A method for hot plastic connection of metal thin-walled tubes of unequal diameters
By designing a machining mold, the metal thin-walled tubes produce curled folds under heating and compression loads, forming a cladding joint, solving the problem of connecting metal thin-walled tubes of varying diameters, and achieving efficient and reliable connection strength and quality.
Patent Information
- Application Number
- CN202210836023.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-15
AI Technical Summary
It is difficult to efficiently and reliably connect metal thin-walled pipes of different diameters in the prior art, and commonly used methods of welding, threaded connection, etc. will cause deformation of the cross-section of the thin-walled pipe.
A machining mold is designed, including an upper mold and a lower mold, and using heating and axial compression loads, the metal thin-walled tubes create inward and outwardly curling plastic folds at the rounded corners of the mold, thereby forming a cover joint.
It realizes efficient and reliable connection of metal thin-walled pipes in different diameters, avoids cross-sectional deformation, improves connection strength and quality, and is suitable for materials with poor plastic forming.
Smart Images

Figure CN115255163B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal thin-walled tube connection processing, in particular to a heating plastic connection processing method for metal thin-walled tubes of unequal diameters. Background Art
[0002] As a structure for transmitting medium and transferring load, pipe parts have been widely used in automobiles, aerospace, and oil pipelines. Among them, metal thin-walled tubes have the advantages of being hollow, light, high rigidity, and high strength. Lightweight metal thin-walled tubes such as high-strength steel, aluminum metal, and magnesium alloy also have the dual advantages of lightweight materials and thin-walled tubes, which can achieve weight reduction effects, mechanical properties, and cost advantages at the same time. Therefore, parts made of metal thin-walled tubes of unequal diameters are also receiving more and more attention. This type of hollow pipe fittings are mainly used for engine intake and exhaust system pipe fittings, air conditioning system pipes, hydraulic system pipes, pipe fittings in engine brackets, chassis structural parts, body frames, seat frames, radiator brackets, front and rear axles, drive shafts, hollow shafts, etc.
[0003] Although metal thin-walled tubes have the above advantages, the application of metal thin-walled tubes still faces a technical challenge - how to efficiently and reliably achieve the connection between metal thin-walled tubes of unequal diameters. On the one hand, due to the different diameters, the two tubes cannot be in direct contact. The existing riveting, bonding, plastic connection and other methods all require the two tubes to have a certain contact surface, so these methods are not suitable for the connection of thin-walled tubes of unequal diameters; on the other hand, due to the limitation of wall thickness, the commonly used methods such as melting welding, threaded connection, flange connection, and snap connection will cause the cross-sectional deformation of the thin-walled tube, so these methods are also not suitable for the connection of thin-walled tubes. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a heating plastic connection processing method for metal thin-walled tubes of unequal diameters, which can efficiently and reliably connect two metal thin-walled tubes of unequal diameters without causing cross-sectional deformation of the thin-walled tubes.
[0005] The object of the present invention can be achieved by the following technical solution: A method for hot plastic connection of metal thin-walled tubes of unequal diameters, comprising the following steps:
[0006] S1. Placing the first metal thin-walled tube and the second metal thin-walled tube to be connected in a processing mold, and using the processing mold to heat the first metal thin-walled tube and the second metal thin-walled tube, wherein the processing mold includes an upper mold and a lower mold, the upper mold can be moved vertically up and down, the bottom of the upper mold is provided with an upper mold fillet, and the lower mold is provided with a lower mold fillet, and the diameter of the first metal thin-walled tube is greater than the diameter of the second metal thin-walled tube; (It should be noted that in actual applications, the two metal thin-walled tubes to be connected can also be pre-heated before being placed in the processing mold. In this case, there is no need to use the processing mold for heating, and then directly execute step S2)
[0007] S2, the upper mold moves downward, carrying the first metal thin-walled tube downward. When the bottom of the first metal thin-walled tube contacts the lower mold, the bottom of the first metal thin-walled tube is deformed inwardly by the fillet of the lower mold, forming a curled portion at the bottom of the first metal thin-walled tube.
[0008] Then, the upper die moves downward to contact the top of the second metal thin-walled tube. Under the action of the upper die radius, the top of the second metal thin-walled tube is deformed and rolled outward to form a curled portion at the top of the second metal thin-walled tube.
