Asphalt membrane with biodegradable binder

By consolidating the nonwoven carrier without crosslinking agent, the nonwoven carrier is solved by consolidating the nonwoven carrier with starch and polyvinyl alcohol aqueous binder in the prior art, the problem of insufficient mechanical characteristics and dimensional stability of the asphalt membrane carrier at high temperatures in the prior art is solved, and high efficiency and environmental protection are achieved Asphalt membrane production, suitable for building applications.

CN115279961BActive Publication Date: 2024-11-05CARL FREUDENBERG KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180021007.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-04
Filing Date
2021-03-25
Publication Date
2024-11-05
Estimated Expiration
2041-03-25

AI Technical Summary

Technical Problem

The nonwoven carriers used in the asphalt film in the prior art lack mechanical properties and dimensional stability at high temperatures, and commonly used adhesives contain crosslinking agents and expensive non-natural additives, which are difficult to meet the high quality standards for building applications.

Method used

Using starch and polyvinyl alcohol without crosslinking agents as binders to consolidate the nonwoven carriers through aqueous adhesives, providing a simple, reliable and inexpensive solution, with the adhesive composition including only starch and Polyvinyl alcohol, suitable for the production of asphalt films.

Benefits of technology

It achieves high mechanical properties and dimensional stability of nonwoven carriers at room temperature and high temperatures, especially at 180°C, and is suitable for automated production of bitumen films, and the adhesive is biodegradable and meets environmental and safety requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004647910850000191
    Figure GDA0004647910850000191
  • Figure GDA0004647910850000201
    Figure GDA0004647910850000201
  • Figure GDA0004647910850000211
    Figure GDA0004647910850000211
Patent Text Reader

Abstract

The subject matter of the present invention relates to a nonwoven carrier, wherein the nonwoven contains organic polymer fibers and is consolidated with an aqueous binder, wherein the binder contains: (a) starch; (b) polyvinyl alcohol, which may contain up to 5 mol.% of other monomer units, wherein (c) the binder contains no crosslinking agent, and (d) the binder contains no filler. The subject matter of the present invention also relates to the use of the nonwoven carrier, a production method, a bituminous membrane and a building material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a nonwoven carrier, comprising a nonwoven bonded with an adhesive, wherein the adhesive comprises starch and polyvinyl alcohol, wherein the adhesive does not contain a crosslinking agent or a filler. The subject matter of the invention also relates to the use of the nonwoven carrier, a production method, an asphalt membrane and a building material. Background Art

[0002] Bitumen membranes with waterproofing and shielding properties are used in building applications, in particular as roofing materials. Bitumen membranes comprise a textile carrier impregnated with bitumen. The bitumen is applied to the textile carrier in a molten bitumen bath at about 180° C. to 200° C., then cooled and cured. The main function of the carrier is to give the bitumen membrane mechanical stability, in this respect especially mechanical resistance and dimensional stability, and to "hold the bitumen together".

[0003] The textile fabric can be a nonwoven, which is consolidated with aqueous adhesives such as acrylic acid, SBR, polyurethane or natural polymer adhesives. The adhesive should increase the mechanical resistance and dimensional stability of the nonwoven. Optionally, the stability of the nonwoven is further increased by reinforcements such as glass fiber yarns or scrims. The nonwoven is impregnated with an aqueous adhesive solution, then dried and cured, thereby obtaining a nonwoven carrier for asphalt impregnation. The nonwoven carrier and asphalt film are usually provided in the form of relatively thin flexible sheets, usually with a thickness of several millimeters, and the flexible sheet can be rolled up and unfolded.

[0004] Such adhesive-consolidated nonwoven carriers for bituminous membranes should have special properties that make them suitable for the production of bituminous membranes. Ideally, the nonwoven carrier should not shrink or stretch in size when subjected to temperature or mechanical forces. It should easily follow all stresses during the asphaltening process (at about 180° C. to 200° C.), thereby having a high initial modulus and high dimensional stability (low deformation). Further, the nonwoven carrier should have high tear resistance and elongation at break (determined by tensile tests at room temperature). This requirement is important because it determines the technical specifications of the membrane, such as tear resistance and elongation at break.

[0005] Bitumen membranes for construction applications are produced in large quantities. Therefore, they are usually produced on a large scale in an automated production line, where a roll of nonwoven carrier is continuously unrolled and guided through a molten bitumen bath. Subsequently, the product is cooled until the bitumen solidifies and the bitumen membrane product is rolled up. In such processes, it is important that the nonwoven carrier is dimensionally stable and therefore deforms as little as possible. When the nonwoven carrier is processed and guided through a hot bath, the nonwoven carrier should not deform at about 180°C. Otherwise, the sheet material may be damaged or an uneven product may be obtained. The adhesive must remain stable at around 180°C. However, the properties of many polymer adhesives deteriorate at high temperatures, thereby reducing the bond strength and nonwoven stability. Therefore, many adhesive-bonded nonwoven carriers that may have mechanical stability at low temperatures are not suitable for producing bitumen membranes. Overall, it is generally expected that nonwoven carriers can produce bitumen membranes in an efficient, automated, large-scale process without damaging the material.

[0006] Further, the bituminous membrane must meet high quality standards for construction applications. Typically, it is used as a building and roof membrane, such as a sarking membrane (sometimes referred to as a lining membrane), a shielding membrane or a waterproof membrane. In such applications, the bituminous membrane must protect the roof and building from moisture for many years. Therefore, it is very important that the bituminous membrane is uniform and free of defects such as cracks and punctures, or even structural irregularities that may cause damage over time. Even small defects may lead to moisture leakage or other problems at the building location over a long period of time. Therefore, relatively thin bituminous roof membranes and the nonwoven carrier embedded therein should have good mechanical properties and high dimensional stability so that they can be easily applied to the building or roof location without damage. High stability is also required after being applied to the construction location, because the building location or roof may be subject to stress and strain over many years.

[0007] In general, it is desirable that such nonwoven carriers for asphalt membranes be flexible while having good mechanical properties and high dimensional stability at hot and cold temperatures. Even a small improvement in the mechanical stability of the nonwoven carrier at hot or cold temperatures can significantly reduce damage, resulting in a more precise and reliable material.

[0008] In the art, various synthetic adhesives are used to consolidate nonwovens, such as acrylic acid, SBR or polyurethane polymers. For environmental reasons, it is also desirable to use natural and biodegradable materials. Therefore, the art has described adhesives based on starch for consolidating the nonwoven carrier for asphalt film. Starch can be obtained in a large number and is relatively cheap as an adhesive. Adhesives based on conventional starch for nonwovens are usually provided in the form of a mixture with another adhesive polymer. Such compositions also include a crosslinking agent covalently linked to the adhesive molecule, thereby forming a three-dimensional polymer matrix. It is also assumed in the art that high dimensional stability is achieved by crosslinking polymer adhesives.

[0009] EP 0 354 023 A2 relates to an adhesive composition for a fiber mat, wherein the adhesive comprises starch, a starch crosslinker and an anti-wicking agent. The crosslinker may be a melamine formaldehyde or urea glyoxal condensate. The adhesive may comprise a polymer strength additive such as polyvinyl alcohol or an acrylic polymer. The anti-wicking agent is typically a surfactant.

[0010] WO 2006 / 120523 A1 discloses a curable aqueous adhesive composition comprising polyvinyl alcohol, starch or sugar, a multifunctional crosslinking agent and a catalyst. It is suggested to use the adhesive to impregnate a glass fiber product.

[0011] WO 2015 / 084372 A1 discloses an aqueous adhesive for impregnating nonwovens, the aqueous adhesive comprising a polyol in colloid form such as starch and a crosslinking agent. The adhesive may contain another polymer. The crosslinking agent is a multifunctional small molecule, such as glyoxal or citric acid.

[0012] WO2019 / 050439A2 relates to a thermal and acoustic insulation material made of mineral fibers. The product is a mat made of mineral fibers and a binder, and the mat is cross-linked with heavy metals or boron compounds and heavy metal salts.

[0013] DE 1 619 127 relates to a method for impregnating fiber products with resins. In a first step, the fiber substrate is impregnated with an intermediate first binder (A), which is washed off after subsequent impregnation with binder (B). The intermediate product is unstable and unsuitable for producing bituminous membranes.

[0014] EP 3 299 514 A1 relates to textile fabrics impregnated with a binder system comprising ≥30% polyvinyl alcohol, ≤70% starch, a crosslinking agent, fillers and additives. However, no specific binder compositions or working examples are disclosed.

[0015] The starch-based adhesive compositions and nonwovens consolidated therewith described in the art can still be improved. Usually, adhesive compositions require various additives and are therefore relatively complex. All concrete adhesive compositions contain a crosslinking agent and usually also contain a catalyst for controlling the crosslinking reaction. The reaction between starch, polyvinyl alcohol and the crosslinking agent must be initiated, controlled and monitored. Insufficient crosslinking degree may result in low product stability, while excessive crosslinking may result in excessive rigidity of the product. Therefore, it is generally desirable to consolidate such nonwoven carriers with simpler and more reliable adhesive systems.

[0016] Further, the mechanical properties of nonwoven carriers impregnated with such adhesives can still be improved. There is a great need for adhesive-consolidated nonwoven carriers that are flexible and have good mechanical properties at cold and hot temperatures; and are therefore suitable for the production of bituminous membranes. However, most prior art documents do not address this issue, especially the mechanical properties at high temperatures.

