Impregnated yarn, ribbed thin-walled composite product containing the impregnated yarn, and method for making the yarn and the composite product
By using impregnation and twisting methods in thin-walled composite materials, the problem of localized impregnation of yarns is solved, better impregnation of yarns and improvement of mechanical properties are achieved, ensuring optimized performance of the materials.
Patent Information
- Application Number
- CN202080093090.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-13
AI Technical Summary
The existing technology has the problem of localized impregnation of yarns in improving the mechanical properties of thin-walled composite materials, resulting in insufficient impregnation of fibers and affecting the optimization and reproducible performance of the materials.
Using at least two continuous strands containing plant fibers, the thermoplastic polymer material in the molten state is impregnated in an impregnation tank, and a total twist between the strands is achieved in a twisting step, ensuring that the thermoplastic material is present throughout the entire volume of the fiber. Evenly distributed, resulting in impregnated yarns with high mechanical properties.
A better impregnation of the yarn is achieved, improving the mechanical strength and mechanical properties, especially in bending, tensile and compression, ensuring that the overall volume of the yarn is fully covered by the thermoplastic material.
Smart Images

Figure CN115298367B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of rib-reinforced thin-walled composite products made of yarns, and to impregnated yarns for use in the manufacture of such ribbed thin-walled composite products.
[0002] Such thin-walled composites are often used to form parts with improved mechanical properties while keeping the part lightweight. Background Art
[0003] If it is desired to reinforce a thin-walled composite product in bending as well as in compression, it is known to provide protruding reinforcements in the form of a ribbed mesh or grid, as in WO2017099585, wherein the ribs are formed above and / or below the substrate by moulding.
[0004] From EP 2648890, certain types of thin-walled composite products are known, in particular with yarns of a first thickness and yarns of a second thickness greater than the first thickness, and these yarns are used as reinforcing profiled ribs on one face of the thin-walled composite product. These yarns of the second thickness consist of twisted vegetable fibers, the twist providing these yarns of the second thickness with improved compression resistance, in particular.
[0005] Document WO2019087141 relates to a method for impregnating a grid formed by an assembly of yarns with a polymer, the method improving the quality of the impregnation, the purpose of which is to improve the bending properties of a thin-walled composite product comprising the grid on a flat base support such as a mat. To this end, polymer particles are sprinkled on one side of a grid of interwoven yarns so as to obtain a grid with a greater amount of polymer on one side, which additionally lightens the thin-walled composite product comprising such a grid. However, this method is not suitable when impregnated yarns with high mechanical properties are required, because the impregnation of the yarns of the grid is very localized.
[0006] EP2813607A1 describes the passage of a fiber bundle through an impregnation unit to form an impregnated yarn, wherein the impregnation unit contains a liquid thermoplastic polymer bath. It turns out that, in practice, the mere passage through the liquid polymer bath does not ensure a complete and perfect impregnation of the fiber bundle throughout its volume, but rather a very localized impregnation on the surface of the fiber bundle. This random and insufficient impregnation does not guarantee an optimized and reproducible performance of the reinforcing yarn in a thin-walled composite product. Summary of the invention
[0007] An object of the present invention is to provide a solution which allows obtaining an impregnated yarn for which the impregnation of the fibers is improved, whereby the mechanical properties of the impregnated yarn are increased.
[0008] Another object of the present invention is to provide a method for manufacturing a dipped yarn and a dipped yarn obtained by the manufacturing method, which are free from the limitations of known manufacturing methods and dipped yarns.
[0009] Another object of the present invention is to provide a method of manufacturing a ribbed thin-walled composite product and a ribbed thin-walled composite resulting from the manufacturing method that is free from the limitations of known manufacturing methods and thin-walled composite materials.
[0010] Another object of the present invention is to provide a method of making a thin wall composite product reinforced with ribs formed from yarns, thereby forming a ribbed thin wall composite product that is superior to the prior art.
[0011] According to the invention, these objects are achieved in particular by means of a method for producing an impregnated yarn based on at least one strand comprising vegetable fibers, in which the following steps are carried out:
[0012] - providing at least two continuous strands comprising vegetable fibers,
[0013] - providing an impregnation tank defining a curved passage between an inlet and an outlet,
[0014] - supplying the tank with a bath of thermoplastic polymer material in a molten state which permanently fills the channel,
[0015] - arranging the strands so that: they separate from one another upstream of the impregnation tank, they enter the impregnation tank through the inlet, they simultaneously follow the channel and, while doing so, are immersed in the liquid thermoplastic material and have at least one contact zone with one face of the channel, and they leave the impregnation tank through the outlet, and
[0016] - impregnating the strands by continuously advancing the strands, thereby forming strands impregnated with thermoplastic material, thereby forming an impregnated yarn;
[0017] - wherein each of the strands has a twist T1 along a first direction when the strands pass through the impregnation tank 20, and
[0018] - wherein, after the impregnation step, a yarn twisting step is also carried out, during which, downstream of the impregnation tank, a total twist of all the strands is achieved, corresponding to the twist T2 between the strands, while the thermoplastic material is still in the liquid state, whereby the thermoplastic material creates bonds between the strands in the state in which they are twisted together, resulting in the formation of an impregnated and twisted yarn, and wherein said total twist T2 is achieved along a second orientation different from the first orientation.
[0019] The advantage of this solution compared to the prior art is that it allows good impregnation of the fibers with the thermoplastic material and in particular does not allow obtaining an impregnated yarn in which only the surface parts of the strands are impregnated without systematically impregnating the strands and the core of the impregnated yarn obtained by the method.
[0020] This impregnated yarn obtained by the manufacturing method according to the invention has better mechanical strength due to this improved impregnation and in particular a more subsequent impregnation, in particular by reaching the fibers of the central part of the strand or strands (or filaments) forming the yarn, which therefore allows to achieve an improved impregnation of the yarn itself thus obtained. A greater proportion of the volume of each strand is impregnated with the thermoplastic material, which results in a greater proportion of the volume of the entire yarn being impregnated.
