Silicone composition for release sheet and release sheet
By using a specific proportion of a combination of alkenyl organopolysiloxane, epoxy organopolysiloxane, Si-H organohydrogensiloxane and platinum group catalyst in the release sheet, the problem of base under high temperature and high humidity is solved. It solves the problem of material adhesion and peel force balance, achieves efficient adhesion and low peel force, and reduces costs.
Patent Information
- Application Number
- CN202080098879.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-03-25
AI Technical Summary
It is difficult for the existing technology to maintain the balance between the adhesion of the substrate and the low peeling force of the release sheet for a long time in a high temperature and high humidity environment, and the existing methods usually affect the peeling characteristics or increase the manufacturing cost.
An addition-curable silicone composition for release sheets is used, which composition contains a specific proportion of alkenyl organopolysiloxane, epoxy organopolysiloxane, Si-H organohydrogen siloxane, Platinum group metal catalysts and organic solvents form a cured film with excellent adhesion and low peeling force on the substrate.
It achieves long-term maintenance of substrate adhesion in high temperature and high humidity environments, while maintaining low peeling force of the peeling sheet without affecting the peeling characteristics and reducing manufacturing costs.
Smart Images

Figure FDA0004927889090000021 
Figure FDA0004927889090000022 
Figure FDA0004927889090000041
Abstract
Description
Technical Field
[0001] The present invention relates to a silicone composition for a release sheet, and a release sheet obtained using the composition. Background Art
[0002] Conventionally, a release property for an adhesive material has been imparted by forming a cured film of a silicone composition on the surface of a sheet-like substrate such as paper or a plastic film.
[0003] As a method for forming a cured film of a silicone composition on a substrate surface, for example, Patent Document 1 proposes a method in which a platinum compound is used as a catalyst to cause an alkenyl-containing organopolysiloxane and an organohydrogenpolysiloxane to undergo an addition reaction, thereby forming a releasable film on the substrate surface.
[0004] Although such silicone compositions adhere well to paper substrates, it has been pointed out that they have the following drawbacks: poor adhesion to plastic films such as polyester films and polypropylene films, and the need for pretreatment of the substrate.
[0005] As a method for improving adhesion to a substrate, Patent Document 2 proposes a base polymer composition having RSiO 3 / 2 However, this method lacks practicality because a large amount of branched organopolysiloxane containing alkenyl groups is used, which leads to increased production costs.
[0006] As a method for improving adhesion to a substrate by using a small amount of additives, Patent Document 3 proposes adding an organopolysiloxane having an epoxy group. However, this method only describes the adhesion to the substrate under high temperature and high humidity conditions, and does not perform evaluations immediately after curing or when stored at room temperature. In addition, there is no description of the effect of the addition of an organopolysiloxane having an epoxy group on the release properties.
[0007] Patent Document 4 improves adhesion to a substrate by adding a reaction product of a liquid polyorganosiloxane containing alkenyl and silanol groups and a hydrolyzable silane containing an epoxy group. However, this method also does not investigate the effect of adding the reaction product on release properties.
[0008] In Patent Document 5, alkenyl-containing low molecular weight siloxane is added and irradiated with ultraviolet rays, and then the coating is cured by heating, thereby improving the substrate adhesion without affecting the release characteristics. However, this method requires a heating dryer and a UV irradiation device.
[0009] Recently, as the performance of release sheets, requirements have begun to be placed on a smaller peeling force than conventional products and the following high durability: in the molding process of the release sheet, good adhesion to the substrate can be maintained even in harsh environments such as high temperature and high humidity. However, the existing compositions for release sheets tend to have poorer adhesion to the substrate as the peeling force is reduced, and as for long-term adhesion in more harsh environments, almost no composition has been found that can meet the requirements. It is believed that the reason for this is that most of the materials effective for light peeling, such as various materials used as transfer components, work in a manner that reduces adhesion to the substrate, and the reality is that it is difficult to achieve both light peeling and excellent adhesion to the substrate.
[0010] Thus, in the prior art, no suitable method has been found that can achieve both easy releasability of a silicone composition and excellent substrate adhesion.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 47-32072
[0014] Patent Document 2: Japanese Patent No. 2965231
[0015] Patent Document 3: Japanese Patent Application Publication No. 2011-132532
[0016] Patent Document 4: Japanese Patent No. 5507246
[0017] Patent Document 5: Japanese Patent No. 5626097 Summary of the invention
[0018] Technical Problems to be Solved by the Invention
[0019] The present invention has been completed in view of the above situation, and its purpose is to provide a silicone composition for a release sheet, which has excellent adhesion to the substrate and almost no increase in peeling force due to improved adhesion, so that a cured film (peeling film) that imparts a smaller peeling force can be formed, and the substrate adhesion of the film can be maintained for a long time not only at room temperature, but also in harsh environments such as high temperature and high humidity.
[0020] Another object of the present invention is to provide a release sheet obtained from the composition of the present invention.
[0021] Technical means to solve technical problems
[0022] The present invention is made to solve the above-mentioned technical problems, and provides an addition-curable silicone composition for a release sheet, characterized in that it comprises:
[0023] 100 parts by mass of (A) an organopolysiloxane having at least two alkenyl groups in one molecule, an alkenyl content of 0.001 to 0.2 mol / 100 g, and a 30% by mass toluene dilution viscosity at 25° C. of 0.01 to 70 Pa·s;
[0024] (B) A component comprising the following compounds (B1) and (B2):
[0025] 0.1 to 20 parts by mass of an organopolysiloxane (B1) containing 10 mol% or more of a siloxane unit having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom, containing 0.002 to 0.02 mol / 100g of a silanol group, containing 0.5 to 2.5 mol / 100g of an alkoxy group, and having an average degree of polymerization of 3 to 50,
[0026] (B2) having 1.3 mol / 100g or more of Si-H groups and a degree of polymerization of 10 to 100 in an amount equivalent to 0.02 to 1 times the mass of the compound (B1);
[0027] a catalytic amount of (D) a platinum group metal catalyst; and
[0028] 0 to 20,000 parts by mass of (E) an organic solvent.
[0029] The silicone composition for release sheets of the present invention can form a cured film (release film) having excellent adhesion to a substrate, especially a plastic film substrate such as a polyester film, by containing specific amounts of the above-mentioned components (A), (B) and (D). In addition, the cured film obtained from the silicone composition for release sheets of the present invention can show a small peeling force, and while showing such a small peeling force, it can also have good adhesion to the substrate, and can maintain good adhesion to the substrate for a long time not only at room temperature but also under severe conditions of high temperature and high humidity.
[0030] The silicone composition for release sheet of the present invention preferably further comprises (C) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule and different from the (B2) compound, wherein the (C) component is an amount such that the total molar number of hydrogen atoms bonded to silicon atoms of the (B2) compound and the (C) component is equivalent to 0.5 to 10 times the molar number of alkenyl groups in the composition.
[0031] By including such a component (C), better curability can be obtained.
[0032] The (B1) compound is preferably a partially hydrolyzed condensate of an organic alkoxysilane represented by the following general formula (1-1) and at least one of the organic alkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), and is an organic polysiloxane having a linear siloxane structure, a branched siloxane structure, or a cyclic siloxane structure, or a mixture thereof.
[0033] [Chemical formula 1]
[0034]
[0035] (R12) 2 -Si(OR1) 2 ····(1-2)
[0036] R12-Si(OR1) 3 ····(1-3)
[0037] Si(OR1) 4 ····(1-4)
[0038] In formulas (1-1), (1-2), (1-3) and (1-4), R1 is optionally the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and not having an aliphatic unsaturated bond, optionally containing an oxygen atom, or a hydrogen atom, R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and n is an integer from 3 to 10.
[0039] By including such a compound (B1), the strength of the cured product can be improved, and a higher adhesion-improving effect can be exhibited.
[0040] The compound (B2) is preferably an organohydrogensiloxane represented by the following general formula (2-1) or (2-2), or a mixture thereof:
[0041] (R12) 3 Si-{(R12)HSiO} m -Si(R12) 3 ····(2-1)
[0042] (R12) 2 HSi-{(R12)HSiO} m -SiH(R12) 2 ····(2-2)
[0043] In the formulae (2-1) and (2-2), R12 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and m is an integer of 2 to 100.
[0044] By including such a compound (B2) in a manner used simultaneously with the compound (B1), the strength of the cured product can be improved, and a higher adhesion improvement effect can be exerted. Since it is difficult to obtain a sufficient adhesion improvement effect even if the compound (B2) is used alone, it is speculated that the following effects may be caused: the compound (B1) increases the strength of the adhesion improvement layer formed at the interface between the organic silicone cured film and the substrate, and strengthens the bonding between the adhesion improvement layer and the organic silicone cured film.
[0045] The silicone composition for release sheets of the present invention preferably further comprises 0.1 to 10 parts by mass of a component (B3) as the component (B), wherein the component (B3) is a compound having a viscosity of less than 0.5 Pa·s at 25° C., having at least two alkenyl groups in one molecule, an alkenyl content of 5 to 500 times the alkenyl content of the component (A), and having no epoxy group, and the component (B3) is such that the number of moles of hydrogen atoms bonded to silicon atoms in the composition is equivalent to 0.5 to 10 times the total number of moles of alkenyl groups in the components (A) and (B3).
[0046] By including this (B3) component, the curability of the composition can be further improved, and the light peeling effect can be maintained, and the adhesion of the obtained cured film to the substrate just after curing is improved. The mechanism of the effect is not yet clear, but the (B3) component, which has a higher alkenyl content than the (A) component and a lower viscosity than the (A) component, has less restriction on molecular movement in the composition and excellent reactivity with SiH groups, so the curability is improved, the residual SiH groups are reduced, and the light peeling effect can also be obtained. Further, it is speculated that by performing a cross-linking reaction, the cross-linking density is improved, so the adhesion of the substrate just after curing is also improved.
[0047] The silicone composition for a release sheet of the present invention preferably further contains 0.1 to 20 parts by mass of the following component (F1) and / or the following component (F2) as a release force control component (F) based on 100 parts by mass of the component (A):
[0048] (F1) a release force control component comprising an acrylic-silicone graft copolymer having a weight average molecular weight of 1,000 to 100,000, wherein the acrylic-silicone graft copolymer is obtained by radically polymerizing (a) an organopolysiloxane compound having an acryloyl group and / or a methacryloyl group represented by the following general formula (3) and (b) a radical polymerizable monomer having one radical polymerizable group in one molecule,
[0049] [Chemical formula 2]
[0050]
[0051] In formula (3), R2 is a hydrogen atom or a methyl group, X is a group selected from an oxygen atom, an NH group and a sulfur atom, Y is a divalent hydrocarbon group having 1 to 12 carbon atoms and optionally containing an oxygen atom, R 3 are optionally the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, hydrogen atoms, hydroxyl groups, alkoxy groups having 1 to 10 carbon atoms, or substituents represented by the following general formula (4), and f is an integer from 0 to 1,000,
[0052] [Chemical formula 3]
[0053]
[0054] In formula (4), R 4 are optionally the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, hydrogen atoms, hydroxyl groups, or alkoxy groups having 1 to 10 carbon atoms. g is an integer of 0 to 300;
[0055] (F2) Linear phenylmethylpolysiloxane.
