A negative electrode sheet and its preparation method and application
By adopting a double-layer structure design in the negative electrode sheet of lithium-ion battery, the inner layer of small-particle graphite and soft or hard carbon and the outer layer of large graphite and lithium silicon oxygen composite oxide are solved in the prior art energy The difficulty of density and rate performance is taken into account, which achieves the balance of high energy density and fast charging performance, and significantly improves the cycle life and charging performance of the battery.
Patent Information
- Application Number
- CN202211050764.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-08-29
AI Technical Summary
The negative electrode sheets of existing lithium-ion batteries are difficult to take into account when improving energy density and rate performance. The commonly used additive methods affect the wetting and compaction density of the electrode sheets, limiting their performance in practical applications.
The negative electrode sheet design adopts a double-layer structure, in which the inner layer is composed of a mixture of small-particle graphite and soft carbon or hard carbon, and the outer layer is a mixed material of large graphite and lithium silicon oxygen composite oxide. This structural design reduces lithium ions The solid phase diffusion impedance and interface impedance improve rate performance, and replenish lithium ions in long-term cycles through LixSiyOz to improve the energy density of the battery.
It achieves good wetting and high energy density, improves the rate performance and long-term cycle life of lithium-ion batteries, and ensures charging performance, porosity can reach more than 40%, 1C discharge capacity at 25℃ can reach more than 2489mAh, and 3C charging The constant current ratio can reach more than 96.9%, and the DCR can reach less than 13.4mΩ.
Smart Images

Figure CN115275097B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries and relates to a negative electrode plate and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries, with their high energy density, high operating voltage, environmental friendliness, and strong manufacturability, are currently widely used in mobile phones, laptops, electric vehicles, and energy storage. As the power battery market continues to expand, the pursuit of longer battery life and faster charging speeds poses greater challenges to the energy density and rate performance of lithium-ion batteries.
[0003] Currently, the methods on the market to improve the energy density and rate performance of lithium-ion batteries mainly rely on battery materials and electrode design. For example, increasing the gram capacity and compaction density of positive and negative electrode materials to improve the energy density of battery cells. However, this method has large technical barriers and is difficult to industrialize. In addition, as the gram capacity of the negative electrode material increases, the supported charging rate will gradually decrease, and it is impossible to achieve a balance between energy density and fast charging performance. If a high-areal-density electrode process is used, the wettability of the electrode will be greatly affected. At the same time, the migration distance of lithium ions will increase, the migration channel will decrease, and the charging rate will be greatly reduced.
[0004] CN113380983A discloses a high-density negative electrode plate, a preparation method thereof, and a lithium-ion battery comprising the plate. The high-density negative electrode plate includes a negative electrode coating and a negative electrode current collector; the negative electrode coating includes a negative electrode active material, an additive, a conductive agent, a suspending agent, and a binder, and the additive is a high-density additive.
[0005] CN113299918A discloses a negative electrode plate and a lithium ion battery comprising the negative electrode plate. A dispersing aid is directly added to the negative electrode plate, which is easy to operate, improves the infiltration of the electrolyte, and can improve the rate charge and discharge performance of the battery.
[0006] The above solution improves the compaction density and wettability of the negative electrode plate by adding additives, which will affect the rate performance and energy density of the plate, limiting its practical application. Summary of the Invention
[0007] The purpose of the present invention is to provide a negative electrode plate and its preparation method and application, wherein the negative electrode plate has a double-layer structure, has good wettability, and meets the requirements of high energy density and fast charging.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a negative electrode plate, the negative electrode plate comprising a negative electrode current collector, a second active material layer and a first active material layer disposed between the negative electrode current collector and the second active material layer, the active material of the first active material layer comprising a mixture of a first graphite and soft carbon and / or hard carbon, the active material of the second active material layer comprising a second graphite and Li x Si y O z , where x is 1 to 4 (1, 2, 3, or 4, etc.), y is 0.1 to 2 (for example, 0.1, 0.5, 1, 1.5, or 2, etc.), and z is 3 to 5 (3, 3.5, 4, 4.5, or 5, etc.).