[0009] S3, the upper mold continues to move downward to combine the bottom curled portion of the first metal thin-walled tube with the top curled portion of the second metal thin-walled tube, and compact to form a coated joint, thus completing the connection process of the first metal thin-walled tube and the second metal thin-walled tube.
[0010] Furthermore, the lower mold is fixedly mounted on a stand of a universal material testing machine, and the universal material testing machine applies a compressive load to the upper mold in the axial direction to move the upper mold downward.
[0011] Furthermore, the lower mold is provided with a first groove and a second groove that are connected, the first groove is located above the second groove, the lower mold radius is provided at the connecting position of the first groove and the second groove, the diameter of the first groove is consistent with the outer diameter of the first metal thin-walled tube, and the diameter of the second groove is consistent with the outer diameter of the second metal thin-walled tube.
[0012] Furthermore, the depth of the first groove is greater than the height of the first metal thin-walled tube, and the depth of the second groove is less than the height of the second metal thin-walled tube.
[0013] Furthermore, when the first metal thin-walled tube is placed in the processing mold in step S1, there is a first height difference between the bottom of the first metal thin-walled tube and the bottom of the upper mold, and the bottom of the upper mold is located inside the first metal thin-walled tube;
[0014] When the second metal thin-walled tube is placed in the processing mold in step S1, there is a second height difference between the top of the second metal thin-walled tube and the top of the second groove, and the top of the second groove is located below the top of the second metal thin-walled tube.
[0015] Furthermore, the calculation formula of the first height difference and the second height difference is specifically:
[0016]
[0017]
[0018] Among them, t1 is the wall thickness of the first metal thin-walled tube, t2 is the wall thickness of the second metal thin-walled tube, d1 is the outer diameter of the first metal thin-walled tube, d2 is the outer diameter of the second metal thin-walled tube, l1 is the first height difference, l2 is the second height difference, r1 is the radius of the upper mold corner, and r2 is the radius of the lower mold corner.
[0019] Furthermore, a heating device is installed in the processing mold.
[0020] Furthermore, the heating device is specifically a resistance wire heater or an electromagnetic induction heater.
[0021] Furthermore, the first metal thin-walled tube and the second metal thin-walled tube are made of the same material, specifically steel alloy, aluminum alloy or magnesium alloy.
[0022] Furthermore, when the material of the first metal thin-walled tube and the second metal thin-walled tube is a steel alloy, the heating temperature of the processing mold is set to 500-600°C;
[0023] When the material of the first metal thin-walled tube and the second metal thin-walled tube is aluminum alloy, the heating temperature of the processing mold is set to 250-300° C.;
[0024] When the first metal thin-walled tube and the second metal thin-walled tube are made of magnesium alloy, the heating temperature of the processing mold is set to 200-300°C.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. The method of the present invention fully considers the problem that metal thin-walled tubes of unequal diameters cannot be directly contacted. By designing a processing mold including an upper mold and a lower mold, the upper mold is nested and connected to the lower mold, and the upper mold is designed to be able to move vertically up and down, and an upper mold fillet is set at the bottom of the upper mold, and a lower mold fillet is set at the lower mold. By using the upper mold fillet and the lower mold fillet, the ends of the two metal thin-walled tubes (i.e., the bottom of the first metal thin-walled tube and the top of the second metal thin-walled tube) are respectively curled inward and outward to form a joint, which can be well suitable for the end connection of metal thin-walled tubes of unequal diameters.
[0027] 2. The present invention fully considers the characteristics of the metal thin-walled tube, uses a processing mold to heat the first metal thin-walled tube and the second metal thin-walled tube, forms wrinkles through plastic deformation, and the two connected metal thin-walled tubes are covered by the wrinkles to form a joint. This joint has high connection strength and effectively avoids the problem that welding, threaded connection and other methods will weaken the mechanical properties of the metal thin-walled tube.
[0028] 3. The present invention fully considers the cracking problem that is easy to occur when connecting metal materials with poor plastic formability. By heating, the deformation resistance of the material is reduced and the formability is improved. It can effectively avoid the cracking of metal thin-walled tubes with poor plastic deformation ability, and at the same time reduce the tonnage requirements of the equipment, so as to achieve the effect of improving the connection quality and connection strength.
