Preparation method of abrasive grains

The asymmetric energy input and sol-gel method of converting aluminum hydroxide to prepare abrasive grains solve the problems of limited number of abrasive grains and large wear in the existing technology, achieving more efficient abrasive grain production and extending the service life of abrasive tools. promote.

CN115279863BActive Publication Date: 2024-10-22TYROLIT SCHLEIFMITTELWERKE SWAROVSKI KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180020275.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-11
Filing Date
2021-02-22
Publication Date
2024-10-22
Estimated Expiration
2041-02-22

AI Technical Summary

Technical Problem

The existing technology has the problem of limited preparation quantity and rapid wear when preparing abrasive particles, resulting in that only a relatively small amount of abrasive particles can be prepared within a specific time.

Method used

The starting mixture containing aluminum hydroxide is converted into alumina using a sol-gel process and formed into a mill by heat treatment and sintering by distorting the extrudate and intermediate particles through asymmetric energy input, resulting in non-uniform geometries. particles, avoiding the wear and tear caused by the use of chip devices.

Benefits of technology

Preparing more abrasive grains in the same time reduces wear and improves the production efficiency of abrasive grains and the service life of abrasive tools.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115279863B_ABST
    Figure CN115279863B_ABST
Patent Text Reader

Abstract

A method for preparing abrasive grains, comprising the steps of: i. providing a starting mixture containing at least aluminum hydroxide, which can be converted into at least aluminum oxide by heat treatment, ii. extruding the starting mixture into extrudates, iii. cutting the extrudates into intermediate particles, and iv. heat treatment of the intermediate particles, wherein the intermediate particles are converted into abrasive grains containing aluminum oxide, wherein the extrudates and / or the intermediate particles are subjected to an asymmetric energy input relative to the geometry of the extrudates and / or the intermediate particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing abrasive grains, which comprises the following process steps:

[0002] i. providing a starting mixture (2) containing at least aluminum hydroxide, which can be converted into at least aluminum oxide by heat treatment,

[0003] ii. extruding the starting mixture into an extrudate (3),

[0004] iii. cutting the extrudate (3) into intermediate particles (4), and

[0005] iv. heat treatment of the intermediate particles (4), wherein the intermediate particles (4) are converted into abrasive particles (5) containing aluminum oxide,

[0006] The invention also relates to a method for preparing a grinding tool for processing metal materials and the grinding tool prepared according to the method. Background Art

[0007] Various methods for producing abrasive grains are known from the prior art. For example, the applicant's own EP 3 342 839 A1 discloses a method in which abrasive grains with non-uniform shapes and / or sizes are produced by cutting extrudates. The purpose of this process is to produce abrasive grains with non-uniform geometry.

[0008] A disadvantage here is that only relatively small amounts of abrasive grain can be produced in a given period of time.

[0009] Furthermore, there is relatively high wear with this method, since the cutting edges are subject to high loads and therefore wear relatively quickly. Summary of the invention

[0010] The object of the present invention is to provide a method for producing abrasive grains that avoid the above-mentioned problems, abrasive grains produced thereby, and a method for producing a grinding tool for metal material processing, wherein the abrasive grains produced according to the present invention and the grinding tool produced by the method are used.

[0011] These objectives are solved by the method for preparing abrasive grains and the abrasive grains prepared therefrom according to the present invention, as well as the method for preparing a grinding tool for machining metal materials using the abrasive grains and the grinding tool prepared therefrom.

[0012] In the process according to the invention, the extrudates and / or intermediate particles are therefore subjected to an asymmetric energy input with respect to the geometry of the extrudates and / or intermediate particles.

[0013] The asymmetrical energy input results in an asymmetrical heating of the extrudate and / or the intermediate particles. Since the extrudate and / or the intermediate particles cannot be cooled uniformly due to the asymmetrical (i.e., non-uniform) heating, stresses occur in the extrudate and / or the intermediate particles. These stresses lead to distortions of the extrudate and / or the intermediate particles, resulting in abrasive particles with non-uniform geometry.

