Composite material patching and repairing method for cracks in aircraft landing gear beam
The cracks of the landing gear beam were determined through eddy current and coloring penetrant testing, and kerosene-resistant composite materials and magnetic pressurization devices were used to achieve safe repair of the aircraft landing gear beam inside the fuel tank, solving the problems of poor accessibility and potential oil and gas explosion risks in traditional methods. problem, reducing the crack growth rate and ensuring the safe use of the aircraft.
Patent Information
- Application Number
- CN202210931681.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-04
AI Technical Summary
Cracks appeared in the aircraft landing gear beam during service. The repair area has poor accessibility, small operating space, and there is a risk of oil and gas explosion. It is difficult to carry out effective pressurization and heating repairs in a semi-enclosed area using traditional methods.
Eddy current testing and coloring penetrant testing methods are used to determine crack information, kerosene-resistant composite material patches and structural adhesives are selected, combined with magnetic attraction and hot air heating, and a pressurizing device is composed of magnets and iron pressure plates to achieve pressurization and pressure inside the fuel tank. Heating repair.
It effectively reduces the crack expansion rate, ensures the safety of aircraft use, solves the problems of pressurization and heating, and meets the repair needs in kerosene environment.
Smart Images

Figure CN115257017B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aircraft repair, and relates to a composite material patching and repairing method for cracks in an aircraft landing gear beam. Background Art
[0002] The landing gear beam is an important load-bearing component of the aircraft. Cracks appear during service. To ensure the safety of the aircraft, it is necessary to repair the cracks in the landing gear beam. Since the landing gear beam is located inside the aircraft fuel tank, the landing gear beam repair area can only be reached through the maintenance cover. The accessibility of the repair area is poor and the operating space is small. Secondly, during the repair of the landing gear beam, the repair area needs to be heated and pressurized. Since the landing gear beam repair area is located inside the aircraft fuel tank, the accessibility is poor and the operating space is small, traditional clamping tools cannot pressurize the repair area. Thirdly, the landing gear beam repair area is inside the aircraft fuel tank, the repair area is small, and there is a risk of oil and gas explosion during the repair process. The problem of directional heating of the repair area needs to be effectively solved. At present, there is no equipment, device or method in this regard in the field of aviation equipment composite material repair technology. Summary of the invention
[0003] In order to solve the above problems, the present invention proposes a composite material patching and repairing method for aircraft landing gear beam cracks, so that when cracks appear in the aircraft landing gear beam, the cracks in the landing gear beam can be repaired in time to reduce the crack propagation rate and ensure the safety of the aircraft in service.
[0004] The technical solution of the present invention is:
[0005] A composite material patching and repairing method for cracks in an aircraft landing gear beam comprises the following steps:
[0006] (1) Crack inspection of the repaired area of the landing gear beam: The repaired area of the landing gear beam is inspected using the eddy current test method and the dye penetrant test method. The two methods are used in turn to determine the crack length and location information, and the dye penetrant test length is used as the final test result.
[0007] (2) Selection of materials for repairing landing gear beam cracks: The repair materials are selected based on the stress conditions of the landing gear beam, crack propagation conditions, and static and fatigue test results. The composite patch is made of T300 grade carbon fiber reinforced QY8911 bismaleimide resin, and a layer of EW100A glass fiber reinforced QY8911 bismaleimide resin is applied on the bonding surface. The adhesive is J-349-1 structural adhesive, which is resistant to kerosene, has high peel strength, is suitable for bonding metals and non-metals, and cures at medium and low temperatures.
[0008] (3) Control of oil and gas concentration in the landing gear beam repair area: Clean the kerosene in the landing gear beam repair area to reduce the kerosene concentration. The kerosene concentration is tested to be no more than 25% LEL of the first alarm point.
[0009] (4) Protection of the landing gear beam repair area: Use non-porous isolation film, medical tape, etc. to isolate the landing gear beam repair area from other non-repair areas, and fill the sharp triangle area of the landing gear beam repair area with fine flat cloth.
[0010] (5) Inspection of surface attachments in the landing gear beam repair area: Remove the sealant, paint layer, etc. on the bonding surface of the landing gear beam repair area.
[0011] (6) Inspection and installation of composite material patches: Determine the bonding surface, 0° ply orientation, shape, size, etc. of the composite material patch based on the shape of the landing gear beam repair area, and cut it; trim the shape of the composite material patch and chamfer the edges of the composite material patch.
