Methods and related devices for exfoliating and / or functionalizing layered objects

By applying voltage difference in liquid to generate plasma, the problems of low treatment efficiency and use of harmful compounds in the prior art are solved, and efficient and low defective layered material peeling and functionalization are achieved.

CN115279693BActive Publication Date: 2024-11-29UNIVERSITY OF LORRAINE +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180020601.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-10
Publication Date
2024-11-29
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

The prior art requires the use of harmful compounds or is inefficient when dealing with layered materials, making it difficult to achieve efficient peeling and functionalization in a single step, and is prone to introduce structural defects.

Method used

By placing the first and second electrodes in the liquid and applying a voltage difference to generate a plasma, the voltage difference, distance and time are controlled, and the gas pressure and electrode surface area are adjusted to achieve peeling and functionalization of the layered material.

Benefits of technology

Efficient peeling and functionalizing of the layered material in a single step is achieved, reducing the introduction of structural defects, avoiding the use of harmful compounds, and energy-intensive but simple implementation, enabling control of the obtained layered material properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115279693B_ABST
    Figure CN115279693B_ABST
Patent Text Reader

Abstract

"Method for exfoliating and / or functionalizing layered objects and related devices" The present invention relates to a method for exfoliating and / or functionalizing layered objects, comprising the following steps: ·- Immersing at least a portion of a first electrode in a liquid containing the layered object to be exfoliated and / or functionalized, ·- Placing a second electrode outside the liquid; at least a portion of the second electrode is opposite to the liquid surface; ·- Generating a plasma between at least a portion of the second electrode opposite to the liquid surface and the liquid surface by applying a pulse voltage difference between the first and second electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of producing nanofillers intended to be incorporated into composite materials, especially polymer composite materials. The nanofillers are in particular layered materials, such as graphene or graphene materials.

[0002] The invention also relates to the processing of such nanofillers, in particular the exfoliation and / or functionalization. Background Art

[0003] Wet functionalization of layered materials by chemical acid and / or oxidative treatments is known from the prior art. Said treatments require the use of hazardous compounds which require stringent operating conditions and have a significant impact on the environment.

[0004] Functionalization of layered materials by plasma treatment is also known from the prior art. These plasma treatment methods involve the interaction of a plasma with the surface of the material to be treated, resulting in a reaction of the active species of the plasma with the material to be treated.

[0005] The technique of exfoliating layered materials by ultrasound is known from the prior art. This method has limited efficiency because it requires several steps to obtain the desired result.

[0006] Prior art also includes micromechanical exfoliation, whereby graphene sheets are mechanically separated by separating a layer or group of graphene sheets or sheets of graphene material. This method is not feasible on an industrial scale.

[0007] The objects of the present invention are in particular:

[0008] - Eliminate the use of chemical compounds that are hazardous or have a significant impact on the environment, and / or

[0009] - obtaining a layered material with few layers, and / or

[0010] - starting from a macroscopic layered material to obtain a layered material with few layers, and / or

[0011] - functionalizing the layered material, and / or

[0012] - obtaining a layered material in a single step and / or functionalizing a layered material in a single step and / or obtaining a functionalized layered material in a single step, and / or

[0013] - almost no structural defects are introduced into the obtained layered material and / or the obtained functionalized layered material, and / or

[0014] - is not very energy intensive, but is easy and simple to implement, and / or

[0015] - Controlling the obtained layered material and / or the obtained functionalized layered material. Summary of the invention

[0016] To this end, a method for exfoliating and / or functionalizing a layered object is proposed, comprising the following steps:

[0017] - immersing at least a portion of the first electrode in a liquid containing the layered object to be exfoliated and / or functionalized,

[0018] - placing a second electrode outside the liquid; at least a portion of the second electrode is opposite to the surface of the liquid,

[0019] - generating a plasma between at least a portion of the second electrode opposite to the surface of the liquid and said surface of the liquid by applying a voltage difference between the first electrode and the second electrode.

[0020] Preferably, the voltage of the first electrode is greater than the voltage of the second electrode.

[0021] The voltage of the first electrode may be less than the voltage of the second electrode so that the stripping is greater than the functionalization. The voltage of the first electrode may be less than the voltage of the second electrode so that the functionalization is reduced or no longer obtained. In other words, the voltage of the first electrode may be less than the voltage of the second electrode so that the stripping of the layered object is mainly or exclusively performed during the implementation of the method.

[0022] According to the invention, layered refers to objects whose structure consists of parallel layers.

[0023] The second electrode and / or a portion of the first electrode may be placed in the gas in contact with the surface of the liquid.

[0024] At least a portion of the second electrode opposite to the liquid surface may be:

[0025] - an end of the second electrode, and / or

[0026] - The whole or part of the electrode surface which is opposite to the surface of the liquid.