[0014] Compared to the methods known from the prior art, more abrasive grains can be produced in the same time, since, for example, a plurality of extruded strands can be provided. In addition, the wear in the method according to the invention is less than in the prior art, since no chip breaking device is required.

[0015] It should be noted that the technology of converting a starting mixture containing at least aluminum hydroxide into at least aluminum oxide by heat treatment has long been known. In this article, it is called the so-called "sol-gel method". In this case, a starting mixture containing at least aluminum hydroxide is used. The aluminum hydroxide can exist in different variants. In the present invention, powdered boehmite (γ-AlOOH) is preferably used. In addition, the boehmite is preferably subsequently converted into a transparent sol by adding water and mixing in a peptizing agent (such as nitric acid). Then, preferably, the reaction of forming a gel, i.e., dehydration and polymerization, is initiated by further adding an acid (such as nitric acid) or a nitrate solution. Due to the gelation, the boehmite is present in a very uniform distribution. In the subsequent step, the water that can be released is evaporated. During the subsequent heat treatment at a temperature between 400°C and 1200°C (preferably between 800°C and 1000°C), the aluminum hydroxide can be converted into the transition phase γ-Al2O3 of aluminum oxide. Under the reaction of the conversion of boehmite into aluminum oxide, nitrogen is released as a residue of acid and water. This low-temperature firing is also called calcination. In a final step, a further heat treatment can then be carried out, preferably in a pressureless manner, in the form of sintering. This step is preferably carried out at a temperature between 1200° C. and 1800° C., particularly preferably between 1200° C. and 1500° C. Depending on the starting mixture, it may occur that, in addition to aluminum oxide (usually as α-aluminum oxide), second phases such as spinel are also produced. The expression "at least converted into aluminum oxide" takes this fact into account.

[0016] "Extrusion" is a process technology in which a solid to viscous hardenable material is continuously forced out of a shaped opening under pressure. This produces a body with an open cross-section, called an extrudate.

[0017] In the present case, the cross section of the extrudate depends on the nozzle body used and is preferably rectangular, square, trapezoidal, parallelogram, triangular, teardrop-shaped, propeller-shaped or star-shaped and / or has at least one convex surface or at least one concave surface.

[0018] The method for producing abrasive grains according to the invention differs from the prior art not only in its simplicity and lower maintenance requirements and wear, but also in the fact that the shape and / or size of the intermediate grains or of the abrasive grains present after sintering can be easily and flexibly varied by replacing the nozzle body and / or by changes during cutting.

[0019] One possibility to influence or control the abrasive grain size is to feed the extrudate to the cutting process step at a variable feed rate and / or in an oscillating motion. In the case of an oscillating motion, the extrudate to be cut has a certain length.

[0020] In addition, it can also be provided that the intermediate particles produced by cutting are comminuted in a further method step before the heat treatment, preferably by a cutting device.Instead of a cutting device, other comminution devices can also be used, for example, they also crush and / or chop the intermediate particles.

[0021] Another possibility for influencing the shape and / or size of the abrasive grains is to change the consistency of the starting mixture. For this purpose, it can be provided that water, a peptizing agent (preferably nitric acid), and / or an additive, such as an acid which can also be nitric acid, and / or cobalt nitrate are added when the starting mixture is provided and / or during the extrusion of the starting mixture.

[0022] Other advantageous embodiments of the invention are also possible. It can be particularly preferably provided that the extrudate and / or the intermediate particle has a longitudinal direction and that the energy input takes place asymmetrically transversely to the longitudinal direction.

[0023] On the one hand, this promotes the distortion of the extrudate and / or the intermediate particle and, on the other hand, makes it easier to achieve an asymmetric energy input.