[0056] By including such a component (F), it is possible to maintain excellent adhesion to the substrate and adjust the peeling force. In addition, it is possible to obtain an excellent peeling film having a high residual adhesive ratio of the adhesive sheet after peeling.
[0057] The present invention also provides a release sheet characterized in that it is obtained by applying the silicone composition for a release sheet of the present invention to a paper substrate or a film substrate and curing the composition.
[0058] The release sheet of the present invention is obtained by coating the silicone composition for release sheet of the present invention on a substrate and curing it, so the cured film obtained by curing can show a small peeling force and can show good substrate adhesion. This good substrate adhesion can be maintained for a long time not only at room temperature but also under severe conditions of high temperature and high humidity.
[0059] Effects of the Invention
[0060] According to the silicone composition for release sheets of the present invention, a non-adhesive cured film with excellent adhesion to the substrate can be obtained, and good release characteristics can be obtained while the non-adhesiveness of the cured film before and after the adhesion improvement is almost unchanged. The existing adhesion improvement methods cannot avoid the influence on the release characteristics, but according to the release sheet formed with the cured film of the silicone composition for release sheets of the present invention, the adhesion to the substrate can be improved without affecting the release characteristics. In addition, the cured film obtained from the silicone composition for release sheets of the present invention can maintain good substrate adhesion for a long time even when placed under harsh conditions of high temperature and high humidity. DETAILED DESCRIPTION
[0061] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0062] In the present invention, the release sheet may be, for example, release paper including a paper substrate or a release film including a film made of plastic, etc. The release sheet composition may be, for example, a silicone composition for release paper or a silicone composition for release film.
[0063] To achieve the above-mentioned object, the inventors of the present application have conducted intensive research and found that a cured film having excellent adhesion to a substrate can be obtained by using a composition, wherein the composition comprises the following components in specific amounts: (A) an organopolysiloxane having at least two alkenyl groups in one molecule, an alkenyl content of 0.001 to 0.2 mol / 100 g, and a 30% by mass toluene dilution viscosity of 0.01 to 70 Pa·s at 25° C.; (B) a compound (B1) and a compound (B2), wherein (B1) The compound is an organopolysiloxane containing 10 mol% or more of a siloxane unit having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom, 0.002 to 0.02 mol / 100g of a silanol group, 0.5 to 2.5 mol / 100g of an alkoxy group, and an average degree of polymerization of 3 to 50 in one molecule, wherein the (B2) compound is an organohydrogensiloxane having 1.3 mol / 100g or more of a Si-H group and a degree of polymerization of 10 to 100; (D) a platinum group metal catalyst; and (E) an organic solvent.
[0064] Furthermore, in the conventional methods for improving adhesion, sufficient substrate adhesion cannot be obtained using a composition with a small peeling force, but it has been found that the composition of the present invention can achieve both a small peeling force and excellent substrate adhesion, and its excellent substrate adhesion can be sustained for a long time, thereby completing the present invention.
[0065] In addition, the inventors of the present application previously achieved the target effect by combining a composition of a high alkenyl-containing siloxane and an epoxy-containing siloxane in Japanese Unexamined Patent Publication No. 2017-25135, but the present inventors have discovered a composition that improves the effect using a cheaper material, thereby completing the present application.
[0066] [Silicone composition for release sheet]
[0067] The addition-curable silicone composition for a release sheet of the present invention comprises:
[0068] 100 parts by mass of (A) an organopolysiloxane having at least two alkenyl groups in one molecule, an alkenyl content of 0.001 to 0.2 mol / 100 g, and a 30% by mass toluene dilution viscosity at 25° C. of 0.01 to 70 Pa·s;
[0069] (B) A component comprising the following compounds (B1) and (B2):
[0070] 0.1 to 20 parts by mass of (B1) an organopolysiloxane containing 10 mol% or more of a siloxane unit having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom, 0.002 to 0.02 mol / 100g of a silanol group, 0.5 to 2.5 mol / 100g of an alkoxy group, and an average degree of polymerization of 3 to 50 in one molecule;
[0071] (B2) having 1.3 mol / 100g or more of Si-H groups and a degree of polymerization of 10 to 100 in an amount equivalent to 0.02 to 1 times the mass part of the compound (B1);
[0072] a catalytic amount of (D) a platinum group metal catalyst; and
[0073] 0 to 20,000 parts by mass of (E) an organic solvent.
[0074] In the silicone composition for release sheets of the present invention, the amount of the organic solvent (E) may be 0 parts by mass relative to 100 parts by mass of the component (A), and therefore it is an optional component. In addition, the silicone composition for release sheets of the present invention may also contain other optional components in addition to the components (A), (B) and (D). Specific examples of the optional components are described below.
[0075] Hereinafter, each component of the silicone composition for a release sheet of the present invention will be described in order.
[0076] [Component (A): organopolysiloxane having alkenyl groups]
[0077] The component (A) used in the present invention is an organopolysiloxane having at least two alkenyl groups in one molecule, an alkenyl content of 0.001 to 0.2 mol / 100 g, and a 30 mass % toluene dilution viscosity at 25°C of 0.01 to 70 Pa·s, and is preferably represented by the following general formula (5).
[0078] [Chemical formula 4]
[0079]
[0080] In the above formula (5), R 5are optionally the same or different, and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms and having no aliphatic unsaturated bond, or alkenyl groups having 2 to 12 carbon atoms and optionally containing oxygen atoms, and at least two R 5 It is an alkenyl group.
[0081] Specific examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms and not having an aliphatic unsaturated bond include monovalent hydrocarbon groups having 1 to 10 carbon atoms selected from the following groups: alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, and butyl; cycloalkyl groups having 5 to 8 carbon atoms, such as cyclohexyl; aryl groups having 6 to 10 carbon atoms, such as phenyl and tolyl; aralkyl groups having 7 to 10 carbon atoms, such as benzyl; and hydroxypropyl, cyanoethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, and the like obtained by replacing some or all of the hydrogen atoms bonded to the carbon atoms of these groups with hydroxyl, cyano, halogen atoms, and the like. In particular, from the viewpoint of releasability, the monovalent hydrocarbon group having 1 to 20 carbon atoms and not having an aliphatic unsaturated bond is preferably an alkyl group or an aryl group, and is more preferably a methyl group, an ethyl group, a propyl group, or a phenyl group.
[0082] The alkenyl group having 2 to 12 carbon atoms which may contain an oxygen atom is preferably -(CH 2 ) x -CH=CH 2 (x is 0 or an integer of 1 to 10) includes vinyl, propenyl, butenyl, hexenyl, octenyl, and decenyl. In addition, the methylene chain may contain an ether bond, for example -(CH 2 ) 2 -O-CH 2 -CH=CH 2 、-(CH 2 ) 3 -O-CH 2 -CH=CH 2 Etc. Among them, vinyl is preferred.
[0083] The number of alkenyl groups in one molecule of the organopolysiloxane of component (A) is more than two. That is, the organopolysiloxane of component (A) has at least two alkenyl groups in one molecule. If the number of alkenyl groups is less than two, there is a high possibility that uncrosslinked molecules remain after curing, and the curability will be reduced, which is not ideal. The organopolysiloxane of component (A) may, for example, have less than 2000 alkenyl groups in one molecule. In addition, the alkenyl content in the organopolysiloxane of component (A) is 0.001 to 0.2 mol per 100 g, and more preferably 0.002 to 0.15 mol. If the content is less than 0.001 mol, the curability may sometimes be reduced, and if the content is greater than 0.2 mol, heavy peeling may sometimes occur.
[0084] In addition, the viscosity of component (A) at 25°C is 0.01 to 70 Pa·s as a 30% by mass toluene dilution viscosity, particularly preferably 0.01 to 60 Pa·s as a 30% by mass toluene dilution viscosity, and further preferably 0.01 to 50 Pa·s as a 30% by mass toluene dilution viscosity. If it is less than 0.01 Pa·s, the coating property when the composition is made is insufficient, and if it is greater than 70 Pa·s, the operability is reduced. In addition, the viscosity can be measured using a rotary viscometer (the same below).
[0085] In the above formula (5), h, i, j, and k are selected from positive numbers that make the viscosity within the above range, and in particular, h is an integer greater than 2, preferably an integer from 2 to 300, i is an integer greater than 100, preferably an integer from 148 to 19,998, and more preferably an integer from 198 to 14,700, j is an integer greater than 0, preferably an integer from 0 to 100, k is an integer greater than 0, preferably an integer from 0 to 100, 150≤h+i+j+k≤20,000, and preferably 200≤h+i+j+k≤15,000.
[0086] Specific examples of the component (A) include the following, but are not limited thereto. In the following formulae, Me, Vi, and Ph represent a methyl group, a vinyl group, and a phenyl group, respectively.
[0087] [Chemical formula 5]
[0088]
[0089] [Chemical formula 6]
[0090]
[0091] [(B) ingredient]
[0092] The (B) component used in the present invention is an adhesion-enhancing component and is a component containing the following (B1) compound and (B2) compound.
[0093] (B1) Compound
[0094] The compound (B1) is a compound having an effect of improving adhesion by being blended into the composition of the present invention, and is an organopolysiloxane containing 10 mol% or more of a siloxane unit having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom, 0.002 to 0.02 mol / 100g of a silanol group, 0.5 to 2.5 mol / 100g of an alkoxy group, and an average degree of polymerization of 3 to 50. The compound (B1) is used in an amount of 0.1 to 20 parts by mass per 100 parts by mass of the component (A).
[0095] The (B1) compound is a compound that has a high effect of maintaining the substrate adhesion of the cured film (peeling film) obtained by using the composition of the present invention even under heating and humidification conditions (under high temperature and high humidity conditions), and is a component added in anticipation of an adhesion improvement effect under particularly severe use conditions. In addition, the average degree of polymerization is a weight average degree of polymerization when converted to polystyrene obtained by gel permeation chromatography (GPC).
[0096] The organopolysiloxane as the compound (B1) is an organopolysiloxane containing 10 mol% or more of a siloxane unit having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom in one molecule. If the siloxane unit is less than 10 mol%, the adhesion effect to the substrate cannot be obtained. The upper limit of the content of the siloxane unit is not particularly limited, and can be set to 100 mol%, for example.
[0097] The organopolysiloxane as the compound (B1) contains 0.002 to 0.02 mol / 100g of silanol groups. When the content of the silanol groups is less than 0.002 mol / 100g, sufficient adhesion to the substrate cannot be obtained. On the other hand, when the content of the silanol groups is greater than 0.02 mol / 100g, the peeling properties may be adversely affected. The content of the silanol groups is preferably 0.003 to 0.02 mol / 100g.