[0021] This good impregnation is ensured in particular due to the contact with the surface of the impregnation tank during the passage of the strand or strands in the bath of liquid thermoplastic material, since by rubbing against the hard surface, the strand or strands flatten, which allows (by this opening of the strand or strands) the fibers to unfold and thus all or most of the fibers of each strand to come into direct contact with the liquid thermoplastic material. The contact with the tank wall delimiting the passage also creates a local overpressure, which forces the thermoplastic material to penetrate into the strand and coat more or even all of its fibers.
[0022] Also according to the present invention, there is provided an impregnated yarn having at least two continuous strands comprising vegetable fibers, wherein a first single twist of the strands is in a first direction (each of the strands having an individual twist in the first orientation), and a second total twist of the strands is in a second direction different from the first direction (all of the strands having a total twist in the second orientation different from the first orientation). Preferably, the strands are impregnated with a thermoplastic material in at least 60% of their volume, each of the strands being individually twisted, and all of the strands being also twisted into a configuration held by the thermoplastic material.
[0023] Thus, such dipped yarns exhibit both a single twist of each strand and a total twist. It will be appreciated that the thermoplastic material allows bonding to be formed between all strands / filaments both in a configuration of individual twists of the strands / filaments (single twist of the strands) and in a configuration of twists of the strands / filaments together (total twist of the strands forming a twisted yarn).
[0024] As will be described in detail below, this results in an impregnated yarn with high mechanical properties, among which are improved bending, tensile and compressive strengths due to the double twist for each strand and between all strands.
[0025] According to one embodiment, the impregnated yarn further comprises at least one binding wire, which is spirally wound around all said strands, thereby forming an impregnated and bound yarn. Such a binding wire improves the shape retention of the yarn cross section and helps in particular to limit the crushing of the yarn, which is intended to form a rib on the surface of the thin-walled composite product. Therefore, this binding wire is optional. If this binding wire is present around the impregnated yarn, two spirally wound binding wires can be provided as an alternative, which can be in the same direction or, preferably, in opposite directions.
[0026] One or more of the following provisions may also be present in the dipped yarn:
[0027] - the outer fibers of the strands make an angle of between -20° and +20° with the longitudinal direction or main direction of the impregnated yarn,
[0028] - the strands have an individual twist of between 50 and 300 tpm, preferably between 100 and 200 tpm,
[0029] The impregnated yarn comprises between three and six strands, each strand having a weight between 200 and 800 tex, preferably between 300 and 600 tex.
[0030] Furthermore, according to the present invention, a method for manufacturing a thin-walled composite product is proposed, the method comprising the following steps:
[0031] - provide support, such as pads,
[0032] - producing an impregnated yarn according to the method described herein,
[0033] - assembling the impregnated yarns to form a grid in which the impregnated yarns cross each other,
[0034] - stacking grids and supports, and
[0035] - Compression moulding of the stacked grids and supports, thereby forming a composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarns.
[0036] Also according to the present invention, a method for manufacturing a thin-walled composite product is provided, the method comprising the following steps:
[0037] - producing an impregnated yarn according to the method described herein,
[0038] - provide a base yarn of smaller size than the dipped yarn,
[0039] - weaving or knitting the base yarn with the impregnated yarn to form a preform,
[0040] - Compression moulding the preform, thereby forming a composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarns.
[0041] Furthermore, according to the present invention, a solution is provided whereby a thin-walled composite product comprising an impregnated yarn as described herein is provided, said composite product having a ribbed face, said ribs being at least partially produced by said impregnated yarn.
[0042] The presence of these ribs makes it possible to increase the flexural rigidity of a part formed by or incorporating such a thin-walled composite product, while slightly increasing the weight of the part. The presence of these ribs also makes it possible to improve the impact performance of the part, during an impact, the ribs slow down the propagation of cracks in the part, thus limiting the damage, avoiding the projection of fragments and increasing the absorption of the impact energy.
[0043] As used herein, the term "thin-walled" composite product refers to a composite product whose wall thickness does not exceed 10% of the smallest dimension of the composite product or an article containing the composite product. Alternatively, within the scope of the present invention, the term "thin-walled" composite product refers to a composite product whose wall thickness does not exceed 5% of the smallest dimension of such composite product or an article containing such composite product.
[0044] The thin-walled composite product thus formed is intended to form, in particular but not exclusively, parts or portions of parts for the interior of a motor vehicle, such as dashboards, door covers, pillar and console covers, roofs, trunk lids. It may also be used to make suitcase shells, vehicle bodies, and the like.