[0029] Fourth, the present invention designs a suitable length of the free end of the metal thin-walled tube that exceeds the processing mold (i.e., a first height difference between the bottom of the first metal thin-walled tube and the bottom of the upper mold, and a second height difference between the top of the second metal thin-walled tube and the top of the second groove) according to the geometric dimensions of the metal thin-walled tubes to be connected, so that the curling deformation forms formed by the upper and lower metal thin-walled tubes can be consistent, the inner and outer metal thin-walled tubes can fit each other, and sufficient plastic curling deformation of the ends of the upper and lower metal thin-walled tubes is guaranteed, so as to reliably form a covering curling and thus form a joint with a stable connection strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the method flow of the present invention;
[0031] Figure 2 It is a schematic diagram of the processing process of the present invention;
[0032] Figure 3 A schematic diagram of the wrinkle morphology between the connected tubes in the compression plastic connection of metal thin-walled tubes with unequal diameters;
[0033] Figure 4 It is a schematic diagram of the effect of placing the first metal thin-walled tube and the second metal thin-walled tube in the processing mold in the present invention;
[0034] Figure 5 Schematic diagram of the aluminum alloy thin-wall pipe joint sample with different diameters manufactured in Example 1;
[0035] Markings in the figure: 1. upper mold, 2. first metal thin-walled tube, 3. upper mold radius, 4. lower mold, 5. lower mold radius, 6. second metal thin-walled tube, 7. end wrinkles. DETAILED DESCRIPTION
[0036] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0037] like Figure 1 and Figure 2 As shown, a method for hot plastic connection of metal thin-walled tubes of unequal diameters comprises the following steps:
[0038] S1, placing the first metal thin-walled tube 2 and the second metal thin-walled tube 6 to be connected in a processing mold, and using the processing mold to heat the first metal thin-walled tube 2 and the second metal thin-walled tube 6, wherein the processing mold comprises an upper mold 1 and a lower mold 4, the upper mold 1 is nested and connected to the lower mold 4, the upper mold 1 can move vertically up and down, the bottom of the upper mold 1 is provided with an upper mold fillet 3, the lower mold 4 is provided with a lower mold fillet 5, and the diameter of the first metal thin-walled tube 2 is greater than the diameter of the second metal thin-walled tube 6;
[0039] S2, the upper mold 1 moves downward, carrying the first metal thin-walled tube 2 downward. When the bottom of the first metal thin-walled tube 2 contacts the lower mold 4, the bottom of the first metal thin-walled tube 2 is deformed inwardly by the fillet 5 of the lower mold, forming a curled portion at the bottom of the first metal thin-walled tube;
[0040] Then, the upper mold 1 moves downward to contact the top of the second metal thin-walled tube 6. Under the action of the upper mold radius 3, the top of the second metal thin-walled tube 6 is deformed and rolled outward to form a curled portion at the top of the second metal thin-walled tube.
[0041] S3, the upper mold 1 continues to move downward, so that the bottom curled portion of the first metal thin-walled tube is combined with the top curled portion of the second metal thin-walled tube, and compacted to form a coated joint (i.e., the end wrinkles 7, the specific shape is as follows Figure 3 As shown), the connection processing of the first metal thin-walled tube 2 and the second metal thin-walled tube 6 is completed.
[0042] In practical applications, the lower mold 4 can be fixedly installed on a bench of a universal material testing machine, and the universal material testing machine applies a compressive load to the upper mold 1 along the axial direction to move the upper mold 1 downward.
[0043] like Figure 2 As shown, the lower mold 4 is provided with a first groove and a second groove which are connected, the first groove is located above the second groove, the lower mold radius 5 is provided at the connecting position of the first groove and the second groove, the diameter of the first groove is consistent with the outer diameter of the first metal thin-walled tube 2, the diameter of the second groove is consistent with the outer diameter of the second metal thin-walled tube 6, the depth of the first groove is greater than the height of the first metal thin-walled tube 2, and the depth of the second groove is less than the height of the second metal thin-walled tube 6.
[0044] This technical solution takes into account that the connecting ends of the two connected metal thin-walled tubes need to form a plastically coated joint, and cracks should not appear on the tube wall in the joint area. The key lies in designing a suitable free end length of the metal thin-walled tube exposed to the mold. If the free end length is too large, the length of the unstable section will be too large, and the curling deformation morphology formed by the upper and lower metal thin-walled tubes will not be consistent, and the inner and outer tubes will not fit well; if the free end length is too small, the plastic curling deformation of the upper and lower tube ends will be insufficient, and the coated curling cannot be formed, resulting in an inability to reliably form a joint. Therefore, this technical solution calculates the free end length of the connected metal thin-walled tube exposed to the mold based on the material diameter and wall thickness of the connected metal thin-walled tubes.