[0098] The organopolysiloxane as the compound (B1) contains 0.5 to 2.5 mol / 100g of alkoxy groups. When the content of the alkoxy groups is less than 0.5 mol / 100g, sufficient adhesion to the substrate cannot be obtained. On the other hand, when the content of the alkoxy groups is greater than 2.5 mol / 100g, the peeling properties may be adversely affected. The content of the alkoxy groups is preferably 0.6 to 2.5 mol / 100g.
[0099] The average polymerization degree of the organopolysiloxane as the compound (B1) is 3 to 50, preferably 3 to 20. If the average polymerization degree is less than 3, the adhesion effect to the substrate is insufficient, and if the average polymerization degree is greater than 50, the adhesion effect to the substrate is reduced or the workability is reduced.
[0100] The organopolysiloxane of the compound (B1) may be any of linear, branched, and cyclic, and may also be a mixture thereof, but is preferably a partial hydrolysis condensate of an organoalkoxysilane. Among the organoalkoxysilanes used as raw materials, alkoxysilanes having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom are preferably mono-trifunctional organoalkoxysilanes, and more preferably organoalkoxysilanes represented by the following general formula (1-1).
[0101] [Chemical formula 7]
[0102]
[0103] In formula (1-1), R1 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and not having an aliphatic unsaturated bond, which may contain an oxygen atom, or a hydrogen atom. n is an integer of 3 to 10.
[0104] Specific examples of the organoalkoxysilane include the following organoalkoxysilanes.
[0105] [Chemical formula 8]
[0106]
[0107] As other organic alkoxysilanes that are co-hydrolyzed and condensed with the above-mentioned alkoxysilane, it is preferred to use at least one of the organic alkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), and it is more preferred to use trifunctional and tetrafunctional alkoxysilanes represented by the following general formulas (1-3) and (1-4). It is believed that by including such a branched structure or a three-dimensional crosslinked structure in the molecule, or by imparting molding ability during the formation of the cured product, the strength of the cured product will be improved. Furthermore, by moderately reducing the solubility and dispersibility of the (B1) compound in the organic silicone cured film layer with excellent mold release properties formed around a linear structure, the (B1) compound will be easily concentrated near the interface between the substrate and the organic silicone cured film, thereby exerting a higher adhesion improvement effect.
[0108] (R12) 2 -Si(OR1) 2 ····(1-2)
[0109] R12-Si(OR1) 3 ····(1-3)
[0110] Si(OR1) 4 ····(1-4)
[0111] In formulae (1-2) to (1-4), R1 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and not having an aliphatic unsaturated bond, which may contain an oxygen atom, or a hydrogen atom, and R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms.
[0112] Specific examples of the organoalkoxysilane to be co-hydrolyzed and condensed with an alkoxysilane having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom (for example, an organoalkoxysilane of the general formula (1-1)) include the following organoalkoxysilanes.
[0113] [Chemical Formula 9]
[0114] (CH 3 ) 2 -Si(OCH 3 ) 2 、(CH 3 ) 2 -Si(OC 2 H 5 ) 2 、
[0115] (CH 3 ) 2 -Si(OC 3 H 7 ) 2 、(C 6 H 5 ) 2 -Si(OCH 3 ) 2 、
[0116] (C 6 H 5 ) 2 -Si(OC 2 H 5 ) 2 、(C 6 H 5 ) 2 Si(OC 3 H 7 ) 2 、
[0117] (CH 3 )-Si(OCH 3 ) 3 、(CH 3 )-Si(OC 2 H 5 ) 3 、
[0118] (CH 3 )-Si(OC 3 H 7 ) 3 、(C 6 H 5 )-Si(OCH 3 ) 3 、
[0119] (C 6 H 5 )-Si(OC 2 H 5 ) 3 、(C 6 H 5)-Si(OC 3 H 7 ) 3 ,
[0120] (C 8 H 17 )-Si(OCH 3 ) 3 , (C 10 H 21 )-Si(OCH 3 ) 3 ,
[0121] Si(OCH 3 ) 4 、Si(OC 2 H 5 ) 4 、Si(OC 3 H 7 ) 4
[0122] In the above formula (1-1), the hydrogen atom on the monovalent organic group having a glycidoxy group may be substituted with a substituent. From the perspective of safety and economy, the substituent here is preferably a substituent other than an epoxycyclohexyl group. Examples of the epoxycyclohexyl group include 3,4-epoxycyclohexylmethyl, 2-(3,4-epoxycyclohexyl)ethyl, and 3-(3,4-epoxycyclohexyl)propyl.
[0123] In addition, R1 is an unsubstituted or substituted hydrocarbon group with 1 to 10 carbon atoms and no aliphatic unsaturated bond, which may contain an oxygen atom, or a hydrogen atom. Specifically, the hydrocarbon group as R1 includes, for example, alkyl groups such as methyl, ethyl, propyl, and butyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl and tolyl; aralkyl groups such as benzyl and phenethyl; or groups obtained by replacing some or all of the hydrogen atoms bonded to the carbon atoms of these groups with hydroxyl groups, such as hydroxypropyl. Among these groups, as R1, a hydrogen atom and an alkyl group are preferred, and an alkyl group with 1 to 5 carbon atoms is more preferred.
[0124] The following siloxane units formed by partial hydrolysis condensation reaction of the organoalkoxysilane represented by the above general formulae (1-1) to (1-4) can be represented by T E , D, T, Q, and the compound (B1) is represented by D a T E b T c Q d The average formula.
[0125] [Chemical formula 10]
[0126]
[0127] (R12) 2 -Si(O 1 / 2 ) 2 ····(D)
[0128] R12-Si(O 1 / 2 ) 3 ····(T)
[0129] Si(OR1) 4 ····(Q)
[0130] Here, a+b+c+d is 3 to 50, b / (a+b+c+d) is 0.1 to 1, a, c and d are each independently 0 to 35, and the molecular end that does not form a siloxane bond with other siloxane units is an alkoxy group or a silanol group.
[0131] The compound (B1) preferably does not have an alkenyl group in the molecule. By including such a compound (B1), the adhesion effect to the substrate can be improved.
[0132] The amount of the compound (B1) is in the range of 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, relative to 100 parts by mass of the organopolysiloxane of the component (A). If it is less than 0.1 parts by mass, the adhesion to the substrate cannot be improved. In addition, if it is greater than 20 parts by mass, the peeling characteristics may be affected or the strength of the cured film may be reduced. In addition, if it is greater than 20 parts by mass, it may not be possible to maintain excellent adhesion to the substrate for a long time under harsh environments.
[0133] Specific examples of the compound (B1) include the following compounds.
[0134] [Chemical formula 11]
[0135] (B1) Compound Example 1
[0136]
[0137] The molecules represented by the above formula and their mixtures, wherein a+b is 3 to 50, a is 1 or more, the molecular ends are capped with (a+b+2) or less methoxy, ethoxy and / or propoxy groups, and a part of them are substituted with hydroxyl groups.
[0138] (B1) Compound Example 2
[0139]
[0140] The molecules and mixtures thereof represented by the above formula, wherein a+b+c is 3 to 50, a is 1 to 50, the molecular ends are capped with (a+b+2×c+2) or less methoxy groups, ethoxy groups and / or propoxy groups, and a portion of them are substituted with hydroxyl groups.
[0141] As more preferable examples, the following compounds and the like can be mentioned.
[0142] [Chemical formula 12]
[0143] (B1) Example 3 of Compound
[0144]
[0145] Molecules represented by the above average hexamer formula and mixtures thereof, wherein the molecular ends are capped with 8 or less methoxy groups, a portion of which are substituted with hydroxyl groups;
[0146] (B1) Example 4 of Compound
[0147]
[0148] The molecules represented by the above average hexamer formula and mixtures thereof, wherein the molecular terminals are capped with 12 or less methoxy groups and / or ethoxy groups, and a part of the methoxy groups are substituted with hydroxyl groups.
[0149] (B2) Compound
[0150] The (B2) compound is an organohydrogensiloxane having 1.3 mol / 100g or more Si-H groups and a degree of polymerization of 10 to 100. When used together with the (B1) compound, the adhesion-enhancing effect is further enhanced. If the Si-H group of the (B2) compound is less than 1.3 mol / 100g, the adhesion-enhancing effect cannot be obtained. The upper limit of the Si-H group of the (B2) compound is not particularly limited, and can be, for example, 1.7 mol / 100g.
[0151] Since it is difficult to obtain a sufficient adhesion-improving effect even if the (B2) compound is used alone, it is presumed that the (B1) compound plays a role in improving the strength of the adhesion-improving layer formed at the interface between the silicone cured film and the substrate and in strengthening the bonding between the adhesion-improving layer and the silicone cured film.
[0152] The degree of polymerization of the compound (B2) is 10 to 100. If the degree of polymerization is less than 10, the adhesion-improving effect is low, and if the degree of polymerization is greater than 100, the stability is reduced, which is not preferred. The degree of polymerization of the compound (B2) is more preferably 15 to 100.
[0153] The preferred structure of the compound (B2) is that the main chain is mainly composed of siloxane units H(R12)SiO2 / 2 Here, R12 may be the same or different and is an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms.
[0154] More preferably, an organohydrogensiloxane represented by the following general formula (2-1) or (2-2) or a mixture thereof is used.
[0155] (R12) 3 Si-{(R12)HSiO} m -Si(R12) 3 …·(2-1)
[0156] (R12) 2 HSi-{(R12)HSiO} m -SiH(R12) 2 …·(2-2)
[0157] In the formulae (2-1) and (2-2), R12 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and m is an integer of 2 to 100.
[0158] The blending amount of the (B2) compound is adjusted according to the blending amount of the (B1) compound used at the same time. Thus, the adhesion improvement effect can be obtained. The specific blending amount is equivalent to 0.02 to 1 times the mass part of the (B1) compound. If it is less than 0.02 times, the adhesion improvement effect is small, and if it is greater than 1 times, it sometimes affects the peeling characteristics such as re-peeling. The blending amount of the (B2) compound is preferably equivalent to 0.03 to 1 times the mass part of the (B1) compound. Even if it is blended in a manner greater than 1 times the mass part, it is not expected to significantly improve the adhesion improvement effect, but the (B2) compound can be further added to make the molar number of hydrogen atoms bonded to the silicon atom of the (B2) compound equivalent to 0.5 to 10 times the molar number of alkenyl groups of the (A) component. Thus, the curability of the composition can be further improved, which is more ideal.
[0159] Specific examples of the compound (B2) include the following compounds.
[0160] [Chemical formula 13]
[0161] (B2) Compound Example 1
[0162]
[0163] Among them, a' is 10-98, and b' is 0-17.
[0164] (B2) Example 2 of Compound
[0165]
[0166] Among them, a' is 8 to 98, and b' is 0 to 17.
[0167] (B2) Example 3 of Compound
[0168]
[0169] Among them, a' is 22-97, b' is 0-13, and c' is 1-6.