[0045] The invention also relates to a method for manufacturing an article comprising a thin-walled portion, wherein the thin-walled portion is formed by or comprises a thin-walled composite product manufactured according to the method described herein, the article belonging to the group comprising:
[0046] Automotive body parts, including doors, roofs, hoods, fenders, spoilers, front and rear bumpers, aerodynamic kits; or automotive interior parts, including door covers, instrument panels, center consoles, pillar trims, trunk trims, roofs; or sporting goods, such as canoe shells, kayak or light boat hulls, bicycle frames; or furniture parts; or aircraft interior parts, including side panels, roof panels, luggage compartments; or light aircraft aerodynamic parts, including hoods, wheel covers; or aerodynamic fairings of any movable machine; or suitcase shells. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Embodiment examples of the invention are shown in the description illustrated by the accompanying drawings, in which:
[0048] Figure 1 The different steps of the method for making an impregnated yarn and the resulting impregnated yarn are shown, which are not part of the present invention,
[0049] Figure 2 shows the different steps of a method for producing an impregnated yarn having two strands and the impregnated yarn resulting from this method of production according to the invention,
[0050] Figure 3 The individual steps of a three-strand variant of the method for producing an impregnated yarn according to the invention and the resulting impregnated yarn are shown,
[0051] Figure 4 A unit for producing impregnated yarn is shown, which allows the implementation of Figure 3 The manufacturing method variant shown in
[0052] Figure 5 A possible embodiment of an impregnation tank is schematically shown, which allows to carry out an impregnation step of one or more strands which will become the impregnated yarn,
[0053] Fig. 6A and 6B showing respectively a first side and a second side of a ribbed thin-walled composite product comprising impregnated yarns according to the invention,
[0054] Figure 7 yes Figure 6B A magnified view of region VII of FIG. Fig. 6A and 6B impregnated yarns forming ribs on one side of the composite product, and
[0055] Figure 8 The various steps of a manufacturing method to form another type of dipped yarn are shown and are outside the scope of the present invention. DETAILED DESCRIPTION
[0056] refer to Figure 1 , Figure 1 from Figure 1From right to left of is shown the manufacturing steps of an impregnated yarn which are not part of the present invention, arrow F1 indicating the input and arrow F2 indicating the output. Here, a single strand 10a is used to continuously form an impregnated yarn 10e. Initially (after arrow F1, step A), the strand 10a is a continuous strip taken from a bobbin and comprises plant fibers 11, the direction of which does not have to be controlled. For example, the strand 10a comprises short flax / linen yarn fibers, which are substantially parallel to each other and to the general direction of the strand 10a. Then, (step B), preferably but not necessarily, a twist T1 of the strand 10a is achieved in a first direction, thereby forming a twisted strand 10b according to a separate twist in a direction which is not parallel to the general direction P0 of the strand 10a ( Figure 1 The purpose of this twist is to increase the tear strength of the strands and thus avoid breakage during the next impregnation step. However, this single twist T1 will be small (for example an angle β between 0° and 20° relative to the direction P0 of the strands 10b) in order to facilitate good impregnation in the next step. According to another possibility (without Figure 1 ), directly starting from strands 10b already individually twisted on a bobbin that feeds the production line. Then, (step C), the twisted strands 10b (or untwisted strands 10a) are impregnated with a liquid thermoplastic material 12a, for example a thermoplastic polymer (or a mixture of thermoplastic polymers) present in an impregnation tank 20. This particular impregnation step C will be described in detail below. Impregnated, possibly twisted strands 10c are obtained, which are then Figure 1 In this case, the dipped yarn 10e is also formed using the single strands.
[0057] In the case of Figure 8 In the case of , an alternative case is shown, in which the manufacturing method includes the above-mentioned steps A, C and the following step E, but does not include steps B and D: there is no single twist T1 and no additional single twist T1'. Figure 8 A single strand 10a (whose fibers 11 are substantially parallel to the direction P0 of the strand 10a) is formed to form an impregnated yarn 10e, but in Figure 8 Within the scope of the method, two strands 10a, three strands 10a or even more strands 10e may be used, which strands therefore remain untwisted throughout the method, in particular during the impregnation step C and the (optional) bundling step E.
[0058] Then, if Figure 1As shown, at the exit of the impregnation tank 20, but optionally and not necessarily, the yarn 10c can be twisted (step D), and if it has been twisted before (step B of twist T1 or twisted strands already provided), this is additional. This separate (additional) twist T1' occurs in the same direction (first twist orientation) as the separate twist T1, which increases the radial compressive strength of the yarn, and the lower twist T1 (angle β) of the outer fibers 11 in the impregnation tank 20 facilitates good impregnation. In addition or as an alternative to the twist T1' (step D) of the yarn at the exit of the tank, a preferred but not essential last step E consists in placing a binding thread 13 around the twisted impregnated strand 10c, so as to form a spiral, and this is after passing through the impregnation tank 20, while the thermoplastic material 12a that has impregnated the impregnated yarn is still liquid and has not yet completely hardened. The result is an impregnated and bound yarn 10e, in which the solidified thermoplastic material 12b acts as a binder to maintain the position and orientation of the fibers 11 between them on the one hand, and on the other hand, within the impregnated and bound yarn 10e together with the binding wire 13, the impregnated and bound yarn 10e having good cohesion, thereby giving it good radial compression resistance. At the outlet (arrow F2), the impregnated and bound yarn 10e has been formed, which can be wound onto a bobbin for further use.
[0059] refer to Figure 2 , Figure 2 Shows the combination Figure 1 and Figure 8 A variant of the method for producing a single-strand dipped yarn just described, which constitutes a method falling within the scope of the invention, is one in which two strands 10a (step A) or 10b (step B) are used to form a dipped yarn according to the invention. Each twisted strand 10b is impregnated with a liquid thermoplastic material 12a in an impregnation tank 20 (step C), and the two impregnated twisted strands 10c are then twisted together with a twist T2. In this way, the dipped yarn 10d formed is larger than each individual dipped twisted strand 10c, and this is while the thermoplastic material is still liquid 12a, without solidification in any case. In this way, this thermoplastic material acts as a bond between the two dipped twisted strands 10c, which maintains the configuration of the total twist between the two dipped twisted strands 10c in the dipped yarn 10d. In the optional but preferred final step E of laying the spiral binding threads 13 around the dipped strands 10d, because the thermoplastic material 12a is still liquid and has not fully solidified, it also acts as a bond, holding the spiral binding threads 13 around the dipped yarn 10d together and forming the dipped and twisted yarn 10e. Once the thermoplastic material 12b solidifies, it holds these bonds.
[0060] Reference now Figure 3 , Figure 3 A variant of the method for producing an impregnated yarn according to the invention is shown, in which three flat strands 10a (step A) or three twisted strands 10b (step B) are used to form the impregnated yarn. Each twisted strand 10b is impregnated with a liquid thermoplastic material 12a in an impregnation tank (step C), and the three impregnated twisted strands 10c are then twisted together in a total twist T2 (step D). In this way, the impregnated yarn 10d formed is larger than each individual impregnated twisted strand 10c, and this is while the thermoplastic material is still liquid 12a, without in any case solidification. In this way, this thermoplastic material 12 provides a bond between the three impregnated twisted strands 10c, which maintains the total twist pattern between the three impregnated twisted strands 10c in the impregnated yarn 10d. As Figure 3 As shown, if the spiral binding thread 13 is used around the impregnated yarn 10d while the thermoplastic material 12a is still liquid and has not yet fully solidified, the thermoplastic material 12a not only provides a bond between the three impregnated twisted strands 10c of the impregnated yarn 10d, but also provides a bond that holds the spiral binding thread 13 around the impregnated yarn 10d and forms the impregnated and tied yarn 10e. Once the thermoplastic material 12b solidifies, it maintains these bonds.