[0017] Another problem is that known binders for nonwoven fabrics often contain formaldehyde-based crosslinking agents, such as melamine formaldehyde. Aldehyde-based binders, such as those derived from formaldehyde and glyoxal, are undesirable for safety and environmental reasons, since they can cause health problems.

[0018] It is also a problem that known adhesive compositions are often relatively expensive, as the components or additives are not readily available in large quantities. As bituminous membranes are industrial products, used in large quantities in construction applications, lower cost adhesives are desirable.

[0019] Another problem with known adhesive compositions is that they contain components or additives that are not obtainable from natural sources and / or are not biodegradable. It would be desirable to provide readily available adhesive compositions that are obtainable from natural sources or are biodegradable.

[0020] The underlying problem of the present invention

[0021] The underlying problem of the present invention is to provide nonwoven fabrics, uses, methods and asphalt membranes that overcome the above problems. The specific problem is to provide a nonwoven carrier that is impregnated and consolidated with an adhesive in a relatively simple, efficient and inexpensive manner. The adhesive composition should be provided and processed simply and reliably. The adhesive should not contain formaldehyde and / or should be obtained from a natural source as far as possible or be biodegradable. In general, the nonwoven carrier should be produced sustainably as far as possible.

[0022] A further problem of the present invention is to provide a nonwoven carrier bonded with an adhesive which is very suitable for the production of bituminous membranes. The nonwoven carrier should have good mechanical properties at room temperature, in particular with regard to maximum tensile strength and toughness before breaking. In addition, the nonwoven carrier should have high dimensional stability at elevated temperatures of about 180° C. Therefore, the nonwoven carrier should be suitable for the production of bituminous membranes in roll form with standard machines in an automated process. Summary of the invention

[0023] The subject matter of the invention is a nonwoven carrier for a bituminous membrane, wherein the nonwoven contains organic polymer fibers and is bonded with an aqueous binder, wherein the binder contains

[0024] (a) starch,

[0025] (b) polyvinyl alcohol, which may contain up to 5 mol.% of other monomer units, wherein

[0026] (c) the adhesive does not contain a cross-linking agent, and

[0027] (d) The adhesive contains no filler.

[0028] The subject matter of the invention also relates to a method for producing and the use of a nonwoven carrier, a bituminous membrane and a building material. Further embodiments are disclosed in the description.

[0029] The nonwoven carrier comprises a nonwoven consolidated with an adhesive. According to ISO 9092, a nonwoven is a sheet of staple fibers or continuous filaments which have been formed into a web by any means and bonded together by any means except weaving or knitting. Preferably, the fibers forming the nonwoven are randomly oriented. Preferably, they are bonded by friction, cohesion and / or adhesion.

[0030] Nonwoven carriers are substrates for the production of bituminous membranes. Bituminous membranes are commonly used in construction applications, especially roofing applications. In a typical production process, the nonwoven carrier is impregnated with molten bitumen.

[0031] The nonwoven carrier of the present invention that is consolidated with an adhesive is porous. Preferably, the void ratio of the nonwoven carrier and / or the nonwoven before the adhesive impregnation is between 60% and 95%, more preferably between 75% and 93%, especially between 80% and 90%. The porosity can be calculated by the weight and density of the product and the components. Therefore, the molten asphalt can penetrate the holes from one side to the other side of the nonwoven carrier sheet, so that a compact and stable composite material can be obtained after the asphalt is solidified. Preferably, the average pore size is between 50 μm and 300 μm, preferably between 80 μm and 200 μm, preferably determined by ISO15901-1:2016.

[0032] The nonwoven carrier is a sheet material. Preferably, the nonwoven carrier is flexible and / or rollable. The subject matter of the present invention also relates to a roll of a nonwoven carrier and / or an asphalt membrane. Such a roll can be easily unrolled and rolled up again by the user. The flexibility and roll form of the nonwoven carrier are conducive to efficient processing in an automated, continuous process. The flexibility and roll form of the asphalt membrane are conducive to application and processing at building locations, etc.

[0033] The nonwoven carrier is consolidated with an aqueous binder. This is a solution or dispersion of polymers and optionally additives in water, which is usually applied to the nonwoven by impregnation, drying and curing in a bath and binds the nonwoven fibers together. The nonwoven binder enhances the stability of the nonwoven.

[0034] The adhesive of the present invention comprises starch and polyvinyl alcohol. The art has described nonwoven adhesives comprising starch and polyvinyl alcohol. However, the adhesive according to the present invention is different because it does not comprise a crosslinking agent. Surprisingly, it was found that an adhesive comprising starch and polyvinyl alcohol as a structural polymer without a crosslinking agent is suitable for producing a nonwoven carrier for asphalt membranes, which meets the high requirements for mechanical resistance and dimensional stability at cold and even at high temperatures of about 180°C. Unexpectedly, in the absence of a crosslinking agent, such nonwoven carriers have sufficient stability even at high temperatures, which is used in conventional adhesives to form a three-dimensional matrix of covalently linked adhesive polymers. Even more surprisingly, it was also found that an adhesive without a crosslinking agent can have even better mechanical properties at cold and hot temperatures, especially better dimensional stability than the corresponding adhesive with a crosslinking agent.

[0035] As used herein, the term cross-linking agent refers to a compound specifically added to an aqueous adhesive and forming a covalent bond of an adhesive polymer in an adhesive composition during consolidation. According to the present invention, there is no such compound that can form a covalent bond between starch and polyvinyl alcohol molecules. Polyvinyl alcohol and starch are polyols characterized in that the polyols have repeated hydroxyl functional groups on the polymer backbone. In the art, the cross-linking agent for an adhesive comprising starch and / or polyvinyl alcohol is typically a compound with two or more functional groups, which can react with hydroxyls, typically carboxyls, but can also be amines or aldehydes. Starch can also be chemically modified, for example, by partial oxidation, in which some of the hydroxyls are converted into carboxyls. Such modified starch can be cross-linked with a cross-linking agent having hydroxyls and carboxyls. The aqueous adhesive used according to the present invention does not include a cross-linking agent compound, which covalently links a specific starch to polyvinyl alcohol during adhesive consolidation.

[0036] The water-based adhesive of the present invention does not include a crosslinking agent. Typical crosslinking agents for corresponding adhesives in the art are formaldehyde or formaldehyde resins, such as urea-formaldehyde resins, melamine-formaldehyde resins or acetone-formaldehyde resins, glyoxal or glyoxal resins, urea or urea resins, or non-polymeric polycarboxylic acids or non-polymeric polycarboxylic acid anhydrides comprising two, three or more carboxyl groups, such as citric acid. In a preferred embodiment, the water-based adhesive does not include other compounds, and the other compounds include two or more functional groups, which are used for crosslinking specific starch and polyvinyl alcohol in the adhesive, particularly for the hydroxyl groups of crosslinked starch and polyvinyl alcohol; such as the functional groups selected from the group consisting of the following: carboxyl, isocyanate group, amine group, aldehyde group, epoxy group or ketone group. The adhesive does not include a crosslinking agent in the form of heavy metals or borate or compounds yet. Preferably, the adhesive does not include a catalyst, especially a crosslinking catalyst, because no catalytic chemical reaction is required.

[0037] Preferably, the nonwoven is not consolidated with an aqueous adhesive in such a way that the adhesive is crosslinked. Under standard conditions, the adhesive without a crosslinking agent does not crosslink starch and polyvinyl alcohol, under which the nonwoven is impregnated, dried and the adhesive is cured. However, under specific harsh conditions, at least some degree of crosslinking may occur despite the absence of a crosslinking agent. Therefore, it is preferred that the nonwoven carrier is not subjected to conditions that may cause crosslinking during or after the adhesive consolidation. For example, it is preferred that very high or very low pH, pressure, temperature and / or water depletion are not adjusted; the aqueous adhesive does not contain a highly reactive additive; or the nonwoven carrier is not subjected to a highly reactive environment such as reactive radiation or plasma.

[0038] Preferably, in the nonwoven carrier of the present invention, starch and polyvinyl alcohol are not cross-linked, or at least not cross-linked substantially. In this respect, "substantially" means that although the conditions have been adjusted so that cross-linking should not occur, for example, due to impurities or structural anomalies of raw materials, a small amount of covalent bonds that are inevitable and negligible may be formed. For example, substantially not cross-linked can mean that starch and / or polyvinyl alcohol molecules are covalently bonded to each other less than 2% or less than 0.5%. The amount of cross-linking can be determined by removing adhesive, molecular analysis (for example, by MALDI TOF) and comparing with aqueous adhesive solutions from the nonwoven carrier.

[0039] The starch may be a modified starch or a native starch. Native starch is obtained directly from a natural source without any physical or chemical treatment. Preferably, the source of the modified or native starch is natural. Preferably, the source is a plant, preferably a vegetable. Preferably, the starch source is a tuber such as potato, cassava, arrowroot, sweet potato, a cereal such as wheat, corn (corn / maize), rye, rice, barley, millet, oats, sorghum, a chestnut, acorn, bean, pea and other legumes, banana or plant pulp, for example, fruits such as sago palm. Preferably, the starch is corn starch, which is preferably modified.