[0012] (7) Surface treatment of bonding surfaces: Remove the anodized layer on the bonding surface of the landing gear beam repair area and grind it to a rough surface. Slightly grind the bonding surface of the composite patch. Use 120# aviation washing gasoline and acetone to wipe the landing gear beam repair area and the bonding surface of the composite patch respectively until there is no contamination. Complete the patch repair within 2 hours after the bonding surface treatment.
[0013] (8) Preparation and application of J-349-1 structural adhesive: Prepare J-349-1 structural adhesive according to the technical specifications; apply a layer of J-349-1 structural adhesive evenly on the adhesive surface of the composite patch to ensure that there are no defects such as poor adhesive, rich adhesive, and bubbles.
[0014] (9) Gluing of composite patch and pressurization of landing gear beam repair area: Glue the composite patch coated with J-349-1 structural adhesive to the repair area of the landing gear beam; a pressurization device is composed of a magnet and an iron pressure plate, wherein the iron pressure plate is placed on the composite patch and the magnet is placed at the bottom of the landing gear beam. The composite patch is pressurized on the repair area of the landing gear beam by the principle of magnetic attraction. The best patching position is determined by adjusting the pressurization device and the position of the composite patch.
[0015] (10) Curing repair: Use a hot repair instrument to control the hot air blower to heat the repair area of the landing gear beam through the air supply duct; the heating and cooling rates are controlled at 2°C / min. After heating to 80°C, keep the temperature for 3 hours, then drop to below 40°C and cool naturally.
[0016] (11) Post-curing treatment: Perform visual and ultrasonic inspections on the adhesive cured repair area. After the inspection, apply H01-101H varnish and H06-1020H-D antistatic primer to the composite patch, and apply a layer of HM109-1 sealant on the J-349-1 structural adhesive remaining around the composite patch.
[0017] Beneficial effects of the present invention: The present invention adopts a magnetic attraction method to effectively solve the pressurization problem during the crack repair process of the landing gear beam in a semi-enclosed area; a material system for repairing the cracks of the landing gear beam is designed and developed according to the stress conditions and working environment of the landing gear beam, and the material system effectively reduces the crack expansion rate and meets the requirements of working in a kerosene environment; the present invention combines magnetic attraction and blowing hot air to achieve the needs of heating and pressurizing the crack repair area inside the aircraft tank. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the composite material patching and repairing of the landing gear beam of the present invention.
[0019] Figure 2 Schematic diagram of the composite material patch of the present invention; (a) is a front view, and (b) is a cross-sectional view.
[0020] Figure 3 It is a schematic diagram of the thermocouple arrangement of the present invention.
[0021] Figure 4 It is the heating curing curve of the present invention.
[0022] In the figure: 1-magnet; 2-landing gear beam; 3-composite material patch; 4-iron pressure plate; 5-thermocouple; 6-rib; 7-hot air blower; 8-compressed air; 9-ground power supply; 10-thermal patch instrument. DETAILED DESCRIPTION
[0023] The specific implementation of the present invention is further explained below in conjunction with the examples and drawings, but is not intended to limit the present invention.
[0024] See also Figure 1 A composite material patching and repairing method for cracks in an aircraft landing gear beam, the steps are as follows:
[0025] (1) Crack inspection in the repair area of the landing gear beam: The eddy current testing method is used to conduct an initial inspection of the repair area of the landing gear beam. When a suspected crack response signal is found, its length is measured; then, the dye penetrant testing method is used to confirm the crack length again, and the dye penetrant testing length is used as the final test result.
[0026] (2) Material selection for repairing landing gear beam cracks:
[0027] Repair materials are selected according to the stress conditions of the landing gear beam, crack propagation, static and fatigue test results; the composite patch is made of T300 grade carbon fiber / QY8911 bismaleimide resin prepreg with a ply ratio of [45 / 0 / 0 / -45 / 0 / 0 / 90 / 0]s, and a layer of glass fiber EW100A / QY8911 bismaleimide resin prepreg is added on the bonding surface; the adhesive is J-349-1 structural adhesive which is resistant to kerosene, has high peel strength, is suitable for bonding metals and non-metals, and cures at medium and low temperatures.
[0028] (3) Control of oil and gas concentration in the landing gear beam repair area: Clean the kerosene in the landing gear beam repair area until there is no oil stain, and use air to reduce the oil and gas concentration. Use the RBBJ-T portable gas detection alarm to detect the oil and gas concentration in at least 3 areas, which should not exceed 25% LEL of the first alarm point. If necessary, blow cold air into the fuel tank to reduce the oil and gas concentration until the repair requirements are met.
[0029] (4) Protection of the landing gear beam repair area: Use non-porous isolation film, medical tape, etc. to isolate the landing gear beam repair area from other areas, and fill the sharp triangle area of the landing gear beam repair area with fine flat cloth.