[0061] about Figure 1 , Figure 8 , Figure 2 and Figure 3 , the case where the dipped yarn is made of a single strand, two strands or three strands has been described, but it should be understood that according to the present invention, even more strands (four strands, five strands or more) twisted together can be used.
[0062] It is to be noted that in this context the expression "impregnated and binding yarn" may be replaced by "impregnated yarn" and vice versa, since the use of binding yarn 13 arranged in a spiral around the impregnated yarn is not consistent in the context of the present invention.
[0063] Our reference Figure 5 , Figure 5 One possibility of implementing the impregnation step is shown, with an impregnation tank 20 filled with liquid thermoplastic material 12a and defining a channel 21 between an inlet 20a and an outlet 20b of the impregnation tank 20. According to the basic provision allowing a good impregnation of the strands 10b by the liquid thermoplastic material 12a, there are one or more contact zones 20c in the channel 21 followed by each twisted strand 10b, which contact zones 20c have walls belonging to the face of the channel 21 and therefore to the inner face of the impregnation tank 20. Figure 5In the figure shown, these contact zones 20c are located on the side of a cylinder 22 placed in an impregnation tank 20 and are bypassed by the twisted strands 10b, which thus pass through the wavy channel 21. Other configurations not shown are also possible to force the twisted strands 10b to contact against the faces of the channel 21 alone while the strands 10b are immersed in the liquid thermoplastic material 12a, for example by means of the zigzag walls of the impregnation tank 20. In general, the channel 21 is curved.
[0064] It is therefore understood that, due to this friction on these contact zones and the pressure of the twisted strands 10b, the penetration of the liquid thermoplastic material 12a into the twisted strands 10b is favoured, and this is especially because this contact tends to separate the fibres 11 of the twisted strands 10b from each other and to generate a local overpressure on the liquid thermoplastic material 12a. At the outlet of the passage 21 and the above-mentioned contact, impregnated twisted strands 10c are obtained, which have individual twists T1 consistent with the twisting before passing through the impregnation tank, these twisted strands being highly impregnated or even completely impregnated with the thermoplastic material 12a. Thanks to this arrangement, an effective impregnation step is carried out, which makes it possible to obtain, at the outlet of the impregnation tank 20, impregnated strands 10c in at least 60% of their volume, generally in at least 70% of their volume, preferably in at least 80%, or even in at least 90% or 95% of their volume impregnated with thermoplastic material. In some cases, impregnation of the thermoplastic material may be obtained in the entire (100%) volume of the impregnated strand 10c. At the end of the manufacturing line implementing the manufacturing method according to the invention, this large amount of thermoplastic material is present in the yarn in this same proportion.
[0065] In the corresponding Figure 3 In the embodiment of the invention, each of the strands has a twist T1 according to a first orientation when the strands pass through the impregnation tank 20: the individual twists are, for example, between 50 and 300 tpm, preferably between 100 and 200 tpm. The first orientation is, for example, S-shaped. The first orientation of the twist T1 results in the formation of a strand 10b having an outer fiber 11 which is at an angle β relative to the general direction P0 of the strand 10a.
[0066] According to the invention, the impregnated yarn 10d comprises at least two twisted strands 10b (preferably three twisted strands 10b) separated from each other upstream of the impregnation tank 20 and simultaneously passing through the passage 21. For example, the impregnated yarn 10d comprises 2 to 10 single strands of 200 to 1500 tex, preferably 3 to 6 single strands of 200 to 800 tex, preferably 3 to 6 single strands of 300 to 600 tex. According to an alternative embodiment, several independent impregnation tanks working in parallel are used, one impregnation tank being used to impregnate each strand 10b.
[0067] For example, the twisted strand 10b passes through a calibrated hole at the inlet 20a of the impregnation tank 20 (at Figure 5 ) into the impregnation tank, the hole being large enough to avoid clogging but small enough to avoid leakage of the liquid thermoplastic material (e.g. polypropylene) (e.g., a hole of 2.5 mm in diameter for three twisted strands 10b each of 555 tex). In addition, for example, the impregnated twisted strands 10c pass through a calibrated hole at the outlet 20b of the impregnation tank 20 (at Figure 5 ) appears on the left side of the diaphragm 10d, which will determine the final radius of the impregnated yarn 10d and the amount of thermoplastic material of this impregnated yarn 10d (for example, a hole with a diameter of 2 mm for three twisted strands 10b of 555 tex each). The diameter of this outlet hole will be adjusted to obtain the desired share of thermoplastic material and fibers in the impregnated yarn 10d. In the impregnated yarn 10d, this share is generally 30% to 70% by weight of thermoplastic material, preferably 40% to 60% by weight of thermoplastic material.
[0068] According to one embodiment, the or each strand 10a or 10b consists only of plant fibers belonging to the group comprising flax, hemp, sisal, jute, abaca, kenaf, nettle, ramie, kapok, abaca, henequen, pineapple, banana plant, palm and wood fibers.
[0069] According to one embodiment, the thermoplastic material used for impregnation comprises a polymer belonging to the group comprising polyolefins, polypropylene (PP), maleic anhydride grafted polypropylene (maPP), polyethylene (PE) polyamide or copolyamide, polyester or copolyester, thermoplastic polyurethane, copolyoxymethylene, thermoplastic cellulose ester (cellulose acetate propionate), polylactic acid (PLA) or its derivatives or mixtures thereof. For example, a mixture of polypropylene and maleic anhydride grafted polypropylene (maPP) is used, which facilitates the bonding of the polymer to natural fibers. For example, such a mixture can be used with 3% to 10% by weight of maPP.
[0070] According to one embodiment, the viscosity of the thermoplastic material in the impregnation tank 20 is such that the melt flow index is greater than 10 g / 10 min, preferably greater than 34 g / 10 min. The melt flow index is a value measured in g / 10 min according to ISO 1133 at 230° C. under a load of 2.16 kg.