[0040] In a preferred embodiment, starch is not native starch. Therefore, starch is modified starch. It is highly preferred that starch is physically modified and / or chemically modified. Modified starch can be obtained by physical and / or chemical treatment of native starch, usually to change its characteristics. According to the present invention, it is found that modified starch can impart high stability to nonwoven carriers. On the contrary, in the absence of a crosslinking agent, it may be more difficult to provide a uniform adhesive with native starch, which can result in low stability of the nonwoven carrier.

[0041] In a preferred embodiment, the starch is chemically modified. In this regard, the term "chemically modified" refers to partially hydrolyzed starch and starch with chemically modified side chains and / or functional groups. For example, the chemically modified starch can be alkali-modified starch, bleached starch, oxidized starch, acetylated starch, hydroxypropylated starch, starch ether, hydroxyethyl starch, cationic starch or carboxymethylated starch.

[0042] In other embodiments, the starch may be a dextrin, such as maltodextrin or cyclodextrin. Dextrins are low molecular weight carbohydrates obtained by starch hydrolysis, characterized by a dextrose equivalent of between 3 and 20. In another embodiment, the starch is not a dextrin. Since the molecular weight of dextrins is relatively low, it may be preferred to use starches with higher molecular weights to obtain a highly stable product.

[0043] In a preferred embodiment, the chemically modified starch is a partially hydrolyzed starch. Partially hydrolyzed starches are characterized by shorter polysaccharide chain lengths compared to corresponding native starches. Partially hydrolyzed starches have been found to impart advantageous properties to nonwoven carriers.

[0044] In one embodiment, the average molecular weight of the starch may be between 500 g / mol and 25,000 g / mol, in particular between 2,500 g / mol and 20,000 g / mol, as determined by MALDI-TOF.

[0045] Preferably, starch, especially chemically modified starch, does not contain chemically modified side chains, i.e. hydroxyl groups that have been converted into other functional groups by chemical reaction. Preferably, starch contains hydroxyl groups as its starch precursor from natural sources. Native starch, physically modified and partially hydrolyzed starch have a characteristic structure, wherein all functional groups on the polymer backbone are hydroxyl groups. In these starches, the amount of other functional groups can be ignored, for example, less than 2%, less than 0.5% or less than 0.2% of total hydroxyl groups and / or total non-terminal hydroxyl groups. It is found that when starch hydroxyl groups are not chemically modified, the stability of nonwoven carriers at cold and hot temperatures can be particularly high.

[0046] In a preferred embodiment, the average size of the starch particles in the aqueous adhesive dispersion is at least 0.1 μm, preferably at least 1 μm, more preferably at least 2 μm or at least 5 μm. The average size can be in the range of 0.1 μm to 50 μm, preferably 1 μm to 50 μm, especially between 5 μm and 25 μm. The average particle size can be determined by dynamic light scattering (DLS), for example according to ISO 22412:2017. In this regard, the term "starch particles" refers to observed starch aggregates, which may also contain some PVOH. It is found that such relatively high particle size can be associated with the high dimensional stability of the nonwoven carrier at high temperatures and the higher mechanical resistance at low temperatures.

[0047] As determined according to ISO 2555 at a concentration of 25 wt.% and 23°C, the starch may have a viscosity of 50 mPa*s to 800 mPa*s, preferably 150 mPa*s to 600 mPa*s, or more preferably 250 mPa*s to 600 mPa*s. The starch viscosity may be at least 50 mPa*s, preferably at least 150 mPa*s, or more preferably at least 250 mPa*s. It was found that if the viscosity of the starch is adjusted accordingly, the mechanical stability of the nonwoven carrier at cold and hot temperatures can be significantly improved. Without being bound by theory, it was found that viscosity may be a more suitable parameter for selecting the type of starch in the adhesive composition than molecular weight, because viscosity depends not only on molecular weight, but also on other properties, such as the three-dimensional structure of the starch molecule.

[0048] Starch is a polysaccharide, mainly composed of amylose and / or amylopectin. In a preferred embodiment, the ratio of amylose in the starch is between 10% and 50%, more preferably between 15% and 30% (dry weight, relative to the total amount of amylose and amylopectin). It is found that starches such as corn starch, which contain a relatively high amylopectin content, can impart high dimensional stability to the nonwoven carrier.

[0049] In a preferred embodiment, the starch is of the type to be cooked. Preferably, the starch is insoluble in water and / or will not pregelatinize at 23°C. Preferably, when 5wt.% of starch is added to cold water and stirred for 2 minutes, the starch is insoluble. Starch is commercially available in soluble or insoluble form. For various practical and industrial applications, soluble starches such as pregelatinized starch are more convenient to use. Soluble starch can be easily dissolved in water at low temperatures. In the starch industry, natural starch is made soluble by physical treatments such as heating, mechanical shearing, drying and grinding. Soluble starch can be provided in the form of a dry powder, which is instantly soluble in cold water and has thickening / gelling ability. Pregelatinized soluble starch particles show a lack of birefringence and retain little if any of the original natural granular structure. According to the present invention, it is found that the type starch to be cooked can provide high stability for nonwoven carriers at cold and hot temperatures. Since the starch to be cooked cannot be simply dissolved in cold water, the adhesive of the present invention should be pretreated before being applied to the nonwoven. Typically, the pretreatment comprises heating and stirring, for example heating to at least 80° C., preferably at least 90° C. After cooling, the homogeneous starch dispersion obtained can be added to the adhesive.

[0050] Preferably, the starch is physically modified. The starch may be subjected to a physical treatment, such as heat and / or mechanical shearing, which may change the physical structure. Here, if no chemical reaction such as cleavage of polysaccharide chains occurs, the modification is considered to be physical. Physical modification may make the starch more uniform, which may improve the adhesive properties.

[0051] In a highly preferred embodiment, the starch is a partially hydrolyzed starch from a natural source, the starch preferably comprising 10 to 50% amylose (dry weight, relative to the total amount of amylose and amylopectin) and having an average molecular weight of between 1000 g / mol and 2500 g / mol, and / or an average size of the starch particles in the starch dispersion and / or the aqueous adhesive dispersion of at least 0.1 μm, preferably at least 1 μm, and / or a viscosity of at least 150 mPa*s, preferably at least 250 mPa*s, determined at a concentration of 25 wt.% at 23° C. according to ISO 2555. It was found that when starches having such properties are used, the stability of the nonwoven carrier at high temperatures can be particularly high.

[0052] In another embodiment, the starch is a chemically modified starch, wherein the functional groups are chemically modified. The hydroxyl groups of the starch substrate can be at least partially converted into different functional groups, for example by etherification, esterification, amidation or oxidation. Chemically modified starches include starch esters such as xanthates, acetates, phosphates, sulfates, nitrates; starch ethers such as methyl ethers or ethyl ethers, nonionic starch ethers, anionic starch ethers or cationic starch ethers; and oxidized starches such as carboxylated starches. In a preferred embodiment, the starch contains at least 90%, preferably at least 95%, more preferably at least 98%, or even at least 99% of hydroxyl groups that are not chemically modified. Most preferably, the starch does not contain chemically modified hydroxyl groups. High levels of hydroxyl groups may be beneficial to the stability of the adhesive, which may be mediated at least in part by hydrogen bonds. In another embodiment, the starch is partially oxidized. Preferably, the degree of oxidation of the hydroxyl groups is low, for example between 0.1% and 10%, or between 0.5% and 5%. Partially oxidized starch may contain more than 90% amylopectin. In embodiments, the starch comprises about 99% amylopectin and has a degree of oxidation of about 0.5% to 2%.

[0053] The aqueous adhesive comprises polyvinyl alcohol which may contain up to 5 mol.% of other monomeric units. Polyvinyl alcohol is a linear polymer consisting of monomeric building blocks having hydroxyl groups. It is assumed that starch has good compatibility with polyvinyl alcohol, also because both polymers contain hydroxyl groups and are able to form intramolecular hydrogen bonds. Another advantage of polyvinyl alcohol is that it is biodegradable, albeit relatively slowly.

[0054] Preferably, the viscosity of the polyvinyl alcohol is at least 25 mPa*s, more preferably at least 30 mPa*s. Preferably, the viscosity is in the range of 25 mPa*s to 100 mPa*s, more preferably between 30 mPa*s and 75 mPa*s. It has been found that if the viscosity of the polyvinyl alcohol is adjusted accordingly, the mechanical properties of the nonwoven carrier are particularly good at cold and hot temperatures. If the viscosity is too low, the mechanical stability of the nonwoven will decrease. If the viscosity is too high, the processability may decrease and the formation of an intimate mixture of starch and polyvinyl alcohol may be impaired. Here, the viscosity of the polyvinyl alcohol is determined according to ISO 2555 at a concentration of 4 wt.% at 23°C.

[0055] Preferably, the degree of saponification (hydrolysis) of the polyvinyl alcohol is at least 90 mol%, more preferably at least 95 mol% or at least 98 mol%. The degree of saponification indicates the degree to which acetate groups from the precursor polymer are converted to hydroxyl groups. A high degree of saponification is advantageous because the binder is more uniform, thereby giving the nonwoven carrier a higher stability.