[0024] An advantageous embodiment of the method for producing abrasive grains also consists in that the intermediate grains produced by cutting are calcined during the heat treatment, preferably at a temperature between 400° C. and 1200° C., particularly preferably between 800° C. and 1000° C., and / or sintered, preferably at a temperature between 1200° C. and 1800° C., particularly preferably between 1200° C. and 1500° C. Furthermore, provision can be made for the intermediate grains produced by cutting to be predried during the heat treatment prior to calcination and / or sintering, preferably at a temperature between 50° C. and 350° C., particularly preferably at a temperature between 80° C. and 100° C.

[0025] As already mentioned above, protection is also sought for a method for producing a grinding tool for machining metallic materials, wherein the abrasive grain produced using the method according to the invention for producing abrasive grain is embedded in a binder, for example a ceramic binder or a synthetic resin binder. Advantageously, a porosity of 2 to 50% and / or 1.5 to 4.5 g / cm 3 Density of the abrasive.

[0026] BRIEF DESCRIPTION OF THE DRAWINGS AND SPECIFIC EMBODIMENTS

[0027] Further details and advantages of the present invention are explained in more detail below in conjunction with the accompanying drawings based on the accompanying drawings description. In it is shown:

[0028] Figure 1 According to a first exemplary embodiment of the method for producing abrasive grains according to the present invention,

[0029] Figure 2 According to a second exemplary embodiment of the method for producing abrasive grains according to the present invention,

[0030] Figure 3 An embodiment of the nozzle body is shown in a sectional view,

[0031] Figure 4a -1 a schematic diagram of the outlet of the nozzle channel of a nozzle body according to the invention,

[0032] Figure 5a / 5b Photograph of abrasive grains prepared according to a preferred embodiment of the preparation method of the present invention,

[0033] Figure 6a is a photograph of abrasive grains prepared according to one embodiment of the method for preparing abrasive grains of the present invention; and

[0034] Figure 6b is a front view photograph of abrasive grains prepared according to one embodiment of the method for preparing abrasive grains of the present invention.

[0035] exist Figure 1 In the first exemplary embodiment of the method for producing abrasive grains according to the invention shown, a starting mixture 2 is provided by introducing boehmite 13, water 14, nitric acid 15 and an additive 16, such as cobalt nitrate, into a mixer 17, wherein the mixer 17 is essentially composed of a mixing container 17a and a rotating unit 17b arranged therein.

[0036] The starting mixture 2 provided in this way is then fed to an extrusion device 18. It can be provided that the extrusion device 18 is arranged on a platform 19 which can be in a swinging motion. This swinging motion is Figure 1 It is schematically indicated by double arrows.

[0037] The extrudate 3 leaving the extrusion device 18 has a specific cross-sectional shape determined by the nozzle body 6 .

[0038] In this first embodiment, the device 8 for asymmetric energy input is arranged directly after the nozzle body 6 and performs an asymmetric energy input on the intermediate particles 4. However, the device 8 for asymmetric energy input can also be arranged at other locations, for example in the region of the belt guide 20.

[0039] The asymmetrical energy input by means of the device 8 for asymmetrical energy input can be carried out in particular in the following way:

[0040] - contact with at least one heating device, preferably wherein the at least one heating device is of platform-like construction at least in regions, and / or

[0041] - introducing an electric current into the extrudate 3 and / or the intermediate particle 4, wherein at least a part of the energy of the electric current is converted into heat via the electrical resistance of the extrudate 3 and / or the intermediate particle 4, and / or

[0042] - convection, preferably by fan heater means, and / or

[0043] - the effect of electromagnetic radiation, preferably wherein the electromagnetic radiation has at least one wavelength between 780 nm and 1 mm or between 380 nm and 100 nm, and / or is emitted by at least one laser or radiant heater, and / or

[0044] - Induction, in which ferromagnetic particles are added to the starting mixture 2 to be extruded.

[0045] The device 8 for asymmetrical energy input can also be designed in the form of drums and / or rollers.