[0071] According to one embodiment, the viscosity of the molten thermoplastic material 12a in the impregnation tank 20 is between 10 and 10,000 Pa.s, preferably between 20 and 1000 Pa.s, and preferably between 50 and 500 Pa.s. This viscosity corresponds to a low shear rate viscosity of 1 sec-1. Typically, during impregnation in the impregnation tank 20, the temperature of the thermoplastic material is between 150°C and 250°C.
[0072] In order to implement the above, especially with regard to Figures 1 to 3 The described method for making dipped yarns can be used as Figure 4 The schematically shown manufacturing unit 100. Between the inlet F1 and the outlet F2, there is still Figures 1 to 3 At the entrance of the manufacturing unit 100, three spools 110 allow the three twisted strands 10b to be fed to the manufacturing unit 100, corresponding to Figure 3 Step B.
[0073] In the case shown, the twisted strands 10b are dried by passing through a drying module 120, which drying can be omitted in other embodiments. However, it can be seen that the natural fibers still have a moisture content of 4-8%. When these fibers 11 enter the impregnation tank, which is heated to, for example, 190°C, this moisture forms water vapor and escapes from the fibers. When the steam escapes, it displaces the thermoplastic material and impairs the impregnation of the fibers forming the strands. Before entering the impregnation tank, the twisted strands 10b can be dried very easily by passing through a drying module 120, which includes a tube with a hot air flow between 100-150°C. It is also possible to pre-dry the twisted strands 10b and keep the coil unwound on the bobbin 110 in a dry atmosphere.
[0074] In this way, the one or more strands 10b are dried before entering the impregnation tank 20.
[0075] The impregnation tank 20 described above is arranged directly downstream of the drying module 120 , and the extruder 23 supplies the liquid thermoplastic material to the tank 20 .
[0076] Downstream of the impregnation tank 20, the end of the manufacturing unit 100 includes a drive, winding and twisting module 140, which includes a bobbin for receiving the impregnated yarn 10d (or the impregnated and tied yarn 10e). In this way, when the free end of the impregnated yarn 10d passes through the drive, winding and twisting module 140 and the drive, winding and twisting module 140 is activated, the impregnated yarn as a whole is advanced and twisted, and is wound on the support as the impregnated yarn advances, thereby obtaining a twisted (and possibly tied) impregnated yarn 10d, which is wound on the bobbin of the drive, winding and twisting module 140.
[0077] In this way, after the impregnation step C, a step of twisting the impregnated yarn 10d is carried out (step D), during which, while the thermoplastic material is still in the liquid state, a total twist corresponding to the T2 twist between all the strands downstream of the impregnation tank 20 is achieved, whereby the thermoplastic material 12a is combined between these strands 10c (these strands 10c are in a state in which they are twisted together), resulting in the formation of the impregnated and twisted yarn 10d.
[0078] According to the present invention, the total twist is achieved in a second orientation T2 different from the first orientation T1. Thus, if the individual twist T1 of each strand 10c is in the S direction (counterclockwise relative to the yarn advancement direction), the total twist of the yarn 10d in the Z direction (clockwise relative to the yarn advancement direction) will be achieved by the drive, winding and twisting module 140.
[0079] Under these conditions, the degree of twist T2 is chosen so that the external fibers 11 of the one or more strands 10c form with the longitudinal direction or main direction P1 of the impregnated yarn 10d an acute angle of between -20° and +20° or a small angle δ of zero. According to another possibility, this angle δ is between +10° and -10°, or even between +5° and -5°, and possibly between +3° and -3°. By "external fibers" is meant the portion of fibers of each strand situated on the surface of the impregnated (and twisted) yarn. In practice, in the case of strands 10b having fibers with a certain twist according to a first orientation (angle δ if there are cumulative twists T1 and T1', or angle β if there is only twist T1), by twisting the strands together according to a second orientation (total twist T2), the angle δ (and possibly ε in the presence of a binding thread 13) formed between the external fibers of the strand and the main direction P1 of the yarn 10d or 10e is reduced, or even eliminated. This can be achieved in particular in the case of strands 10b having fibers with a certain twist according to a first orientation (angle δ if there are cumulative twists T1 and T1', or angle β if there is only twist T1). Figure 3As can be seen in FIG. 1 , fibers 11 are visible in portion D representing the dipped yarn 10 d having a total twist and forming outer fibers, which fibers 11 are substantially parallel to the main direction P1 of the dipped yarn 10 d (with respect to P1 , the angle ε is marked as close to 0, i.e. ε~0).
[0080] This situation in which the outer fibers 11 are oriented at 0° (longitudinal) in the impregnated yarns 10d results in the impregnated yarns having maximum stiffness in bending, which leads to good bending strength qualities when these yarns are integrated as surface ribs in thin-walled composite products.
[0081] Since the outer fibers of the impregnated yarn are mainly subject to bending stresses, a yarn geometry with outer yarn fibers at 0° (longitudinal) is advantageous. This can be achieved by twisting several single yarns (T2 twist) in the twist direction opposite to the single strands (if the single strands have S-shaped twist T1, then for T2 twist the yarn is twisted in the Z direction) so that the outer fibers are at or close to 0°. For example, twisting three single strands of 555 tex with 158 tpm twist with 73 tpm results in a fiber angle of 0° on the outside of a 1665 tex yarn (e.g. linen). Therefore, by twisting the single strands to form a large yarn, the fiber angle 11 can be optimized to have good bending properties (outer fibers 11 at 0°) and good radial compressive strength of the yarn (inner fibers 11 have a sufficiently large twist angle).
[0082] Because step D of twisting all of the single yarns 10c into a larger yarn 10d is performed while the thermoplastic material 12a is still molten, this total twist creates additional compression of the yarn 10d, which further presses the thermoplastic material into the interior of the single yarns 10c and enhances its impregnation.
[0083] exist Figures 1 to 3 In the embodiment shown, the following steps are performed (step E): a binding thread 13 is provided and wound around the impregnated yarn 10d impregnated with the thermoplastic material downstream of the impregnation tank, thereby forming an impregnated and binding yarn 10e. The binding thread 13 is placed in a spiral around the impregnated yarn 10d while the thermoplastic material 12a is still in liquid state, so as to ensure that the binding thread 13 is fixed to the impregnated yarn 10d and to obtain good cohesion of the impregnated and binding yarn 10e. For example, the linear weight of such a binding thread is between 10 and 60 tex, preferably between 15 and 45 tex. The weight added by the binding thread is generally 1-15%, preferably 2-10%, of the total weight of the impregnated and binding yarn 10e.
