight and the content of the auxiliary agent is 0.001-25% by weight, based on the total amount of the oxidized catalyst and calculated as oxide.
[0016] The third aspect of the present invention provides a Fischer-Tropsch synthesis catalyst prepared by the preparation method described in the second aspect.
[0017] The fourth aspect of the present invention provides use of the Fischer-Tropsch synthesis catalyst described in the first aspect or the third aspect in a Fischer-Tropsch synthesis reaction.
[0018] Through the above technical scheme, the Fischer-Tropsch synthesis catalyst carrier provided by the present invention is a raspberry-shaped oxide microsphere, which has a short diffusion distance and a large macroscopic surface area during application. In addition, the Fischer-Tropsch synthesis catalyst provided by the present invention has more active centers and has better Fischer-Tropsch synthesis performance when applied in the Fischer-Tropsch synthesis process, especially a higher CO conversion rate and C5+ hydrocarbon selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a SEM photograph of the catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] In the present invention, the gas-to-catalyst ratio refers to the ratio of the volume of gas passing through the catalyst bed per hour to the volume of the catalyst. In the reduction process (or re-reduction process), the gas in the gas-to-catalyst ratio refers to the reducing gas (i.e., hydrogen-containing gas), and in the passivation process, the gas in the gas-to-catalyst ratio refers to the passivating gas (i.e., oxygen-containing passivating gas, also called oxygen-containing gas).
[0022] In the present invention, for the purpose of distinction, the reduction of the catalyst before passivation is referred to as "reduction", and the reduction of the catalyst after passivation is referred to as "re-reduction".
[0023] The first aspect of the present invention provides a Fischer-Tropsch synthesis catalyst, which includes a carrier and an active component supported on the carrier, wherein the active component includes cobalt and an additive, wherein the additive is selected from at least one of Group IA metal elements, Group IIA elements, Group IB elements, Group IIB elements, Group IIIB elements, Group IVB elements, Group VB elements, Group VIB elements, Group VIIB elements and Group VIII elements, and the content of cobalt is 20-60% by weight and the content of the additive is 0.001-25% by weight, based on the total amount of the catalyst and calculated as oxide;
[0024] The carrier is a raspberry-shaped oxide microsphere, which is a hollow microsphere with a large hole on the surface, and a hollow structure inside the hollow microsphere, wherein the large hole and the hollow structure are connected to form a cavity with one end open; wherein the oxide in the raspberry-shaped oxide microsphere is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide;
[0025] Among them, the number of active centers of the catalyst after the re-reduction treatment is 0.06-0.3mmol hydrogen / g catalyst, and the re-reduction treatment conditions include: temperature of 200°C, time of 2 hours, re-reduction atmosphere of an atmosphere containing hydrogen and argon with a hydrogen concentration of 10 volume%, and a gas-to-agent volume ratio of 15000.
[0026] Preferably, the number of active centers of the catalyst after the re-reduction treatment is 0.09-0.29 mmol hydrogen / g catalyst, more preferably 0.1-0.29 mmol hydrogen / g catalyst.
[0027] In the present invention, the number of active centers of the catalyst is obtained by performing a H2-programmed temperature desorption (H2-TPD) test on an Autochem2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics Corporation of the United States. The test method includes: weighing 0.2000g of a 40-60 mesh sample, first performing re-reduction activation, and the re-reduction conditions are: H2-Ar mixed gas with a hydrogen content of 10 volume %, a flow rate of 50mL / min, heating to 200°C at a heating rate of 10°C / min for reduction for 2h. The reduced catalyst is cooled in a H2-Ar mixed gas with a hydrogen content of 10 volume %, and after the temperature drops to 55°C, it is switched to Ar gas for purging, with an Ar flow rate of 20mL / min, until the baseline is stable, and then a H2-TPD experiment is performed. The experimental conditions and procedures of H2-TPD were as follows: the carrier gas was Ar, the carrier gas flow rate was 20 mL / min, the heating rate was 10 °C / min, the final temperature was 400 °C, and the thermal conductivity detector (TCD) detected the signal to obtain the TPD curve.
[0028] According to a preferred embodiment of the present invention, the catalyst is characterized by TPR, and in its TPR curve, the temperature corresponding to the peak of the low-temperature reduction peak with the largest area is 140-270°C, preferably 150-260°C, and more preferably 150-210°C. The temperature corresponding to the peak of the low-temperature reduction peak with the largest area in the TPR spectrum curve can be used as an indicator for evaluating the regenerative performance of the passivated catalyst. The lower the temperature corresponding to the peak of the low-temperature reduction peak with the largest area, the easier the catalyst is to regenerate. The Fischer-Tropsch synthesis catalyst provided by the present invention has good regenerative performance.
[0029] In the present invention, the TPR (i.e., programmed temperature reduction) characterization is carried out on an Autochem2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics, USA. The specific test conditions include: taking 0.20g of sample, first heating the sample to 120°C for dehydration treatment for 1 hour under 50mL / min Ar gas flow at a heating rate of 10°C / min, and after the temperature drops to 50°C, performing a TPR experiment. The experimental conditions and procedures of TPR are: the reducing gas is 10 volume % H2-Ar mixed gas, the flow rate is 50mL / min, and the temperature is increased to 900°C at a heating rate of 10°C / min; in the above-mentioned heating process, the signal is detected by a thermal conductivity detector (TCD) to obtain a TPR spectrum curve.
[0030] According to the present invention, preferably, based on the total amount of the catalyst, the content of cobalt is 25-55% by weight, and the content of the auxiliary agent is 0.001-10% by weight, calculated as oxide.
[0031] According to the present invention, specifically, in the catalyst, based on the total amount of the catalyst, the content of the carrier is 15-80% by weight, preferably 35-75% by weight.
[0032] The present invention has a wide range of selection of the auxiliary agent. Preferably, the auxiliary agent is selected from one or more of La, Zr, Mn, V, Cr, Cu, Ce, W, Ti, Zn, Sc, Mg, Ca, Be, Na, K, Ru, Ag, Au, Re, Pt and Pd, and more preferably selected from one or more of La, Zr, Cu, Ce, W, Ti, Ru, Ag, Au, Re, Pt and Pd. In the preferred case of the present invention, the catalyst exhibits better CO conversion rate and C5+ hydrocarbon selectivity in the Fischer-Tropsch synthesis reaction.
[0033] In a preferred embodiment of the present invention, in addition to cobalt and additives, the active components may optionally contain other components, and those skilled in the art may select them according to their needs, as long as they are beneficial to improving the catalytic performance of the catalyst in the Fischer-Tropsch synthesis reaction.
[0034] According to the Fischer-Tropsch synthesis catalyst provided by the present invention, the oxide in the raspberry-shaped oxide microspheres is an inorganic oxide, which can be selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide, preferably aluminum oxide and / or silicon oxide.
[0035] According to the Fischer-Tropsch synthesis catalyst provided by the present invention, in the raspberry-shaped oxide microspheres, the diameter of the hollow structure is 1-2000 μm, preferably 1-400 μm.
[0036] According to the present invention, in the raspberry-shaped oxide microspheres, the pore size of the macropores is 0.2-1000 μm, preferably 0.5-200 μm.
[0037] According to the present invention, in the raspberry-shaped oxide microspheres, the shell thickness of the hollow microspheres is 0.2-1000 μm, preferably 0.5-200 μm.
[0038] According to the present invention, the appearance of the raspberry-shaped oxide microspheres is close to spherical. Preferably, the sphericity of the raspberry-shaped oxide microspheres is 0.5-0.99.
[0039] According to the Fischer-Tropsch synthesis catalyst provided by the present invention, the particle size of the raspberry-shaped oxide microspheres is preferably 3-2500 μm, preferably 10-500 μm.
[0040] The sphericity of the microsphere blank is given by the formula σ=4πA / L 2 Calculated. Where: σ is the sphericity; A is the projected area of the microsphere, unit is m 2 ; L is the projected circumference of the microsphere, in m; A and L are obtained from the SEM photos of the microspheres using the image processing software Image-ProPlus.
[0041] The raspberry-shaped oxide microspheres of the present invention are calcined at 400-1300°C, preferably 450-1100°C, and more preferably 500-700°C to obtain oxides having a specific surface area of about 0.1-900 m 2 / g, preferably 10-300m 2 / g, and the pore volume is about 0.01-3.6 ml / g, preferably 0.1-0.9 ml / g.
[0042] The crushing rate of the raspberry-shaped oxide microspheres of the present invention is preferably 0-1%, and the crushing rate is measured according to the method provided by the similar strength standard number Q / SH3360 226-2010, and the specific method is:
[0043] First, select sieves S1 and S2 with mesh numbers M1 and M2 respectively, where M1 < M2. Pass the microspheres to be tested through sieve S1 with mesh number M1 first, and then pass the sieved microsphere powder through sieve S2 with mesh number M2. Finally, use the microsphere powder retained by sieve S2 as the sample to be tested.