[0056] Polyvinyl alcohol can comprise other monomeric units of up to 5mol.%, preferably up to 2mol.%. These other monomeric units are intentionally incorporated into the polymer chain during polymerization. Therefore, other monomers are part of a monomer mixture, and polyvinyl alcohol or a polyvinyl alcohol precursor, typically polyvinyl acetate, is polymerized by the monomer mixture. Therefore, the monomer is not vinyl alcohol or residual vinyl acetate, and the monomer is not yet hydrolyzed when polyvinyl acetate is converted into polyvinyl alcohol. Polyvinyl alcohol derivatives with other monomeric units are known in the art and are commercially available. For example, a small amount of other monomeric groups such as ethylene or carboxyl can be incorporated into the polymer to give the desired functionality of the polymer. In a preferred embodiment, polyvinyl alcohol does not comprise other monomeric units and / or groups, except residual acetic acid groups. This may be advantageous because the polymer is homogeneous and can give the nonwoven carrier high stability.

[0057] In one embodiment, the degree of polymerization of the polyvinyl alcohol is at least 600, more preferably at least 1000. The relatively high degree of polymerization associated with the relatively high polymer chain length can provide good mechanical stability to the nonwoven carrier.

[0058] In a preferred embodiment, starch and / or polyvinyl alcohol are produced from natural raw materials. Starch can be produced from natural sources, and polyvinyl alcohol can be produced from natural building blocks, for example based on bioethanol. Therefore, sustainable adhesives can be produced, which are also biodegradable. Preferably, the nonwoven fibers are from recycled PET, for example from used PET bottles. Therefore, sustainable nonwoven carriers can be provided.

[0059] In a preferred embodiment, the amount of polyvinyl alcohol in the adhesive is less than 30 wt.%, less than 25 wt.% or less than 20 wt.%. The advantage is that the proportion of starch in the composition can be significantly higher than the proportion of polyvinyl alcohol, because commercially available starch is cheaper than polyvinyl alcohol. Since no crosslinking agent is included, the additive (if any) does not include a crosslinking agent.

[0060] In a preferred embodiment, the adhesive comprises only starch and polyvinyl alcohol as solid components. According to the present invention, it is found that highly advantageous properties can be imparted to nonwoven carriers by adhesives that are completely or mainly composed of starch and polyvinyl alcohol. In industrial applications, it is highly advantageous if such adhesives are composed of a small amount of components. First, it can be easily prepared and is inexpensive. Further, both polymer components are biodegradable. Another advantage of adhesives without crosslinking agents is that no chemical reaction is carried out during or after the nonwoven is impregnated. In contrast, reactive adhesives used in the art require controlled chemical reactions. If the reaction is incomplete or excessive, the product may have undesirable properties. Overall, simple adhesive compositions can improve product uniformity, reproducibility, and quality control. Another advantage of adhesives without crosslinking agents is that excess aqueous adhesives in the production process can be reused. In contrast, crosslinked aqueous adhesives cannot be used again and must be discarded. Therefore, the present invention can reduce waste and provide a more sustainable nonwoven carrier. Surprisingly, it is also found that adhesives without crosslinking agents can impart even better mechanical properties to substrates than comparable adhesives with crosslinking agents, including dimensional stability. For example, it was found that adhesives without crosslinking agents can have lower heat deformation, which is particularly important for the asphaltification process. This is unexpected because it is generally assumed in the art that crosslinking agents increase dimensional stability by forming a polymer network.

[0061] In a preferred embodiment, adhesive does not comprise the structural polymer that is different from starch and polyvinyl alcohol.Preferably, adhesive does not comprise the other structural polymer that is generally used for nonwoven adhesive, such as acrylic polymer, SBR, polyurethane, polyamide, polyester or its copolymer, or other natural polymer, such as protein, gelatin or alginate.Preferably, adhesive does not comprise other polymer at all, and is therefore not used as functional additive yet.Due to only using starch and polyvinyl alcohol as structural polymer, the nonwoven carrier with high mechanical stability can be obtained, therefore do not need to comprise other structural polymer.This is also favourable for the simplicity, quality control and cost reason of production process.

[0062] The adhesive may contain additives. Preferably, the total amount of additives is relatively low. Preferably, it is less than 15 wt.%, more preferably less than 10 wt.%, or less than 5 wt.%, all wt.% being related to the total adhesive dry weight. Particularly preferred is that the amount of additives is less than 2 wt.%, less than 1 wt.% or that additives are not present at all. Therefore, it is preferred that the adhesive is completely or substantially composed of starch and polyvinyl alcohol as solid components.

[0063] The additive can be a functional additive that imparts the desired characteristic of the adhesive. Such functional additives are known in the art and comprise UV stabilizers, adhesion promoters, coloring agents and processing aids. Preferably, the additive is not a polymer. In a preferred embodiment, only the additive is an additive in an aqueous adhesive solution, and the additive will not become a part of the adhesive of the consolidation on the nonwoven carrier, such as salt and buffer substances.

[0064] Highly preferably the total amount of additive is low.According to the present invention, surprisingly find that substantially or only very simple adhesive composition based on starch and polyvinyl alcohol can give nonwoven carrier highly favorable characteristic.Therefore, adhesive solution can be very simple, and this is conducive to large-scale production and processing.For environmental reasons, a small amount of additives may also be favorable.Usually, the adhesive containing no additive or only containing a small amount of additives can be more efficiently recovered.This type of adhesive can be recovered from the adhesive bath and / or can be peeled off and recovered from the nonwoven carrier.On the contrary, crosslinked adhesive or the adhesive comprising high-level synthetic additives can not be efficiently recovered.

[0065] The adhesive contains no fillers. This can be advantageous, since fillers are usually used in relatively high amounts and can significantly impair the stability of the polymer matrix formed by starch and polyvinyl alcohol. In particular, since the adhesive is not crosslinked, the stability of the nonwoven carrier can be reduced by fillers.

[0066] According to the present invention, it is found that the common functional additives used in this type of adhesive in the present field can have a negative impact on the mechanical properties of the nonwoven carrier. In a preferred embodiment, the adhesive does not include surfactants, detergents, wetting agents, emulsifiers, protective colloids and / or dispersants, preferably does not include any of these additives. Preferably, the adhesive does not include additives, and the additives are amphiphilic molecules or nonionic surfactants. More preferably, the adhesive does not include hydrocarbons containing 8 to 18 carbon atoms connected with polar or ionic moieties, and / or ethoxylated surfactants, such as ethoxylated sorbitan esters. Without being bound by theory, this type of functional additive may damage the internal hydrogen bonds between the adhesive molecules, thereby reducing the stability of the nonwoven carrier. However, the adhesive may include inevitable impurities such as salts, which have no relevant effects on the consolidated adhesive structure.

[0067] Preferably, the polyvinyl alcohol is provided to the adhesive in the form of an aqueous solution. Preferably, the polyvinyl alcohol is not provided in the form of a dispersion. In this embodiment, additives required for the preparation of such dispersions, such as emulsifiers or protective colloids, are not provided.

[0068] In another embodiment, the adhesive does not contain an additive comprising a hydrophilic group, such as a hydroxyl, carboxyl, amine, aldehyde or ketone group and / or an ionic group. More preferably, the adhesive does not contain an additive comprising a hydroxyl. Without being bound by theory, the hydrophilic group can affect the hydrogen bonds in the adhesive structure, thereby reducing the stability of the nonwoven carrier.

[0069] In a preferred embodiment, the adhesive comprises

[0070] 5 wt.% to 95 wt.%, preferably 10 wt.% to 90 wt.% of starch,

[0071] 5 wt.% to 95 wt.%, preferably 10 wt.% to 90 wt.% of polyvinyl alcohol, and

[0072] 0 wt.% to 15 wt.%, preferably 0 % to 2 % of additives,

[0073] The sum of all percentages is 100 wt.%. All percentages of adhesive components herein refer to dry weight unless otherwise stated. It has been found that even in the absence of a crosslinking agent, the amounts of starch and polyvinyl alcohol can be varied widely to provide various nonwoven carriers with high dimensional stability at high or low temperatures.

[0074] In a preferred embodiment, adhesive comprises 50wt.% to 95wt.%, preferably 72wt.% to 95wt.% starch, 5wt.% to 50wt.%, preferably 5wt.% to 28wt.% polyvinyl alcohol, and 0wt.% to 15wt.%, preferably 0wt.% to 2wt.% additives, wherein the sum of all percentages is 100wt.% (dry weight). It is found that the adhesive composition comprising such relatively large amounts of starch can impart high dimensional stability to nonwoven carriers.

[0075] In another preferred embodiment, the adhesive comprises 5wt.% to 69wt.% starch, 31wt.% to 95wt.% polyvinyl alcohol and 0wt.% to 15wt.%, preferably 0wt.% to 2wt.% additives, wherein the sum of all percentages is 100wt.% (dry weight). It is found that the adhesive composition comprising such a relatively large amount of polyvinyl alcohol can impart high mechanical resistance to the nonwoven carrier.

[0076] In another preferred embodiment, the adhesive comprises 30wt.% to 70wt.% starch, 30wt.% to 70wt.% polyvinyl alcohol and 0wt.% to 15wt.%, preferably 0wt.% to 2wt.% additives, wherein the sum of all percentages is 100wt.% (dry weight). It is found that the adhesive composition comprising relatively similar amounts of polyvinyl alcohol and starch can impart high dimensional stability to the nonwoven carrier, especially at high temperatures.