[0170] [Chemical formula 14]
[0171] (B2) Compound Example 4
[0172]
[0173] Among them, a' is 11-97, b' is 0-15, and c' is 1-7.
[0174] (B2) Example 5 of Compound
[0175]
[0176] Among them, a'+b'+c'+d'+e' is 10 to 100, c' is less than 13, d' is less than 6, and the molecular end is Me 3 SiO 1 / 2 Unit termination.
[0177] (B2) Compound Example 6
[0178]
[0179] Wherein, a'+b'+c'+d'+e' is 10 to 100, c' is 15 or less, d' is 7 or less, and the molecular end is (Me) 2 HSiO 1 / 2 Unit termination.
[0180] More preferably, the compounds represented by the following average structural formulas can be mentioned.
[0181] [Chemical formula 15]
[0182]
[0183] (B3)Ingredients
[0184] The component (B3) may be further included as the component (B). The component (B3) is a compound having a viscosity of less than 0.5 Pa·s at 25° C., having at least two alkenyl groups in one molecule, an alkenyl content of 5 to 500 times the alkenyl content of the component (A), and having no epoxy group.
[0185] (B3) component is blended as a component that improves the curability of the composition and the adhesion of the obtained cured film to the substrate just after curing. The curability and substrate adhesion improvement effect brought about by the addition of (B3) component is obtained by the large difference in viscosity and alkenyl content with (A) component. (A) component is a high-viscosity organopolysiloxane, which will be high-molecular-weighted through a slight cross-linking reaction. Therefore, as the reaction proceeds, the movement of molecules in the composition is restricted, and sometimes unreacted alkenyl and SiH groups remain. On the other hand, compared with (A) component, (B3) component has a higher alkenyl content and lower viscosity. Therefore, the restriction on the movement of molecules in the composition is less, and the reactivity with SiH groups is excellent, so the curability can be improved. In addition, since the residual SiH groups are reduced, a light peeling effect can also be obtained. Further, it is speculated that the cross-linking density is increased due to the cross-linking reaction, so the substrate adhesion just after curing is also improved.
[0186] The number of alkenyl groups in one molecule of the component (B3) is two or more, and the amount is 5 to 500 times, preferably 15 to 400 times, the amount of alkenyl groups contained in the component (A). If the number of alkenyl groups in one molecule of the component (B3) is 5 to 500 times the amount of alkenyl groups contained in the component (A), the light peeling effect can be maintained, and the adhesion of the obtained cured film to the substrate immediately after curing can be sufficiently improved.
[0187] Here, the alkenyl group contained in the component (B3) is preferably an alkenyl group having 2 to 12 carbon atoms, and more preferably -(CH 2 ) x -CH=CH 2 (x is 0 or an integer from 1 to 10), -(C=O)-CH=CH 2 or -O-(C=O)-CH=CH 2 Specific examples include vinyl, propenyl, butenyl, hexenyl, octenyl, decenyl, acryloyl, and acryloyloxy. In addition, the methylene chain may contain an ether bond, for example, -(CH 2 ) 2 -O-CH 2 -CH=CH 2 、-(CH 2 ) 3 -O-CH 2 -CH=CH 2etc. Industrially, vinyl groups and acryloyloxy groups are more preferably used.
[0188] In addition, the viscosity of the component (B3) at 25°C is less than 0.5 Pa·s, and more preferably less than 0.3 Pa·s. By being less than 0.5 Pa·s, the effect of improving the adhesion to the substrate can be fully obtained. The lower limit of the viscosity of the component (B3) at 25°C is not particularly limited, and can be set to 0.005 Pa·s, for example.
[0189] The component (B3) is preferably a hydrocarbon compound having at least two alkenyl groups, optionally containing a hydroxyl group, and optionally having an aryl group or an oxygen atom (ether bond, ester bond, etc.) in one molecule, or an organopolysiloxane represented by the following general formula (6).
[0190] [Chemical formula 16]
[0191]
[0192] In the above formula (6), R 6 are optionally the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms and having no aliphatic unsaturated bond, or alkenyl groups having 2 to 12 carbon atoms and optionally containing oxygen atoms, at least two R 6 It is an alkenyl group.
[0193] As the above-mentioned monovalent hydrocarbon group having 1 to 20 carbon atoms and not having an aliphatic unsaturated bond, specifically, there can be listed a monovalent hydrocarbon group having 1 to 10 carbon atoms selected from the following groups: alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, and butyl; cycloalkyl groups having 5 to 8 carbon atoms, such as cyclohexyl; aryl groups having 6 to 10 carbon atoms, such as phenyl and tolyl; aralkyl groups having 7 to 10 carbon atoms, such as benzyl; or hydroxypropyl, cyanoethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, etc., obtained by replacing some or all of the hydrogen atoms bonded to the carbon atoms of these groups with hydroxyl, cyano, halogen atoms, etc. In particular, from the viewpoint of releasability, alkyl groups and aryl groups are preferred, and methyl, ethyl, propyl, and phenyl groups are further more preferred.
[0194] Examples of the alkenyl group having 2 to 12 carbon atoms which may have an oxygen atom include the same groups as those mentioned above for the alkenyl group having 2 to 12 carbon atoms. Among them, a vinyl group and an alkenyloxy group are preferred.
[0195] In the above formula (6), m', n', o' and p' are selected from positive numbers that make the viscosity within the above range, and in particular, m' is an integer greater than 2, preferably an integer from 2 to 100, n' is an integer greater than 0, preferably an integer from 0 to 500, more preferably an integer from 0 to 300, and further preferably an integer from 0 to 140, o' is an integer greater than 0, preferably an integer from 0 to 30, p' is an integer greater than 0, preferably an integer from 0 to 30, 2≤m'+n'+o'+p'≤502, preferably 2≤m'+n'+o'+p'≤300, and further preferably 2≤m'+n'+o'+p'≤150.
[0196] The organopolysiloxane represented by the formula (6) may be linear, branched or cyclic.
[0197] More preferably, the component (B3) is a partially hydrolyzed condensate of an alkoxysilane mixture containing 10 mol % or more of an organoalkoxysilane represented by the following general formula (6-1), and is a compound having a linear or branched and / or cyclic siloxane structure, or a mixture thereof.
[0198] Alkenyl-Si(OR11) 3 ···(6-1)
[0199] In formula (6-1), Alkenyl is a monovalent organic group having an alkenyl group, and R11 may be the same or different and is an unsubstituted or substituted hydrocarbon group or a hydroxyl group having 1 to 20 carbon atoms and not having an aliphatic unsaturated bond and optionally containing an oxygen atom.
[0200] When the (B3) component is blended, the number of moles of hydrogen atoms bonded to silicon atoms in the composition of the present invention is preferably an amount equivalent to 0.5 to 10 times the total number of moles of alkenyl groups in the (A) component and the (B3) component. Here, the hydrogen atoms bonded to silicon atoms can constitute, for example, Si-H groups. Therefore, the hydrogen atoms bonded to silicon atoms in the composition include hydrogen atoms of the Si-H group of the (B2) compound. When the composition of the present invention includes the (C) component described below, the hydrogen atoms bonded to silicon atoms in the composition further include hydrogen atoms bonded to silicon atoms possessed by the (C) component.
[0201] In addition, the amount of the component (B3) when blended can be set, for example, in the range of 0.1 to 10 parts by mass, preferably in the range of 0.1 to 5 parts by mass, relative to 100 parts by mass of the organopolysiloxane of the component (A). By setting the blending amount of the component (B3) to 0.1 to 10 parts by mass relative to 100 parts by mass of the component (A), the light peeling effect can be maintained and the substrate adhesion can be sufficiently improved.
[0202] Specific examples of the component (B3) include the following.
[0203] [Chemical formula 17]
[0204] Example 1 of component (B3)
[0205]
[0206] Among them, a"+b" is 2 to 150, a" is 2 or more, and the molecular ends are blocked with (a"+b"+2) or less methoxy groups, ethoxy groups, and propoxy groups, and a part of them may be substituted with hydroxyl groups.
[0207] Example 2 of component (B3)
[0208]
[0209] Among them, c"+d"+e" is 2 to 150, e" is 2 or more, and the molecular ends are blocked with (c"+2) or less methoxy, ethoxy, or propoxy groups, and a part of them may be substituted with hydroxyl groups.
[0210] Example 3 of component (B3)
[0211]
[0212] Among them, a"+b"+c"+d"+e" is 2 to 150, a" is greater than 2, and the molecular ends are capped with (a"+b"+c"+2) or less methoxy, ethoxy, or propoxy groups, and a part of them may be substituted by hydroxyl groups.
[0213] The following examples can be more preferably cited.
[0214] [Chemical formula 18]
[0215]
[0216] A compound represented by the above average formula and having 7 or less methoxy groups at the molecular ends.
[0217]
[0218] A compound represented by the above average formula and having 10 or less methoxy groups at the molecular ends.
[0219] [(C): Organohydrogenpolysiloxane]
[0220] The silicone composition for release sheets of the present invention may further include (C) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule and different from the compound (B2). In the composition of the present invention, the component (C) is an optional component.
[0221] The organohydrogenpolysiloxane of the component (C) has at least two hydrogen atoms bonded to silicon atoms (hereinafter also referred to as "SiH groups") in one molecule, and the SiH groups undergo addition reaction with the alkenyl groups in the component (A) and the optional component (B3) to form a cured film.
[0222] The organohydrogenpolysiloxane of component (C) is not particularly limited as long as it has at least two hydrogen atoms bonded to silicon atoms in one molecule and is different from compound (B2). Specific differences from compound (B2) include, for example, having an amount of Si-H groups of less than 1.3 mol / 100 g.
[0223] Examples of the component (C) include a component represented by the following average composition formula (7).
[0224] R 7 s H t SiO (4-s-t) / 2 (7)
[0225] In the above formula (7), R 7 They may be the same or different and are unsubstituted or substituted monovalent hydrocarbon groups without aliphatic unsaturated bonds. Specifically, examples include: alkyl groups preferably having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, and butyl; cycloalkyl groups preferably having 5 to 8 carbon atoms, such as cyclohexyl; aryl groups preferably having 6 to 10 carbon atoms, such as phenyl and tolyl; aralkyl groups preferably having 7 to 10 carbon atoms, such as benzyl; or hydroxypropyl, cyanoethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, etc., obtained by replacing some or all of the hydrogen atoms bonded to the carbon atoms of these groups with hydroxyl, cyano, halogen atoms, etc. Among them, alkyl groups and aryl groups are preferred, and methyl groups are more preferred from the viewpoint of increasing the addition reaction rate.
[0226] s is a positive number of 0.1 to 2, preferably a positive number of 0.2 to 1.5, t is a positive number of 0.1 to 3, preferably a positive number of 0.2 to 2, and s+t satisfies 3.1 or less, and particularly satisfies 0.5 to 2.7.