[0027] According to the present invention:

[0028] - the voltage difference between the first electrode and the second electrode is greater than 1000 volts, and / or

[0029] - the distance d1 between at least a portion of the second electrode facing the liquid surface and the liquid surface is greater than 1 μm, and / or

[0030] - the voltage difference between the first electrode and the second electrode is applied for a time longer than 10 picoseconds, and / or

[0031] - the time interval between two consecutive applications of the voltage difference between the first electrode and the second electrode is greater than 0.1 ns, and / or

[0032] - The pressure of the gas in which the second electrode is placed is greater than 1 Pa and / or less than 1×10 7 Pa.

[0033] Preferably, the voltage difference between the first electrode and the second electrode can be adjusted according to the product of the gas pressure and the distance d1, or vice versa, so as to generate plasma, ie, to meet the breakdown condition of the gas.

[0034] Preferably, the gas in which the second electrode is placed is a gas in contact with the surface of the liquid.

[0035] Non-limiting examples of the gas in which the second electrode is placed may be air, nitrogen, a noble gas such as xenon, krypton, argon, neon or helium, or a gas mixture.

[0036] The first electrode and / or the second electrode may comprise a refractory material, preferably a major proportion of a refractory material.

[0037] The first electrode and / or the second electrode may consist primarily or essentially of a refractory material.

[0038] The first electrode and the second electrode may contain tungsten and / or carbon.

[0039] The layered object to be exfoliated and / or to be functionalized may include graphite, clay materials, transition metal chalcogenides, layered silicates and / or graphene materials.

[0040] Preferably, the layered object to be exfoliated and / or to be functionalized mainly or substantially comprises graphite, clay materials, transition metal chalcogenides, layered silicates and / or graphene materials. The layered object to be exfoliated and / or to be functionalized may mainly or substantially consist of graphite, clay materials, transition metal chalcogenides, layered silicates and / or graphene materials.

[0041] According to the invention, the number of layers of the exfoliated layered object and / or the functionalized layered object is less than 25.

[0042] The layered object to be exfoliated and / or to be functionalized may include graphite and / or graphene materials, and the exfoliated and / or functionalized object may be made of graphene.

[0043] Within the framework of the present application, graphene is considered to consist of layers having a number of less than 25.

[0044] At least one dimension of the layered object to be exfoliated and / or to be functionalized may be larger than 100 nanometers.

[0045] The layered object to be functionalized and / or to be exfoliated may have a single dimension greater than 100 nanometers, two dimensions greater than 100 nanometers, or three dimensions greater than 100 nanometers.

[0046] Methods may include regulating:

[0047] - a voltage difference between the first electrode and the second electrode so as to:

[0048] ● increasing the exfoliation and / or functionalization of a layered object contained in a liquid by increasing or decreasing the voltage difference between the first electrode and the second electrode, and / or

[0049] ● reducing the exfoliation and / or functionalization of a layered object contained in a liquid by reducing or increasing the voltage difference between the first electrode and the second electrode, and / or

[0050] - the nature of the gas in which the second electrode is placed and / or the pressure of the gas in which the second electrode is placed, so as to:

[0051] ● Increased exfoliation and / or functionalization of layered objects contained in liquids by reducing the breakdown voltage of the gas, and / or

[0052] ● Reduce the exfoliation and / or functionalization of layered objects contained in liquids by increasing the breakdown voltage of the gas, and / or

[0053] - the nature of the liquid containing the layered object to be exfoliated and / or to be functionalized and / or the conductivity of the liquid containing the layered object to be exfoliated and / or to be functionalized, in order to:

[0054] ● increasing the exfoliation and / or functionalization of layered objects contained in a liquid by lowering the pH by adding one or more acids and / or increasing the conductivity of the liquid by adding one or more salts, and / or

[0055] ● reducing the exfoliation and / or functionalization of layered objects contained in the liquid by increasing the pH by adding one or more bases and / or by reducing the salinity of the solution to reduce the conductivity of the liquid, and / or

[0056] - the surface area of ​​the second electrode so that:

[0057] ● increasing the exfoliation and / or functionalization of layered objects contained in the liquid by increasing the surface area of ​​the second electrode that interacts with the plasma, and / or

[0058] ● Reduce exfoliation and / or functionalization of layered objects contained in liquids by reducing surface leakage and / or collecting charges interacting with the plasma.

[0059] Preferably, and unless otherwise stated in this application, adjustment of a parameter that has the effect of increasing release and / or functionalization (or reducing release and / or functionalization, respectively) does not have the effect of reducing release and / or functionalization (or increasing release and / or functionalization, respectively).