[0010] The negative electrode plate of the present invention adopts a double-layer structure design. The first active material layer is the inner layer. The material of this layer is a mixture of small-particle graphite and soft carbon or hard carbon. When lithium ions are embedded, the small-particle graphite has a shorter migration distance, which can effectively reduce the solid-phase diffusion impedance of lithium ions and reduce the anode polarization. At the same time, the mixed soft carbon and hard carbon are amorphous carbon, and there are more lithium ion embedding channels, which effectively reduces the interface impedance when lithium ions are embedded, and can also achieve the effect of reducing anode polarization and improving rate performance. The second active material layer is the outer layer. The material of this layer is a mixture of large graphite and lithium silicon oxygen composite oxide. Li x Si y O z To pre-lithiate SiO, during the long-term cycle, as lithium ions are consumed, a potential difference will appear between the anode and the cathode. x Si y O z It will gradually release lithium ions to replenish the lost lithium ions, improve the long-term cycle life of the battery, and provide higher energy density.
[0011] Preferably, the median particle size D50 of the first graphite is 5 to 15 μm, for example, 5 μm, 8 μm, 10 μm, 12 μm or 15 μm.
[0012] Preferably, the median particle size D50 of the soft carbon and / or hard carbon is 6 to 10 μm, for example, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm.
[0013] Preferably, the mass ratio of the first graphite to soft carbon and / or hard carbon is (70-87):(13-30), for example: 70:30, 75:25, 80:20, 82:18 or 87:13.
[0014] The inner layer of the negative electrode plate of the present invention adopts a mixture of small-particle graphite and soft carbon or hard carbon to improve the conductivity between the negative electrode plate and the current collector, while shortening the lithium ion embedding distance, accelerating the lithium ion embedding speed, and reducing the internal resistance of the battery cell.
[0015] Preferably, the median particle size D50 of the second graphite is 15-25 μm, for example, 15 μm, 18 μm, 20 μm, 22 μm or 25 μm.
[0016] Preferably, the Li x Si y O z For nanomaterials.
[0017] Preferably, the second graphite and Li x Si y O z The mass ratio is (87-95):(5-13), for example: 87:13, 88:12, 90:10, 92:8 or 95:5, etc.
[0018] The outer layer of the negative electrode plate of the present invention is made of large-grained graphite and Li x Si y O z Nanomaterial mixing and large-particle graphite increase the compaction density of the pole piece, while ensuring that the outer graphite layer still has a high porosity after cold pressing, ensuring that lithium ions can enter the interior of the pole piece smoothly. x Si y O z Nanomaterials improve the energy density of battery cells by pre-lithiation of SiO.
[0019] In a second aspect, the present invention provides a method for preparing the negative electrode sheet as described in the first aspect, the preparation method comprising the following steps:
[0020] (1) The first graphite, soft carbon and / or hard carbon, conductive agent and binder are mixed with the first solvent to obtain a first slurry, and the second graphite, Li x Si y O z , a conductive agent and a binder are mixed with a second solvent to obtain a second slurry;
[0021] (2) The first slurry is coated on the surface of the negative electrode current collector, and the second slurry is coated on the surface of the first slurry, and the negative electrode sheet is obtained by cold pressing.
[0022] Preferably, the conductive agent in step (1) includes any one of conductive carbon black, carbon nanotubes or graphene, or a combination of at least two of them.
[0023] Preferably, the binder comprises sodium carboxymethyl cellulose and / or styrene-butadiene rubber, preferably sodium carboxymethyl cellulose and styrene-butadiene rubber.
[0024] Preferably, the first solvent comprises deionized water.
[0025] Preferably, the oil-based solvent includes any one of dimethyl sulfoxide, N,N-dimethylformamide, dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof.
[0026] Preferably, the mass ratio of the first graphite and the mixture of soft carbon and / or hard carbon, the conductive agent, sodium carboxymethyl cellulose, and styrene-butadiene rubber is (94-97):(1.0-2.0):(1.2-1.8):(1.5-2.5), for example: 94:1.8:1.7:2.5, 95:1.5:1.5:2, 96:1.8:1.5:1.7 or 96:1:1.2:1.8, etc.
[0027] Preferably, the second graphite and Li x Si y O z The mass ratio of the mixture, the conductive agent sodium carboxymethyl cellulose, and styrene-butadiene rubber is (94-96):(0.5-1.7):(1.0-3.2):(1.2-2.8), for example: 94:1.8:1.7:2.5, 95:1.5:1.5:2, 96:1.8:1.5:1.7 or 96:1:1.2:1.8, etc.
[0028] Preferably, the solid content of the first slurry in step (1) is 55-60%, for example, 55%, 56%, 57%, 58%, 59% or 60%.
[0029] Preferably, the viscosity of the first slurry is 3000-5500 mPa·s, for example, 3000 mPa·s, 3500 mPa·s, 4000 mPa·s, 4500 mPa·s or 5500 mPa·s.