[0227] Examples of the organohydrogenpolysiloxane represented by the above formula (7) include: 7 HSiO 2 / 2 Unit (R 7 With the above R 7 Same, the following are the same), HSiO 3 / 2 Unit and R 7 2 HSiO 1 / 2 At least one of the units may further include R 7 2 SiO 2 / 2 Unit, R7 SiO 3 / 2 Unit and R 7 3 SiO 1 / 2 The polymer or copolymer preferably has at least two, preferably 10 to 100, R 7 HSiO 2 / 2 Unit or R 7 2 HSiO 1 / 2 In addition, any amount of SiO 4 / 2 unit.
[0228] The content of SiH groups in the organopolysiloxane of the component (C) is preferably 0.1 mol / 100 g or more and less than 1.3 mol / 100 g, and particularly preferably 0.2 mol / 100 g or more and less than 1.3 mol / 100 g.
[0229] The organohydrogenpolysiloxane may be linear, branched, or cyclic, or a mixture thereof.
[0230] The viscosity of the component (C) at 25° C. is preferably 0.001 to 10 Pa·s, particularly preferably 0.005 to 5 Pa·s. When the viscosity of the component (C) is 0.001 to 10 Pa·s, both appropriate curability and workability can be achieved.
[0231] Specific examples of the component (C) include the following, but are not limited thereto. In the following formulae, Me and Ph represent a methyl group and a phenyl group, respectively.
[0232] [Chemical formula 19]
[0233]
[0234] [Chemical formula 20]
[0235]
[0236] The amount of component (C) is preferably such that the number of moles of hydrogen atoms bonded to silicon atoms is equivalent to 0.5 to 10 times the number of moles of alkenyl groups in the composition, and particularly preferably such that the number of moles of hydrogen atoms bonded to silicon atoms is equivalent to 1 to 5 times the number of moles of alkenyl groups in the composition. In the composition, by making the number of moles of hydrogen atoms bonded to silicon atoms equivalent to 0.5 to 10 times the number of moles of alkenyl groups, it is possible to maintain light peelability and further improve curability and adhesion to the substrate.
[0237] As described above, the (B2) compound contains Si-H groups and therefore contains hydrogen atoms bonded to silicon atoms. Therefore, when the (C) component is included, the hydrogen atoms bonded to silicon atoms in the composition include the (C) component and the hydrogen atoms bonded to silicon atoms of the (B2) compound. In addition, as described above, when the composition of the present invention contains the (B3) component, it is preferred that the number of moles of hydrogen atoms bonded to silicon atoms in the composition of the present invention is an amount equivalent to 0.5 to 10 times the total number of moles of alkenyl groups in the (A) component and the (B3) component. That is, when the composition of the present invention contains components (B3) and (C), it is preferred that the total molar number of hydrogen atoms bonded to silicon atoms of the components (C) and (B2) is in the range of 0.5 to 10 times the total molar number of alkenyl groups of the components (A) and (B3), and it is particularly preferred that the total molar number of hydrogen atoms bonded to silicon atoms of the components (C) and (B2) is in the range of 1 to 5 times the total molar number of alkenyl groups of the components (A) and (B3).
[0238] Furthermore, in order to obtain an appropriate crosslinking density, the amount of the component (C) is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass based on 100 parts by mass of the component (A).
[0239] [(D): Platinum group metal catalyst]
[0240] The platinum group metal catalyst of component (D) is a catalyst for promoting the addition reaction of component (A) and component (B3) with compound (B2) and component (C). As a catalyst for promoting the so-called hydrosilylation reaction, any catalyst known to those skilled in the art can be used. As such a platinum group metal catalyst, for example, catalysts such as platinum, palladium, rhodium, and ruthenium can be listed, among which platinum catalysts are particularly preferably used. As such a platinum catalyst, for example, chloroplatinic acid, an alcohol solution or an aldehyde solution of chloroplatinic acid, a complex of chloroplatinic acid and various olefins or vinylsiloxanes, various olefins or vinylsiloxane complexes of platinum, etc. can be listed.
[0241] The amount of component (D) is a catalytic amount and is preferably within a range of 10 to 1,000 ppm, particularly preferably 20 to 500 ppm, based on the mass of component (A) in terms of mass of platinum group metals in order to obtain a good cured film.
[0242] [(E): Organic solvent for dilution]
[0243] The silicone composition of the present invention may contain an organic solvent for dilution as an optional component. Specifically, 0 to 20,000 parts by mass of the organic solvent of the component (E) is used per 100 parts by mass of the component (A).
[0244] The silicone composition of the present invention may be a solvent-free composition obtained by blending specific amounts of the above-mentioned components (A), (B) and (D), and optional components. By diluting with an organic solvent, practical advantages such as improved coating workability, improved coating film thickness, improved surface smoothness, and other coating film conditions can be obtained.
[0245] As the organic solvent that can be used, there are aromatic hydrocarbon compounds such as toluene and xylene; aliphatic hydrocarbon compounds such as hexane, heptane, and isoparaffin; ketone compounds such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester compounds such as ethyl acetate and butyl acetate; ether compounds such as diisopropyl ether and 1,4-dioxane. Any organic solvent can be used as long as it is a compound that can dissolve silicone. It can also be dispersed or diluted in water in any proportion and used.
[0246] The amount of component (E) when added is preferably 100 to 20,000 parts by mass, particularly preferably 200 to 10,000 parts by mass, relative to 100 parts by mass of component (A). By setting the amount of component (E) to 100 to 20,000 parts by mass, the above-mentioned advantages due to dilution can be fully obtained.
[0247] [(F) Peel force controlling ingredient]
[0248] Furthermore, the composition of the present invention may contain a peeling force control component (F). As the (F) component, the following (F1) component and / or the following (F2) component may be used, and the blending amount is 0.1 to 20 parts by mass relative to 100 parts by mass of the (A) component. By including the (F) component in this amount, the adhesion to the substrate can be maintained, and the peeling force can be appropriately controlled.
[0249] (F1): A peel force control component containing an acrylic-silicone graft copolymer
[0250] Component (F1) is a peeling force control component containing an acrylic-silicone graft copolymer. By blending this component, a very small peeling force can be obtained, and an excellent cured film (peeling film) with a high residual adhesive ratio of the adhesive sheet after peeling can be obtained.
[0251] The acrylic-silicone graft copolymer used in the present invention is a copolymer having a weight average molecular weight of 1,000 to 100,000, which is obtained by radically polymerizing an organopolysiloxane compound (a) having an acryloyl group and / or a methacryloyl group (hereinafter also referred to as a (meth)acryloyl group) and a radical polymerizable monomer (b) having one radical polymerizable group in one molecule.
[0252] According to the measurement results of gel permeation chromatography (hereinafter referred to as "GPC") using toluene as a developing solvent, the weight average molecular weight of the copolymer is 1,000 to 100,000, preferably 1,500 to 50,000, and more preferably 2,000 to 30,000 when converted to polystyrene. When the weight average molecular weight is 1,000 to 100,000, a high residual adhesion rate and excellent dispersibility in the silicone composition can be achieved.
[0253] [Component (a): Organopolysiloxane compound having a (meth)acryloyl group]
[0254] The organopolysiloxane compound (a) used in the present invention is not particularly limited as long as it has a (meth)acryloyl group. From the perspectives of ease of copolymerization with a radical polymerizable monomer (b) having one radical polymerizable group in one molecule, ease of synthesis of the organopolysiloxane compound itself, and the effect of the release force control component, it is preferably a radical polymerizable silicone macromonomer represented by the following general formula (3).
[0255] [Chemical formula 21]
[0256]
[0257] In the above general formula (3), R 2 is a hydrogen atom or a methyl group, and X is a group selected from an oxygen atom, an NH group and a sulfur atom (a divalent functional group).
[0258] Y is a divalent hydrocarbon group having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, which may contain an oxygen atom, and specifically includes: alkylene groups such as methylene, ethylene, propylene (trimethylene, methylethylene), butylene (tetramethylene, methylpropylene), hexamethylene, and octamethylene; arylene groups such as phenylene; combinations of two or more of these groups (alkylene-arylene, etc.); -CH 2 CH 2 -O-CH 2 CH 2 -;-CH 2 CH 2 -O-CH 2 CH 2 -O-CH 2 CH 2 -;-CH(CH 3 )CH 2 -O-CH(CH 3 )CH 2 -;-CH 2 CH 2 CH 2 CH 2 -O-CH 2CH 2 CH 2 CH 2 -, etc. As Y, ethylene, propylene and butylene are preferred.
[0259] f is an integer of 0 to 1,000, preferably an integer of 0 to 500, and more preferably an integer of 0 to 200.
[0260] R 3 They may be the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20, preferably 1 to 18 carbon atoms, hydrogen atoms, hydroxyl groups, alkoxy groups having 1 to 10, preferably 1 to 8 carbon atoms, or substituents represented by the following general formula (4).
[0261] [Chemical formula 22]
[0262]
[0263] In formula (4), R 4 They may be the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, preferably 1 to 18 carbon atoms, hydrogen atoms, hydroxyl groups, or alkoxy groups having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms. g is an integer of 0 to 300.
[0264] Here, as R 3 , R 4 The unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms includes: alkyl groups such as methyl, ethyl, propyl, and butyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl and tolyl; aralkyl groups such as benzyl and phenethyl; or hydroxypropyl, cyanoethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, etc. obtained by replacing some or all of the hydrogen atoms bonded to the carbon atoms of these groups with hydroxyl, cyano, halogen atoms, etc. Specific examples of alkoxy groups having 1 to 10 carbon atoms include methoxy, ethoxy, propoxy, butoxy, etc. As R 3 , preferably an alkyl group or an aryl group, and more preferably an alkyl group having 1 to 5 carbon atoms. 4 , preferably an alkyl group or an aryl group, and more preferably an alkyl group having 1 to 5 carbon atoms.
[0265] g is an integer of 0-300, preferably an integer of 0-100, and more preferably an integer of 0-50.
[0266] Specific examples of the component (a) include the following, but are not limited thereto: Me, Ome, and Ph in the following formulae represent a methyl group, a methoxy group, and a phenyl group, respectively.
[0267] [Chemical formula 23]
[0268]
[0269] [Chemical formula 24]
[0270]
[0271] [Chemical formula 25]
[0272]
[0273] [Component (b): Radical polymerizable monomer]
[0274] The radical polymerizable monomer (b) used in the present invention may be used alone or in combination of two or more. There are no particular limitations as long as the monomer has one radical polymerizable group in one molecule.
[0275] As the component (b), there can be exemplified compounds having one radical polymerizable group such as an acryloyl group, a methacryloyl group, a styryl group, a cinnamate group, a vinyl group, an allyl group, etc. in one molecule, and specifically, there can be exemplified (meth)acrylic acid ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearate (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, trifluoropropyl (meth)acrylate, perfluorobutyl ethyl (meth)acrylate, and perfluorooctyl ethyl (meth)acrylate; epoxy radical polymerizable monomers such as glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, propylene glycol, and 1,2-dextrin; 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate and other hydroxyl radical polymerizable monomers; γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyldimethoxysilane, γ-methacryloxypropyl dimethylmethoxysilane, γ-methacryloxypropyl triethoxysilane, γ-methacryloxypropyl methyldiethoxysilane, γ-methacryloxypropyl tributoxysilane, γ-methacryloxypropyl triisopropenoxysilane, γ-acryloxypropyl trimethoxysilane, acryloxymethyl trimethoxysilane, γ-acryloxypropyl triethoxysilane, γ-acryloxypropyl methyldiethoxysilane, styryl trimethoxysilane, styryl triethoxysilane, α-methylstyryl trimethoxysilane and other free radical polymerizable silane compounds; polyoxyalkylene radical polymerizable monomers; glycerol (meth)acrylate.