[0060] An acid may refer to a substance that behaves like an acid during an acid-base reaction, while a base may refer to a substance that behaves like a base during an acid-base reaction. In particular, a base may refer to a substance that is able to accept one or more protons (H + ), while an acid can be a chemical substance that can donate one or more protons (H + ) chemical substances.

[0061] According to the invention, adjusting may be modifying or adjusting.

[0062] According to the present invention, increasing or decreasing the exfoliation and / or functionalization may be defined as increasing or decreasing the exfoliation rate and / or the functionalization rate.

[0063] Preferably, the method may be carried out at atmospheric pressure.

[0064] Methods may include regulating:

[0065] - a distance d1 between at least a portion of the second electrode opposite the surface of the liquid and the surface of the liquid, so that:

[0066] ● increasing the exfoliation and / or functionalization of the layered objects contained in the liquid by promoting a uniform state or a filamentous state of the layered objects contained in the liquid by reducing the distance between at least a portion of the second electrode opposite to the surface of the liquid and the surface of the liquid, and / or

[0067] reducing the exfoliation and / or functionalization of the layered objects contained in the liquid by promoting a filamentous state or a uniform state of the layered objects contained in the liquid by increasing the distance between at least a portion of the second electrode opposite to the surface of the liquid and the surface of the liquid, and / or

[0068] - the time for which a voltage difference is applied between the first electrode and the second electrode so as to:

[0069] ● increasing the exfoliation and / or functionalization of the layered object contained in the liquid by increasing the time for which the voltage is applied between the first electrode and the second electrode, and / or

[0070] ● reducing the exfoliation and / or functionalization of the layered object contained in the liquid by reducing the time during which the voltage is applied between the first electrode and the second electrode, and / or

[0071] - the frequency between two consecutive applied voltage differences so that:

[0072] ● increasing the exfoliation and / or functionalization of layered objects contained in a liquid by increasing the frequency between two consecutive applied voltage differences, and / or

[0073] • Reducing the exfoliation and / or functionalization of layered objects contained in liquid by reducing the frequency between two consecutive applied voltage differences.

[0074] In the case of adjusting distance d1, as a non-limiting example of increasing functionalization, decreasing distance d1 can have the same effect as increasing distance d1. This effect is due to a change in the plasma discharge state, such as from a uniform discharge state to a filamentary discharge state or vice versa.

[0075] According to the present invention, a device for exfoliating and / or functionalizing a layered object is also proposed, comprising:

[0076] at least one first electrode comprising at least one portion intended to be immersed in a liquid comprising the layered object to be exfoliated and / or to be functionalized,

[0077] - at least one second electrode intended to be placed outside the liquid; at least a portion of the at least one second electrode intended to be opposite to the surface of the liquid,

[0078] - a pulse power generator for emitting electrical pulses between the at least one first electrode and the at least one second electrode, the pulse power generator being arranged to apply a voltage difference greater than 1000 volts between the at least one first electrode and the at least one second electrode.

[0079] Preferably, the at least one first electrode and the at least one second electrode are placed relative to each other and / or the generator is arranged such that no plasma is generated between the at least one first electrode and the at least one second electrode.

[0080] Preferably, no plasma extends between the surface of the at least one first electrode and the surface of the at least one second electrode.The surface of the at least one second electrode may be at least a portion of the at least one second electrode intended to be placed opposite the surface of the liquid.

[0081] Preferably, the at least one first electrode and the at least one second electrode are placed relative to each other and / or the generator is arranged such that the plasma is generated starting from at least a portion of the at least one second electrode intended to be placed opposite the surface of the liquid. Preferably, the plasma is generated starting from at least a portion of the at least one second electrode opposite the surface of the liquid to the surface of the liquid intended to immerse at least a portion of the at least one first electrode.

[0082] The at least one first electrode and the at least one second electrode may be arranged relative to each other such that a distance d2 separating the at least one first electrode and the at least one second electrode is greater than a distance d2 denoted as dE1E2 distance d, starting from that distance and going below it E1E2 generating a plasma in a spatial region extending between at least one first electrode and at least one second electrode, and / or

[0083] The generator may be arranged so as to apply between at least one first electrode and at least one second electrode a voltage less than V cl-elec A voltage V of the voltage d2 is applied so that plasma is generated in a region extending between the at least one first electrode and the at least one second electrode along the distance d2.