[0030] Preferably, the solid content of the second slurry is 51-55%, for example, 51%, 52%, 53%, 54% or 55%.
[0031] Preferably, the viscosity of the first slurry is 3000-5500 mPa·s, for example, 3000 mPa·s, 3500 mPa·s, 4000 mPa·s, 4500 mPa·s or 5500 mPa·s.
[0032] Preferably, in step (2), the coating thickness of the first slurry, the coating thickness of the second slurry and the compaction density after cold pressing satisfy the relationship c=(0.047b-0.021a) / 3, and c is 1.50-1.68 g / cm 3 , for example: 1.50g / cm 3 , 1.52g / cm 3 , 1.55g / cm 3 , 1.6g / cm3 or 1.68g / cm 3 etc., wherein the coating thickness of the first slurry is a μm, the coating thickness of the second slurry is b μm, and the compaction density after cold pressing is cg / cm 3 .
[0033] The inner slurry is a combination of small-particle graphite and soft carbon or hard carbon. When lithium ions are embedded, small-particle graphite has a shorter migration distance, which can effectively reduce the solid-phase diffusion impedance of lithium ions and reduce anode polarization. At the same time, the mixed soft carbon and hard carbon are amorphous carbon, and there are more lithium ion embedding channels, which effectively reduce the interface impedance when lithium ions are embedded, and can also achieve the effect of reducing anode polarization. Since the particle size of the inner slurry is small and the fast charging performance needs to be guaranteed, the compaction density is small; the outer slurry is large-particle graphite and Li X Si y O z In industrial production, the cold pressing speed of the mixture can often reach 40-80m / min. The outer and inner layers of the electrode are subjected to uneven force, so the outer graphite of the electrode is often subjected to greater pressure. Therefore, large-particle graphite is used in the outer layer. Large-particle graphite has a higher compaction density, which can ensure that there are still good pore channels after cold pressing, ensuring electrolyte infiltration and lithium ion channels.
[0034] In a third aspect, the present invention provides a lithium-ion battery, comprising the negative electrode sheet as described in the first aspect.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The negative electrode plate of the present invention adopts a double-layer structure design. The first layer is the inner layer, and the material of this layer is a mixture of small-particle graphite and soft carbon or hard carbon to improve the rate performance. The second layer is the outer layer, and the material of this layer is a mixture of large graphite and lithium silicon oxygen composite oxide to provide higher energy density.
[0037] (2) The porosity of the negative electrode plate of the present invention can reach more than 40%, showing good liquid absorption rate and plate wettability. After the battery is manufactured, the 25°C 1C discharge capacity can reach more than 2489mAh, the 3C charging constant current ratio can reach more than 96.9%, and the DCR can reach less than 13.4mΩ. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a schematic structural diagram of the negative electrode sheet described in Example 1, ①-current collector, ②-first active material layer, ③-second active material layer. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described below by way of specific embodiments. It should be understood by those skilled in the art that the embodiments are merely to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0040] Unless otherwise specified, all ratios in the Examples and Comparative Examples of the present invention are by mass.
[0041] Example 1
[0042] This embodiment provides a negative electrode plate, which is manufactured by the following method:
[0043] (1) A first graphite with a D50 of 10 μm and a soft carbon mixture with a D50 of 8 μm, conductive carbon black, sodium carboxymethyl cellulose (hereinafter referred to as CMC) and styrene-butadiene rubber (hereinafter referred to as SBR) were mixed with deionized water at a ratio of 95:1.1:1.8:2.1 and stirred to obtain a first slurry with a solid content of 58% and a viscosity of 4500 mPa·s, wherein the mass ratio of the first graphite to the soft carbon was 80:20. A second graphite and a mixture of Li2Si1O3, conductive carbon black, CMC and SBR were mixed with dimethyl sulfoxide at a ratio of 95:1.8:1.6:1.6 and stirred to obtain a second slurry with a solid content of 54% and a viscosity of 4500 mPa·s, wherein the mass ratio of the second graphite to Li2Si1O3 was 90:10;
[0044] (2) The first slurry is coated on the surface of the negative electrode current collector, and the second slurry is coated on the surface of the first slurry, and the negative electrode sheet is obtained by cold pressing, wherein the coating thickness of the first slurry is a=60 μm, the coating thickness of the second slurry is b=130 μm, and the compaction density after cold pressing is 1.62 g / cm 3 .
[0045] The structural diagram of the negative electrode plate is as follows Figure 1 As shown, ① is the current collector, ② is the first active material layer, and ③ is the second active material layer.