[0044] In a cylindrical steel container with a cross-sectional diameter of 10 mm, add a certain mass of the sample to be tested. Then, apply a certain pressure to the microspheres through a cylinder for a certain period of time. After that, use sieve S2 with mesh number M2 to screen the pressed microsphere powder, record the mass of the microsphere powder passing through the sieve, and then divide the mass of the microsphere powder passing through the sieve by the total mass of the added microspheres to obtain the crushing rate of the microspheres.
[0045] In the present invention, M1 can be 100 mesh, M2 can be 150 mesh, the pressure can be 100 N, and the time can be 10 s.
[0046] The strength of the microspheres can be evaluated using this crushing rate; the smaller the crushing rate, the higher the strength of the microspheres.
[0047] Under pressurized conditions, the raspberry-shaped oxide microspheres of the present invention have a low crushing rate and significantly higher strength than the existing known oxide microspheres, such as the apple-shaped hollow molecular sieve microspheres disclosed in CN108404970A. This is determined by the differences in their raw materials and preparation methods. The higher strength enables the raspberry-shaped oxide microspheres to have a larger porosity, a significant reduction in pressure drop, and excellent processing performance and wear resistance.
[0048] The Fischer-Tropsch synthesis catalyst provided by the present invention has the advantages of a large number of active centers, high catalytic activity, and good renewable performance.
[0049] The second aspect of the present invention provides a method for preparing a Fischer-Tropsch synthesis catalyst, which includes:
[0050] (1) Prepare raspberry-shaped oxide microspheres;
[0051] (2) Introduce active components onto the raspberry-shaped oxide microspheres by an impregnation method to obtain an oxidized catalyst; the active components include cobalt and promoters, and the promoters are selected from at least one of the metal elements in Group IA, Group IIA, Group IB, Group IIB, Group IIIB, Group IVB, Group VB, Group VIB, Group VIIB, and Group VIII elements;
[0052] (3) Reduce the oxidized catalyst in a hydrogen-containing atmosphere;
[0053] (4) after the temperature of the catalyst obtained by reduction in step (3) drops below 50° C., the catalyst obtained by reduction in step (3) is passivated, wherein the passivation comprises: continuously introducing an oxygen-containing gas below 50° C. and controlling the passivation temperature to be no higher than 70° C.; wherein the oxygen concentration of the oxygen-containing gas is continuously increased;
[0054] The amount of the raspberry-shaped oxide microspheres and the active component is such that the cobalt content in the oxidized catalyst is 20-60% by weight, preferably 25-55% by weight, based on the total amount of the oxidized catalyst, and the content of the auxiliary agent is 0.001-25% by weight, preferably 0.001-10% by weight, calculated as oxide.
[0055] The specific selection and content of the active components are as described above and will not be repeated here.
[0056] The composition and structure of the raspberry-shaped oxide microspheres are as described above and will not be repeated here.
[0057] Any method that can obtain the above-mentioned raspberry-shaped oxide microspheres of composition and structure can be used to prepare raspberry-shaped oxide microspheres in step (1) of the present invention. Preferably, step (1) of preparing raspberry-shaped oxide microspheres comprises:
[0058] (1-1) adding nitrate, peptizing agent, pore former, the oxide and / or its precursor into a dispersant and stirring to obtain a dispersed slurry;
[0059] (1-2) subjecting the dispersed slurry to an aging treatment;
[0060] (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded under the conditions of an inlet air temperature of 400-1200° C., preferably 450-700° C., and an outlet air temperature of 50-300° C., preferably 120-200° C., to obtain the raspberry-shaped oxide microspheres.
[0061] In the present invention, preferably, the mass ratio of the nitrate, the peptizing agent, the pore former and the oxide and / or its precursor is (10-500):(1-10):(10-500):(10-1000).
[0062] In the present invention, nitrate, peptizing agent, pore former and oxide and / or its precursor can be added to the dispersant in sequence or simultaneously. The order of addition can also be adjusted according to the solubility of each raw material. It is preferred to stir while adding to mix them evenly.
[0063] In the present invention, preferably, the nitrate is selected from one or more of zirconium nitrate, aluminum nitrate, lanthanum nitrate and yttrium nitrate. Nitrate ions in the nitrate can promote the oxidant that can be used as a pore-forming agent under high temperature conditions. They undergo a self-propagating combustion reaction at high temperatures to generate gas and steam, so that the oxide material forms a cavity.
[0064] In the present invention, preferably, the peptizing agent is selected from one or more of acids, bases and salts. The acids can be selected from: inorganic acids (such as hydrochloric acid, sulfuric acid, nitric acid, etc.), organic acids (formic acid, acetic acid, oxalic acid, etc.) and combinations of one or more of inorganic acids or organic acids; the bases can be selected from: inorganic bases (sodium hydroxide, potassium hydroxide, calcium hydroxide, barium hydroxide, aluminum hydroxide, lithium hydroxide, magnesium hydroxide, zinc hydroxide, copper hydroxide, iron hydroxide, lead hydroxide, cobalt hydroxide, chromium hydroxide, zirconium hydroxide, nickel hydroxide, ammonium hydroxide, soda ash (anhydrous sodium carbonate), sodium carbonate (monohydrate, heptahydrate, decahydrate), sodium bicarbonate (baking soda), potassium carbonate, potassium bicarbonate, etc.), organic bases (such as amine compounds, alkali metal salts of alcohols, alkaloids, alkyl metal lithium compounds, etc.) and combinations of one or more of inorganic bases or organic bases; the salts can be selected from: inorganic acid salts (such as hydrochloric acid, sulfates, nitrates, etc.), organic acid salts (formates, acetates, oxalates, etc.) and combinations of one or more of inorganic acid salts or organic acid salts.
[0065] According to the present invention, preferably, the pore-forming agent is selected from one or more of synthetic cellulose, starch, polymeric alcohol and surfactant. The synthetic cellulose is preferably one or more of carboxymethyl cellulose, methyl cellulose, ethyl cellulose and hydroxycellulose fatty alcohol polyvinyl ether; the polymeric alcohol is preferably one or more of polyethylene glycol, polypropylene glycol, polyvinyl alcohol and polypropylene glycol PPG; the surfactant is preferably one or more of fatty alcohol polyvinyl ether, fatty alcohol amide and its derivatives, acrylic acid copolymer and maleic acid copolymer with a molecular weight of 200-2000000.
[0066] According to the present invention, specifically, the oxide and / or its precursor can directly adopt aluminum oxide, silicon oxide, zirconium oxide and titanium oxide, or the precursors of these oxides can be selected, specifically, one or more selected from silicon source, aluminum source, zirconium source and titanium source, wherein the aluminum source is preferably selected from one or more of pseudo-boehmite, aluminum alcohol, aluminum sulfate, aluminum nitrate, aluminum chloride and sodium aluminate, the silicon source is preferably selected from one or more of sodium silicate, silicate, water glass and silica sol, the zirconium source is preferably selected from one or more of zirconium dioxide, zirconium tetrachloride, zirconium oxychloride, zirconium hydroxide, zirconium sulfate, zirconium phosphate, zirconium oxynitrate, zirconium nitrate, basic zirconium carbonate and tetrabutoxy zirconium, and the titanium source is preferably selected from one or more of titanium dioxide, titanium nitrate, metatitanic acid, titanyl sulfate, titanium dichloride, titanium trichloride, titanium tetrachloride, titanium aluminum chloride, tetraethyl titanate, tetrabutyl titanate, tetra-n-propyl titanate and tetraisopropyl titanate.
[0067] In the present invention, when using the above-mentioned aluminum source, silicon source, zirconium source and titanium source, it also includes chemical reagents for precipitating or gelling them, such as acids (such as inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid or organic acids such as acetic acid), and / or alkalis (such as sodium carbonate, sodium hydroxide, etc.).
[0068] When it is necessary to prepare an oxide composition containing other components, oxides such as vanadium oxide, chromium oxide, manganese oxide, iron oxide, cobalt oxide, molybdenum oxide, tungsten oxide, nickel oxide, copper oxide, etc. may also be added, and precursors that can form these oxides may also be added.
[0069] In the present invention, preferably, the dispersant is selected from one or more of water, alcohols, ketones and acids, wherein the alcohols are preferably methanol, ethanol, propanol, etc., the ketones are preferably acetone, butanone, etc., and the acids are preferably formic acid, acetic acid, propionic acid, etc. The dispersant is preferably a mixture of water and a small amount of ethanol. A small amount of ethanol in water can have a better dispersing effect and can be used as a boiling point regulator. By adjusting the dispersant, the water evaporation effect and the droplet shrinkage effect are more matched and matched, so that the appearance of the microspheres is more regular and smooth.