[0084] Preferably, for a given gas and gas pressure:

[0085] - for a voltage V applied between at least one first electrode and at least one second electrode app The at least one first electrode and the at least one second electrode are arranged relative to each other so that the distance d2 between the at least one first electrode and the at least one second electrode is greater than the distance d separating the at least one first electrode and the at least one second electrode. E1E2 , starting from this distance and going below it along a distance d E1E2 generating a plasma in a spatial region extending between at least one first electrode and at least one second electrode, and / or

[0086] - for the arrangement of the at least one first electrode and the at least one second electrode relative to each other, such that the at least one first electrode and the at least one second electrode are spaced apart by a distance denoted as d elec The generator is arranged so that a voltage less than V is applied between at least one first electrode and at least one second electrode. cl-elec A voltage V is provided at a voltage of 100° so that plasma is generated in a region extending between the at least one first electrode and the at least one second electrode along the distance d2.

[0087] Preferably, the arrangement of the at least one first electrode and the at least one second electrode and / or the voltage V applied between the at least one first electrode and the at least one second electrode is such that the breakdown voltage V of the gas in the spatial region extending along the distance d2 between the at least one first electrode and the at least one second electrode is cl-elec greater than the distance d1 in a spatial region extending between at least a portion of at least one second electrode intended to be placed opposite the liquid surface and the liquid surface, referred to as V cl-liq The breakdown voltage of the gas.

[0088] In other words, the voltage difference applied between the at least one first electrode and the at least one second electrode and / or the arrangement of the at least one first electrode and the at least one second electrode relative to each other is such that no plasma is generated in the spatial region extending between the at least one first electrode and the at least one second electrode.

[0089] Preferably, only a portion of the second electrode, referred to as the exposed portion, is intended to be placed in the gas.

[0090] According to the present invention, "placing a portion of an object such as an electrode in a medium such as a gas or a liquid" means that the surface of the object is in direct contact with the medium.

[0091] As non-limiting examples, at least one first electrode and / or at least one second electrode may be in the form of an elongated strip or in the form of a plate.

[0092] The at least one first electrode and / or the at least one second electrode may be a single electrode or may comprise several electrodes.

[0093] The at least one first electrode and / or the at least one second electrode may be a group of electrodes that are connected or not connected to each other. The at least one first electrode and / or the at least one second electrode may be an electrode network.

[0094] A device may contain a single generator or several generators.

[0095] The device may comprise several generators, and the at least one first electrode and / or the at least one second electrode preferably comprises several electrodes; each generator being connected to a single electrode or to several electrodes of the several electrodes.

[0096] Preferably, the voltage of the first electrode is greater than the voltage of the second electrode.

[0097] The at least one first electrode may:

[0098] - comprises a portion intended to be placed in the gas in which at least one second electrode is placed and at a distance d2 from the at least one second electrode, said distance d2 being adjusted according to the nature and / or the pressure of the gas in which at least one second electrode is placed, so that the voltage difference applied by the generator is less than the breakdown voltage of the gas, or

[0099] - does not contain a portion intended to be placed in a gas in which at least one second electrode is placed.

[0100] The distance d2 may be defined as the minimum distance separating the portion of the at least one first electrode intended to be placed in the gas in which the at least one second electrode is placed from the at least one second electrode.

[0101] Preferably, the portion intended to be placed in the gas in which the at least one second electrode is placed is the portion of the second electrode intended to be exposed.

[0102] The entire at least one first electrode may be intended to be immersed in the liquid. Excluding the portion intended to be placed in the gas in which the at least one first electrode is placed may correspond to the case where the entire at least one first electrode is intended to be immersed in the liquid.

[0103] At least one first electrode may be in the form of an elongated strip, and:

[0104] ● Mainly extends in direction b1, direction b1 connects:

[0105] ■ a plane p1 comprising at least a portion of at least one second electrode intended to be placed opposite the surface of the liquid, and

[0106] ■ an end of at least a portion of at least one first electrode intended to be immersed in the liquid,

[0107] ● A portion of at least one first electrode including at least a portion of at least one first electrode intended to be immersed in the liquid protrudes along the b1 direction relative to the plane p1; the distance d3 between the end of at least a portion of at least one first electrode immersed in the liquid and the plane p1 is greater than 2 mm.

[0108] The at least one second electrode and / or the at least one first electrode and the at least one second electrode may be in the form of an elongated strip.

[0109] According to the present invention:

[0110] - the distance d1 between the plane p1 and the surface of the liquid may be greater than 1 μm, and

[0111] - the distance d4 between the plane p2 containing the end of at least a portion of at least one first electrode intended to be immersed in the liquid and the surface of the liquid may be greater than 1 mm, said distance d4 being equal to the difference between d3 and d1 .

[0112] The device may comprise a liquid containing a layered object to be exfoliated and / or functionalized; at least one first electrode and at least one second electrode are positioned relative to each other and / or the generator is arranged to apply a voltage difference suitable for generating a plasma between at least a portion of at least one second electrode positioned opposite to the surface of the liquid and the surface of the liquid.