[0045] like Figure 4 As shown, when the first metal thin-walled tube 2 is placed in the processing mold in step S1, there is a first height difference between the bottom of the first metal thin-walled tube 2 and the bottom of the upper mold 1 (i.e., the free end length l1 of the first metal thin-walled tube 2), and the bottom of the upper mold 1 is located inside the first metal thin-walled tube 2;
[0046] When the second metal thin-walled tube 6 is placed in the processing mold in step S1, there is a second height difference between the top of the second metal thin-walled tube 6 and the top of the second groove (i.e., the free end length l2 of the second metal thin-walled tube 6), and the top of the second groove is located below the top of the second metal thin-walled tube 6.
[0047] Specifically, the free end lengths (in mm) of the first metal thin-walled tube 2 and the second metal thin-walled tube 6 are determined according to formula (1) and formula (2):
[0048]
[0049]
[0050] In formula (1) and formula (2), t1 is the tube wall thickness of the first metal thin-walled tube 2, t2 is the tube wall thickness of the second metal thin-walled tube 6, d1 is the outer diameter of the first metal thin-walled tube 2, d2 is the outer diameter of the second metal thin-walled tube 6, r1 is the radius of the upper die fillet 3, r2 is the radius of the lower die fillet 5, l1 is the free end length of the first metal thin-walled tube 2, l2 is the free end length of the second metal thin-walled tube 6; the unit of all symbols in the formula is mm. The free end length is the length of the first metal thin-walled tube 2 or the second metal thin-walled tube 6 exposed outside the mold after being placed in the processing mold.
[0051] In addition, in order to ensure that the processing mold can reliably heat the metal thin-walled tube, a heating device is installed in the processing mold. Specifically, heating can be performed by setting a resistor in the processing mold, or by electromagnetic induction, that is, the heating device can be a resistance wire heater or an electromagnetic induction heater.
[0052] In practical applications, the first metal thin-walled tube 2 and the second metal thin-walled tube 3 are made of the same material, specifically steel alloy, aluminum alloy or magnesium alloy. When the processing mold heats the first metal thin-walled tube 2 and the second metal thin-walled tube 3, the heating temperature is determined according to the material: the heating temperature of the low-carbon steel thin-walled tube is 500-600°C, the heating temperature of the aluminum alloy thin-walled tube is 250-300°C, and the heating temperature of the magnesium alloy thin-walled tube is 200-300°C.
[0053] Embodiment 1
[0054] This embodiment applies the above technical solution to realize a heating plastic connection processing method for aluminum alloy thin-walled tubes of unequal diameters, wherein the outer diameter and wall thickness of the first metal thin-walled tube are 44 mm and 1 mm respectively, and the outer diameter and wall thickness of the second metal thin-walled tube are 30 mm and 1 mm respectively, comprising the following steps:
[0055] 1) The two aluminum alloy thin-walled tubes to be connected are placed in a processing mold, which is installed on a universal material testing machine. According to equations (1) and (2), l1=14mm and l2=15mm are calculated;
[0056] 2) Use resistance heating to heat the mold to a temperature of 300°C;
[0057] 3) Apply axial compression load through a universal material testing machine to cause the ends of the two connected aluminum alloy thin-walled tubes to curl and deform and form plastic wrinkles.
[0058] The final processed product is Figure 5 shown.
[0059] Embodiment 2
[0060] This embodiment applies the above technical solution to realize a method for hot plastic connection of magnesium / magnesium alloy thin-walled tubes of unequal diameters, comprising the following steps:
[0061] 1) Place the two magnesium / magnesium alloy tubes to be connected into a processing mold, and the processing mold is installed on a universal material testing machine;
[0062] 2) Use resistance heating to heat the mold to a temperature of 250°C;
[0063] 3) Applying axial compression load through a universal material testing machine causes the ends of the two connected magnesium / magnesium alloy thin-walled tubes to curl and deform and form plastic wrinkles.