[0070] According to a preferred embodiment of the present invention, step (1-1) further comprises adding a blasting agent to the dispersant. The blasting agent may be added before or after the oxide. Preferably, the blasting agent is selected from one or more of picric acid, trinitrotoluene, digested glycerol, nitrocellulose, dynamite, hexogen and C4 plastic explosive. Preferably, before drying and forming, the blasting agent is mixed evenly with other materials. Preferably, the amount of blasting agent added is 0-1% of the total dry weight of nitrate, peptizing agent, pore-forming agent and oxide and / or its precursor.
[0071] According to a preferred specific embodiment of the present invention, nitrate, peptizing agent, pore-forming agent and oxide precursor are sequentially added to a dispersant for slurrying, and the slurry is stirred evenly and then pumped into a sand mill or a colloid mill for grinding to obtain a dispersed slurry. The solid content of the slurry during slurrying is preferably 5-60% by weight, and the grinding time is preferably 1-30 minutes. After mixing and grinding, the average particle size of the aluminum source, silicon source, zirconium source and titanium source particles in the slurry can be ground to 0.01-10 μm.
[0072] After the raw material mixing and grinding process, it is fully dissolved and dispersed to make the dispersed slurry uniform. The grinding equipment used can be a colloid mill, a sand mill or other equipment. The selection standard is that the catalyst fine powder reaches the required average particle size after grinding, preferably less than 10 μm.
[0073] In the present invention, the range of selection of the conditions for the aging treatment is relatively wide. Preferably, in step (1-2), the temperature of the aging treatment is 0-90°C, preferably 20-60°C.
[0074] Preferably, the aging treatment time is 0.1-24 hours, preferably 0.5-2 hours.
[0075] In the present invention, the drying device used can be a flash drying device and a spray drying device, preferably a spray drying device. Flash drying and spray drying are commonly used methods for drying materials. After the wet material is dispersed in a drying tower, the water vaporizes rapidly in contact with hot air to obtain a dry product. The spray drying method can directly dry a solution or emulsion into a powder or granular product, eliminating the processes of evaporation and crushing.
[0076] According to a preferred embodiment of the present invention, the aged dispersed slurry is sent to a spray drying device for drying and molding at an inlet air temperature of 400-1200° C., preferably 450-700° C., and an outlet air temperature of 50-300° C., preferably 120-200° C. The pressure in the spray tower can be equivalent to that of conventional spraying, and raspberry-shaped oxide microspheres can be obtained.
[0077] In the present invention, the working principle of spray drying is to disperse the material to be dried into very fine mist-like particles through mechanical action (such as pressure, centrifugation, and airflow spray), increase the water evaporation area, accelerate the drying process, contact with hot air, remove most of the water in a short time, and dry the solid matter in the material into powder.
[0078] The spray drying device used in the present invention is a conventional device in the existing process, and the present invention has no special restrictions on it. The spray drying device usually includes: a feeding system, a hot air system, a drying tower system, a collecting system and a sealing system. The feeding system is connected to the drying tower system in the middle of the top, the hot air system is connected to the top side of the drying tower system, the collecting system is connected to the bottom of the drying tower system, and the sealing system is connected to the hot air system. In the spray drying process, it is basically necessary to have three functions: spraying of the stock solution; drying of tiny droplets in the spray; separation and recovery of fine powder products. The spray drying device is usually equipped with an atomizer, a drying chamber and a fine powder recoverer corresponding to the above functions.
[0079] Due to the large number of control parameters and complex factors in the spray drying process, the particle size and shape after spray drying are very complex. The general product particle size range is micron-level, and is generally a mixture of spheres, discs, apples, grapes, cavities, meniscuses, etc. How to selectively shape them into an ideal single shape, such as a cavity, is one of the difficulties.
[0080] One method in the prior art is to form a spherical emulsion under the action of the surface tension of a surfactant, and then at a relatively low temperature, the pore-forming agent is vaporized or pyrolyzed inside the spherical emulsion. The gases generated by these vaporizations and pyrolysis will cause the internal cavities of the microsphere emulsion; the slow release of the gas leads to the formation of large pores on the surface that are connected to the internal hollow structure, and the molecular sieve particles form secondary stacking pores during the spray molding process to become mesopores on the surface of the molecular sieve microspheres. Combined with the subsequent calcination process, large-particle hollow molecular sieve microspheres are obtained.
[0081] In the present invention, under the high temperature of 400-1200℃ inlet air temperature, the oxide and the reducing agent in the slurry undergo a strong redox self-propagating combustion reaction, instantly generating a large amount of gas; at the same time, the droplet spray enters the high temperature zone and evaporates strongly, and the surface tension formed by the concentrated slurry causes the droplets to shrink sharply. The strong explosion inside and the strong contraction outside form a raspberry-shaped hollow material with good strength. The obtained raspberry-shaped oxide microspheres have high strength, high sphericity and high yield rate.
[0082] In the present invention, the raspberry-shaped oxide microspheres can be calcined before step (2) and then used as a carrier. Preferably, the calcination temperature can be 400°C-1300°C, preferably 450-1100°C, and more preferably 500-700°C; the calcination time can be 1-12h, preferably 2-8h, and more preferably 3-4h.
[0083] The present invention does not particularly limit the specific implementation of step (2), as long as the active component is introduced into the raspberry-type oxide microspheres by an impregnation method. Preferably, it includes preparing an impregnation solution of a compound containing an active metal component, and then impregnating the raspberry-type oxide microspheres with the solution. The impregnation method is a conventional method, for example, it can be an excess liquid impregnation or a pore saturation impregnation. Among them, by adjusting and controlling the concentration, dosage of the impregnation solution of the compound containing the active component or the dosage of the raspberry-type oxide microspheres, a catalyst of a specified content can be prepared, which is easily understood and implemented by those skilled in the art.
[0084] In the present invention, there are more than two types of active components, and the active components can be co-impregnated into the raspberry-shaped oxide microspheres, or can be impregnated into the raspberry-shaped oxide microspheres in steps, preferably co-impregnated. The specific operation is well known to those skilled in the art, and the present invention will not be repeated here.
[0085] According to a preferred embodiment of the present invention, the raspberry-shaped oxide microspheres are impregnated with an impregnation solution containing an active component precursor, and then dried and calcined. Preferably, the drying temperature can be 80°C-200°C, and more preferably 100-150°C. Preferably, the calcination temperature is 200°C-800°C, and preferably 300-600°C. The present invention does not have any restrictions on the drying and calcination time, and conventional drying and calcination time can be used. The calcination device used and its operating conditions are conventional equipment and operating parameters in existing calcination technology, and the present invention has no special restrictions on them.
[0086] The present invention has no particular limitation on the type of the precursor of the active component, which can be selected from water-soluble compounds corresponding to the active component, such as nitrates, acetates, chlorides, etc. For example, the precursor of cobalt can be at least one of cobalt nitrate, cobalt chloride, basic carbonate and cobalt acetate, and the precursor of the auxiliary agent can be at least one of cobalt nitrate, cobalt chloride, basic cobalt carbonate and cobalt acetate.
[0087] The present invention adopts raspberry-shaped oxide microspheres, which can reduce the waste of carriers and catalysts and save materials; at the same time, due to the improvement of the shape efficiency factor, it can also promote diffusion, improve reaction efficiency and target product selectivity. In reactions with relatively large thermal effects, the hollow carrier can also reduce the generation of hot spots and has good intrinsic safety.
[0088] According to the present invention, the hydrogen-containing atmosphere contains hydrogen and may optionally contain a protective gas. The protective gas is a gas that does not participate in the reaction, and the protective gas is preferably selected from at least one of nitrogen, helium, argon and neon, and more preferably nitrogen.
[0089] Preferably, the concentration of hydrogen in the hydrogen-containing atmosphere is not less than 5% by volume, more preferably 5-90% by volume, and further preferably 40-90% by volume.
[0090] In the present invention, specifically, before the reduction, the method further comprises introducing a protective gas into the reduction device for replacement, then introducing hydrogen to obtain the hydrogen-containing atmosphere, and then performing the reduction. According to the present invention, specifically, the oxidized catalyst is loaded into the pre-reduction reactor, the system is replaced with a protective gas (e.g., N2), preferably ensuring that the volume percentage of O2 in the system is ≤0.5%, starting the compressor, maintaining the system pressure at 0.0-2MPa (gauge pressure), and performing the reduction according to the temperature increase and hydrogen preparation procedure.
[0091] Further preferably, the preparation method further comprises a heat exchange step: the introduced hydrogen and optionally the protective gas are first heat exchanged with the reduced gas, then optionally heated, and then introduced into the reduction system. The reduced tail gas is cooled by heat exchange and preferentially separated by gas-liquid separation, and the tail gas after water removal can be recycled for the reduction process.
[0092] In the present invention, there is no particular limitation on the equipment for performing the reduction, but it is preferably a rotary kiln reactor, a fluidized bed reactor or a drum reactor, more preferably a fluidized bed reactor, and most preferably a fluidized reactor with a riser.