[0113] Preferably, the arrangement of the at least one first electrode and the at least one second electrode and / or the voltage V applied between the at least one first electrode and the at least one second electrode is such that:

[0114] - the breakdown voltage V of the gas in the spatial region extending along the distance d2 between the at least one first electrode and the at least one second electrode cl-elecgreater than the distance d2 in a spatial region extending between at least a portion of at least one second electrode intended to be placed opposite the liquid surface and the liquid surface, referred to as V cl-liq The breakdown voltage of the gas, and - a voltage V applied between at least one first electrode and at least one second electrode:

[0115] ●Greater than voltage V cl-liq ,and

[0116] ●Less than voltage V cl-elec .

[0117] Preferably, the device according to the invention is arranged to carry out the method according to the invention. Any features of the method according to the invention can be integrated in the device according to the invention.

[0118] Preferably, the method according to the invention is implemented by the device according to the invention. Any features of the device according to the invention can be integrated into the method according to the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0119] Other advantages and features of the invention will become apparent from a reading of the detailed description of non-limiting embodiments and implementations and the following drawings:

[0120] [ Figure 1 ] Figure 1 is a schematic diagram of an embodiment of an apparatus according to the present invention,

[0121] [ Figure 2 ] Figure 2 is a graph showing the changes in the pH of a solution, the conductivity of a solution and the temperature of a solution as a function of time during the implementation of the method according to the invention,

[0122] [ Figure 3 ] Figure 3 A comparison photograph of a layered filler treated by the method in a suspended state and a reference layered filler in a suspended state is shown,

[0123] [ Figure 4 ] Figure 4 The Raman spectra of the layered filler before treatment and the Raman spectra of the layered filler after treatment are shown. DETAILED DESCRIPTION

[0124] Since the embodiments described below are by no means limiting, it is particularly contemplated that a variant of the invention consists in selecting only the features described, considered separately from the other features described (even if the selection is considered separately in the sentence containing these other features), provided that the selection of this feature is sufficient to confer a technical advantage or to differentiate the invention with respect to the state of the art. This selection includes at least one preferably functional feature without structural details, or at least one preferably functional feature with only a part of the structural details, provided that this part alone is sufficient to confer a technical advantage or to differentiate the invention with respect to the state of the art.

[0125] Reference Figure 1 A device 1 and a method according to the invention are described. The layered object used during the implementation of the exfoliation and / or functionalization method according to the invention by means of the device 1 is a graphite filler sold under the trade name "KNG-180" by the company "Knano". The graphite filler has macroscopic dimensions greater than 100 nanometers. The exfoliated and / or functionalized object is made of graphene. The exfoliated and / or functionalized object may include graphene and graphene materials. The method is implemented at ambient temperature. The gas 2 in which at least one second electrode 6, i.e., a single second electrode 6 according to an embodiment, is placed is air 2. The pressure of the gas 2 in which the second electrode 6 is placed is greater than 1 Pa and / or less than 1×10 7 Pa. According to an embodiment, the air 2 is at atmospheric pressure. The liquid 3 containing the layered object and intended to immerse at least one first electrode 5, i.e., at least a portion 4 of a single first electrode 5 according to an embodiment, is deionized water 3. The method is implemented on a solution with a volume of 300 ml of liquid 3, and the mass of the graphite filler is 200 mg. Unless otherwise stated, the method is implemented for more than one hour. The second electrode 6 is intended to be placed outside the liquid 3. At least a portion 7 of the second electrode 6 is intended to be opposite to the surface 8 of the liquid 3. The device 1 includes a pulse power generator 10 that emits electrical pulses between the first electrode 5 and the second electrode 6. The pulse generator 10 is arranged so as to apply a voltage difference greater than 1000 volts between the first electrode 5 and the second electrode 6. According to an embodiment, the voltage difference is 6 kV. Preferably, the voltage of the first electrode 5 is greater than the voltage of the second electrode 6. According to an embodiment, the second electrode 6 is grounded and the first electrode 5 is connected to the pulse generator 10.

[0126] When implementing the method, the portion 4 of the first electrode 5 is immersed in the liquid 3. The first electrode 5 and the second electrode 6 are placed relative to each other and / or the generator 10 is arranged to apply a voltage difference suitable for generating a plasma 9 between the portion 7 of the second electrode 6 placed opposite the surface 8 of the liquid 3 and said surface 8 of the liquid 3. In practice, the generation of the plasma, called breakdown, occurs under conditions that comply with Paschen's law, i.e., when the product of the pressure of the gas and the distance between the electrodes minimizes the breakdown voltage of the gas. Typically, a distance of a few millimeters between the second electrode 5 and the surface 8 of the liquid 3 is chosen, combined with a voltage greater than the breakdown voltage, so as to ensure a plasma discharge 9 in the gas mixture 2 or pure gas 2.