[0030] (5) Removal of attachments on the surface of the landing gear beam repair area: Use a scraper to remove the sealant in the landing gear beam repair area; use a neutral paint stripper to remove the paint layer on the surface of the repair area. If the neutral paint stripper cannot remove the paint layer, use an acidic cleaning agent to continue removing it. After the paint layer is removed, immediately remove the cleaning agent. Use a reflector and a handheld lamp to inspect. No sealant or paint layer is allowed to remain in the repair area.
[0031] (6) Inspection and installation of composite patch: First, determine the bonding surface (glass cloth laying surface) of the composite patch and the 0° direction of the carbon fiber laying layer. According to the shape of the landing gear beam repair area, determine the shape and size of the composite patch. See the schematic diagram of the composite patch for details. Figure 2 ; Second, the composite material patch that has been inspected and installed is trimmed to ensure that the edge of the composite material patch does not touch the R-angle edge of the landing gear beam and rib, and to ensure that the bonding surface of the composite material patch is in contact with the web surface of the landing gear beam; Third, the composite material patch is chamfered to ensure a smooth transition in the chamfered area; After the inspection and installation, no delamination, splitting or other damage is allowed to occur around the composite material patch.
[0032] (7) Surface treatment of the bonding surface: Use 60-120 grit sandpaper to remove the anodized layer of the bonding surface and grind it rough to improve the bonding strength between the composite patch and the repair area. The surface should be smooth and have a metallic luster after grinding. Use 300 grit sandpaper to lightly grind the bonding surface of the composite patch along the 0° laying direction of the carbon fiber, taking care not to damage the fibers.
[0033] (8) Cleaning of impurities in the repair area of the landing gear beam: First, use a vacuum cleaner to clean the dust, debris and other impurities in the repair area of the landing gear beam; Second, soak the plain silk with 120# aviation washing gasoline and wipe the repair area of the landing gear beam and the adhesive joint of the composite material patch from top to bottom in one direction. Do not reuse the plain silk. Wait until there is no black mark or obvious adhesion on the surface of the plain silk and let it dry for 10 to 15 minutes until the acetone is completely evaporated after the surface of the plain silk is soaked. Complete the patch repair within 2 hours after the surface treatment of the adhesive joint.
[0034] (9) Preparation and application of J-349-1 structural adhesive: Prepare J-349-1 structural adhesive according to the technical specifications; apply a layer of J-349-1 structural adhesive evenly on the bonding surface of the composite patch to ensure that there are no defects such as poor adhesive, rich adhesive, and bubbles.
[0035] (10) Pressurizing the repair area of the landing gear beam: The composite patch 3 coated with J-349-1 structural adhesive is glued to the repair area of the landing gear beam 2; the magnet 1 and the iron pressure plate 4 form a pressurizing device using the principle of magnetic attraction, wherein the iron pressure plate 4 is placed on the composite patch 3, and the magnet 1 is placed at the bottom of the landing gear beam, so that the composite patch 3 is pressurized on the repair area of the landing gear beam, and the best patching position is determined by adjusting the pressurizing device and the position of the composite patch. Use an endoscope or a reflector to check to ensure that the edge of the composite patch does not contact the landing gear beam or the R-angle edge of the rib, and that the adhesive surface of the composite patch fits the web surface of the landing gear beam.
[0036] (11) Thermocouple arrangement: Figure 3 Thermocouple 5 is arranged at the position and fixed with pressure-sensitive tape.
[0037] (12) Curing repair: Before curing, use breathable felt to fill the repair area for insulation; use HCS9200B hot patch instrument 10 to control HCS-2041 hot air blower 7 to heat the landing gear beam repair area through the air supply pipe; keep a certain distance (about 200mm) between the air outlet of HCS-2041 hot air blower 7 and the landing gear beam repair area to avoid uneven heating temperature due to too close distance; control the heating and cooling rate at 2℃ / min, heat to 80℃, keep warm for 3h, then cool down to below 40℃, and cool naturally; control the temperature according to the average temperature, collect and record the thermocouple temperature with the help of the hot patch instrument, and the curing curve is shown in Figure 4 .
[0038] (13) Post-curing treatment:
[0039] Carry out a visual inspection of the visible parts of the landing gear beam repair area. No glue bumps should be squeezed out around the composite material patch. Abnormalities such as bubbles, cracks, voids, inconsistent color, etc. are not allowed. Use ultrasonic testing to check the quality of the bonding after repair. No bonding defects are allowed.