[0093] The present invention has no particular limitation on the amount of reducing gas, and it is preferably selected based on the principle of keeping the powder in a fluidized state.
[0094] Preferably, the reduction conditions in step (3) include: the oxidized catalyst is in a fluidized state and in contact with a reducing gas; the temperature is 100-750°C, more preferably 150-700°C.
[0095] Preferably, the reduction conditions in step (3) include: a time of no more than 2 hours, more preferably no more than 1.5 hours. The time refers to the residence time of the oxidized catalyst at the highest reduction temperature in the equipment for performing the reduction.
[0096] Preferably, the reduction conditions in step (3) include: the reduction gas-agent ratio is 500-5000, more preferably 600-4500.
[0097] The present invention has a wide range of pressure selection for the reduction, preferably 0-2 MPa. The pressure is a gauge pressure.
[0098] The oxidized catalyst using raspberry-shaped oxide microspheres as carriers can be quickly reduced, and the obtained Fischer-Tropsch synthesis catalyst has good regeneration performance and a large number of active centers.
[0099] According to the present invention, in step (4), preferably, after the temperature of the catalyst obtained by reduction in step (3) drops below 50° C., oxygen-containing gas below 50° C. is continuously introduced to passivate the catalyst obtained by reduction in step (3).
[0100] In the present invention, there is no limitation on the method of cooling the catalyst obtained by reduction in step (3), as long as the catalyst can be cooled to the desired temperature, for example, by heat exchange, cold exchange, water cooling, ammonia cooling, purging, etc.
[0101] According to a preferred embodiment of the present invention, the method provided by the present invention further comprises a process of replacing the hydrogen in the system before the passivation. According to a specific embodiment of the present invention, carbon dioxide or carbon dioxide and nitrogen are used to replace H2 in the system. The purge process can not only achieve rapid cooling but also achieve the replacement of hydrogen in the system.
[0102] Preferably, when the temperature of the catalyst obtained by reduction in step (3) drops to below 45° C. (more preferably below 35° C.), and the hydrogen content in the system is ≤1% by volume, the catalyst obtained by reduction in step (3) is passivated.
[0103] In the preparation method of the present invention, it can be understood that the passivation temperature is not higher than 70° C. means that the passivation temperature of the catalyst bed is not higher than 70° C. Preferably, the passivation temperature is controlled to be no higher than 65° C.
[0104] According to the method provided by the present invention, as long as the concentration of the oxygen-containing gas introduced during the passivation process shows an increasing trend, it is within the scope of "the oxygen concentration of the oxygen-containing gas continues to increase" described in the present invention. The oxygen concentration of the oxygen-containing gas continues to increase may be a uniform increase or an irregular increase, and the present invention has no particular limitation on this.
[0105] According to a specific embodiment of the present invention, for ease of operation, a certain concentration of oxygen-containing gas may be introduced for a certain period of time, and then a higher concentration of oxygen-containing gas may be introduced for a certain period of time, and so on. In this case, that is, the oxygen concentration increases in stages, for example, in multiple stages, in one specific embodiment, the oxygen concentration in the latter stage is higher than the oxygen concentration in the previous stage, and in another specific embodiment, the oxygen concentrations in the first few stages are the same and lower than the oxygen concentration in the subsequent stages, thereby showing an overall upward trend.
[0106] In the present invention, preferably, the oxygen concentration of the oxygen-containing gas is continuously increased in stages. In this case, the present invention has a wide range of optional durations for the various stages, as long as it is beneficial to improving the performance of the obtained catalyst. More preferably, during the passivation process, when the oxygen-containing gas introduced in the previous stage makes the oxygen concentration in the passivation outlet gas equal to the oxygen concentration of the introduced oxygen-containing gas, the operation of introducing the oxygen-containing gas in the next stage is entered.
[0107] According to the present invention, preferably, during the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in at least 2 stages, more preferably in 2-10 stages, and more preferably in 3-8 stages, for example, the number of stages may be 3, 4, 5, 6, 7, 8. By adopting this preferred solution, the catalyst can be passivated more uniformly, so that the catalyst has more active centers after re-reduction activation.
[0108] It is understood that, under the preferred embodiment, the oxygen concentration of the oxygen-containing gas in the first stage is lower than the oxygen concentration of the oxygen-containing gas in the second stage, and the oxygen concentration of the oxygen-containing gas in the second stage is lower than the oxygen concentration of the oxygen-containing gas in the third stage, and so on. Further, it is understood that the relative multiples of the oxygen concentration of the oxygen-containing gas in each adjacent two stages can be independently the same or different, for example, the relative multiple of the oxygen concentration of the oxygen-containing gas in the first stage and the second stage is 1.5, and the relative multiple of the oxygen concentration of the oxygen-containing gas in the second stage and the third stage can be 1.5 or 2.
[0109] Preferably, the gas-to-agent ratio of the passivation is 200-4500, more preferably 300-4000.
[0110] In the passivation process of the present invention, the gas-to-agent ratio of each stage of passivation can be independently the same or different, as long as it is conducive to promoting the uniform passivation process of the catalyst and improving the passivation efficiency. Those skilled in the art can freely choose according to needs.
[0111] According to a preferred embodiment of the present invention, the passivation time is no more than 5 hours, preferably no more than 1.5 hours, for example, 0.5-1.5 hours. The passivation method provided by the present invention can be completed in a short time, and the passivation effect is good.
[0112] In the present invention, preferably, the oxygen concentration of the oxygen-containing gas is continuously increased in stages. In this case, the present invention has a wide range of optional durations for the various stages, as long as it is beneficial to improving the performance of the obtained catalyst. More preferably, during the passivation process, when the oxygen-containing gas introduced in the previous stage makes the oxygen concentration in the passivation outlet gas equal to the oxygen concentration of the introduced oxygen-containing gas, the oxygen-containing gas is introduced into the next stage.
[0113] In the present invention, the oxygen-containing gas is preferably a mixture of a protective gas and oxygen, and the protective gas is selected from one or more of helium, argon, carbon dioxide and nitrogen.
[0114] Preferably, the concentration of the oxygen-containing gas is 0.05-21% by volume, preferably 0.1-21% by volume.
[0115] According to a preferred embodiment of the present invention, during the passivation process, the initial oxygen concentration of the oxygen-containing gas introduced is 0.05-0.2% by volume. The use of oxygen-containing gas with a lower initial oxygen concentration can make the passivation uniform and controllable, and is more conducive to obtaining a catalyst with good reproducibility.
[0116] According to a preferred embodiment of the present invention, during the passivation process, the oxygen concentration of the oxygen-containing gas introduced in the second stage is 0.1-1% by volume.
[0117] According to a preferred embodiment of the present invention, during the passivation process, the oxygen concentration of the oxygen-containing gas introduced in the latter stage is 1-8 times the oxygen concentration of the oxygen-containing gas introduced in the previous stage. Under this preferred embodiment, the catalyst can be passivated more uniformly and controllably, so that the obtained catalyst has more active centers after the re-reduction treatment, and the passivation efficiency is high.
[0118] The present invention has no particular limitation on the device for passivation, which can share the same set of devices with the reduction or can be set separately. Its type can refer to the device used in the reduction process, such as a fluidized bed reactor, in which the catalyst is in a fluidized state.
[0119] In the present invention, when the reduction and passivation are carried out using the same equipment, the method further comprises: before the passivation, firstly introducing a protective gas (preferably carbon dioxide and N2 in a volume ratio of 10-20) to replace the H2 in the system, rapidly cooling down, and when the volume percentage of H2 in the system is ≤1%, then introducing oxygen so that the amount of oxygen in the passivation atmosphere meets the required oxygen concentration, and then carrying out the passivation. The gas after passivation is recycled or directly discharged. Preferably, the passivation temperature is ensured to be no higher than 70°C by adjusting the amount of protective gas (preferably carbon dioxide) pumped in.
[0120] In the present invention, the reducing gas (ie, the hydrogen-containing atmosphere) and the passivating gas (ie, the oxygen-containing gas) may be used once or recycled; preferably, the hydrogen-containing gas is recycled and the passivating gas is not recycled.
[0121] According to a preferred embodiment of the present invention, before the reduction in step (3), the method further comprises: preheating the reducing gas (i.e., hydrogen-containing gas) and the oxidized catalyst at the same time, and then contacting the preheated reducing gas and the oxidized catalyst to perform the reduction. Furthermore, the product obtained after the reduction is preferably subjected to gas-solid separation, preferably in a cyclone dust collector.
[0122] In the present invention, reduction and passivation preferably adopt a dual reactor form, for example, after the oxidation state catalyst is reduced in the first stage rapid reduction reactor, the reduced material is then transported to an intermediate tank, cooled and then transported to a second reactor for passivation. The supporting equipment may include a powder preheating furnace, a gas preheating furnace, a feeding device, a powder reduction device, an intermediate tank, a powder passivation device, etc.