[0276] Considering the light peeling effect and high residual adhesion rate effect obtained by the (F) peeling force control component, it is preferred to contain an alkyl (meth)acrylate having 1 to 30 carbon atoms, and more preferably to contain methyl (meth)acrylate.
[0277] [(a) component / (b) component ratio]
[0278] The polymerization mass ratio [(a) / (b)] of the organopolysiloxane compound (a) having a (meth)acryloyl group and the radical polymerizable monomer (b) having one radical polymerizable group in one molecule is preferably in the range of 30 / 70 to 99 / 1, more preferably 40 / 60 to 97 / 3, and further preferably 50 / 50 to 95 / 5. When the polymerization mass ratio [(a) / (b)] is in the range of 30 / 70 to 99 / 1, the light release effect can be maintained and sufficient compatibility with the organosilicon composition can be exhibited, thereby preventing the (F) release force control component from separating.
[0279] [Synthesis method of acrylic acid-silicone graft copolymer]
[0280] The copolymerization of the monomer raw material comprising an organic polysiloxane compound (a) having a (meth)acryloyl group and a radical polymerizable monomer (b) having one radical polymerizable group in one molecule is carried out in the presence of the following common radical polymerization initiators: peroxides such as benzoyl peroxide, diisopropylbenzene peroxide, lauroyl peroxide, tert-butyl peroxy-2-ethylhexanoate; azo compounds such as 2,2'-azobis(2-methylbutyronitrile), etc., and any of the methods of solution polymerization, emulsion polymerization, suspension polymerization, and bulk polymerization can also be applied.
[0281] In the present invention, among these polymerization methods, the solution polymerization method is particularly preferred because it is easy to adjust the molecular weight of the obtained acrylic acid-organic silicone graft copolymer to the optimal range. Examples of the solvent used in this case include: aromatic hydrocarbons such as benzene, toluene, and xylene; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; esters such as ethyl acetate, n-butyl acetate, and isobutyl acetate; alcohols such as ethanol, isopropanol, n-butanol, and isobutanol, etc., or a mixture of two or more thereof.
[0282] The polymerization temperature is preferably in the range of 50 to 180° C., particularly preferably in the range of 60 to 120° C. Under this temperature condition, the polymerization reaction can be completed in about 1 to 10 hours. The method for extracting the copolymer from the copolymerization solution is not particularly limited, and examples thereof include a method of evaporating the solvent, a method of adding a poor solvent such as water or methanol to the copolymerization solution to precipitate the copolymer, and a method of drying the copolymer.
[0283] The amount of component (F) is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of component (A). When component (F) is contained in the above preferred amount, both excellent light release effect and excellent curability can be achieved.
[0284] (F2): Linear phenyl methyl polysiloxane
[0285] The component (F2) is a phenylmethyl polysiloxane having a linear structure, and may have no functional group or may have an alkoxy group and / or a silanol group at the terminal.
[0286] The component (F2) is preferably an organopolysiloxane having a 30% by mass toluene dilution viscosity of 0.01 to 70 Pa·s at 25° C. By including the component (F2) having a viscosity within such a range, both an excellent peel force control effect and excellent productivity can be achieved.
[0287] [Other optional ingredients]
[0288] The silicone composition of the present invention is obtained by blending the above-mentioned component (A), the (B1) compound, the (B2) compound and the (D) component in specific amounts, and may further contain the above-mentioned component (B3), the (C) component, the (E) component and the (F) component as optional components in the above-mentioned preferred amounts, and other components may be added in any amounts as required. Components known as components generally used in silicone-based release agent compositions may be added in normal blending amounts.
[0289] As other optional components, for example, as pot life extenders, known components such as various organic nitrogen compounds, organic phosphorus compounds, acetylene compounds, oxime compounds, and organic chlorine compounds can be used. For example, acetylene alcohols such as 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-pentene-3-ol, and phenylbutynol; acetylene compounds such as 3-methyl-3-1-pentene-1-yne and 3,5-dimethyl-1-hexyn-3-yne; reactants of these acetylene compounds with alkoxysilanes, siloxanes, or hydrosilanes; vinyl siloxanes such as tetramethylvinylsiloxane rings; organic nitrogen compounds such as benzotriazole; and other organic phosphorus compounds, oxime compounds, and organic chromium compounds.
[0290] The amount of these compounds added may be an amount that can obtain a good pot life, and is generally preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the component (A).
[0291] When the composition of the present invention is made into an emulsion composition, a surfactant or a high molecular weight emulsifier may be blended, and the appropriate blending amount is within the range of 0.1 to 10 parts by mass based on 100 parts by mass of the component (A).
[0292] Furthermore, other known antioxidants, pigments, stabilizers, antistatic agents, defoamers, adhesion improvers other than the component (B), thickeners, and inorganic fillers such as silica may be blended as optional components as necessary.
[0293] In terms of pot life, the preparation of the silicone composition for a release sheet is preferably carried out by premixing the component (A), the compound (B1), the compound (B2), and the optional components uniformly and then adding the component (D) immediately before use.
[0294] As another preparation method, the following method is beneficial for optimizing the peeling properties of the cured product: after pre-mixing the (A) component and the optional components, add the (B) component (the (B1) compound and the (B2) compound, and the optional (B3) component) and the (D) component as the adhesion-enhancing component immediately before use.
[0295] Furthermore, it is also preferable to use a method of adding the (B1) compound and the (B2) compound separately. The (B1) and (B2) compounds have different effects on improving adhesion, so from the perspective of adhesion, peeling properties, and cost, it is ideal to adjust the optimal addition amounts of the (B1) and (B2) compounds according to the use of the composition and use them.
[0296] When used as an additive as described above, the compound (B1) and / or (B2) may be used as an additive composition in which the compound (B1) and / or (B2) is mixed with other components.
[0297] [Release sheet (coated product)]
[0298] The release sheet of the present invention is obtained by applying the silicone composition for a release sheet of the present invention to a paper substrate or a film substrate and curing the composition.
[0299] The release sheet of the present invention may include, for example, a sheet-like substrate such as a paper substrate or a film substrate, and a cured product (cured film) of the silicone composition for a release sheet of the present invention formed on the substrate.
[0300] The cured film can be formed on the substrate by diluting the silicone composition for release sheet of the present invention as is or further diluting it with the diluting solvent or water within the above range, and applying the composition by a coating method such as coating with a comma coater, a die lip coater, a roll coater, a die coater, a knife coater, a blade coater, a rod coater, a kiss coater, a gravure coater, a wire bar coater, screen coating, dip coating, or cast coating at a concentration of 0.01 to 100 g / m 2 After coating on one or both sides of a sheet substrate such as paper or film, heat at 50 to 200° C. for 1 to 120 seconds. When a cured film (release layer) is formed on both sides of the substrate, it is preferred to perform the cured film formation operation on each side of the substrate.
[0301] Examples of substrates include: various coated papers such as polyethylene laminated paper, glassine paper, high-grade paper, kraft paper, and clay-coated paper; synthetic paper such as YUPO; polyethylene film, polypropylene film such as CPP or OPP; polyester film such as polyethylene terephthalate film (PET film); polyamide film, polyimide film, polylactic acid film, polyphenol film, polycarbonate film, etc. In order to improve the adhesion between these substrates and the cured film (peeling layer), a substrate subjected to corona treatment, etching treatment, or plasma treatment may also be used.
[0302] Example
[0303] Hereinafter, the present invention will be specifically described with reference to synthesis examples, examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, parts represent parts by mass.
[0304] Preparation of silicone composition and release film
[0305] <Raw materials used>
[0306] (A)Ingredients
[0307] (A-1)
[0308] The composition is composed of 0.04 mol% (CH 2 =CH) 3 SiO 1 / 2 The trivinylsiloxane units represented by 3 )(CH 2 =CH)SiO 2 / 2 The methylvinylsiloxane units represented by 3 ) 2 SiO 2 / 2 Organopolysiloxane composed of dimethylsiloxane units represented by
[0309] 30 mass% toluene dilution viscosity at 25°C is 15 Pa·s
[0310] Alkenyl content = 0.01 mol / 100g
[0311] (A-2)
[0312] The 0.02 mol% (CH 3 ) 2 (CH 2 =CH)SiO 1 / 2 dimethylvinylsiloxane units, 3.4 mol% (CH 3 )(CH 2 =CH)SiO 2 / 2 The methylvinylsiloxane units represented by 3 ) 2 SiO 2 / 2 The organopolysiloxane composed of dimethylsiloxane units represented by the formula (I) has a 30% by mass toluene dilution viscosity at 25° C. of 10 Pa·s.
[0313] Alkenyl content = 0.04 mol / 100g
[0314] (B) Ingredients
[0315] (B1-1) Compound
[0316] 118.2 parts by mass (0.5 mol) of 3-glycidoxypropyltrimethoxysilane, 68.1 parts by mass (0.5 mol) of methyltrimethoxysilane, and 15 parts by mass (0.83 mol) of water were subjected to partial hydrolysis condensation at 70° C. for 5 hours in the presence of hydrochloric acid to obtain an epoxy group-containing siloxane oligomer
[0317] The viscosity at 25°C is 0.05 Pa·s
[0318] The average degree of polymerization is 5
[0319] Siloxane units having epoxy groups bonded to silicon atoms via carbon atoms are 50 mol%
[0320] The silanol group content was 0.012 mol / 100 g, and the silanol content was measured by the Grignard method of quantifying the amount of methane generated using methylmagnesium iodide.