[0046] Example 2
[0047] This embodiment provides a negative electrode plate, which is manufactured by the following method:
[0048] (1) A first graphite with a D50 of 12 μm and a hard carbon mixture with a D50 of 8.5 μm, conductive carbon black, sodium carboxymethyl cellulose (hereinafter referred to as CMC), and styrene-butadiene rubber (hereinafter referred to as SBR) were mixed with deionized water at a ratio of 95:1.1:1.8:2.1 and stirred to obtain a first slurry with a solid content of 57% and a viscosity of 4800 mPa·s, wherein the mass ratio of the first graphite to the hard carbon was 75:25. A second graphite and a Li2Si1O3 mixture, conductive carbon black, CMC, and SBR were mixed with dimethylformamide at a ratio of 95:1.8:1.6:1.6 and stirred to obtain a second slurry with a solid content of 53% and a viscosity of 4800 mPa·s, wherein the mass ratio of the second graphite to Li2Si1O3 was 90:10;
[0049] (2) The first slurry is coated on the surface of the negative electrode current collector, and the second slurry is coated on the surface of the first slurry, and the negative electrode sheet is obtained by cold pressing, wherein the coating thickness of the first slurry is a=50 μm, the coating thickness of the second slurry is b=120 μm, and the compaction density after cold pressing is 1.53 g / cm 3 .
[0050] Example 3
[0051] The only difference between this embodiment and embodiment 1 is that the mass ratio of the first graphite to the soft carbon is 95:5, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0052] Example 4
[0053] The only difference between this embodiment and embodiment 1 is that the mass ratio of the second graphite to Li2Si1O3 is 98:2, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0054] Example 5
[0055] The only difference between this embodiment and embodiment 1 is that the mass ratio of the second graphite to Li2Si1O3 is 80:20, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0056] Example 6
[0057] The only difference between this embodiment and embodiment 1 is that the compaction density after cold pressing is 1.72 g / cm 3 , other conditions and parameters are exactly the same as those in Example 1.
[0058] Example 7
[0059] The only difference between this embodiment and embodiment 1 is that the compaction density after cold pressing is 1.45 g / cm 3 , other conditions and parameters are exactly the same as those in Example 1.
[0060] Comparative Example 1
[0061] The only difference between this comparative example and Example 1 is that no soft carbon is added to the inner layer, and other conditions and parameters are exactly the same as those in Example 1.
[0062] Comparative Example 2
[0063] The only difference between this comparative example and Example 1 is that Li2Si1O3 is not added to the outer layer, and other conditions and parameters are exactly the same as those in Example 1.
[0064] Comparative Example 3
[0065] The only difference between this comparative example and Example 1 is that only the inner layer is provided, and other conditions and parameters are exactly the same as those in Example 1.
[0066] Comparative Example 4
[0067] The only difference between this comparative example and Example 1 is that only the outer layer is provided, and other conditions and parameters are exactly the same as those in Example 1.
[0068] Performance testing:
[0069] The porosity of the negative electrode plates obtained from Examples 1-7 and Comparative Examples 1-4 was tested, and the liquid absorption rate and wettability of the plates were characterized by the plate porosity. The negative electrode plates were assembled with LFP positive electrode plates, diaphragms, and electrolytes to form lithium iron phosphate batteries. 25℃1C discharge capacity test method: Under 25℃ environment, 1C current constant current and constant voltage were used to charge to 3.65V, and then 1C current constant current was used to discharge to 2.5V, and the discharge capacity C0 was recorded as the 25℃1C discharge capacity; 25℃3C charging constant current ratio test method: Under 25℃ environment, 1C current constant current was used to discharge to 2.5V, and then 3C current constant current and constant voltage was used to charge to 3.65V, and the constant current charging capacity was recorded as C1, and the constant current and constant voltage charging was recorded. The capacitance is C2, and the 3C charging constant current ratio is: C1 / C2*100%. The DCR test method is: Under a 25°C environment, use a 1C constant current to discharge to 2.5V, then use a 1C constant current to charge to 50% SOC, use a 1C constant current to charge for 10 seconds, record the end point as V0, then discharge at a constant current for 10 seconds, record the end voltage as V1, and record the current as I. The DCR is: (V0-V1) / I. The test results are shown in Table 1:
[0070] Table 1
[0071]
[0072] As can be seen from Table 1, from Examples 1-2, the porosity of the negative electrode plate of the present invention can reach more than 40%, showing good liquid absorption rate and plate wettability. After the battery is manufactured, the 25°C 1C discharge capacity can reach more than 2489 mAh, the 3C charging constant current ratio can reach more than 96.9%, and the DCR can reach less than 13.4 mΩ.