[0064] Embodiment 3
[0065] This embodiment applies the above technical solution to realize a method for hot plastic connection of unequal diameter steel / steel alloy thin-walled tubes, comprising the following steps:
[0066] 1) Place the two steel / steel alloy thin-walled tubes to be connected into a processing mold, which is installed on a universal material testing machine;
[0067] 2) Use resistance heating to heat the mold to a temperature of 600°C;
[0068] 3) Applying axial compression load through a universal material testing machine causes the ends of the two connected steel / steel alloy thin-walled tubes to curl and deform and form plastic wrinkles.
[0069] It can be seen that the technical scheme proposes a new heating connection processing method suitable for metal thin-walled tubes of unequal diameters. By designing a processing mold, the two metal thin-walled tubes to be connected are heated by the processing mold, and then the axial compression load is applied to the metal thin-walled tubes through the processing mold. When the upper tube and the lower tube contact the lower mold and the upper mold respectively, under the guidance of the mold radius, the bottom of the upper metal thin-walled tube with a larger diameter will produce an inward curling deformation to form an inner fold; the top of the lower metal thin-walled tube with a smaller diameter will produce an outward curling deformation to form an outer fold. The two folds are coated to form a self-locking joint. This connection process is based on the principle of plastic deformation, integrating the advantages of plastic connection and heating softening materials. It can be mass-produced under the action of molds and presses, and has the characteristics of high precision, high efficiency and high reliability. At the same time, there is no emission of harmful substances such as light, radiation, exhaust gas, etc. during the construction process, no filling materials are required, and the working environment is friendly.
[0070] Compared with the existing connection methods, the most significant advantage of this technical solution is that it is suitable for the connection of thin-walled tubes of unequal diameters, especially the connection of metal thin-walled tubes of unequal diameters and poor plastic formability. In addition, compared with welding, the heating temperature is much lower than the temperature reached by welding, and will not cause the thin-walled tube to burn through; compared with threaded connection, this method does not need to thin the tube wall, does not affect the strength of the tube blank itself, and is particularly suitable for the connection of thin-walled tubes; compared with flange connection, this method does not require opening holes at the joints, does not require other thinning treatments, and reduces the number of parts required for flange connection; compared with single bonding, the joints connected by this method have better high and low temperature resistance; compared with conventional plastic connection, this method can achieve the connection of metal thin-walled tubes with poor plastic formability by heating, and is applicable to a wider range of materials. Therefore, this method can prepare tubes / tube joints of unequal diameters, and can prepare tubes / tube joints that are difficult to connect, such as aluminum alloys and magnesium alloys, with a wide range of material adaptability and higher joint strength.
[0071] In summary, the advantages of this technical solution are:
[0072] 1. Suitable for connecting thin-walled tubes of unequal diameters. Existing welding, threaded connection, riveting, bonding, etc. all require direct contact between two metal tubes, while the connection method of the present invention is suitable for connecting thin-walled metal tubes of unequal diameters, and has a wider application range.
[0073] Second, it is suitable for connecting thin-walled metal tubes. Existing welding and threaded connections will weaken the mechanical properties of thin-walled tubes and affect the strength of the parent material. Single bonding is not resistant to high and low temperatures. The connection method of the present invention only causes plastic deformation of the thin-walled tube, and the strength of the parent material is higher after deformation.
[0074] 3. Suitable for connecting metal pipes with poor plastic formability, such as aluminum alloy and magnesium alloy thin-walled pipes. The present invention uses heating to improve the plasticity of the metal pipe, ensuring that no cracking defects occur in the connection area, and the joint strength is more reliable.
[0075] Fourth, the connection method of the present invention has no damage to the mechanical properties of the connected pipes, no emission of light, heat, exhaust gas, etc., and no need for filling materials.
[0076] 5. The connection method of the present invention adopts the method of processing molds for production, and the production accuracy is guaranteed by the molds. Therefore, the quality stability of the manufactured products is good, and the degree of automation is high, which is suitable for assembly line production.