[0077] In a preferred embodiment, the adhesive comprises 60 wt.% to 90 wt.% of starch, 10 wt.% to 40 wt.% of polyvinyl alcohol and 0 wt.% to 5 wt.% of additives, wherein the total is 100 wt.% (dry weight). In another preferred embodiment, the adhesive comprises 70 wt.% to 90 wt.% of starch, especially 72 wt.% to 90 wt.% of starch, 10 wt.% to 30 wt.% of polyvinyl alcohol and 0 wt.% to 5 wt.% of additives, wherein the total is 100 wt.% (dry weight).

[0078] Nonwovens can be spinning, spunlace, melt spinning or staple nonwovens. As used herein, the term fiber comprises staple fibers and filaments. Staple fibers have a definite length, and filaments can be "endless" filaments. Staple fibers can be processed and arranged by conventional methods such as carding. Preferably, the length of the staple fibers is between 20 mm and 200 mm, more preferably between 60 mm and 100 mm.

[0079] The nonwoven comprises organic polymer fibers. In a preferred embodiment, the organic fibers are synthetic fibers. Preferably, the nonwoven is composed of organic polymer fibers, preferably synthetic fibers. Preferably, the nonwoven does not comprise inorganic and / or mineral fibers such as nonwoven glass fibers. Nonwovens from organic and polymer fibers are advantageous because they are lighter than glass fibers, and adhesives can provide high stability for such nonwovens. In a preferred embodiment, the organic polymer is polyester. Polyester can be selected from polyethylene terephthalate, polybutylene terephthalate and polyester copolymers. Preferably, polyester is polyethylene terephthalate (PET). This polymer is particularly suitable for the carrier of asphalt membranes because it has high melting temperature, low cost and good mechanical properties. It is also assumed that the adhesive based on starch and polyvinyl alcohol used in the present invention has good adhesion to polyester fibers, especially PET fibers. In a preferred embodiment, the nonwoven fibers are only polyester fibers. The nonwoven can comprise single component and / or multicomponent fibers, such as bicomponent fibers. The nonwoven may optionally contain further reinforcing inorganic fibers.If the nonwoven consists of organic polymer fibers, preferably synthetic fibers, preferably polyester fibers, especially PET fibers, it may optionally contain reinforcements which are not made of nonwoven fibers.

[0080] In an embodiment, the nonwoven fiber is a mixture of organic fibers and inorganic fibers. The nonwoven can include a mixture of polyester fibers and other nonwoven fibers, such as less than 50 wt %, less than 20 wt % or less than 10 wt % for all fibers. The nonwoven can include other fibers that are relatively stable at high temperatures, such as natural fibers or inorganic nonwoven fibers.

[0081] Preferably, the linear density of the nonwoven fibers is 0.5 dtex to 20 dtex, more preferably 1 dtex to 10 dtex, especially in the range of 2 dtex to 6 dtex. Such fiber nonwovens can provide strength and flexibility for the asphalt membrane. Preferably, the diameter of the nonwoven fibers is in the range of 5 μm to 50 μm, preferably 10 μm to 30 μm. Preferably, the fiber fineness is at least 2.5 dtex.

[0082] In a preferred embodiment, the nonwoven comprises a reinforcement. As used herein, reinforcement relates to any fiber structure, i.e. fiber, filament, yarn, line or other elongated structures. Reinforcement fibers are different from nonwoven fibers, because they are not randomly arranged in the fleece fabric (nonwoven precursor) during the nonwoven production process like other nonwoven fibers. On the contrary, reinforcement fibers are added in different ways during or after the nonwoven production process. Usually, reinforcement is directional, i.e. it particularly strengthens the nonwoven in a specific direction. For example, reinforcement can be a linear yarn or a discrete layer, such as a scrim. Reinforcement fibers are not a part for fiber raw material, and the fiber raw material is arranged to form a nonwoven or fleece fabric precursor. Preferably, reinforcement is embedded in the inside of the nonwoven carrier.

[0083] The reinforcement can be multifilament and / or monofilament. The reinforcement can be from aramid, preferably so-called high modulus aramid, carbon, glass, glass roving, mineral fiber (basalt), high-strength polyester monofilament or multifilament, high-strength polyamide monofilament or multifilament, and yarn, such as mixed multifilament yarn (yarn containing reinforcing filaments and low-melting point binder fibers), or a line (monofilament) made of metal or metal alloy. Preferably, the reinforcement is made of inorganic fibers, such as glass fiber or glass fiber yarn.

[0084] In a preferred embodiment, the reinforcement is a yarn, preferably a glass fiber yarn. Preferably, the amount of the glass fiber yarn in the nonwoven carrier is 2wt.% to 20wt.%, preferably 5wt.% to 15wt.%. Such a level is usually enough to increase strength without damaging the nonwoven properties. Preferably, the yarns are aligned with each other, preferably parallel. The glass fiber yarn can increase the mechanical strength of the nonwoven carrier.

[0085] Preferably, the nonwoven carrier is made up of nonwoven, and the nonwoven is consolidated with an adhesive and optionally comprises a reinforcement. In another embodiment, the nonwoven carrier is a composite substrate, and the composite substrate comprises other, independent inorganic fiber layers. Other layers can be nonwoven, woven fabric, net or scrim or fiber and / or yarn layers. In another embodiment, the nonwoven does not comprise other layers.

[0086] In a preferred embodiment, the nonwoven has a basis weight of 50 g / m2 prior to impregnation with the binder. 2 Up to 500g / m 2 , more preferably 100g / m 2 Up to 300g / m 2 , especially 150g / m 2 Up to 250g / m 2 . Such basis weights are particularly suitable for bituminous membranes. The nonwoven can be pre-consolidated, especially mechanically consolidated, for example by hydraulic needling or pre-needling, before being impregnated with the binder. Preferably, the binder (additional) loading is 1 wt.% to 50 wt.%, preferably 5 wt.% to 40 wt.%, more preferably 10 wt.% to 30 wt.%, of the nonwoven (dry weight without binder). Preferably, water is the only solvent in the aqueous binder.

[0087] Preferably, the thickness of the nonwoven carrier is between 0,25 mm and 6 mm, more preferably between 0,5 mm and 4 mm, in particular between 0.8 mm and 2 mm, as determined according to ISO 9073-2, 1997, paragraph 5.1 "Nonwovens in general".

[0088] In a preferred embodiment, the nonwoven carrier has a thermal tensile deformation of less than 1.8% at 180° C. and 120 N, more preferably less than 1.5%, preferably less than 1.5% at 180 g / m 2 Due to this high dimensional stability, the nonwoven carrier can advantageously be used to produce bituminous membranes with standard machines. Furthermore, the high stability at high temperatures means that the bituminous membranes remain stable for a long time in building and roofing applications. Even in mild climates, roof temperatures can rise to 100°C, for example when the sun shines directly on the metal parts of the roof. In hot geographical areas and for specific applications, the temperature may rise even higher. Therefore, the high dimensional stability at high temperatures is also advantageous for building and roofing applications.

[0089] In a preferred embodiment, the maximum glass tensile strength of the nonwoven carrier at 180°C is at least 150N / 50mm, more preferably at least 200N / 50mm, especially when reinforcing glass fiber yarns are included. The maximum glass tensile strength is related to dimensional stability. It defines the threshold at which the nonwoven collapses due to the fracture of the reinforcement (usually glass fiber). This is defined by the peak value defined in the tensile strength and elongation diagram. High maximum glass hot tensile strength is desirable because it shows that the material can withstand higher tension and tension on the asphalt production line at 180°C, especially at higher speeds. When a force higher than the maximum glass tensile strength is applied to the nonwoven carrier, it loses its shape (collapses) and cannot be reprocessed. Therefore, high maximum glass tensile strength shows that the nonwoven carrier is suitable for efficient production of high-quality asphalt membranes in industrial processes.

[0090] At low temperatures, bituminous membranes are used in construction applications and are subjected to mechanical forces, such as bending to cover irregular building parts, nailing or to withstand stress and strain. Therefore, it is important that the material is mechanically stable at low temperatures to avoid punctures, cracks, etc.

[0091] Preferably, the total maximum tensile strength of the nonwoven carrier is at least 600 N / 5 cm, more preferably at least 625 N / 5 cm, at room temperature (23° C.), determined according to ISO 9073-3. Preferably, the peak tenacity at room temperature is at least 0.28 daN / 5 cm / g / m 2 Preferably, the elongation at break, determined in accordance with ISO 9073-3, at room temperature is at least 40%.

[0092] Unless otherwise stated, the above parameters regarding mechanical stability are determined in the longitudinal direction, preferably in the longitudinal direction and in the transverse direction. Preferably, the properties are for a 180 g / m 2 The basis weight of the spunbond is determined.

[0093] Preferably, the air permeability of the nonwoven carrier is 250÷2500 l / m 2 , as determined by ISO 9037-15.

[0094] The subject matter of the present invention also relates to a method for producing the nonwoven carrier according to the invention, said method comprising the following steps:

[0095] (a) providing a nonwoven fabric,

[0096] (b) impregnating the nonwoven with an aqueous binder comprising starch and polyvinyl alcohol, wherein the binder does not contain a crosslinking agent, and

[0097] (c) drying and curing the binder to obtain the nonwoven carrier.