[0321] Alkoxy content is 0.9 mol / 100g
[0322] (B1-2) Compound
[0323] 166.7 parts by mass (0.7 mol) of tetraethoxysilane, 47.3 parts by mass (0.2 mol) of 3-glycidoxypropyltrimethoxysilane, 17.8 parts by mass (0.1 mol) of methyltriethoxysilane, and 15 parts by mass (0.83 mol) of water were subjected to partial hydrolysis condensation at 80° C. for 5 hours in the presence of hydrochloric acid to obtain an epoxy group-containing siloxane oligomer
[0324] The viscosity at 25°C is 0.02 Pa·s
[0325] The average degree of polymerization is 5
[0326] 20 mol% of siloxane units having epoxy groups bonded to silicon atoms via carbon atoms
[0327] The silanol content is 0.015 mol / 100g
[0328] Alkoxy content is 1.4 mol / 100g
[0329] (B1-3) Compound
[0330] An epoxy-containing siloxane oligomer obtained by partially hydrolyzing and condensing 236.3 parts by mass (1 mol) of 3-glycidoxypropyltrimethoxysilane and 9 parts by mass (0.5 mol) of water at 70° C. for 5 hours in the presence of hydrochloric acid
[0331] The viscosity at 25°C is 0.005 Pa·s
[0332] The average degree of polymerization is 2
[0333] Siloxane units having epoxy groups bonded to silicon atoms via carbon atoms are 100 mol%
[0334] The silanol content is 0.015 mol / 100g
[0335] Alkoxy content is 0.9 mol / 100g
[0336] (B1-4) Compound
[0337] The organopolysiloxane represented by the following formula
[0338] [Chemical formula 26]
[0339]
[0340] w1=42,w2=33,Ep 1 is 2-(3,4-epoxycyclohexyl)ethyl, and Me is methyl.
[0341] (B1-5) Compound
[0342] The organopolysiloxane represented by the following formula
[0343] [Chemical formula 27]
[0344]
[0345] w=20,Ep 1 is 2-(3,4-epoxycyclohexyl)ethyl, and Me is methyl.
[0346] (B1-6) Compound
[0347] Ep of compound (B1-4) 1 3-(2,4-epoxypropoxy)propyl organopolysiloxane
[0348] (B1-7) Compound
[0349] Ep of compound (B1-5) 1 3-(2,4-epoxypropoxy)propyl organopolysiloxane
[0350] (B2-1) Compound
[0351] 5 mol% (CH 3 ) 3 SiO 1 / 2 The trimethylsiloxane units represented by 3 )HSiO 2 / 2 Organohydrogenpolysiloxane composed of methylhydrogensiloxane units represented by
[0352] The viscosity at 25°C is 0.02 Pa·s
[0353] Si-H group content = 1.5 mol / 100 g
[0354] The degree of polymerization is 40
[0355] (B2-2) Compound
[0356] 2 mol% (CH 3 ) 3 SiO 1 / 2 The trimethylsiloxane units represented by 78 mol% (CH 3 )HSiO 2 / 2 methylhydrogensiloxane units, and 20 mol% of (CH 3 ) 2 SiO 2 / 2 Organohydrogenpolysiloxane composed of dimethylsiloxane units represented by
[0357] The viscosity at 25°C is 0.1 Pa·s
[0358] Si-H group content = 1.2 mol / 100 g
[0359] The degree of polymerization is 100
[0360] (B3-1)Ingredients
[0361] 27.2 parts by mass (0.2 mol) of methyltrimethoxysilane, 187.5 parts by mass (0.8 mol) of 3-(acryloyloxy)propyltrimethoxysilane, and 15.0 parts by mass (0.83 mol) of water were subjected to partial hydrolysis condensation at 70° C. for 5 hours in the presence of hydrochloric acid to obtain an alkenyl group-containing siloxane oligomer
[0362] The viscosity at 25°C is 0.04 Pa·s
[0363] The average degree of polymerization is 6
[0364] 80 mol% of siloxane units having an alkenyl group bonded to a silicon atom via a carbon atom
[0365] The alkenyl content is 0.24 mol / 100g
[0366] The silanol content is 0.009 mol / 100g
[0367] (B3-2)Ingredients
[0368] 54.1 parts by mass (0.45 mol) of dimethyldimethoxysilane, 73.3 parts by mass (0.3 mol) of diphenyldimethoxysilane, 37.1 parts by mass (0.25 mol) of vinyltrimethoxysilane, and 15.3 parts by mass (0.85 mol) of water were subjected to partial hydrolysis condensation at 70° C. for 5 hours in the presence of hydrochloric acid to obtain an alkenyl group-containing siloxane oligomer
[0369] The viscosity at 25°C is 0.10 Pa·s
[0370] The average degree of polymerization is 7
[0371] 25 mol% of siloxane units having an alkenyl group bonded to a silicon atom via a carbon atom
[0372] The alkenyl content is 0.078 mol / 100g
[0373] The silanol content is 0.011 mol / 100g
[0374] (C) Ingredients
[0375] (C-1)
[0376] 2 mol% (CH 3 ) 3 SiO 1 / 2 The trimethylsiloxane units represented by 70 mol% (CH 3)HSiO 2 / 2 methylhydrogensiloxane units, and 28 mol% of (CH 3 ) 2 SiO 2 / 2 Organohydrogenpolysiloxane composed of dimethylsiloxane units represented by
[0377] The viscosity at 25°C is 0.1 Pa·s
[0378] Si-H group content = 1.1 mol / 100 g
[0379] (D) Ingredients
[0380] Platinum-vinylsiloxane complex as catalyst
[0381] (E) Ingredients
[0382] A mixed solvent of toluene and hexane with a mass ratio of 1:1
[0383] (F)Ingredients
[0384] (F-1) Ingredient
[0385] Release force control component: acrylic acid-organic silicon graft copolymer obtained by the following Synthesis Example 1
[0386] [Synthesis example 1]
[0387] 30.0 parts of toluene were added to a glass reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a dropping device. After heating to 90-100°C, a mixture of 55.7 parts (0.067 mol) of a radical polymerizable silicone macromonomer represented by the following formula (8), 9.8 parts (0.098 mol) of methyl methacrylate, 2.5 parts (0.012 mol) of tert-butyl peroxy-2-ethylhexanoate, and 51.8 parts of toluene was added dropwise over 4 hours under nitrogen flow. Further, after polymerization at 90-100°C for 2 hours, 0.4 parts (0.002 mol) of tert-butyl peroxy-2-ethylhexanoate was added and polymerization was carried out for 2 hours. Subsequently, the mixture was dried in a vacuum dryer at 150°C / 10 mmHg to obtain an acrylic-silicone graft copolymer. The weight average molecular weight when converted to polystyrene measured by GPC was 12,000.
[0388] [Chemical formula 28]
[0389]
[0390] (F-2)Ingredients
[0391] Composed of 0.7 mol% (CH 3 ) 3 SiO1 / 2 The trimethylsiloxane units represented by 3 ) 2 SiO 2 / 2 The dimethylsiloxane units represented by 6 H 5 ) 2 SiO 2 / 2 The organopolysiloxane composed of diphenylsiloxane units represented by
[0392] The viscosity at 25°C is 3.00 Pa·s
[0393] (Ingredient G)
[0394] Pot life extender: 3-methyl-1-butyn-3-ol
[0395] <Examples 1 to 20, Comparative Examples 1 to 20>
[0396] Using the above-described components (A) to (E) and (G) as raw materials, a coating composition was prepared according to the following procedures.
[0397] Components (A) to (C) were placed in a flask according to the ratios shown in Tables 1 and 2, and 3,200 parts of component (E) and 3 parts of component (G) were added and stirred to dissolve. Component (D) was added to the resulting solution in an amount of 100 ppm relative to component (A) in terms of platinum mass, and stirred and mixed to obtain a coating composition. A release film (coated product) was prepared using the composition in the following manner and evaluated.
[0398] <Examples 21 to 24>
[0399] Using the above-described components (A) to (G) as raw materials, a coating composition was prepared according to the following procedures.
[0400] Components (A) to (C) and (F) were placed in a flask according to the ratios shown in Table 2, and 3,200 parts of component (E) and 3 parts of component (G) were added and stirred to dissolve. Component (D) was added to the resulting solution in an amount of 100 ppm relative to component (A) in terms of platinum mass, and stirred and mixed to obtain a coating composition. A release film (coated product) was prepared using the composition in the following manner and evaluated.
[0401] <Evaluation>
[0402] [Curing properties (adhesion immediately after curing)]
[0403] A bar coater was used to coat the solid content at 0.1 g / m 2The obtained composition was coated on a PET film having a thickness of 38 μm, and heated in a hot air dryer at 100°C for a specified number of seconds (30 seconds or 60 seconds) to form a release agent layer (cured film) to obtain a release film. The release agent layer was scratched 10 times with a finger, and the presence of turbidity and peeling was observed visually, and evaluated based on the following criteria.
[0404] A: No turbidity or shedding was observed at 30 seconds.
[0405] B: Turbidity and shedding were observed at 30 seconds, but neither turbidity nor shedding was observed at 60 seconds.
[0406] C: Turbidity and shedding were observed at 60 seconds.
[0407] The results are shown in Tables 1 and 2 below.
[0408] [Adhesion]
[0409] A bar coater was used to coat the solid content at 0.1 g / m 2 The obtained composition was coated on a PET film having a thickness of 38 μm, and heated in a hot air dryer at 120° C. for 40 seconds to form a release agent layer to obtain a release film. The obtained release film was stored at 25° C. and 50% RH for one week, or at 60° C. and 90% RH for one week. The release agent layer was scratched 10 times with a finger, and the presence of turbidity and peeling was observed visually, and evaluated based on the following criteria.
[0410] A: No turbidity or shedding was observed.
[0411] B: Turbidity was observed, but no shedding was observed.
[0412] C: Turbidity or shedding was observed.
[0413] The results are shown in Tables 1 and 2 below.
[0414] [Peel force]
[0415] A bar coater was used to coat the solid content at 0.1 g / m 2 The compositions obtained in Examples 5 to 7, 13, 18 to 21 and 23, and Comparative Examples 1, 3 and 20 were coated on a PET film having a thickness of 38 μm, heated in a hot air dryer at 120° C. for 40 seconds to form a release agent layer (cured film), and evaluated according to the FINAT method in the following steps.
[0416] An adhesive tape (Tesa 7475 tape, a product name manufactured by Tesa Tape Inc.) with a width of 25 mm was attached to the surface of the release agent layer and processed under the following two pressure bonding conditions: 70 g / cm at 25°C.2 Load of 20g / cm2, treated for 20 hours (compression bonding A); applied in a dryer at 70°C 2 After air cooling for about 30 minutes, the Tesa7475 tape was stretched at an angle of 180° and a peeling speed of 0.3 m / min using a tensile tester (manufactured by Shimadzu Corporation, DSC-500 type tester) to measure the force (N / 25 mm) required for peeling.
[0417] The results are shown in Table 3 below.
[0418] [Residual Adhesion Ratio]
[0419] A release agent layer was formed in the same manner as in the above-mentioned peeling force evaluation, and a polyester adhesive tape (Nitto 31B, trade name manufactured by NITTO DENKO CORPORATION) with a width of 25 mm was attached to the surface of the release agent layer. 2 The polyester adhesive tape was then peeled off from the release agent layer and attached to a SUS stainless steel plate. Then, a tensile tester was used to peel off the polyester adhesive tape from the SUS stainless steel plate and the peeling force F was measured.
[0420] In addition, a polyester adhesive tape was attached to a tetrafluoroethylene plate instead of a release agent layer, and the treatment was carried out in the same manner, and the peeling force F was measured. 0 .