[0084] Among the various advantages of the presence of this binding thread 13, it should be noted that it helps to keep the cross section of the impregnated and bound yarn 10e circular and mainly helps to increase its resistance to radial compression. This is advantageous when the impregnated and bound yarn 10e is used as a rib on its surface in a thin-walled composite product, because during the manufacturing process of the thin-walled composite product, the product is compressed by a flexible film or a flexible pad (such as a silicone substrate) under pressure. In this process, the threads of the rib tend to be crushed and the effectiveness of the rib is thereby reduced. Since the stiffness in bending stress depends on the cube of the thickness of the structure, the thickness of the rib has a major influence on the bending stiffness of the thin-walled composite product.
[0085] The binding thread 13 may be a vegetable fiber yarn (e.g. flax / linen, cotton, hemp, etc.) or may be a synthetic fiber (polymer yarn, such as polyester, polyamide or glass fiber, carbon fiber, aramid). The binding thread 13 may not melt or become too soft at the processing temperature of the composite product (180-210°C), otherwise when the part is compressed, the binding thread 13 will deform and it will lose all its effectiveness in restraining and maintaining the shape of the impregnated and bound yarn 10e.
[0086] Therefore, if there is a twisted binding thread 13 in the impregnated yarn 10e, the binding thread 13 is laid (step E) after step D of twisting the yarn as a whole, and the binding thread laying module 130 is arranged upstream (before) of the driving, winding and twisting module 140. It should be understood that the twist of all yarn strands (total twist T2) is achieved by the driving, winding and twisting module 140, but this total twist is propagated all the way to the outlet of the impregnation tank 20 (at Figure 4 , at the outlet of the impregnation tank 20 located on the left side, the three twisted impregnated strands 10c are differentiated (separated) and then combined in the impregnated yarn 10d).
[0087] According to an embodiment not shown, at least two binding wires 13 are provided downstream of the impregnation tank, and when the impregnated yarn 10d advances through the outlet of the impregnation tank, the binding wires are arranged spirally in different directions around the impregnated yarn 10d successively, thereby forming the impregnated and tying yarn 10e. In one embodiment, exactly two binding wires 13 are arranged spirally around the impregnated yarn 10d in opposite rotation directions, whereby the two binding wires 13 intersect at the surface of the impregnated and tying yarn 10e.
[0088] Different methods are possible for the installation of the binding wire 13 or two or more binding wires 13. In a first solution, the impregnated yarn passes inside a binding wire spool which rotates at a determined speed to achieve the desired binding wire density. When the spool rotates at high speed, the tension on the small binding wire is generated by the inertia of the binding wire rotating at high speed around the impregnated yarn. Alternatively, the spool of the binding wire can rotate around the impregnated yarn and the tension in the binding wire is generated by braking the unwinding of the spool. In either case, the impregnated yarn does not come into contact with the binding wire transport unit, except for the binding wire itself, and this is so as not to interfere with the twisting process occurring between the drive, winding and twisting module 140 and the impregnation tank 20.
[0089] For the drive, winding and twisting module 140, a winding system can be used, in which the bobbin on which the impregnated yarn is wound rotates both on its own axis to wind the impregnated yarn and on the axis of the impregnated yarn to produce twist. The second way is the spinning wheel method, in which a flywheel (épinglier) rotates around the bobbin. The rotation speed of the flywheel determines the twist, and the speed difference between the bobbin and the flywheel controls the feeding rate of the impregnated yarn. The precise control of these two speeds can be done with a stepper motor, a synchronous motor or a servo motor.
[0090] according to Figure 8 Another possibility, which is not part of the present invention, can be seen in Figure 1 , where the initial strand 10a is in the form of a ribbon with aligned fibers 11 (the fibers 11 have an angle close to 0° with respect to the main direction P0 of the ribbon or strip), which passes through a bath of molten thermoplastic polymer in an impregnation tank and then the binding wire 13 is laid spirally around the impregnated yarn 10c.
[0091] As previously indicated, the present invention also relates to a thin-walled composite product comprising an impregnated yarn as previously described, the composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarn, and in some cases all of the ribs being formed by the impregnated yarn.
[0092] According to one possibility, such a ribbed thin-walled composite product is produced by a method comprising the following steps:
[0093] - provide support, such as pads,
[0094] - producing an impregnated yarn according to the method described above,
[0095] - assembling the impregnated yarns to form a grid in which the impregnated yarns cross each other,
[0096] - stacking grids and supports, and
[0097] - Compression moulding of the stacked grids and supports, thereby forming a composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarns.
[0098] An example of such a thin-walled ribbed composite product 30 is Fig. 6A and Figure 6B as well as Figure 7 30 is shown in the form of a part of a component which can be used, for example, as a decorative component for the interior of an automobile. This thin-walled ribbed composite product 30 comprises a grid 32 and a support 34 superimposed and connected to each other. The grid 32 is formed by impregnated and bound yarns 10e, which are held together in an interlocking manner by an assembly line, for example polyester, for example 10 to 100 dtex, which is applied by sewing, knitting or braiding with the impregnated and bound yarns 10e of the grid 32.
[0099] The bond between the mesh 32 and the support 34 is formed by the polymer itself, either during the compression molding step or during the thermal pre-lamination step. Alternatively, the mesh 32 may be sewn to the substrate 34.
[0100] According to another manufacturing method, two supports 34 are provided and the grid 32 is stacked together with the two supports 34 , located on either side of said grid 32 , to form a sandwich stack.
[0101] According to one embodiment, the support 34 (or the two supports) is selected from a woven material support, a non-woven material support or a non-woven material support 34 belonging to the following list: a unidirectional fiber web (11), a superposition of unidirectional fiber webs (11) (multidirectional web) and a randomly distributed fiber mat.