[0123] Compared with the prior art, the present invention has the advantages of improving the reduction speed and equipment utilization coefficient, high efficiency, low energy consumption and low production cost. The above advantages are as follows: when the particle size of the powder is ground to less than 2000 microns, the fine powder can use a fast circulating fluidized bed or a conveying reactor, and the required gas velocity is lower than the fluidization gas velocity of the coarse powder. At the same time, the reaction speed of the fine powder is fast, so the efficiency of the reactor is high.
[0124] The third aspect of the present invention provides a Fischer-Tropsch synthesis catalyst prepared by the preparation method described in the second aspect. The Fischer-Tropsch synthesis catalyst has the composition and structure of the Fischer-Tropsch synthesis catalyst described in the first aspect, which will not be described in detail here.
[0125] According to the present invention, preferably, the reduction degree of the Fischer-Tropsch synthesis catalyst is 50-98% as characterized by TPR. The Fischer-Tropsch synthesis catalyst provided by the present invention has a suitable reduction degree and higher activity. However, the pre-reduction catalyst of the prior art has a higher reduction degree (close to 100%) and lower activity.
[0126] In the present invention, the test method of reduction degree is as follows: The test method of reduction degree is as follows: first test the TPR spectrum curve of the pre-reduced catalyst; then calcine 0.2g of the pre-reduced catalyst in an air atmosphere at 450°C for 2h to obtain an oxidized catalyst, test the TPR spectrum curve of the oxidized catalyst according to the TPR test method described in the first aspect, and calculate the reduction degree of the pre-reduced catalyst. Wherein, reduction degree = (direct reduction TPR peak area of oxidized catalyst - high temperature unreduced peak area of pre-reduced catalyst) / direct reduction TPR peak area of oxidized catalyst * 100%.
[0127] The Fischer-Tropsch synthesis catalyst provided by the present invention can be reactivated by hydrogen at a temperature below 300°C.
[0128] The Fischer-Tropsch synthesis catalyst provided by the present invention uses raspberry-shaped oxide microspheres as carriers, so that in the reduction and passivation process, the diffusion distance is short, the macroscopic surface area is large, better reduction and passivation can be performed, and the efficiency is high, and the Fischer-Tropsch synthesis performance is better. In addition, the preparation method of the present invention is low in cost and can be applied in large-scale industry.
[0129] The fourth aspect of the present invention provides use of the Fischer-Tropsch synthesis catalyst described in the first aspect or the third aspect in a Fischer-Tropsch synthesis reaction.
[0130] The present invention reduces smaller particles quickly, which, on the one hand, fully reduces the oxides in the catalyst, improves the reduction degree of the catalyst, and can keep the crystals smaller. Thus, the oxidized catalyst is efficiently reduced to a catalyst precursor with high activity. On the other hand, the method of the present invention has the advantages of high efficiency, and can obtain a very uniform and easily regenerated catalyst with many active centers. Thus, the overall reaction activity of the catalyst is improved. It has a good industrial application prospect.
[0131] The present invention will be described in detail below by way of examples. In the following examples, the test method is as follows:
[0132] The temperature corresponding to the peak of the low-temperature reduction peak with the largest area in the TPR spectrum curve is used as a measure to evaluate the regeneration of the passivated catalyst: the lower the temperature corresponding to the peak of the low-temperature reduction peak with the largest area, the easier the catalyst is to regenerate. The programmed temperature reduction (TPR) was carried out on an Autochem2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics, USA. The test conditions were: 0.20g of the sample was first heated to 120℃ for dehydration treatment for 1 hour under a 50mL / min Ar gas flow at a heating rate of 10℃ / min, and the TPR experiment was carried out after the temperature dropped to 50℃. The experimental conditions and procedures of TPR were: the reducing gas was a H2-Ar mixed gas with a hydrogen content of 10 volume%, the reducing gas flow rate was 50mL / min, and the temperature was raised to 900℃ at a heating rate of 10℃ / min; during the above heating process, the signal was detected by a thermal conductivity detector (TCD) to obtain a TPR spectrum curve.
[0133] The reduction degree of the catalyst is characterized by TPR. The test method is: The test method of the reduction degree is: first test the TPR spectrum curve of the pre-reduced catalyst; then calcine 0.2g of the pre-reduced catalyst in an air atmosphere at 450°C for 2h to obtain an oxidized catalyst, and test the TPR spectrum curve of the oxidized catalyst according to the aforementioned TPR test method to calculate the reduction degree of the pre-reduced catalyst. Among them, the reduction degree = (TPR peak area of the oxidized catalyst directly reduced - the high temperature unreduced peak area of the pre-reduced catalyst) / TPR peak area of the oxidized catalyst directly reduced * 100%.
[0134] The number of active centers was obtained by H2-programmed temperature desorption (H2-TPD) test on the Autochem2950 fully automatic high-pressure chemical adsorption instrument produced by Micromeritics, USA. The test method is as follows: weigh 0.2000g of a 40-60 mesh sample, first perform re-reduction activation, and the re-reduction conditions are: H2-Ar mixed gas with a hydrogen content of 10 volume%, a mixed gas flow rate of 50mL / min, and a temperature increase rate of 10℃ / min to 200℃ for reduction for 2h. The reduced catalyst is cooled in a H2-Ar mixed gas with a hydrogen content of 10 volume%. After the temperature drops to 55℃, it is switched to Ar gas for purging, with an Ar flow rate of 20mL / min, until the baseline is stable, and then the H2-TPD experiment is performed. The experimental conditions and procedures of H2-TPD are: the carrier gas is Ar, the carrier gas flow rate is 20mL / min, the heating rate is 10℃ / min, the final temperature is 400℃, and the thermal conductivity detector (TCD) detects the signal to obtain the TPD curve.
[0135] In the following examples, preparation examples and comparative examples, the specifications of some raw materials used are as follows:
[0136] Pseudo-boehmite powder (produced by Changling Catalyst Factory, with a solid content of 69.5% by weight and a γ-Al2O3 content of not less than 98% by weight);
[0137] Alumina sol (produced by Zhoucun Catalyst Factory, containing 22 wt% Al2O3);
[0138] Sodium silicate (Jinan Huifengda Chemical Co., Ltd., modulus 3.1-3.4, insoluble matter less than 0.4%);
[0139] Ammonia water, hydrochloric acid, nitric acid, sulfuric acid, aluminum sulfate, aluminum chloride, zirconium hydroxide, zirconium oxychloride, titanium tetrachloride, titanium dioxide (Sinopharm Chemical Reagent Co., Ltd., industrial grade);
[0140] Polyethylene glycol PEG4000 powder (Wenzhou Shuangxiao Rubber and Plastic Material Co., Ltd.);
[0141] Methyl cellulose (Hubei Jiangmin Taihua Chemical Co., Ltd.);
[0142] Tetraethyl orthosilicate (TEOS, Jinan Huate Chemical Co., Ltd., content about 99%);
[0143] Cobalt nitrate, aluminum nitrate, titanium nitrate, zirconium nitrate, yttrium nitrate, magnesium nitrate (Yutai Qixin Chemical Co., Ltd., industrial grade).
[0144] The breakage rate of the carrier and catalyst can be measured as follows:
[0145] First, the microspheres to be tested are passed through a 100-mesh sieve, and then the sieved microsphere powder is passed through a 150-mesh sieve. Finally, the microsphere powder intercepted by the 150-mesh sieve is used as the sample to be tested. In a cylindrical steel container with a cross-sectional diameter of 10mm, a certain mass of microspheres (particle size of 100-150 mesh) is added, and then a certain pressure (100N) is applied to the microspheres through a cylinder for a certain period of time (10 seconds), and then the pressed microsphere powder is sieved with a 150-mesh sieve, and the mass of the microsphere powder under the sieve is recorded, and then the mass of the microsphere powder under the sieve is divided by the total mass of the added microspheres to obtain the crushing rate of the microspheres.
[0146] The following preparation example is used to illustrate the preparation of raspberry-shaped oxide microspheres.
[0147] Preparation Example 1
[0148] Add 20 kg of water into the reactor, add 1.2 kg of aluminum nitrate, then add 200 g of concentrated nitric acid, add 2.3 kg of PEG4000, and finally add 4.0 kg of pseudo-boehmite powder, stir evenly and grind to obtain a dispersed slurry.
[0149] The dispersion slurry was aged at 35°C with stirring for 1.5 hours.
[0150] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 580°C, and the air outlet temperature at the end of the drying is 160°C.
[0151] According to the SEM photograph of the obtained raspberry-shaped oxide microspheres, the microsphere surface has a hollow microsphere with a large hole, the hollow microsphere has a hollow structure inside, and the large hole and the hollow structure are connected to form a cavity with one end open.
[0152] Preparation Example 2
[0153] Add 20 kg of water into the reactor, add 0.5 kg of zirconium nitrate, then add 175 g of concentrated nitric acid, add 2 kg of PEG4000, and finally add 4.6 kg of pseudo-boehmite powder, stir evenly and grind to obtain a dispersed slurry.