[0098] During production, curing can be achieved by drying. Since there is no cross-linking agent, there is no need to induce, monitor and / or terminate the cross-linking reaction.

[0099] The subject matter of the present invention also relates to the use of the nonwoven carrier of the present invention as a substrate for producing an asphalt film. The subject matter of the present invention also relates to an asphalt film, which comprises the nonwoven carrier of the present invention. The subject matter of the present invention also relates to a method for producing an asphalt film, which method comprises the following steps:

[0100] (A) providing a nonwoven carrier of the present invention, and

[0101] (B) Impregnation of a nonwoven carrier with bitumen.

[0102] Typically, the impregnation of the nonwoven carrier with bitumen is carried out in a bath containing molten bitumen, in which the nonwoven carrier is immersed. The nonwoven carrier with the bitumen attached is subsequently removed from the bath and dried. Preferably, the method is carried out as an automated process, preferably a continuous process, wherein an "endless" roll of the nonwoven carrier is fed into the process and a roll of bitumen film is obtained as the final product.

[0103] In order to efficiently produce the bitumen film from the nonwoven carrier, the nonwoven carrier and the bitumen film should be flexible. Therefore, the nonwoven carrier and / or the bitumen film are rollable. On the contrary, the nonwoven carrier and / or the bitumen film are not rigid.

[0104] Bitumen membranes can be obtained by conventional processes, in which a nonwoven carrier bonded with an adhesive is impregnated with molten bitumen in a bath. Typically, the nonwoven carrier is supplied to a production line in the form of a roll, where it is unrolled and guided through a hot bitumen bath by standard machinery, drawn out of the bath, followed by cooling and solidification of the bitumen adhered to the carrier. After solidification, the bitumen membrane is rolled up so that it can be stored, transported and supplied to the building site.

[0105] Bitumen membranes can be used for building and roofing applications. Typically, the bitumen membrane is unrolled at the building site, optionally cut into the desired shape, subjected to temporary heating by burning to soften at least one bitumen surface, arranged at the application site, and optionally deformed and thus aligned with the surface of the application site. Subsequently, additional layers, such as insulating layers or tiles, are arranged on the bitumen membrane. Methods for applying bitumen membranes in building applications are standardized in DIN V 20000-201. In the bitumen membrane, the ratio of bitumen to nonwoven carrier is preferably 60% by weight to 97% by weight to 3% by weight to 40% by weight.

[0106] The subject of the present invention also relates to a roof, a building material or a building, which comprises the bituminous membrane of the present invention. For example, the bituminous membrane can be used as a shielding membrane, a sealing membrane or a waterproof sheet.

[0107] The nonwoven carrier of the invention can also be used in other applications such as reinforcing inserts, optionally in combination with further textile fabrics, for masking films, as a textile backing or textile reinforcement, for floor coverings, in particular laminated carpets and PVC floor coverings, as a finish for wall coatings or decorative surfaces in building interiors and exteriors.

[0108] The nonwoven carrier, asphalt film, use and method of the present invention solve the potential problems of the present invention. A nonwoven carrier for producing asphalt film is provided, which is easy to obtain, easy to produce, cheap and has excellent mechanical properties. Surprisingly, although no crosslinking agent is added to stabilize the adhesive system, the nonwoven carrier has high mechanical resistance, especially dimensional stability at room temperature and high temperature, which is even better than comparable adhesives containing crosslinking agents. This is unexpected because the stability of many thermoplastic polymer adhesives deteriorates at high temperatures. Due to high mechanical resistance (as shown in tensile strength, toughness) and dimensional stability (as shown in thermal deformation), the nonwoven carrier is suitable for producing high-quality asphalt films with efficient high-speed automated processes. High dimensional stability at high temperature and very good mechanical properties at room temperature make the nonwoven carrier particularly suitable for construction and roof applications. The present invention also provides guidance on how to provide a specific starch / polyvinyl alcohol adhesive without crosslinking agent with particularly advantageous properties. Another advantage is that the adhesive is biodegradable and formaldehyde-free, and can be based on natural sources, so that a sustainable product can be provided.

[0109] Examples

[0110] In the following working examples, recycled bottle polyester (RPET) nonwovens were consolidated with various starch / polyvinyl alcohol adhesive compositions in the absence of a crosslinking agent.

[0111] Materials and methods

[0112] Dynamic Light Scattering - Size Distribution Analysis

[0113] The average particle size of the solution was determined by dynamic light scattering (DLS) using a 90Plus particle size analyzer (Brookhaven Instruments Corporation, US) at 25.0 ± 0.1 ° C. The autocorrelation function was measured at 90 °, while the laser beam was operated at 658 nm. The average particle size and standard deviation (± SD) were obtained directly from the instrument fitting data by the inverse "Laplace transformation" method and Contin. All analyses were performed three times and expressed as mean ± standard deviation. The SD was found to be 10 nm.

[0114] starch

[0115] Four different corn starches were used to prepare adhesives. Starch A consisted of 99% amylopectin that was partially slightly oxidized. Starch B and Starch C contained about 20% to 25% amylose (dry weight) and were partially hydrolyzed to reduce the M w Starch D contains about 20% to 25% (dry weight) amylose, is pregelatinized and water soluble. It has been pretreated by the supplier by cooking and removing water to make the starch soluble in water, so that no cooking step is required before use.

[0116] The viscosity of the starches was measured according to ISO 2555 using a 25% (w / w) aqueous dispersion or solution at 23°C. The determined properties of the starches are summarized in Table 1 below.

[0117] Table 1 :Characteristics of starch

[0118] starch A B C D Viscosity (mPa*s) 450 370 100 200

[0119] Polyvinyl alcohol (PVOH)

[0120] Polyvinyl alcohol is available in various grades, characterized by different molecular weights. The higher the molecular weight, the higher the viscosity of the polymer in aqueous solution. All grades are characterized by 98% hydrolysis (acetate groups). The pH of PVOH aqueous solutions is 6 as determined according to ISO 976. The viscosity is determined according to ISO 2555 at 23°C using a 4% (w / w) aqueous solution and is summarized in Table 2.

[0121] Table 2 : Viscosity of PVOH grade

[0122] type PVOH 498 PVOH 698 PVOH 1098 PVOH 2098 Viscosity (mPa*s) 22 26 32 50 Degree of hydrolysis (saponification) 98–98.8 98–98.8 98–98.8 98–98.8

[0123] method

[0124] Adhesive preparation

[0125] Adhesive is prepared by mixing starch dispersion (20% solid content) with PVOH solution (10% solid content). In a typical procedure, starch dispersion (500g-20% solid content) is prepared by dispersing 100g dry starch in 400g water. Starch dispersion is heated to 90°C and kept at this temperature for 15 minutes, so that the system is kept mechanically stirred. Finally, the system is cooled to 60°C. PVOH aqueous solution (10% solid content) is prepared by introducing 60g PVOH and 540g water into a three-necked flask equipped with a mechanical stirrer. Then the mixture is heated to 95°C and kept at this temperature for at least 40 minutes. Afterwards, the temperature is cooled to 60°C. 500g of adhesive formulation with a solid content of 12.5% ​​is prepared by mixing 219g starch dispersion, 187g PVOH solution and 94g water. If indicated, 1g wetting agent is added. Finally, the mixture is stirred at 60°C for 10 minutes and used for nonwoven impregnation.

[0126] Nonwoven impregnation

[0127] The nonwoven substrate was a spunbonded nonwoven fabric made of recycled polyethylene terephthalate (PET) fibers (4.4 dtex; reinforced with 68 tex glass yarn, basis weight 180 g / m 2 , pre-consolidated by needle punching and thermosetting). The nonwoven substrate was impregnated with the adhesive formulation using a Mathis Foulard setup (speed: 2.5 m / min; cylinder pressure: 3.5 bar). A sample of the nonwoven (33 cm x 44 cm) was immersed in a bath containing the adhesive formulation. A final add-on of 20% on a dry basis was adjusted after oven drying. The adhesive applied to the nonwoven fabric sample was dried in an oven at 200°C for 3 minutes and 45 seconds.

[0128] Test Method

[0129] A set of 15 samples were obtained from the produced samples and subjected to mechanical tensile testing using a dynamometer (Instron). At low temperature (23°C), 5 samples of 50mm×300mm were used in MD and CD respectively. At high temperature (180°C), 5 samples of 50mm×180mm were used. Hot tensile deformation is the elongation at a specific tensile strength. The lower the value, the more stable the material is, and therefore the better the product. The tensile stress test at 180°C was carried out under modified conditions based on US2008 / 0214716. The heat deformation resistance of the PET nonwoven was characterized by a tensile stress experiment at T=180°C using a tensile machine (dynamometer) with an integrated thermostatic chamber. The clamping length was 80mm and the unwinding speed was 100 mm / min. Under loads of 80N, 100N and 120N, the elongation of the nonwoven was determined in the longitudinal direction (MD) as the tension increased, thereby also determining the maximum tensile strength.