[0102] According to one embodiment, the substrate 34 (or both substrates) is pre-impregnated with a polymer (or more generally a thermoplastic material) that is the same as or different from the polymer (or more generally a thermoplastic material) impregnating the yarns of the mesh.
[0103] According to one embodiment, the grid 32 comprises a mesh with a mesh greater than or equal to 1 cm, preferably between 1 cm and 6 cm, preferably between 1 cm and 3 cm.
[0104] The impregnated yarns described above are used to form a grid 32 or a grille. The grille can have parallel yarns in two directions to produce a square, rectangular or parallelepiped mesh. It can also have three or four yarn directions. Depending on the size of the yarn used, the square mesh grid typically has a mesh size of 5-100 mm, and if 1500 tex impregnated linen yarn is used, the square mesh grid typically has a mesh size of 10-30 mm. The grille can be made by a textile method, for example by knitting the impregnated yarns together with fine threads. The grille can also be obtained by heat welding the impregnated yarns at their intersections by heating or by ultrasound. In order to obtain the desired final composite product, the grille is combined with other composite layers (such as a mat of natural fibers and PP, or a mat of polyester fibers and PP, etc.) in a hot pressing step.
[0105] According to another possibility, a method for manufacturing a ribbed thin-walled composite product is proposed, the method comprising the following steps:
[0106] - producing an impregnated yarn according to one of the methods described above,
[0107] - provide a base yarn of smaller size than the dipped yarn,
[0108] - weaving or knitting the base yarn with the impregnated yarn to form a preform,
[0109] - Compression moulding the preform, thereby forming a composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarns.
[0110] The preform with the impregnated yarn must be shaped in order to obtain the composite product with reinforced ribs. Several methods are feasible. For hot pressing, the preform is heated in an oven to melt the thermoplastic polymer. The base layer and the preform containing the impregnated yarn can either be pre-combined and heated together (if their temperature and heating method match), or heated separately but simultaneously. The preform and the base layer are placed in the mold of the press, and the press is closed to compact and form the composite product. Once the polymer has cooled and solidified, the part is demoulded. The mold used is rigid on the smooth side of the part, but has a soft substrate on the ribbed side, such as a 2-10 mm silicone layer, so as not to crush the ribs produced by the impregnated yarn 10d or 10e described earlier. Alternatively, pressure can be applied by a flexible film pressurized on the ribbed side. In addition, the heating and cooling cycle can be completed in the mold.
[0111] The ribs can be obtained at specific selected locations using a deposition robot which will precisely deposit the desired impregnated yarns 10d or 10e on a base layer (eg a mat) according to a specific reinforcement pattern. The bonding to the base layer can be achieved by melting the polymer or by local stitching of the impregnated yarns.
[0112] The composite product described herein is thin-walled, meaning that it is typically initially in the form of a sheet or plate with one dimension being much smaller (at least 10 times smaller) than the other two dimensions.
[0113] Such composite products may have a variety of geometric shapes, including: flat sheets, non-planar sheets (including sheets with convex and concave sides) or corrugated sheets, three-dimensional hollow shapes (including hollow tubes with circular cross-sections, polygonal cross-sections), or other shapes (including any three-dimensional thin-walled shells).
[0114] Thus, and in a non-limiting manner, it is proposed to manufacture an article comprising a thin-walled portion, wherein said thin-walled portion is formed by a thin-walled composite product manufactured according to one of the methods described hereinabove. Such an article comprising a thin-walled composite product can be used in various applications and in particular belongs to the group comprising:
[0115] Automotive body parts, in particular doors, roofs, hoods, fenders, spoilers, front and rear bumpers, aerodynamic kits; or automotive interior parts, in particular door covers, dashboards, center consoles, pillar trims, trunk trims, roofs; or sports goods, such as canoe hulls, kayak or light boat hulls, bicycle frames; or furniture parts; or aircraft interior parts, including side panels, ceilings, luggage compartments; or light aircraft aerodynamic parts, including hoods, wheel covers; or aerodynamic fairings of any movable machine; or suitcase shells.
[0116] [Table 1]
[0117] Reference numerals list
[0118] A. Supplying step of (plural) strands 10a
[0119] B. Twisting step of the strands 10a
[0120] C. Impregnation step of strand(s) 10b
[0121] D. Twisting step of the entire strand 10c
[0122] E Steps for laying the binding thread 13 on the yarn 10d
[0123] F1 Input
[0124] F2 Output
[0125] T1 Single strand twisting
[0126] T1' Additional single strand twist
[0127] T2 Total yarn twist
[0128] P0 Main direction of the strand
[0129] P1 Main direction of the yarn
[0130] α Angle between outer fiber 11 and strand 10a (step A)
[0131] β Angle between outer fiber 11 and strand 10b (step B)
[0132] δ Angle between the external fiber 11 and the impregnated and twisted yarn 10d (step D)
[0133] ε Angle between the outer fiber 11 and the impregnated, twisted and bound yarn 10e (step E)
[0134] 10a Flat Wire
[0135] 10b Twisted strands
[0136] 10c Twisted impregnated strands (impregnated yarn if only one strand)
[0137] 10d impregnated yarn with total twist
[0138] 10e Dipping and bundling yarn
[0139] 11. Fiber
[0140] 12a Liquid thermoplastic material
[0141] 12b Hardened thermoplastic material
[0142] 13. Binding wire
[0143] 20 Dipping tank
[0144] 20a Tank inlet
[0145] 20b Tank outlet
[0146] 20c Contact area of strands in channel 21
[0147] 21 channels
[0148] 22 Column
[0149] 23 Extruder
[0150] 30 Thin-walled ribbed composite products
[0151] 32 Grid
[0152] 34 Support
[0153] 100 Manufacturing Units
[0154] 110 Spool
[0155] 120 Drying module
[0156] 130 Cable laying module
[0157] 140 Driving, winding and twisting unit.