[0046] Furthermore, the device 8 for asymmetrical energy input can in principle be arranged at any desired location between the extrusion device 18 and the sintering furnace 23 .

[0047] The extrudate 3 is then cut by a separating device 10 designed as a rotating or oscillating knife. It can also be provided that the cutting into intermediate particles is carried out by means of at least one laser or at least one water jet cutter or at least one plasma cutter, preferably wherein the extrudate 3 to be cut by means of at least one laser or at least one water jet cutter or at least one plasma cutter is placed on a conveyor before cutting.

[0048] The intermediate particles 4 produced by cutting the extrudate 3 are conveyed to a predrying device 21 by means of a belt conveyor 20 .

[0049] The predried intermediate particles 4 are then transported to a calcining furnace 22, where the intermediate particles 4 are calcined.

[0050] After calcination, a sintering furnace 23 follows, in which the intermediate particles 4 are sintered into abrasive particles 5. Figure 5a and 5b The shape and / or size of the abrasive particles 5 produced in this way are discussed in more detail.

[0051] Instead of three spatially separate, sequential heat treatment devices: predrying device 21 , calcining furnace 22 and sintering furnace 23 , it is also possible to use an integrated device for heat treatment, for example a tunnel furnace, which has temperature zones that can be controlled independently of one another.

[0052] The sintered abrasive grains 5 are positioned on a belt guide 24. During the transport through the belt guide 24, the abrasive grains 5 produced by sintering are cooled.

[0053] The produced abrasive grains 5 are then transferred to a storage device 25 and can be used for further processing, for example to provide a method for producing an abrasive tool for machining metallic materials.

[0054] Figure 2 A second exemplary embodiment of the method according to the invention is shown. This exemplary embodiment differs essentially only in the position of the device 8 for asymmetrical energy input and the separation device 10.

[0055] It can be seen here that the extrusion device 18 is rotated and the extrudate 3 emerges from the nozzle body 6 in the form of a plurality of extrudate strands 9 in the direction of gravity acceleration. The device 8 for asymmetric energy input is arranged here so that the extrudate strands 9 that sag due to gravity are subjected to an asymmetric heat input. Therefore, the extrudate 3, rather than the intermediate particles 4, is subjected to an asymmetric heat supply.

[0056] The extrudate 3 subjected to asymmetrical heating is then placed on a belt guide 20 and cut by a separating device 10 .

[0057] The remainder of the method according to the invention according to the second exemplary embodiment is similar to Figure 1 The first exemplary embodiment shown operates similarly.

[0058] Figure 3 An exemplary embodiment of a nozzle body 6 is shown in cross section. It can be seen that the nozzle channel 7 is substantially cylindrical and has the same diameter as the inlet 7a.

[0059] In accordance with Figure 3 In the nozzle body 6 of FIG. 1 , the starting mixture 2 to be extruded enters the nozzle body 6 via the inlet 7a and experiences an increase in its density and / or its velocity via the outlet 7b.

[0060] The starting mixture 2 to be extruded then emerges from the nozzle body 6 through the outlet 7b as extrudate 3. The outlet 7b in this exemplary embodiment is similar in shape to a three-blade rotor.

[0061] according to Figure 3 The nozzle body 6 can be produced by an additive manufacturing process or by at least one material removal manufacturing process.

[0062] In the case of material removal production, it can be provided, for example, that blind holes are produced in the metal blank. The outlets 7b can then be cut into these blind holes by laser cutting. However, any other suitable production method can also be provided.

[0063] Figures 4a to 4l A schematic diagram of an outlet 7b of a nozzle channel 7 of a nozzle body 6 is shown. It can be seen that the outlet 7b can have the most diverse geometries. Figures 4a to 4l The outlet 7b shown in FIG. 5 is intended only as an example; in principle, all suitable geometries can be used for the outlet 7b.

[0064] The shape of the outlet 7 b also determines the cross-sectional shape of the extrudate 3 , and thus determines the cross-sectional shape of the intermediate particles 4 and the abrasive particles 5 .