[0040] After the inspection, apply a layer of H01-101H varnish on the surface of the composite patch, and then apply a layer of H06-1020H-D antistatic primer. Apply a layer of HM109-1 sealant to the residual J-349-1 structural adhesive around the composite patch to isolate it and prevent direct contact between the structural adhesive and the fuel.
Claims
1. A composite material patching and repairing method for cracks in an aircraft landing gear beam, characterized in that: The method comprises the following steps: (1) Crack inspection of the repaired area of the landing gear beam: The repaired area of the landing gear beam is inspected using the eddy current testing method and the dye penetrant testing method. The two methods are used in turn to determine the crack length and location information, and the dye penetrant testing length is used as the final test result; (2) Material selection for landing gear beam crack repair: The composite patch is made of T300 grade carbon fiber reinforced QY8911 bismaleimide resin, and a layer of EW100A glass fiber reinforced QY8911 bismaleimide resin is laid on the bonding surface; the adhesive is J-349-1 structural adhesive that is resistant to kerosene, has high peel strength, is suitable for bonding metals and non-metals, and cures at medium and low temperatures; (3) Control of oil and gas concentration in the landing gear beam repair area: Clean the kerosene in the landing gear beam repair area to reduce the kerosene concentration. The kerosene concentration is tested to be no more than 25% LEL of the first alarm point; (4) Protection of the landing gear beam repair area: Use non-porous isolation film and medical tape to isolate the landing gear beam repair area from the non-repair area, and fill the sharp triangle area of the landing gear beam repair area with fine flat cloth; (5) Check the surface attachments of the landing gear beam repair area: remove the sealant and paint layer on the bonding surface of the landing gear beam repair area; (6) Inspection and installation of composite patch: Determine the bonding surface, 0° ply orientation, shape and size of the composite patch according to the shape of the landing gear beam repair area, and cut it; trim the shape of the composite patch and chamfer the edges of the composite patch; (7) Surface treatment of bonding surface: remove the anodized layer on the bonding surface of the landing gear beam repair area and grind it to a rough surface, lightly grind the bonding surface of the composite patch, and use 120# aviation washing gasoline and acetone to wipe the landing gear beam repair area and the bonding surface of the composite patch in turn until there is no contamination. After the bonding surface treatment, complete the patch repair within 2 hours; (8) Preparation and application of J-349-1 structural adhesive: Prepare J-349-1 structural adhesive; apply a layer of J-349-1 structural adhesive evenly on the adhesive surface of the composite patch to ensure that there is no poor adhesive, rich adhesive, or bubbles; (9) Gluing of composite patch and pressurization of landing gear beam repair area: Glue the composite patch coated with J-349-1 structural adhesive to the repair area of the landing gear beam; a pressurization device is composed of a magnet and an iron pressure plate, wherein the iron pressure plate is placed on the composite patch and the magnet is placed at the bottom of the landing gear beam. The composite patch is pressurized on the repair area of the landing gear beam by the principle of magnetic attraction. The best patching position is determined by adjusting the pressurization device and the position of the composite patch; (10) Curing repair: Use a hot repair instrument to control the hot air blower to heat the repair area of the landing gear beam through the air supply pipe; the heating and cooling rates are controlled at 2°C / min. After heating to 80°C, keep the temperature for 3 hours, then cool down to below 40°C, and then cool naturally; (11) Post-curing treatment: Perform visual and ultrasonic inspections on the adhesive cured repair area. After the inspection, apply H01-101H varnish and H06-1020H-D antistatic primer to the composite patch. Apply a layer of HM109-1 sealant to the J-349-1 structural adhesive remaining around the composite patch to isolate it and prevent direct contact between the structural adhesive and the fuel.
2. The method according to claim 1, characterized in that The specific operations of step (6) are as follows: first, determining the bonding surface of the composite patch and the 0° direction of the carbon fiber ply, and determining the shape and size of the composite patch according to the shape of the repair area of the landing gear beam; second, trimming the composite patch after inspection and installation to ensure that the edge of the composite patch does not contact the landing gear beam and the R-angle edge of the rib, and to ensure that the bonding surface of the composite patch fits the web surface of the landing gear beam; third, chamfering the composite patch to ensure a smooth transition in the chamfered area; and no delamination or splitting damage is allowed to occur around the composite patch after inspection and installation.
3. The method according to claim 1 or 2, characterized in that: A distance of 200 mm is maintained between the air outlet of the hot air blower and the repair area of the landing gear beam.
Citation Information
Patent Citations
Tissue engineering methods and compositions
AU2013222002A1
Composite material gluing repairing method for crack of airplane structure oil tank aluminium alloy main load-bearing part
CN109570902A