[0154] The dispersion slurry was aged at 25°C with stirring for 1 hour.
[0155] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 600°C, and the air outlet temperature at the end of the drying is 180°C.
[0156] The SEM of the obtained raspberry-shaped oxide microspheres is similar to that of Preparation Example 1.
[0157] Preparation Example 3
[0158] Add 30 kg of water to the reactor, add 0.7 kg of zirconium nitrate, then add 2 L of concentrated ammonia water, add 1.5 kg of PEG4000 and 8 g of picric acid, and finally add 7 kg of zirconium hydroxide, stir evenly and grind to obtain a dispersed slurry.
[0159] The dispersion slurry was aged at 25°C with stirring for 2 hours.
[0160] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 560°C, and the air outlet temperature at the end of the drying is 140°C.
[0161] The SEM of the obtained raspberry-shaped oxide microspheres is similar to that of Preparation Example 1.
[0162] Preparation Example 4
[0163] Add 30 kg of water to the reactor, add 0.7 kg of titanium nitrate, then add 2.6 L of concentrated ammonia water, add 1.5 kg of PEG4000 and 6 g of picric acid, and finally add 500 g of concentrated nitric acid and 7 kg of titanium nitrate, stir evenly and grind to obtain a dispersed slurry.
[0164] The dispersion slurry was aged at 25°C with stirring for 2 hours.
[0165] The aged dispersed slurry is sent to a spray drying device for drying and forming to obtain raspberry-shaped oxide microspheres, wherein the atomization pressure of the spray drying is 0.3 to 3.0 MPa, the pressure in the tower is -0.0010 to -0.0090 MPa; the initial air inlet temperature of the drying is 560°C, and the air outlet temperature at the end of the drying is 141°C.
[0166] The SEM of the obtained raspberry-shaped oxide microspheres is similar to that of Preparation Example 1.
[0167] The following examples are used to illustrate the Fischer-Tropsch synthesis catalyst provided by the present invention.
[0168] Example 1
[0169] The raspberry-shaped oxide microspheres obtained in Preparation Example 1 were calcined at 600° C. for 3 hours to obtain carrier ZT1, whose physical properties are shown in Table 1.
[0170] The carrier ZT1 was impregnated with cobalt nitrate and zirconium nitrate solutions several times to prepare a catalyst with a Co content of 35 wt% and a Zr content of 1 wt%. The catalyst was dried at 120°C for 2 hours and calcined at 420°C for 2 hours to obtain catalyst CAT1.
[0171] The calcined powder was transported to a fluidized bed reduction system. First, a nitrogen replacement system was introduced into the reactor until the oxygen content was qualified (oxygen content ≤ 0.5 volume %). Then, hydrogen was added to make the hydrogen content in the hydrogen-nitrogen mixed gas 40 volume %, and then a one-step reduction process was started: the above mixed gas with a gas-to-agent ratio of 2000 was introduced to make the catalyst in a fluidized state, and the temperature of the catalyst was raised to 400°C at a heating rate of 80°C / hour, and the temperature was kept constant for 1 hour; the reduction step was ended.
[0172] Then, nitrogen is introduced to replace the hydrogen in the system, and the reduced catalyst is cooled to below 45°C, and an oxygen-containing gas with an oxygen concentration of 0.2-21% by volume, which is composed of air and nitrogen, is introduced at normal pressure below 45°C. Oxygen-containing gases with oxygen concentrations of 0.2%, 0.6%, 1.0%, 3.0%, 8.0% and 21% by volume are introduced in 6 stages, wherein after the oxygen-containing gas of the previous stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the next stage is introduced, and the oxygen concentration is gradually increased for passivation until the passivation is completed. The passivation gas-agent ratio is 2000, during which the passivation temperature of the catalyst bed is controlled to be less than 65°C, and the total passivation time is 1 hour. A Fischer-Tropsch synthesis catalyst is obtained.
[0173] The SEM photo of the catalyst prepared in Example 1 is as follows: Figure 1 shown.
[0174] Comparative Example 1
[0175] The method of Example 1 is different in that the passivation is not segmented, and specifically includes: introducing an oxygen-containing gas with an oxygen concentration of 21% by volume at a temperature below 55°C under normal pressure, a gas-to-agent ratio of 500, a passivation time of 0.5 hours, and controlling the passivation temperature of the catalyst bed to be less than 150°C.
[0176] Comparative Example 2
[0177] The method of Example 1 is different in that the passivation process is different. Specifically, an oxygen-containing gas with an oxygen concentration of 1.5-21% by volume and a temperature below 55° C. is introduced under normal pressure. The passivation is divided into two stages. The gas-to-agent ratio is 500. The oxygen-containing gas used in the first stage of passivation has an oxygen concentration of 1.5% by volume; the oxygen-containing gas used in the second stage of passivation has an oxygen concentration of 21% by volume. After the oxygen-containing gas in the first stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas in the second stage is introduced. The total passivation time is 1 hour. During this period, the passivation temperature of the catalyst bed is controlled to be less than 150° C.
[0178] Example 2
[0179] The raspberry-shaped oxide microspheres obtained in Preparation Example 2 were calcined at 500° C. for 3 hours to obtain carrier ZT2, whose physical properties are shown in Table 1.
[0180] The carrier ZT2 was impregnated with solutions containing cobalt nitrate and zirconium nitrate several times to prepare a catalyst with a Co content of 35 wt% and a Zr content of 2 wt%. The catalyst was dried at 110°C for 4 hours and calcined at 350°C for 3 hours to obtain the catalyst CAT2.
[0181] The catalyst CAT2 was reduced and passivated according to the method of Example 1, except that the oxygen concentration of the oxygen-containing gas used in the first stage of passivation was 0.1% by volume, the oxygen concentration of the oxygen-containing gas used in the second stage was 0.8% by volume, the third stage and subsequent stages were the same as in Example 1, and the total passivation time was 1.5 hours. A Fischer-Tropsch synthesis catalyst was obtained.
[0182] Example 3
[0183] The raspberry-shaped oxide microspheres obtained in Preparation Example 3 were calcined at 550° C. for 3 hours to obtain carrier ZT3, whose physical properties are shown in Table 1.
[0184] The carrier ZT3 was impregnated with cobalt nitrate and Re(NO3)3 solutions multiple times to prepare a catalyst with a Co content of 35 wt% and a Re content of 0.002 wt%. The catalyst was dried at 120°C for 2 hours and calcined at 420°C for 2 hours to obtain the catalyst CAT3.
[0185] Catalyst CAT3 was reduced according to the method of Example 1, except that the reduction temperature was 450° C. and the temperature was kept constant for 1.5 hours; then passivation was performed according to the method of Example 1, except that the oxygen concentration of the oxygen-containing gas used in the first stage of passivation was 0.15% by volume, the oxygen concentration of the oxygen-containing gas used in the second stage was 0.9% by volume, the third stage and subsequent stages were the same as in Example 1, and the total passivation time was 1 hour. A Fischer-Tropsch synthesis catalyst was obtained.
[0186] Example 4
[0187] The raspberry-shaped oxide microspheres obtained in Preparation Example 4 were calcined at 700° C. for 3 hours to obtain carrier ZT4, whose physical properties are shown in Table 1.
[0188] The carrier ZT4 was impregnated with cobalt nitrate and copper nitrate solutions for multiple times to prepare a catalyst with a Co content of 35.0 wt% and a Cu content of 1.0 wt%. The catalyst was dried at 130°C for 2 hours and calcined at 370°C for 4 hours to obtain catalyst CAT4.
[0189] Catalyst CAT4 was reduced and passivated according to the method of Example 3, except that during the reduction process, the reduction temperature was 450° C. and the temperature was kept constant for 1.5 hours; and during the passivation process, the oxygen concentration of the oxygen-containing gas used in the first stage of passivation was 0.2% by volume, the oxygen concentration of the oxygen-containing gas used in the second stage was 1% by volume, and the third stage and subsequent stages were the same as in Example 1, and the total passivation time was 2 hours. A Fischer-Tropsch synthesis catalyst was obtained.
[0190] Table 1 Physical properties of carriers
[0191]
[0192] As can be seen from Table 1, when the raspberry-shaped oxide microspheres prepared in the present invention are used as carriers, although the specific surface area, pore volume and average pore diameter are similar to those of the comparative example, the sphericity and strength are greatly improved, which are significantly better than the oxide microspheres prepared in the comparative example, providing the possibility of utilizing these carriers.
[0193] Example 5
[0194] According to the method of Example 1, the difference is that the reduction process specifically includes: firstly, a nitrogen replacement system is introduced into the reactor until the oxygen content is qualified (oxygen content ≤ 0.5 volume %), and a hydrogen-containing gas (a mixture of 70 volume % hydrogen and nitrogen) is used for reduction at 410° C. for 1 hour, and the gas-to-agent ratio is 2200. The Fischer-Tropsch synthesis catalyst CAT5 is obtained.