[0421] Then, according to (peel force F / peel force F 0 The residual adhesive ratio is calculated by the formula of )×100(%). The higher the residual adhesive ratio, the smaller the effect of contact with the release agent layer on the adhesiveness of the adhesive surface of the adhesive tape, and the release agent layer can be evaluated as an excellent release agent layer that can suppress the decrease in the adhesive force of the adhesive tape after peeling.
[0422] The results are shown in Table 3 below.
[0423] [Table 1]
[0424]
[0425] [Table 2]
[0426]
[0427] [Table 3]
[0428]
[0429] Peel force: Peel off from the adhesive surface at a peeling speed of 0.3m / min and 180 degrees
[0430] Crimp A: 70g / cm 2 Load, press-fit at 25℃ for 20 hours
[0431] Crimp B: 20g / cm 2 Load, press-fit at 70℃ for 20 hours
[0432] Residual adhesion rate: 20g / cm2 with Nitto 31B tape 2 The peeled tape was attached to a SUS plate and pressed once back and forth with a 2 kg tape roller. The adhesion force was measured in the same manner as the peeling force. The blank group used a Teflon (registered trademark) plate treated in the same manner as the test piece and set the measured value to 100%.
[0433] As can be seen from the results of Table 1 and Table 2, the compositions of Examples 1 to 24 of the present invention have excellent curing properties and can show excellent adhesion to the substrate, and can form a release agent layer (cured film) that can maintain the excellent adhesion for a long time even in harsh environments such as high temperature and high humidity. In addition, as can be seen from the results of Table 3, the compositions of Examples 5 to 7, 13, 18 to 21 and 23 of the present invention can show that the peeling force will not increase due to the addition of a close-fitting agent, and can provide a release agent layer that does not significantly damage the adhesion of the tape. The compositions of Examples 1 to 4, 8 to 12, 14 to 17, 22 and 24 of the present invention are also the same as the compositions of the embodiments whose results are shown in Table 3, and the peeling force will not increase due to the addition of a close-fitting agent, and can provide a release agent layer that does not significantly damage the adhesion of the adhesive tape.
[0434] On the other hand, the composition of Comparative Example 1 contains neither the (B1) compound nor the (B2) compound. The compositions of Comparative Examples 2 and 3 contain no (B1) compound. The compositions of Comparative Examples 4 and 19 contain no (B2) compound. As a result, the release agent layers obtained from the respective compositions of Comparative Examples 1 to 4 and 19 cannot maintain adhesion to the substrate for a long time under a harsh environment. In addition, as can be seen from the comparison between Comparative Example 4 and Comparative Example 19, even if the amount of the (B1) compound is increased, if the (B2) compound is not included, adhesion to the substrate cannot be maintained for a long time under a harsh environment.
[0435] The amount of the (B1) compound in Comparative Examples 5 and 6 is 25 parts by mass relative to 100 parts by mass of the (A) component, which is too much. As a result, the release agent layer obtained from the compositions of Comparative Examples 5 and 6 cannot maintain the adhesion to the substrate for a long time under a harsh environment. On the other hand, the amount of the (B1) compound in the composition of Comparative Example 20 is 0.05 parts by mass relative to 100 parts by mass of the (A) component, which is too little. As a result, the release agent layer obtained from the composition of Comparative Example 20 cannot maintain the adhesion to the substrate for a long time under a harsh environment.
[0436] The Si-H group content of the compound (B2-2) used in Comparative Examples 7 and 8 was 1.2 mol / 100 g. As a result, the release agent layers obtained from the compositions of Comparative Examples 7 and 8 could not maintain adhesion to the substrate for a long period of time under a 25° C. (harsh) environment.
[0437] The average degree of polymerization of the (B1-3) compound used in Comparative Examples 9 and 10 was 2. As a result, the release agent layers obtained from the compositions of Comparative Examples 9 and 10 could not maintain adhesion to the substrate for a long period of time under a severe environment.
[0438] The compounds (B1-4) to (B1-7) used in Comparative Examples 11 to 18 all contained no silanol group or alkoxy group. As a result, the release agent layers obtained from the compositions of Comparative Examples 11 to 18 could not maintain adhesion to the substrate for a long period of time under a severe environment.
[0439] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any technical solution having substantially the same structure and having the same function and effect as the technical concept described in the claims of the present invention is included in the protection scope of the present invention.
Claims
1. An addition-curable silicone composition for a release sheet, characterized in that: It contains: 100 parts by mass of (A) an organopolysiloxane having at least two alkenyl groups in one molecule, an alkenyl content of 0.001 to 0.2 mol / 100 g, and a 30% by mass toluene dilution viscosity at 25° C. of 0.01 to 70 Pa·s; (B) A component comprising the following compounds (B1) and (B2): 0.1 to 20 parts by mass of an organopolysiloxane (B1) containing 10 mol% or more of a siloxane unit having a glycidyl group and / or a glycidoxy group bonded to a silicon atom via a carbon atom, containing 0.002 to 0.02 mol / 100g of a silanol group, containing 0.5 to 2.5 mol / 100g of an alkoxy group, and having an average degree of polymerization of 3 to 50, (B2) an organohydrogensiloxane having 1.3 mol / 100 g or more of Si-H groups and a degree of polymerization of 10 to 100; a catalytic amount of (D) a platinum group metal catalyst; and 0 to 20,000 parts by mass of (E) an organic solvent, The mass fraction of the compound (B2) is 0.02 to 1 times the mass fraction of the compound (B1).
2. The silicone composition for a release sheet according to claim 1, wherein It further comprises (C) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule and being different from the compound (B2), wherein the amount of the component (C) is such that the total number of moles of hydrogen atoms bonded to silicon atoms of the compound (B2) and the component (C) is 0.5 to 10 times the number of moles of alkenyl groups in the composition.
3. The silicone composition for a release sheet according to claim 1, wherein The compound (B1) is an organoalkoxysilane represented by the following general formula (1-1), and a partially hydrolyzed condensate of at least one of the organoalkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), and is an organopolysiloxane having a linear siloxane structure, a branched siloxane structure, or a cyclic siloxane structure, or a mixture thereof. (R12)2-Si(OR1)2····(1-2) R12Si(OR1)3····(13) Si(OR1)4····(1-4) In formulas (1-1), (1-2), (1-3) and (1-4), R1 is optionally the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and not having an aliphatic unsaturated bond, optionally containing an oxygen atom, or a hydrogen atom, R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and n is an integer from 3 to 10.
4. The silicone composition for a release sheet according to claim 2, wherein: The compound (B1) is an organoalkoxysilane represented by the following general formula (1-1), and a partially hydrolyzed condensate of at least one of the organoalkoxysilanes represented by the following general formulas (1-2), (1-3), and (1-4), and is an organopolysiloxane having a linear siloxane structure, a branched siloxane structure, or a cyclic siloxane structure, or a mixture thereof. (R12)2-Si(OR1)2····(12) R12-Si(OR1)3····(1-3) Si(OR1)4····(1-4) In formulas (1-1), (1-2), (1-3) and (1-4), R1 is optionally the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and not having an aliphatic unsaturated bond, optionally containing an oxygen atom, or a hydrogen atom, R12 is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and n is an integer from 3 to 10.
5. The silicone composition for a release sheet according to claim 1, wherein The compound (B2) is an organohydrogensiloxane represented by the following general formula (2-1) or (2-2), or a mixture thereof: (R12)3Si-{(R12)HSiO} m -Si(R12)3····(2-1) (R12)2HSi-{(R12)HSiO} m -SiH(R12)2····(2-2) In the formulae (2-1) and (2-2), R12 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and m is an integer of 2 to 100.
6. The silicone composition for a release sheet according to claim 2, wherein: The compound (B2) is an organohydrogensiloxane represented by the following general formula (2-1) or (2-2), or a mixture thereof: (R12)3Si-{(R12)HSiO} m -Si(R12)3····(2-1) (R12)2HSi-{(R12)HSiO} m -SiH(R12)2····(2-2) In the formulae (2-1) and (2-2), R12 may be the same or different and is an unsubstituted or substituted hydrocarbon group having 1 to 20 carbon atoms, and m is an integer of 2 to 100.
7. The silicone composition for a release sheet according to claim 1, wherein: It further comprises 0.1 to 10 parts by mass of a component (B3) as the component (B), wherein the component (B3) is a compound having a viscosity of less than 0.5 Pa·s at 25° C., wherein the component (B3) has at least two alkenyl groups in one molecule, the alkenyl content of which is 5 to 500 times the alkenyl content of the component (A), and does not have an epoxy group. The number of moles of hydrogen atoms bonded to silicon atoms in the composition is 0.5 to 10 times the total number of moles of alkenyl groups in the component (A) and the component (B3).
8. The silicone composition for a release sheet according to claim 2, wherein: It further comprises 0.1 to 10 parts by mass of a component (B3) as the component (B), wherein the component (B3) is a compound having a viscosity of less than 0.5 Pa·s at 25° C., wherein the component (B3) has at least two alkenyl groups in one molecule, the alkenyl content of which is 5 to 500 times the alkenyl content of the component (A), and does not have an epoxy group. The number of moles of hydrogen atoms bonded to silicon atoms in the composition is 0.5 to 10 times the total number of moles of alkenyl groups in the component (A) and the component (B3).
9. The silicone composition for a release sheet according to any one of claims 1 to 8, wherein It further contains the following (F1) component and / or the following (F2) component as a peel force control component (F), wherein the (F) component is 0.1 to 20 parts by mass based on 100 parts by mass of the (A) component: (F1) a release force control component comprising an acrylic-silicone graft copolymer having a weight average molecular weight of 1,000 to 100,000, wherein the acrylic-silicone graft copolymer is obtained by free radical polymerization of (a) an organopolysiloxane compound having an acryloyl group and / or a methacryloyl group represented by the following general formula (3) and (b) a radical polymerizable monomer having one radical polymerizable group in one molecule, In formula (3), R 2 is a hydrogen atom or a methyl group, X is a group selected from an oxygen atom, an NH group and a sulfur atom, Y is a divalent hydrocarbon group having 1 to 12 carbon atoms and optionally containing an oxygen atom, R 3 are optionally the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, hydrogen atoms, hydroxyl groups, alkoxy groups having 1 to 10 carbon atoms, or substituents represented by the following general formula (4), and f is an integer from 0 to 1,000, In formula (4), R 4 are optionally the same or different and are unsubstituted or substituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, hydrogen atoms, hydroxyl groups, or alkoxy groups having 1 to 10 carbon atoms, and g is an integer of 0 to 300; (F2) Linear phenylmethylpolysiloxane.
10. A peeling sheet, characterized in that: The release sheet is obtained by applying the silicone composition for a release sheet according to any one of claims 1 to 9 to a paper substrate or a film substrate and curing the resulting composition.
Citation Information
Patent Citations
Foamable bath salt having improved storage stability
JP1980007246A
Production of photoconductive treated paper
JP1981026097A
Silicone composition for forming releasable cured film
JP2011132532A
Silicone composition for release paper or release film, release paper or release film
JP2017025135A
Compositions for thermosetting silicone resins
CN102268186A