[0065] Figure 5a and 5b A photograph of abrasive grains produced according to the method of the invention for producing abrasive grains 5 is shown. The photographs show the size of the abrasive grains 5 on the one hand and the shape of the abrasive grains 5 on the other hand. It can be seen that most of the abrasive grains 5 from the sample photographed have a twist angle of 90° to 180°. However, it is particularly possible to provide abrasive grains 5 with a twist angle of up to 360°.

[0066] Figure 6a A photograph of abrasive grains prepared by the method for preparing abrasive grains 5 according to the present invention is shown, which have Figure 3 Embodiment of a produced nozzle body The photographs show, on the one hand, the size of the abrasive grains 5 and, on the other hand, their shape.

[0067] It can be seen that most of the abrasive grains 5 from the sample recorded have a twist angle of 90° to 180°. However, it is particularly possible to provide abrasive grains 5 with a twist angle of up to 360°.

[0068] Figure 6b A photograph of abrasive grains prepared by the method for preparing abrasive grains 5 according to the present invention is shown in front view, having a Figure 3 The size of the abrasive grains and their cross-section can be seen in the photo.

[0069] Tags list:

[0070] 1. Process

[0071] 2 Starting mixture

[0072] 3 Extrudate

[0073] 4 Intermediate particles

[0074] 5 Abrasive

[0075] 6 Nozzle body

[0076] 7 nozzle channels

[0077] Entrance 7a

[0078] Exit 7b

[0079] 7c Funnel-shaped cross section

[0080] 7d twisted section

[0081] 8. Devices for asymmetric energy input

[0082] 9 Extrusion Strip

[0083] 10 Separation device

[0084] 11Transmission Device

[0085] 12 Abrasives

[0086] 13 Boehmite

[0087] 14 Water

[0088] 15 nitric acid

[0089] 16 Additives

[0090] 17. Blender

[0091] 17a Mixing tank

[0092] 17b Rotating unit

[0093] 18 Extrusion device

[0094] 19 Platform

[0095] 20 belt guide device

[0096] 21 Pre-drying device

[0097] 22 Calcination furnace

[0098] 23 Sintering furnace

[0099] 24 belt guide device

[0100] 25 storage devices.

Claims

1. A method for preparing abrasive particles (5), comprising the following process steps: i. providing a starting mixture (2) containing at least aluminum hydroxide, which can be converted into at least aluminum oxide by heat treatment, ii. extruding the starting mixture into an extrudate (3), iii. cutting the extrudate (3) into intermediate particles (4), and iv. heat treatment of the intermediate particles (4), wherein the intermediate particles (4) are transformed into abrasive particles (5) containing aluminum oxide, characterized in that The extrudate (3) and / or the intermediate particle (4) are subjected to an asymmetric energy input with respect to the geometry of the extrudate (3) and / or the intermediate particle (4), resulting in an abrasive particle with a non-uniform geometry.

2. A method according to claim 1, wherein the asymmetric energy input is carried out at at least one outlet (7b) of at least one nozzle body (6) of an extrusion device (18) and / or on at least one belt guide device (20) and / or in at least one device (8) for asymmetric energy input.

3. The method according to claim 2, wherein the at least one device (8) for asymmetric energy input comprises at least one drum and / or roller.

4. A method according to claim 2, wherein the asymmetric energy input is carried out at at least one outlet (7b) of at least one nozzle body (6) of the extrusion device (18), wherein at least one extruded strip (9) drooping under the influence of gravity is subjected to the asymmetric energy input.

5. The method according to claim 1, wherein: The asymmetric energy input - by contact with at least one heating device, and / or - by introducing an electric current into the extrudate (3) and / or the intermediate particle (4), wherein at least a portion of the energy of the electric current is converted into heat via the electrical resistance of the extrudate (3) and / or the intermediate particle (4), and / or - by convection, and / or - through the action of electromagnetic radiation, and / or - by induction, in which ferromagnetic particles are added to the starting mixture to be extruded (2).