[0195] Example 6
[0196] According to the method of Example 1, the difference is that the passivation process specifically includes: cooling the above-mentioned reduced catalyst to below 40°C, and introducing an oxygen-containing gas with an oxygen concentration of 0.05-21% by volume composed of air and nitrogen below 40°C under normal pressure. Introducing oxygen-containing gases with oxygen concentrations of 0.05%, 0.2%, 0.4%, 0.8%, 1.2%, 3.0%, 8.0%, and 21% by volume in 8 stages, wherein after the oxygen-containing gas of the previous stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the next stage is introduced, and the oxygen concentration is gradually increased for passivation until the passivation is completed. The gas-agent ratio of the first two stages of passivation is 1000, and the gas-agent ratio of the last six stages of passivation is 500. During the period, the passivation temperature of the catalyst bed is controlled to be less than 55°C, and the total passivation time is 1 hour. Obtain Fischer-Tropsch synthesis catalyst CAT6.
[0197] Example 7
[0198] According to the method of Example 1, the difference is that the passivation process specifically includes: cooling the reduced catalyst to below 45°C, introducing oxygen-containing gas with an oxygen concentration of 0.15-21% by volume under normal pressure, and sequentially introducing oxygen-containing gas with oxygen concentrations of 0.15%, 0.3%, 1.0%, 6%, 12% and 21.0% by volume in 6 stages; the gas-to-agent ratio in the first 2 stages of passivation is 2000, and the gas-to-agent ratio in the last 4 stages of passivation is 1000, during which the passivation temperature of the catalyst bed is controlled to be less than 55°C, and the total passivation time is 1 hour. The Fischer-Tropsch synthesis catalyst CAT7 is obtained.
[0199] Example 8
[0200] According to the method of Example 1, the difference is that the passivation process is different, specifically: an oxygen-containing gas with an oxygen concentration of 1-21% by volume composed of air and nitrogen at a temperature below 45°C is introduced under normal pressure. Oxygen-containing gases with oxygen concentrations of 1.0%, 3.0%, 8.0% and 21% by volume are introduced in 4 stages, wherein after the oxygen-containing gas of the previous stage is introduced, when the oxygen concentration at the gas outlet is equal to the oxygen concentration at the gas inlet, the oxygen-containing gas of the next stage is introduced, and the oxygen concentration is gradually increased for passivation until the passivation is completed. During this period, the passivation temperature of the catalyst bed is controlled to be less than 65°C, and the total passivation time is 2 hours. Fischer-Tropsch synthesis catalyst CAT8 is obtained.
[0201] The catalysts prepared in the above examples and comparative examples were characterized and analyzed. The number of active centers of the catalysts after re-reduction treatment, the temperature corresponding to the peak of the low-temperature reduction peak with the largest area in the TPR spectrum curve, and the degree of reduction are listed in Table 2.
[0202] Table 2
[0203]
[0204] It can be seen from Table 2 that the Fischer-Tropsch synthesis catalyst obtained by the method of the present invention has a higher number of active centers, and the peak temperature corresponding to the peak of the low-temperature reduction peak with the largest area is lower, and the catalyst is easier to regenerate.
[0205] Test Example 1
[0206] The reaction performance of the catalyst prepared above was tested in a small microchannel reactor (the minimum dimension of the channel cross section is 1000 μm). The small microchannel reactor module has 16 reaction channels and 36 cooling channels. The reaction channel is 200 mm long and the maximum catalyst loading is 6 mL.
[0207] 4.0 ml of the above catalyst was loaded into the constant temperature zone of a small microchannel reactor, and the pre-reduced catalysts obtained in the above examples and comparative examples were tested respectively. Before using the catalyst, the catalyst needs to be reduced. The reduction atmosphere is hydrogen; the reduction reaction conditions are: pressure is normal pressure, the heating rate is 5°C / min, and the hydrogen space velocity is 600h -1 The re-reduction temperature is 200°C and the re-reduction time is 2 hours.
[0208] After re-reduction, the reaction performance test was carried out. The specific reaction conditions were: the raw gas was synthesis gas, wherein the H2 / CO molar ratio was 2 / 1, the pressure was 2.5 MPa, the temperature was 220°C, and the raw gas volume space velocity was 24000 h -1 After the reaction was carried out for 12 hours, a gas sample was taken for chromatographic analysis.
[0209] The reaction performance indicators include: CO conversion rate, methane selectivity, C5+ hydrocarbon selectivity and CO2 selectivity. The reaction performance test results are shown in Table 3.
[0210] The calculation formula of methane selectivity is:
[0211]
[0212] Among them, n CH4 is the number of moles of CO converted to methane, n con is the total molar number of CO converted.
[0213] The formula for calculating the selectivity of C5+ hydrocarbons is: (total moles of CO converted - moles of carbon monoxide converted to carbon dioxide and C1-C4 hydrocarbons) / total moles of CO converted.
[0214] The formula for calculating CO2 selectivity is: moles of C converted to CO2 / total moles of CO converted.
[0215] Table 3
[0216]
[0217]
[0218] The test results in Table 3 show that the catalyst provided by the present invention has better FT synthesis performance, i.e., higher CO conversion rate and C5+ hydrocarbon selectivity, lower methane selectivity and CO2 selectivity. Moreover, the methane selectivity of the catalyst of the present invention does not increase significantly due to the increase in temperature, which significantly solves the diffusion problem of the FT synthesis reaction.
[0219] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A Fischer-Tropsch synthesis catalyst, comprising a carrier and an active component supported on the carrier, wherein the active component comprises cobalt and an additive, wherein the additive is selected from at least one of Group IA metal elements, Group IIA elements, Group IB elements, Group IIB elements, Group IIIB elements, Group IVB elements, Group VB elements, Group VIB elements, Group VIIB elements and Group VIII elements, wherein the content of cobalt is 20-60% by weight and the content of the additive is 0.001-25% by weight, based on the total amount of the catalyst and calculated as oxide; The carrier is a raspberry-shaped oxide microsphere, which is a hollow microsphere with a large hole on the surface, and a hollow structure inside the hollow microsphere, wherein the large hole and the hollow structure are connected to form a cavity with an open end; wherein, The oxide in the raspberry-shaped oxide microspheres is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide; The number of active centers of the catalyst after the reduction treatment is 0.06-0.3 mmol hydrogen / g catalyst, and the reduction treatment conditions include: temperature of 200° C., time of 2 hours, reduction atmosphere of 10% by volume hydrogen-containing and argon-containing atmosphere, and gas-to-agent volume ratio of 15000; The preparation of raspberry-shaped oxide microspheres includes: (1-1) adding nitrate, peptizing agent, pore former, the oxide and / or its precursor into a dispersant and stirring to obtain a dispersed slurry; (1-2) subjecting the dispersed slurry to an aging treatment; (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded at an inlet air temperature of 400-1200° C. and an outlet air temperature of 50-300° C. to obtain the raspberry-shaped oxide microspheres.
2. The catalyst according to claim 1, wherein After the catalyst is subjected to re-reduction treatment, the number of active centers of the catalyst is 0.09-0.29 mmol hydrogen / g catalyst.
3. The catalyst according to claim 1 or 2, wherein The catalyst is characterized by TPR. In its TPR curve, the temperature corresponding to the peak of the low-temperature reduction peak with the largest area is 140-270°C.
4. The catalyst according to claim 3, wherein The catalyst is characterized by TPR. In its TPR curve, the temperature corresponding to the peak of the low-temperature reduction peak with the largest area is 150-260°C.
5. The catalyst according to claim 1 or 2, wherein Based on the total amount of the catalyst, the content of cobalt is 25-55% by weight, and the content of the auxiliary agent is 0.001-10% by weight, calculated as oxide.
6. The catalyst according to claim 1 or 2, wherein The auxiliary agent is selected from one or more of La, Zr, Mn, V, Cr, Cu, Ce, W, Ti, Zn, Sc, Mg, Ca, Be, Na, K, Ru, Ag, Au, Re, Pt and Pd.
7. The catalyst according to claim 6, wherein The auxiliary agent is selected from one or more of La, Zr, Cu, Ce, W, Ti, Ru, Ag, Au, Re, Pt and Pd.
8. The catalyst according to claim 1 or 2, wherein The oxide in the raspberry-shaped oxide microspheres is aluminum oxide and / or silicon oxide.
9. The catalyst according to claim 1 or 2, wherein The particle size of the raspberry-shaped oxide microspheres is 3-2500 μm; and / or, The diameter of the hollow structure is 1-2000 μm; and / or, The pore size of the macropores is 0.2-1000 μm; and / or, The shell thickness of the hollow microsphere is 0.2-1000 μm.
10. The catalyst according to claim 9, wherein The particle size of the raspberry-shaped oxide microspheres is 10-500 μm.