[0130] Examples 1 to 5: Effects of different types of corn starch on mechanical properties

[0131] In the first series of experiments, the nonwoven was consolidated with an adhesive comprising different types of starch and the same PVOH (grade 1098). The product was a thin porous sheet that was flexible and rollable. Adhesive compositions and results are summarized in Table 3. In Comparative Example 1, a conventional adhesive for a nonwoven carrier of an asphalt roofing membrane was used, the adhesive being composed of 70% acrylic acid / melamine / formaldehyde adhesive (63% acrylic resin, trademark Acronal S888S, BASF, DE, 7% melamine formaldehyde crosslinking agent, trademark Saduren 163, BASF, DE) and 30% starch C, all percentages being dry wt.%).

[0132] Table 3 :Effects of different types of corn starch on mechanical properties

[0133]

[0134]

[0135] The results show that despite not including a crosslinker, the starch / PVOH adhesive has favorable properties compared to conventional crosslinked acrylic / melamine formaldehyde adhesives.

[0136] First, starch / PVOH adhesives do not contain formaldehyde, which is beneficial for safety and environmental reasons. Further, the cost of starch / PVOH adhesives is significantly reduced, which is related to large-scale industrial products. Third, starch / PVOH adhesives can be produced without cross-linking agents and cross-linking catalysts. Therefore, the composition and production process are much simpler than cross-linked compositions in which reactive components must be adapted to each other and reaction control is required.

[0137] In addition, the results provide evidence that starch / PVOH adhesives, although not cross-linked, can impart improved mechanical properties to the product, making it very suitable as a carrier for asphalt films. For the production of asphalt films, the dimensional stability of the nonwoven carrier at 180°C is extremely important. The results show that the deformation of the nonwoven consolidated by starch / PVOH adhesive is much lower and the maximum glass tensile strength is higher than that of the comparative standard nonwoven with cross-linked melamine acrylic adhesive. This represents a great advantage when the nonwoven carrier is impregnated with asphalt in an industrial process. Low thermal tensile deformation indicates that the nonwoven carrier can maintain its shape when passing through the production line under significant tension and loading a large amount of asphalt. High maximum glass tensile strength indicates that the nonwoven carrier can withstand a relatively high maximum force in the asphalt impregnation line. The maximum force is significantly higher for the nonwoven carrier of the present invention than for the comparative nonwoven with standard adhesive. Therefore, asphalt films can be produced by the nonwoven carrier of the present invention at a higher speed and productivity, and have a higher product quality, i.e., less failure, product abnormality and damage. Particularly high dimensional stability at high temperatures was observed in Example 3 using Starch B. Only Example 4 provided a deformation level comparable to the standard adhesive at high temperatures. However, this is still a good and unexpected result for an adhesive without a crosslinker.

[0138] Further, the result shows that mechanical properties under low temperature are favourable.As shown in example 2 and 3, the cold toughness of the nonwoven fabric of starch / PVOH consolidation is suitable with the comparative example 1 using standard adhesive.The adhesive in example 4 and 5 can not provide tensile strength and toughness identical with conventional adhesive, but for the natural adhesive that does not comprise crosslinking agent, the result is still good and also unexpected.The nonwoven carrier also can stretch and elongate according to the needs of building and roof application.The result under low temperature shows that the nonwoven carrier also gives the good mechanical properties of the bituminous membrane in final building or roof application.

[0139] Example 6: Starch granule size

[0140] The size of starch aggregates in only starch-containing dispersions and starch / PVOH adhesive dispersions is determined by DLS. As shown in Table 4, the size of starch aggregates present in the dispersion is different for different aqueous starch dispersions and aqueous starch / PVOH dispersions. Specifically, starch B and starch B / PVOH dispersions are characterized in that particles are relatively large. Further, the average particle size of starch B / PVOH dispersion is significantly higher than that of only starch-containing dispersions. On the contrary, the dispersion of starch A or C mixed with PVOH shows an aggregate size similar to that of only starch-containing A or C. Without being bound by theory, PVOH seems to be able to play a self-assembly role on the starch molecules in starch B. This can explain the favorable properties of starch / PVOH adhesive system in above-mentioned Example 3.

[0141] Table 4 : Starch granule size determined by DLS (in nm)

[0142]

[0143] in conclusion

[0144] In general, the working examples show that the highly efficient crosslinker-free water-based adhesive composed of starch and PVOH can be used for the nonwoven carrier of the consolidation asphalt film. Analyzing cold mechanical properties, particularly tensile strength and toughness, starch A and starch B show the best values, which are comparable to or even slightly better than melamine / acrylic adhesive standards (total toughness and tensile strength). Regarding thermomechanical properties, starch B provides the lowest MD deformation at 120N. These values ​​are supported by physicochemical studies. In fact, rheological characterization shows the highest G* value (data not shown) of the mixture starch B / PVOH, which shows that this adhesive has a stronger biopolymer network. Compared with other adhesives, the aggregate size measured by DLS is the highest. The largest aggregates can lead to better fiber adhesion and better thermomechanical properties.

[0145] The presence of a small amount of carboxylated groups in the starch in Example 2 due to chemical oxidation does not appear to have a significant effect on the binding properties. The pregelatinized starch used in Example 5 is water soluble and can be dissolved instantly in cold water. The results suggest that these modifications of the starch structure may result in reduced binding properties compared to cooked starch.

[0146] Example 7: Adhesive Analysis

[0147] In another experiment, the water-based adhesive was heated to 200°C for 3 minutes, and the size of the adhesive molecules was analyzed by MALDI-TOF. It was observed that the size of the adhesive molecules was not affected by the thermal treatment. Therefore, the esterification reaction between starch and PVOH can be ruled out. This confirms that although the adhesive is not cross-linked, good mechanical properties of the adhesive-consolidated nonwovens of Examples 2 to 5 are obtained.

[0148] Examples 8 to 12: Impact of different types of PVOH

[0149] In a second series of experiments, nonwovens were consolidated with adhesives comprising Starch A and four PVOHs with different viscosities. In Comparative Example 8, the same conventional adhesive was used as in Comparative Example 1. The results are summarized in Table 5.

[0150] Table 5 :The impact of different grades of PVOH

[0151]

[0152]

[0153] The viscosity of polyvinyl alcohol with linear polymer chains is directly related to the average molecular weight. PVOH 498 and 698 are characterized by low molecular weight and viscosity. The hot tensile deformation of PVOH 698, 1098 and 2098 is lower than that of traditional adhesives. The hot glass tensile strength is always significantly higher than that of standard adhesives. Therefore, these products are very suitable as nonwoven carriers for the production of asphalt membranes. Overall, the results show that if the PVOH has a higher molecular weight, the bonding properties can be improved.

[0154] Examples 13 to 16: Effect of Wetting Agents (Surfactants) on Mechanical Properties of Starch / PVOH Adhesives

[0155] In additional experiments, the effect of wetting agents (surfactants) on starch / PVOH adhesive compositions was examined. Some starch / PVOH adhesives are prepared with additional wetting agents, which are used in the art as additives to improve the processability of adhesives and nonwoven properties. A silicon-free nonionic ethoxylated surfactant (Example 14) was used, which is characterized by a low tendency to produce foam and high efficiency in reducing the surface tension of water-based solutions and dispersions. Adding 0.2% (v / v%) of this substance to an aqueous dispersion can reduce the surface tension to below 30 mN / m. A polyethoxylated monoester of 3,6-sorbitan was also used (Example 16), which is hydrophilic and soluble or dispersible in dilute solutions of water and electrolytes. The solubility in aqueous solution increases with increasing degree of ethoxylation. Adhesives with wetting agents were compared with adhesives of the present invention without additives (Examples 13, 15), respectively. When the sorbitan polyethoxylate wetting agent was added, a significant decrease in cold tensile strength (MD and CD) and cold glass tensile strength was observed (Example 14). When the ethoxylated wetting agent was added, a decrease in cold tensile properties was also observed (Example 16). Both wetting agents also affect the hot tensile deformation in an undesirable manner, because higher deformations were observed compared to the adhesive without additives, respectively. Without being bound by theory, the high tensile strength of the starch / PVOH adhesive may be due to the large number of hydrogen bonds between the molecules and / or the high compatibility between the two polymers. Therefore, when the wetting agent is added, the hydrogen bond network may be at least partially disturbed, resulting in potential delamination of the two polymers. In addition, the surfactant has a tendency to migrate at the interface, resulting in a decrease in the adhesion between the adhesive and the surface of the PET fiber. This can be confirmed by electron microscopy images of the product. The wetting agent has an adverse effect on the adhesive microstructure because undesirable phase separation is observed in the adhesive film. In contrast, a uniform adhesive film is observed in Comparative Example 15. This can explain the lower tensile strength of the nonwoven samples in Examples 14 and 16. Overall, these examples show that standard additives such as surfactants can significantly reduce the stability of nonwoven carriers.

[0156] Examples 17 to 21: Effects of different types of crosslinkers on mechanical properties

[0157] In examples 19 to 21, nonwovens were consolidated with adhesives as described in example 2 above, which additionally comprised a crosslinking agent. Three specific types of crosslinking agents preferred in the art, such as EP 3 299 514 A1, were selected for crosslinking a starch-based adhesive for nonwoven substrates (see Table 6). The adhesives were prepared as described in example 2 above, wherein 5% (solids content) of starch B was replaced by 5% (solids content) of a crosslinking agent, respectively.