[0073] By comparing Example 1 and Example 2-3, it can be seen that in the first active material layer of the negative electrode plate described in the present invention, the mass ratio of the first graphite to soft carbon and / or hard carbon will affect its performance. The mass ratio of the first graphite to soft carbon and / or hard carbon is controlled at (70-87): (13-30), and the negative electrode plate with better performance is obtained. If the proportion of the first graphite is too large and the proportion of soft carbon and / or hard carbon is too small, the lithium ion embedding channel is reduced, the solid phase migration speed is reduced, the anode polarization is increased, the internal resistance of the battery cell is increased, and the lithium embedding speed is reduced, resulting in poor charging rate performance of the battery cell. If the proportion of the first graphite is too small, the anode lithium storage position is reduced, the NP ratio of the battery cell is reduced, and lithium plating is likely to occur, resulting in battery cell capacity attenuation. In severe cases, it may cause the battery cell to short-circuit and cause a safety accident.
[0074] From the comparison between Example 1 and Example 4-5, it can be seen that in the second active material layer of the negative electrode sheet of the present invention, the second graphite and Li x Si y O z The mass ratio of the first graphite and Li x Si y O z The mass ratio of the second graphite is controlled at (87-95): (5-13), and the performance of the negative electrode is better. If the proportion of the second graphite is too large, Li x Si y O z The proportion of the second graphite decreases, the battery capacity decreases, the lithium loss in the cycle process cannot be replenished in time, and the battery cycle life is reduced. If the proportion of the second graphite is too small, Li x Si y O z The proportion of is too large, the anode compaction is reduced, the second active material layer of the anode is subjected to greater pressure during cold pressing, the porosity of the electrode is reduced, the liquid absorption performance of the electrode is deteriorated, and the battery cell is easily susceptible to lithium deposition.
[0075] From the comparison between Example 1 and Examples 6-7, it can be seen that the cold pressing density of the negative electrode sheet of the present invention will affect its performance. The cold pressing density c and the coating thickness a of the first slurry and the coating thickness b of the second slurry need to satisfy the relationship c=(0.047b-0.021a) / 3, and c is 1.50-1.68 g / cm 3If the compaction density is too small, the contact of the anode active material is not close and the conductivity is poor. At the same time, the migration distance of lithium ions during charging is long, and the rate performance deteriorates. If the compaction density is too large, the anode active material layer is over-pressured, the pores between the particles are reduced, the liquid absorption of the electrode is deteriorated, and when lithium ions are embedded, the channels are reduced, which affects the rate performance of the battery cell. Moreover, due to excessive compaction, the graphite particles are easily broken. Due to the broken graphite, the active sites increase, which aggravates the side reactions with the electrolyte, resulting in varying degrees of reduction in the battery cell cycle, rate, and life.
[0076] By comparing Example 1 and Comparative Example 1, it can be seen that the inner layer of the negative electrode plate of the present invention adopts a mixture of small-particle graphite and soft carbon or hard carbon, which improves the conductivity between the negative electrode plate and the current collector, shortens the lithium ion embedding distance, accelerates the lithium ion embedding speed, and reduces the internal resistance of the battery cell.
[0077] From the comparison between Example 1 and Comparative Example 2, it can be seen that the outer layer of the negative electrode sheet of the present invention is made of large-grained graphite and Li X Si y O z Nanomaterial mixing and large-particle graphite increase the compaction density of the pole piece, while ensuring that the outer graphite layer still has a high porosity after cold pressing, ensuring that lithium ions can enter the interior of the pole piece smoothly. X Si y O z Nanomaterials improve the energy density of battery cells by pre-lithiation of SiO.
[0078] From the comparison between Example 1 and Comparative Examples 3-4, it can be seen that the negative electrode plate of the present invention adopts a double-layer structure design, the first active material layer is the inner layer, and the material of this layer is a mixture of small-particle graphite and soft carbon or hard carbon. When lithium ions are embedded, the small-particle graphite has a shorter migration distance, which can effectively reduce the solid-phase diffusion impedance of lithium ions and reduce the anode polarization. At the same time, the mixed soft carbon and hard carbon are amorphous carbon, and there are more lithium ion embedding channels, which effectively reduces the interface impedance when lithium ions are embedded, and can also achieve the effect of reducing anode polarization and improving rate performance. The second active material layer is the outer layer, and the material of this layer is a mixture of large graphite and lithium silicon oxygen composite oxide. Li x Si y O z To pre-lithiate SiO, during the long-term cycle, as lithium ions are consumed, a potential difference will appear between the anode and the cathode. x Si y O z It will gradually release lithium ions to replenish the lost lithium ions, improve the long-term cycle life of the battery, and provide higher energy density.