[0127] The first electrode 5 and the second electrode 6 are placed relative to each other and / or the generator 10 is arranged so that no plasma is generated between the first electrode 5 and the second electrode 6. Plasma 9 is generated between a portion 7 of the second electrode 6 opposite to the surface 8 of the liquid 3 and the surface 8 of the liquid 3 by applying a voltage difference between the first electrode 5 and the second electrode 6. As a non-limiting example, the plasma generated according to the present invention has a thickness of about 1 mm. 3 The size of the plasma can be considered as a small size. 3 or larger than 10cm 3 A plasma of the size of can be regarded as a large-size plasma.

[0128] The distance d1 between the portion 7 of the second electrode 6 intended to be opposite to the surface 8 of the liquid 3 and the surface 8 of the liquid 3 is greater than 1 μm, and according to one embodiment it is 1 mm. The device 1 comprises a nanosecond chopper 11 arranged so as to apply a voltage between the first electrode 5 and the second electrode 6 for an application time longer than 10 picoseconds. According to the invention, the application time is 1 μs. The average electric power of the pulse is about 36 W. The nanosecond chopper 11 is arranged so that the time interval between two consecutive applications of a voltage difference between the first electrode 5 and the second electrode 6 is preferably longer than 0.1 ns. According to one embodiment, the time interval is about 170 μs. The benefit of the high-voltage pulse scheme (usually with a voltage greater than 1000 volts) is to promote the process of exfoliating graphite by causing a shock wave during the plasma breakdown 9 in the air 2 at atmospheric pressure. Then, the graphite fillers located on the surface 8 of the liquid 3 can undergo mechanical separation of their graphene planes. Another benefit of this discharge scheme is that it allows high-energy plasma functionalization while having a method that is not very energy-intensive, with an average power of 10 W to 120 W depending on the discharge conditions. By requiring only the breakdown voltage of gas 2 (here air), the method can be continued until the current reaches several amperes.

[0129] The portion 12 of the first electrode 5 is intended to be located in the gas 3 in which the second electrode 6 is placed. The portion 12 is separated from the second electrode 6 by a distance d2. The distance d2 is adjusted according to the properties and / or the pressure of the gas in which the second electrode 6 is placed so that the voltage difference applied by the generator 10 is less than the breakdown voltage of the gas.

[0130] According to one embodiment, the first electrode 5 and the second electrode 6 are in the form of elongated strips. The first electrode 5 mainly extends in the direction b1, and the direction b1 connects:

[0131] ■ a plane p1 containing a portion 7 of the second electrode 6 intended to be placed opposite the surface 8 of the liquid 3, and

[0132] ■ The end 13 of the portion 4 of the first electrode 5 which is intended to be immersed in the liquid 3 .

[0133] The portion of the first electrode 5 comprising the portion 4 of the first electrode 5 intended to be immersed in the liquid 3 protrudes in the direction b1 relative to the plane p1. The distance d3 between the end 13 of the portion 4 of the first electrode 5 intended to be immersed in the liquid 3 and the plane p1 is greater than 2 mm. The distance d4 between the plane p2 comprising the end 13 of the portion 4 of the first electrode 5 intended to be immersed in the liquid 3 and the surface of the liquid 3 is greater than 1 mm, the distance d4 being equal to the difference between d3 and d1.

[0134] Reference Figure 2 The effect of the method on the solution 3 is described. The aqueous phase 3 will undergo significant changes in its initial intrinsic properties, in particular in its composition, which will modify its pH and conductivity. This change in the composition of the liquid 3 is due in particular to the interaction between the plasma 9 and the liquid 3, and more particularly to the progressive solvation of species originating from the plasma 9, such as electrons, ions and other radicals or energetic species, on the surface 8 of the liquid 3. The changes in the medium 3, its acidification and the gradual heating are likewise variable parameters, which also promote the exfoliation process of graphite on the surface and in the volume of the liquid 3, as well as the reaction mechanism of the functionalization of the graphene plane.