6. The method according to claim 5, wherein the at least one heating device is of platform-like construction at least in regions.

7. The method of claim 5, wherein the convection is performed by a fan heater device.

8. The method of claim 5, wherein the electromagnetic radiation has at least one wavelength between 780 nm and 1 mm or 380 nm and 100 nm.

9. The method of claim 5, wherein the asymmetric energy input is emitted by at least one of a laser or a radiant heater.

10. The method according to claim 1, wherein the extrudate (3) and / or the intermediate particle (4) has a longitudinal direction and the asymmetric energy input is performed transversely to the longitudinal direction.

11. The method according to claim 1, wherein during the extrusion process the starting mixture (2) is extruded through at least one nozzle body (6) having at least one nozzle channel (7). 12 . The method according to claim 11 , wherein the at least one nozzle channel ( 7 ) is a plurality of nozzle channels ( 7 ) extending in parallel.

13. The method according to claim 11, wherein the at least one nozzle body (6) is produced by an additive manufacturing process.

14. The method according to claim 11, wherein the at least one nozzle channel (7) of the at least one nozzle body (6) has an inlet (7a) and an outlet (7b), the starting mixture (2) entering the at least one nozzle channel (7) through the inlet (7a), and the extrudate (3) leaving the at least one nozzle channel (7) via the outlet (7b).

15. The method according to claim 14, wherein the inlet (7a) is circular or elliptical.

16. The method according to claim 14, wherein the outlet (7b) is rectangular, square, triangular, teardrop-shaped or star-shaped and / or has at least one convex surface or at least one concave surface.

17. A method according to claim 11, wherein the at least one nozzle channel (7) has a funnel-shaped portion (7c) adjacent to the inlet (7a), the diameter of which decreases in the direction of the outlet (7b), thereby increasing the pressure, density and / or speed of the starting mixture (2) to be extruded.

18. The method according to claim 1, wherein the extrudate (3) is divided into intermediate particles (4) by a separation device (10).

19. The method according to claim 18, wherein the extrudate (3) is divided into intermediate particles (4) by means of at least one laser and / or at least one water jet cutter and / or at least one plasma cutter.

20. The method according to claim 18, wherein the separating device (10) is a rotating or oscillating knife.

21. The method according to claim 18, wherein the extrudate (3) to be cut by the separating device (10) is placed on a conveyor before cutting.

22. The method according to claim 1, wherein the intermediate particles (4) produced by cutting during the heat treatment - calcined, and / or - Sintered.

23. The method according to claim 22, wherein the intermediate particles (4) are calcined at a temperature between 400°C and 1200°C.

24. The method according to claim 22, wherein the intermediate particles (4) are calcined at a temperature between 800°C and 1000°C.

25. The method according to claim 22, wherein the intermediate particles (4) are sintered at a temperature between 1200°C and 1800°C.

26. The method according to claim 22, wherein the intermediate particles (4) are sintered at a temperature between 1200°C and 1500°C.

27. The method according to claim 22, wherein the intermediate particles (4) produced by cutting are pre-dried during heat treatment prior to calcination and / or sintering.

28. The method according to claim 27, wherein the pre-drying is carried out at a temperature between 50°C and 350°C.

29. The method of claim 27, wherein the pre-drying is performed at a temperature between 80°C and 100°C.

30. The method according to claim 1, wherein the abrasive grain (5) present after the heat treatment is cooled.

31. The method according to any one of claims 1 to 30, wherein water (14), a peptizing agent (15), and / or an additive (16) are added when providing the starting mixture (2) and / or when extruding the starting mixture (2).

32. The method according to claim 31, wherein the peptizing agent (15) is nitric acid.

33. The method according to claim 31, wherein the additive (16) is an acid and / or cobalt nitrate.