[0079] The applicant declares that the above is only a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention fall within the scope of protection and disclosure of the present invention.
Claims
1. A negative electrode plate, characterized in that: The negative electrode sheet includes a negative electrode current collector, a second active material layer, and a first active material layer disposed between the negative electrode current collector and the second active material layer, wherein the active material of the first active material layer includes a mixture of a first graphite and soft carbon and / or hard carbon, and the active material of the second active material layer includes a second graphite and Li x Si y O z , where x is 1 to 4, y is 0.1 to 2, and z is 3 to 5; The median particle size D50 of the first graphite is 10-12 μm, the median particle size D50 of the soft carbon and / or hard carbon is 6-9 μm, the median particle size D50 of the second graphite is 15-25 μm, and the Li x Si y O z The first active material layer is a nanomaterial; the compaction density of the first active material layer is less than that of the second active material layer; The mass ratio of the first graphite to the soft carbon and / or the hard carbon is 80:20; the mass ratio of the second graphite to the Li x Si y O z The mass ratio is 90:10; The compaction density of the negative electrode sheet after cold pressing is 1.62 g / cm 3 .
2. A method for preparing a negative electrode sheet as claimed in claim 1, characterized in that: The preparation method comprises the following steps: (1) mixing a first graphite, soft carbon and / or hard carbon, a conductive agent and a binder with a first solvent to obtain a first slurry, and mixing a second graphite, Li x Si y O z , a conductive agent and a binder are mixed with a second solvent to obtain a second slurry; (2) The first slurry is coated on the surface of the negative electrode current collector, and the second slurry is coated on the surface of the first slurry, and the negative electrode sheet is obtained by cold pressing.
3. The preparation method according to claim 2, characterized in that: The conductive agent in step (1) includes any one of conductive carbon black, carbon nanotubes or graphene, or a combination of at least two of them.
4. The preparation method according to claim 2, characterized in that: The binder in step (1) includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber.
5. The preparation method according to claim 4, characterized in that: The binder in step (1) is sodium carboxymethyl cellulose and styrene-butadiene rubber.
6. The preparation method according to claim 2, characterized in that: In step (1), the first solvent comprises deionized water.
7. The preparation method according to claim 2, characterized in that: In step (1), the second solvent comprises an oil-based solvent.
8. The preparation method according to claim 7, characterized in that: The oil-based solvent includes any one of dimethyl sulfoxide, N,N-dimethylformamide, dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof.
9. The preparation method according to claim 2, characterized in that: Step (1) The mass ratio of the first graphite and the mixture of soft carbon and / or hard carbon, the conductive agent, sodium carboxymethyl cellulose, and styrene-butadiene rubber is (94-97):(1.0-2.0):(1.2-1.8):(1.5-2.5).
10. The preparation method according to claim 2, characterized in that: Step (1) Second Graphite and Li x Si y O z The mass ratio of the mixture, the conductive agent sodium carboxymethyl cellulose, and styrene-butadiene rubber is (94-96):(0.5-1.7):(1.0-3.2):(1.2-2.8).
11. The preparation method according to claim 2, characterized in that: Step (1) The solid content of the first slurry is 55-60%.
12. The preparation method according to claim 2, characterized in that: Step (1) The viscosity of the first slurry is 3000 to 5500 mPa·s.
13. The preparation method according to claim 2, characterized in that: Step (1) The solid content of the second slurry is 51-55%.
14. The preparation method according to claim 2, characterized in that: Step (1) The viscosity of the second slurry is 3000 to 5500 mPa·s.
15. The preparation method according to claim 2, characterized in that: Step (2) The coating thickness of the first slurry, the coating thickness of the second slurry and the compaction density after cold pressing satisfy the relationship c=(0.047b-0.021a) / 3, c is 1.62 g / cm 3 , wherein the coating thickness of the first slurry is aμm, the coating thickness of the second slurry is bμm, and the compaction density after cold pressing is cg / cm 3 .
16. A lithium ion battery, characterized in that: The lithium-ion battery comprises the negative electrode sheet as claimed in claim 1.