11. The catalyst according to claim 9, wherein The pore size of the macropores is 0.5-200 μm.
12. The catalyst according to claim 9, wherein The shell thickness of the hollow microsphere is 0.5-200 μm.
13. The catalyst according to claim 1 or 2, wherein The sphericity of the raspberry-shaped oxide microspheres is 0.5-0.99; and / or The crushing rate of the raspberry-shaped oxide microspheres is 0-1%.
14. A method for preparing a Fischer-Tropsch synthesis catalyst, the method comprising: (1) preparing raspberry-shaped oxide microspheres; (2) introducing active components into the raspberry-shaped oxide microspheres by an impregnation method to obtain an oxidized catalyst; The active component comprises cobalt and an auxiliary agent, wherein the auxiliary agent is selected from at least one of Group IA metal elements, Group IIA elements, Group IB elements, Group IIB elements, Group IIIB elements, Group IVB elements, Group VB elements, Group VIB elements, Group VIIB elements and Group VIII elements; (3) reducing the oxidized catalyst under a hydrogen-containing atmosphere; (4) after the temperature of the catalyst obtained by reduction in step (3) drops below 50° C., the catalyst obtained by reduction in step (3) is passivated, wherein the passivation comprises: continuously introducing an oxygen-containing gas below 50° C. and controlling the passivation temperature to be no higher than 70° C.; wherein the oxygen concentration of the oxygen-containing gas is continuously increased; The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of cobalt in the oxidized catalyst is 20-60% by weight and the content of the auxiliary agent is 0.001-25% by weight, based on the total amount of the oxidized catalyst and calculated as oxide; Wherein, the preparation of raspberry-shaped oxide microspheres in step (1) comprises: (1-1) adding nitrate, peptizing agent, pore former, the oxide and / or its precursor into a dispersant and stirring to obtain a dispersed slurry; (1-2) subjecting the dispersed slurry to an aging treatment; (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded at an inlet air temperature of 400-1200° C. and an outlet air temperature of 50-300° C. to obtain the raspberry-shaped oxide microspheres.
15. The preparation method according to claim 14, wherein: The amount of the raspberry-shaped oxide microspheres and the active component is such that the content of cobalt in the oxidized catalyst is 25-55% by weight and the content of the auxiliary agent is 0.001-10% by weight, calculated as oxide, based on the total amount of the oxidized catalyst.
16. The preparation method according to claim 14 or 15, wherein: The auxiliary agent is selected from one or more of La, Zr, Mn, V, Cr, Cu, Ce, W, Ti, Zn, Sc, Mg, Ca, Be, Na, K, Ru, Ag, Au, Re, Pt and Pd; and / or, The oxide in the raspberry-shaped oxide microspheres is selected from one or more of aluminum oxide, silicon oxide, zirconium oxide, magnesium oxide, calcium oxide and titanium oxide.
17. The preparation method according to claim 16, wherein: The auxiliary agent is selected from one or more of La, Zr, Cu, Ce, W, Ti, Ru, Ag, Au, Re, Pt and Pd.
18. The preparation method according to claim 16, wherein: The oxide in the raspberry-shaped oxide microspheres is aluminum oxide and / or silicon oxide.
19. The preparation method according to claim 16, wherein: The particle size of the raspberry-shaped oxide microspheres is 3-2500 μm.
20. The preparation method according to claim 19, wherein: The particle size of the raspberry-shaped oxide microspheres is 10-500 μm.
21. The preparation method according to claim 14 or 15, wherein: (1-3) The aged dispersed slurry is sent to a drying device, and dried and molded under the conditions of an inlet air temperature of 450-700° C. and an outlet air temperature of 120-200° C. to obtain the raspberry-shaped oxide microspheres.
22. The preparation method according to claim 14 or 15, wherein: The mass ratio of the nitrate, the peptizing agent, the pore former and the oxide and / or its precursor is (10-500):(1-10):(10-500):(10-1000).
23. The preparation method according to claim 14 or 15, wherein: The nitrate is selected from one or more of aluminum nitrate, zirconium nitrate, lanthanum nitrate and yttrium nitrate; and / or, The peptizing agent is selected from one or more of acids, bases and salts; and / or, The pore-forming agent is selected from one or more of starch, synthetic cellulose, polymer alcohol and surfactant; and / or, The oxide and / or its precursor is selected from one or more of an aluminum source, a silicon source, a zirconium source and a titanium source, wherein the aluminum source is selected from one or more of pseudo-boehmite, aluminum alcohol, aluminum nitrate, aluminum sulfate, aluminum chloride and sodium aluminate, the silicon source is selected from one or more of silicates, sodium silicate, water glass and silica sol, the zirconium source is selected from one or more of zirconium dioxide, zirconium tetrachloride, zirconium oxychloride, zirconium hydroxide, zirconium sulfate, zirconium phosphate, zirconium oxynitrate, zirconium nitrate, basic zirconium carbonate and tetrabutoxy zirconium, the titanium source is selected from one or more of titanium dioxide, metatitanic acid, titanium nitrate, titanium oxysulfate, titanium dichloride, titanium trichloride, titanium tetrachloride, titanium aluminum chloride, tetraethyl titanate, tetrabutyl titanate, tetra-n-propyl titanate and tetraisopropyl titanate; and / or, The dispersant is selected from one or more of water, alcohols, ketones and acids.
24. The preparation method according to claim 14 or 15, wherein: Step (1-1) further comprises adding a blasting agent to the dispersant, wherein the blasting agent is selected from one or more of picric acid, trinitrotoluene, digested glycerol, nitrocellulose, dynamite, hexogen and C4 plastic explosive.
25. The preparation method according to claim 24, wherein: The added amount of the blasting agent is 0-1% of the total dry weight of the nitrate, the peptizing agent, the pore-forming agent and the oxide and / or its precursor.
26. The preparation method according to claim 14 or 15, wherein: In step (1-2), the aging treatment temperature is 0-90°C; and / or, In step (1-3), the drying device is a flash drying device or a spray drying device.
27. The preparation method according to claim 26, wherein: In step (1-2), the temperature of the aging treatment is 20-60°C.
28. The preparation method according to claim 14 or 15, wherein: The reduction conditions of step (3) include: the oxidized catalyst is in a fluidized state and in contact with the reducing gas; the temperature is 100-750°C, the time is not more than 2 hours, and the reducing gas-to-agent ratio is 500-5000.
29. The preparation method according to claim 28, wherein The reduction conditions in step (3) include: temperature of 150-700° C., time of no more than 1.5 h, and reduction gas-agent ratio of 600-4500.
30. The preparation method according to claim 14 or 15, wherein: The hydrogen-containing atmosphere contains hydrogen and optionally a protective gas, and the hydrogen concentration in the hydrogen-containing atmosphere is not less than 5 volume %.
31. The preparation method according to claim 30, wherein: The hydrogen concentration in the hydrogen-containing atmosphere is 5-90 volume %.
32. The preparation method according to claim 14 or 15, wherein: The reduction is carried out in a fluidized bed reactor.
33. The preparation method according to claim 14 or 15, wherein: The passivation time is no more than 5 hours.
34. The preparation method according to claim 33, wherein: The passivation time is no more than 1.5h.
35. The preparation method according to claim 14 or 15, wherein: During the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in at least two stages.
36. The preparation method according to claim 35, wherein: During the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in 2-10 stages.
37. The preparation method according to claim 36, wherein During the passivation process, the oxygen concentration of the oxygen-containing gas is continuously increased in 3-8 stages.
38. The preparation method according to claim 14 or 15, wherein: The gas-to-agent ratio of the passivation is 200-4500.
39. The preparation method according to claim 38, wherein The gas-to-agent ratio of the passivation is 300-4000.
40. The preparation method according to claim 14 or 15, wherein: The passivation is carried out in a fluidized bed reactor, and the catalyst is in a fluidized state.
41. The preparation method according to claim 14 or 15, wherein: The concentration of the oxygen-containing gas is 0.05-21 volume %.
42. The preparation method according to claim 41, wherein The concentration of the oxygen-containing gas is 0.1-21% by volume.
43. The preparation method according to claim 35, wherein: During the passivation process, the initial oxygen concentration of the oxygen-containing gas introduced is 0.05-0.2 volume %.
44. The preparation method according to claim 43, wherein During the passivation process, the oxygen concentration of the oxygen-containing gas introduced in the second stage is 0.1-1% by volume.
45. The preparation method according to claim 44, wherein During the passivation process, the oxygen concentration of the oxygen-containing gas introduced in the latter stage is 1-8 times the oxygen concentration of the oxygen-containing gas introduced in the former stage.
46. A Fischer-Tropsch synthesis catalyst obtained by the preparation method described in any one of claims 14 to 45.
47. Use of the Fischer-Tropsch synthesis catalyst according to any one of claims 1 to 13 and 46 in a Fischer-Tropsch synthesis reaction.