[0135] Reference Figure 3 The efficiency of the method for the functionalization effect of the obtained graphene nanofillers is presented. The sedimentation rate of the nanofiller suspension is an indicator of the surface condition of the nanofillers in the suspension. The functionalization of the nanofiller introduces chemical groups or chemical functional groups, especially polar groups or polar functional groups, especially polar groups or polar functional groups containing oxygen atoms, such as hydroxyl, carbonyl and / or carboxyl groups, on the surface of the nanofiller, which promotes the suspension and stability of the nanofiller. Figure 3 a), Figure 3 b) and Figure 3In each of c), the sample on the left is an aqueous solution in which the nanofiller obtained by this method is suspended, while the sample on the right is an aqueous solution in which the nanofiller sold under the trade name "KNG-180" by the company "Knano" is suspended. Figure 3 a), Figure 3 b) and Figure 3 C) shows the sample images of stirring just finished, stirring after 5 minutes and stirring after 1 hour respectively. After 1 hour, no obvious sedimentation was observed in the sample containing the nanofiller in suspension obtained by the method, and after 5 minutes, obvious sedimentation was observed in the solution containing the reference nanofiller in suspension. This proves the efficiency of the method for functionalizing the nanofiller according to the present invention. The detection of carboxyl on the graphene plane surface disclosed by thermogravimetric analysis in combination with mass spectrum and X-ray photoelectron spectroscopy also confirms this change of filler surface condition. Therefore, these groups can be used for specific functionalization or promote the dispersion of graphene plane in polymer matrix.

[0136] Reference Figure 4 , the left figure shows the Raman spectrum of the initial graphite filler before the implementation of the method. The right figure shows the Raman spectrum of the graphene nanofiller obtained after the implementation of the method. Note the small degradation of the carbon plane, which is one tenth of that observed at the end of the chemical treatment of the prior art. D / I G The “defect rate” is evaluated by the ratio of the spectral band denoted D, which is equal to the ratio of the spectral band denoted G, which is characteristic of the sp2 hybridization state of carbon.

[0137] Thus, in a variant that can be combined with another of the above embodiments:

[0138] - the layered object to be exfoliated and / or functionalized comprises a clay material, a transition metal chalcogenide, a layered silicate and / or a graphene material, and / or

[0139] - the first electrode 5 and the second electrode 6 comprise a refractory material, preferably a major proportion of a refractory material, and / or

[0140] - the first electrode 5 and the second electrode 6 contain tungsten and / or carbon, and / or

[0141] The first electrode 5 is completely immersed in the liquid 3 ; therefore, the first electrode 5 does not comprise a portion 12 intended to be placed in the gas 2 where the second electrode 6 is placed.

[0142] Furthermore, unless the different features, forms, variations and embodiments of the present invention are incompatible or mutually exclusive, they can be combined together in various combinations.

Claims

1. A method for exfoliating and / or functionalizing a layered object, comprising the following steps: - immersing at least a portion (4) of the first electrode (5) in a liquid (3) containing the layered object to be exfoliated and / or functionalized, - placing a second electrode (6) outside the liquid; at least a portion (7) of the second electrode is opposite to the surface (8) of the liquid, - generating a plasma (9) between at least a portion of the second electrode opposite to the surface of the liquid and said surface of the liquid by applying a pulsed voltage difference of greater than 1000 volts between the first electrode and the second electrode, so as to induce a shock wave during the breakdown of the plasma in the gas in which the second electrode is intended to be placed.

2. The method according to claim 1, wherein: - at least a portion (7) of the second electrode (3) opposite to the surface (8) of the liquid (3) is at a distance d1 greater than 1 μm from the surface of the liquid, and / or - the voltage difference between the first electrode and the second electrode is applied for a time longer than 10 picoseconds, and / or - the time interval between two consecutive pulse voltage differences applied between the first electrode and the second electrode is greater than 0.1 ns, and / or - the pressure of the gas (2) in which the second electrode is placed is greater than 1 Pa and / or less than 1×10 7 Pa.

3. The method according to claim 1 or 2, wherein the first electrode (5) and / or the second electrode (6) comprises a refractory material.

4. The method according to claim 1 or 2, wherein the first electrode (5) and / or the second electrode (6) comprises a major proportion of a refractory material.

5. The method according to claim 1 or 2, wherein the first electrode (5) and / or the second electrode (6) comprises tungsten and / or carbon.

6. The method according to claim 1 or 2, wherein the layered object to be exfoliated and / or functionalized comprises graphite, clay materials, transition metal chalcogenides, layered silicates and / or graphene materials.

7. The method according to claim 1 or 2, wherein the layered object to be exfoliated and / or functionalized comprises graphite and / or graphene material, and wherein the exfoliated and / or functionalized object is made of graphene.

8. The method according to claim 1 or 2, wherein at least one dimension of the layered object to be exfoliated and / or to be functionalized is greater than 100 nanometers.