Claims
1. A method for hot plastic connection of metal thin-walled tubes of unequal diameters, characterized in that: The following steps are involved: S1. Placing the first metal thin-walled tube (2) and the second metal thin-walled tube (6) to be connected in a processing mold, and using the processing mold to heat the first metal thin-walled tube (2) and the second metal thin-walled tube (6), wherein the processing mold comprises an upper mold (1) and a lower mold (4), the upper mold (1) can be moved vertically up and down, the bottom of the upper mold (1) is provided with an upper mold fillet (3), and the lower mold (4) is provided with a lower mold fillet (5), and the diameter of the first metal thin-walled tube (2) is greater than the diameter of the second metal thin-walled tube (6); S2, the upper mold (1) moves downward, carrying the first metal thin-walled tube (2) downward, and when the bottom of the first metal thin-walled tube (2) contacts the lower mold (4), the bottom of the first metal thin-walled tube (2) is deformed and rolled inwards under the action of the lower mold radius (5), forming a curled portion at the bottom of the first metal thin-walled tube (2); Subsequently, the upper mold (1) moves downward until it contacts the top of the second metal thin-walled tube (6), and under the action of the upper mold radius (3), the top of the second metal thin-walled tube (6) is deformed to roll outward, forming a curled portion at the top of the second metal thin-walled tube (6); S3, the upper mold (1) continues to move downward, so that the bottom curled portion of the first metal thin-walled tube (2) is combined with the top curled portion of the second metal thin-walled tube (6), and compacted to form a coated joint, thus completing the connection process of the first metal thin-walled tube (2) and the second metal thin-walled tube (6); The lower mold (4) is provided with a first groove and a second groove which are connected, the first groove is located above the second groove, the lower mold fillet (5) is provided at the connection position between the first groove and the second groove, the diameter of the first groove is consistent with the outer diameter of the first metal thin-walled tube (2), and the diameter of the second groove is consistent with the outer diameter of the second metal thin-walled tube (6); When the first metal thin-walled tube (2) is placed in the processing mold in step S1, there is a first height difference between the bottom of the first metal thin-walled tube (2) and the bottom of the upper mold (1), and the bottom of the upper mold (1) is located inside the first metal thin-walled tube (2); When the second metal thin-walled tube (6) is placed in the processing mold in step S1, there is a second height difference between the top of the second metal thin-walled tube (6) and the top of the second groove, and the top of the second groove is located below the top of the second metal thin-walled tube (6); The calculation formulas for the first height difference and the second height difference are specifically: Wherein, t1 is the wall thickness of the first metal thin-walled tube (2), t2 is the wall thickness of the second metal thin-walled tube (6), d1 is the outer diameter of the first metal thin-walled tube (2), d2 is the outer diameter of the second metal thin-walled tube (6), l1 is the first height difference, l2 is the second height difference, r1 is the radius of the upper die fillet (3), and r2 is the radius of the lower die fillet (5).
2. The method for hot plastic connection of metal thin-walled tubes of unequal diameters according to claim 1, characterized in that: The lower mold (4) is fixedly mounted on a platform of a universal material testing machine, and the universal material testing machine applies a compressive load to the upper mold (1) in the axial direction, so that the upper mold (1) moves downward.
3. The method for hot plastic connection of metal thin-walled tubes of unequal diameters according to claim 1, characterized in that: The depth of the first groove is greater than the height of the first metal thin-walled tube (2), and the depth of the second groove is less than the height of the second metal thin-walled tube (6).
4. The method for hot plastic connection of metal thin-walled tubes of unequal diameters according to claim 1, characterized in that: A heating device is installed in the processing mold.
5. The method for hot plastic connection of metal thin-walled tubes of unequal diameters according to claim 4, characterized in that: The heating device is specifically a resistance wire heater or an electromagnetic induction heater.
6. The method for hot plastic connection of metal thin-walled tubes of unequal diameters according to claim 1, characterized in that: The first metal thin-walled tube (2) and the second metal thin-walled tube (6) are made of the same material, specifically steel alloy, aluminum alloy or magnesium alloy.
7. The method for hot plastic connection of metal thin-walled tubes of unequal diameters according to claim 6, characterized in that: When the material of the first metal thin-walled tube (2) and the second metal thin-walled tube (6) is a steel alloy, the heating temperature of the processing mold is set to 500-600° C.; When the material of the first metal thin-walled tube (2) and the second metal thin-walled tube (6) is aluminum alloy, the heating temperature of the processing mold is set to 250-300° C.; When the material of the first metal thin-walled tube (2) and the second metal thin-walled tube (6) is a magnesium alloy, the heating temperature of the processing mold is set to 200-300°C.