[0158] Table 6: Crosslinking agents added in Examples 19 to 21

[0159] Crosslinker 1 Crosslinker 2 Crosslinker 3 Chemical name Melamine formaldehyde Polyacrylic acid + sodium hypophosphite (catalyst) Polyamine epichlorohydrin concentration 70% (aqueous solution) 50% (aqueous solution) 20% (aqueous solution)

[0160] Impregnated nonwoven as described above.Product is a thin porous sheet, which is flexible and can be rolled.Adhesive composition and results are summarized in Table 7.Comparative Example 17 is a conventional adhesive for the nonwoven carrier of bituminous roof membrane, which is composed of 70% acrylic acid / melamine / formaldehyde adhesive (63% acrylic resin, 7% melamine formaldehyde crosslinking agent 1) and 30% starch C, and all percentages are dry wt.%.Results are compared with the results obtained for the corresponding adhesive without crosslinking agent and melamine / acrylic acid standard adhesive.

[0161] Table 7 : Examples 17 to 21

[0162]

[0163] The results in Table 7 are as follows:

[0164] (A) The starch / PVOH adhesive mixture without crosslinker (Example 18) provides the same cold PET toughness as the comparative standard formulation based on melamine formaldehyde crosslinker (Example 17). In addition, the adhesive of Example 18 provides the lowest hot tensile deformation at 120N and the highest hot glass tensile strength of all examples, which is the reason for the best running performance during bitumen impregnation in a continuous production line.

[0165] (B) Starch / PVOH + Crosslinker 1 (Comparative Example 19) gives the substrate the same PET cold toughness as the starch / PVOH adhesive blend, but the MD and CD cold PET elongations (%) are low. This is a disadvantage because higher cold elongations are preferred to prevent roof tearing. The hot tensile deformation at 120 N is higher than without a crosslinker (Example 18), making the product less processable during asphalt impregnation.

[0166] (C) Starch / PVOH+Crosslinker 2 and Crosslinker 3 adhesive mixtures (Comparative Examples 20, 21) impart lower cold PET toughness to the substrate than starch B / PVOH without crosslinker (Example 18) and standard formulation (Comparative Example 17). Hot tensile deformation (1.84% and 1.92%) is much higher than that without crosslinker and similar to the standard formulation.

[0167] In summary, starch / PVOH adhesives without crosslinkers showed the best properties for the substrates:

[0168] - Very good thermomechanical stability (lowest tensile deformation and highest tensile strength of glass)

[0169] - Very good cold mechanical properties (PET toughness and PET elongation)

[0170] - FA-free, simpler ingredients, low cost, 100% biodegradable adhesive from natural raw materials, original components can be recycled.

[0171] As demonstrated by DLS measurements, PVOH can very effectively aggregate starch particles, which is due to their very good hot and cold tensile properties. Without being bound by theory, the crosslinker may interfere with the aggregation phenomenon, which leads to a decrease in tensile properties.

[0172] Examples 22 to 25: Industrial scale production of nonwoven carriers

[0173] A binder comprising starch B and PVOH (98% degree of hydrolysis, pH 6, viscosity 32 mPa*s at 23° C., determined according to DIN EN ISO 2555 with a 4% (w / w) aqueous solution) was used for large-scale production of a nonwoven carrier.

[0174] Adhesives are prepared on a large scale by mixing starch dispersion (25% solid content) with PVOH solution (15% solid content). In a typical procedure, starch dispersion (500Kg-25% solid content) is prepared by dispersing 125kg dry starch in 375kg water. Starch dispersion is heated to 90°C to 100°C by a jet cooking system. Finally, the system is cooled to 60°C. PVOH aqueous solution (15% solid content) is prepared by introducing 90Kg PVOH and 510kg water into a heating tank equipped with a mechanical stirrer. The mixture is then heated to 95°C and maintained at this temperature for at least 40 minutes. Afterwards, the temperature is cooled to 60°C. By mixing starch, PVOH and water according to the amount described in detail in Table 8, 500Kg of adhesive formulations with a solid content of 15% are prepared. Finally, the mixture is stirred at 60°C for 10 minutes and used for nonwoven impregnation. Nonwoven impregnation is carried out on a typical Foulard for adhesive liquid impregnation, and mechanical properties are determined as described above.

[0175] Table 8 : Adhesive Composition Examples 23 to 25

[0176] Examples Adhesive formulation Starch amount [kg] PVOH amount [kg] Water [kg] 23 69% starch – 31% PVOH 210 150 140 24 50% starch–50% PVOH 150 250 100 25 33% starch–66% PVOH 99 330 71

[0177] The product was a thin porous sheet that was flexible and rollable. The adhesive compositions and results are summarized in Table 9. In Example 22, the comparative adhesive was applied as described above.

[0178] Table 9 : Large-scale production according to Examples 23 to 25

[0179]

[0180]

[0181] The results provide evidence that starch / PVOH adhesives can impart mechanical properties to products that make them well suited as carriers for asphalt membranes. Although the adhesive does not contain a crosslinker, the nonwoven carrier of the present invention has improved properties compared to a standard with a conventional crosslinked acrylic / melamine formaldehyde adhesive. In particular, adhesive formulations containing at least 50% PVOH can have favorable mechanical properties.

[0182] For the production of bituminous membranes, the mechanical stability of the nonwoven carrier at 180°C is very important. In this regard, the results show that the starch / PVOH adhesive-consolidated nonwoven has lower deformation and significantly higher glass tensile strength compared to the standard. This represents a major advantage for customer production lines, as lower hot tensile deformation means less deformation during bitumen impregnation, and therefore higher speed and productivity, with fewer failures, product irregularities and damage. Particularly low deformation at high temperatures was observed in Examples 24 and 25 with at least 50% PVOH. With regard to cold mechanical properties, especially tensile strength and toughness, starch / PVOH adhesive formulations can show especially better values ​​than standard adhesives, especially when the amount of PVOH is above 30%wt.

Claims

1. A nonwoven carrier for an asphalt membrane, wherein the nonwoven comprises organic polymer fibers and is consolidated with an aqueous binder, wherein the binder comprises (a) starch, and (b) polyvinyl alcohol, said polyvinyl alcohol comprising no or at most 5 mol.% of other monomer units, in, The adhesive does not contain a crosslinking agent, wherein the adhesive does not contain fillers, wherein the starch is physically modified starch and / or chemically modified starch from natural sources, wherein the average size of the starch particles in the aqueous adhesive dispersion is at least 0.1 μm as determined by dynamic light scattering (DLS), and The viscosity of the starch is 50 to 800 mPa*s, the viscosity being determined according to ISO 2555 at a concentration of 25 wt. % at 23°C.

2. The nonwoven carrier according to claim 1, characterized in that The starch is partially hydrolyzed.

3. The nonwoven carrier according to claim 1, characterized in that The adhesive comprises less than 2% additives based on total dry weight.

4. The nonwoven carrier according to claim 1, characterized in that Based on total dry weight, the adhesive contained 0% additives.

5. The nonwoven carrier according to claim 1, characterized in that The starch has a viscosity of at least 150 mPa*s, the viscosity being determined according to ISO 2555 at a concentration of 25 wt. % at 23°C.

6. The nonwoven carrier according to claim 1, characterized in that The starch is insoluble in water at 23° C. and / or does not pregelatinize, and / or the starch comprises from 10% to 50% by dry weight of amylose relative to the total amount of amylose and amylopectin.

7. The nonwoven carrier according to claim 1, characterized in that Less than 2% of the starch and the polyvinyl alcohol are crosslinked or the starch and the polyvinyl alcohol are not crosslinked and / or the polyvinyl alcohol has a viscosity of at least 25 mPa*s, determined according to DIN EN ISO 2555 at a concentration of 4 wt.% at 23°C.

8. The nonwoven carrier according to claim 1, characterized in that The adhesive comprises 5 wt.% to 95 wt.% starch, 5 wt.% to 95 wt.% polyvinyl alcohol and 0 wt.% to 15 wt.% additives, all percentages refer to dry weight and the sum of all percentages is 100 wt.%.

9. The nonwoven carrier according to claim 1, characterized in that The adhesive does not contain structural polymers other than starch and polyvinyl alcohol, and / or the adhesive does not contain additives containing hydroxyl groups.

10. The nonwoven carrier according to claim 1, characterized in that The nonwoven consists of organic polymer fibers and / or the nonwoven comprises reinforcements.

11. The nonwoven carrier according to claim 10, characterized in that The nonwoven fabric consists of polyester fibers.

12. The nonwoven carrier according to claim 10, characterized in that The reinforcement is an inorganic fiber yarn.

13. A method for producing a nonwoven carrier according to any one of the preceding claims, comprising the following steps: (a) providing a nonwoven fabric, (b) impregnating the nonwoven with an aqueous binder comprising starch and polyvinyl alcohol, wherein the binder does not contain a crosslinking agent, and (c) drying and curing the binder to obtain the nonwoven carrier.

14. Use of the nonwoven carrier according to any one of claims 1 to 12 as a substrate for producing bituminous membranes.

15. A method for producing an asphalt film, the method comprising the following steps: (A) providing a nonwoven carrier according to any one of claims 1 to 12, and (B) Impregnating the nonwoven carrier with bitumen.

16. A bituminous film comprising the nonwoven carrier according to any one of claims 1 to 12.

17. A building material or a building, comprising the asphalt membrane according to claim 16.

18. A roof comprising the asphalt membrane according to claim 16.