9. The method according to claim 1 or 2, comprising adjusting: - a voltage difference between the first electrode (5) and the second electrode (6) so as to: ● increasing the exfoliation and / or functionalization of the layered objects contained in the liquid (3) by increasing or decreasing the voltage difference between the first electrode and the second electrode, and / or ● reducing the exfoliation and / or functionalization of a layered object contained in a liquid by reducing or increasing the voltage difference between the first electrode and the second electrode, and / or - the nature of the gas (2) in which the second electrode is placed and / or the pressure of the gas in which the second electrode is placed, so as to: ● Increased exfoliation and / or functionalization of layered objects contained in liquids by reducing the breakdown voltage of the gas, and / or ● Reduce the exfoliation and / or functionalization of layered objects contained in liquids by increasing the breakdown voltage of the gas, and / or - the nature of the liquid containing the layered object to be exfoliated and / or to be functionalized and / or the conductivity of the liquid containing the layered object to be exfoliated and / or to be functionalized, in order to: ● increasing the exfoliation and / or functionalization of layered objects contained in a liquid by lowering the pH by adding one or more acids and / or increasing the conductivity of the liquid by adding one or more salts, and / or • Reducing the exfoliation and / or functionalization of layered objects contained in a liquid by increasing the pH by adding one or more than one base and / or by reducing the salinity of the solution to reduce the conductivity of the liquid.

10. The method of claim 2, comprising adjusting: - the application time of the voltage difference between the first electrode (5) and the second electrode, so as to: ● increasing the exfoliation and / or functionalization of the layered object contained in the liquid by increasing the time for which the voltage is applied between the first electrode and the second electrode, and / or ● reducing the exfoliation and / or functionalization of the layered object contained in the liquid by reducing the time during which the voltage is applied between the first electrode and the second electrode, and / or - the frequency between two consecutive applied voltage differences so that: ● increasing the exfoliation and / or functionalization of layered objects contained in a liquid by increasing the frequency between two consecutive applied voltage differences, and / or • Reducing the exfoliation and / or functionalization of layered objects contained in liquid by reducing the frequency between two consecutive applied voltage differences.

11. An apparatus for exfoliating and / or functionalizing a layered object, comprising: at least one first electrode (5) comprising at least one portion (4) intended to be immersed in a liquid (3) comprising the layered object to be exfoliated and / or functionalized, at least one second electrode (6) intended to be placed outside the liquid; at least one portion (7) of the at least one second electrode is intended to be opposite to the surface (8) of the liquid, - a pulse power generator (10) for emitting electrical pulses between at least one first electrode and at least one second electrode, the pulse power generator being arranged so as to apply a voltage difference greater than 1000 volts between at least one first electrode and at least one second electrode; The at least one first electrode and the at least one second electrode are placed relative to each other and / or the generator is arranged such that: - no plasma is generated between the at least one first electrode and the at least one second electrode, and - Inducing a shock wave during the breakdown of the plasma in the gas in which the second electrode is intended to be placed.

12. The device according to claim 11, wherein at least one first electrode (5): - comprises a portion (12) intended to be placed in the gas (2) in which at least one second electrode (6) is placed and at a distance d2 from the at least one second electrode, the distance d2 being adjusted according to the nature and / or the pressure of the gas in which the at least one second electrode is placed, so that the voltage difference applied by the generator is less than the breakdown voltage of the gas, or - does not contain a portion intended to be placed in a gas in which at least one second electrode is placed.

13. The device according to claim 11 or 12, wherein at least one first electrode (5) is in the form of an elongated strip, and: ● Mainly extends in direction b1, direction b1 connects: ■ a plane p1 comprising at least a portion (7) of at least one second electrode (6) intended to be placed opposite a surface (8) of the liquid (3), and ■ having an end (13) of at least a portion (4) of at least one first electrode intended to be immersed in the liquid, ● A portion of at least one first electrode comprising at least a portion of at least one first electrode intended to be immersed in the liquid protrudes in direction b1 relative to plane p1; a distance d3 between an end of at least a portion of at least one first electrode intended to be immersed in the liquid and plane p1 is greater than 2 mm.

14. The device according to claim 11 or 12, wherein: - the distance d1 between the plane p1 and the surface (8) of the liquid (3) is greater than 1 μm, and The distance d4 between a plane p2 containing the end (13) of at least a portion (4) of at least one first electrode (5) intended to be immersed in the liquid and the liquid surface is greater than 1 mm, said distance d4 being equal to the difference between d3 and d1.

15. A device according to claim 11 or 12, comprising a liquid (3) containing a layered object to be exfoliated and / or functionalized; at least one first electrode (5) and at least one second electrode (6) are placed relative to each other so as to and / or a generator (10) is arranged so as to apply a voltage difference, the voltage difference being suitable for generating a plasma (9) between at least a portion (7) of at least one second electrode placed opposite to the liquid surface and the liquid surface.

Citation Information

Patent Citations

  • Method for preparing graphene with controllable layers, and graphene

    CN107628609A

  • Manufacturing method of two-dimensional material

    CN109264708A

  • Large-scale electrochemical stripping device for preparing graphene oxide

    CN203021301U

  • apparatus and method for expanding graphite to graphene

    DE102016202202A1

  • Method for producing graphene

    JP2014152095A