Claims
1. A method for producing an impregnated yarn (10d; 10e) based on at least two strands (10a; 10b) comprising plant fibers (11), wherein: In the method the following steps are performed: - providing at least two continuous strands (10a; 10b) comprising vegetable fibers (11), - providing an impregnation tank (20) defining a curved passage (21) between an inlet and an outlet, - supplying the tank with a bath of molten thermoplastic polymer material (12a) which permanently fills said channel (21), - arranging the strands (10a; 10b) so that: they are separated from one another upstream of the impregnation tank (20), so that they enter the impregnation tank (20) through the inlet, so that they simultaneously follow the channel (21) and, while doing so, are immersed in the thermoplastic polymer material (12a) and have at least one contact zone (20c) with one face of the channel (21), and so that they leave the impregnation tank (20) through the outlet, and - impregnating said strands (10a; 10b) by continuously advancing said strands (10a; 10b) so as to form strands (10a; 10b) impregnated with a thermoplastic polymer material (12a), thereby forming an impregnated yarn (10d; 10e); - wherein, during the passage (21) of said strands (10a; 10b) through said impregnation tank (20), each of said strands (10a; 10b) has a twist (T1) in a first orientation, and - wherein, after the impregnation step, a yarn twisting step is further performed, during which yarn twisting step, downstream of the impregnation tank (20), a total twist of all the strands (10a; 10b) is achieved, the total twist corresponding to the twist (T2) between the strands, while the thermoplastic polymer material (12a) is still in a liquid state, whereby the thermoplastic polymer material (12a) produces bonding between the strands (10a; 10b) in their twisted-together state, resulting in the formation of an impregnated and twisted yarn, and wherein the total twist (T2) is achieved in a second orientation different from the first orientation, wherein the outer vegetable fibers (11) of one or more strands (10a; 10b) form an angle (δ) between -20° and +20° with the longitudinal direction or main direction of the impregnated yarn; Wherein, the following steps are further performed while the thermoplastic polymer material (12a) is still in a liquid state: - providing at least one binding wire (13) and winding said binding wire (13) around an impregnated yarn (10d) of thermoplastic polymer material downstream of said impregnation tank (20), thereby forming an impregnated and bound yarn.
2. The method for producing an impregnated yarn (10d; 10e) according to claim 1, wherein: The outer vegetable fibers (11) of one or more strands (10a; 10b) form an angle (δ) between +10° and -10° with the longitudinal direction or main direction of the impregnated yarn.
3. The method for producing an impregnated yarn (10d; 10e) according to claim 1, wherein: The strands (10a; 10b) consist exclusively of vegetable fibers (11).
4. The method for producing yarn according to claim 3, wherein: The plant fibers (11) belong to the group comprising flax, hemp, sisal, jute, abaca, kenaf, nettle, ramie, kapok, sisal, pineapple, banana plant, palm and wood fibers.
5. The method for producing yarn according to claim 1, wherein: The thermoplastic polymer material belongs to the group comprising polyolefins, polypropylene (PP), maleic anhydride grafted polypropylene (maPP), polyethylene (PE) polyamide or copolyamide, polyester or copolyester, thermoplastic polyurethane, copolyoxymethylene, thermoplastic cellulose ester, polylactic acid (PLA) or its derivatives or mixtures thereof.
6. The method for producing yarn according to claim 1, wherein: The viscosity of the thermoplastic polymer material (12a) in the impregnation tank is such that the melt flow index measured at 230° C. under a load of 2.16 kg according to ISO 1133 standard is greater than 10 g / 10min.
7. The method for producing yarn according to claim 1, wherein: The viscosity of the molten thermoplastic polymer material (12a) in the impregnation tank (20) is between 10 and 10,000 Pa.s.
8. The method for producing yarn according to claim 1, wherein: The impregnated yarn (10d) comprises 30 to 70% by weight of a thermoplastic polymer material.
9. The method for producing yarn according to claim 1, wherein: Before the yarn (10a; 10b) enters the impregnation tank (20), the yarn (10a; 10b) is also dried.
10. The method for producing yarn according to claim 1, wherein: Further follow these steps: - providing at least two binding wires (13) downstream of the impregnation tank (20), - When the impregnated yarn (10d) advances through the outlet of the impregnation tank (20), the binding wires (13) are continuously arranged spirally in different directions around the impregnated yarn (10d), thereby forming an impregnated and bound yarn.
11. The method for producing yarn according to claim 1, wherein: Further follow these steps: - providing a driving, winding and twisting module (140) arranged downstream of said impregnation tank (20), - passing the free end of the impregnated yarn (10d; 10e) into the driving, winding and twisting module, and - activating the driving, winding and twisting module (140) so that the impregnated yarn (10d; 10e) advances and achieves its total twist (T2), and the impregnated yarn (10d; 10e) is wound onto a support as the impregnated yarn (10d; 10e) advances.
12. The method for producing yarn according to claim 5, wherein: The thermoplastic cellulose ester is cellulose acetate propionate.
13. The method for producing an impregnated yarn (10d; 10e) according to claim 1, wherein: The outer vegetable fibers (11) of one or more strands (10a; 10b) form an angle (δ) between +5° and -5° with the longitudinal direction or main direction of the impregnated yarn.
14. The method for producing yarn according to claim 1, wherein: The viscosity of the thermoplastic polymer material (12a) in the impregnation tank is such that the melt flow index measured at 230° C. under a load of 2.16 kg according to ISO 1133 standard is greater than 34. g / 10min.
15. A method for manufacturing a thin-walled composite product, comprising the steps of: - providing a support (34), - manufacturing the impregnated yarn according to the method of claim 1, - assembling the yarns to form a grid (32) in which the impregnated yarns are crossed, - stacking the grid (32) and the support (34), and - Compression moulding of the stacked grids (32) and supports (34) thereby forming a composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarns.
16. The method of manufacturing a thin-walled composite product according to claim 15, wherein: The yarns of the mesh (32) are held together in a crossed manner by assembly threads which are applied by sewing, knitting or braiding with the yarns of the mesh (32).
17. The method of manufacturing a thin-walled composite product according to claim 15, wherein: Two supports (34) are provided and the grid (32) is stacked with the two supports (34) located on opposite sides of the grid (32) to form a sandwich stack.
18. The method of manufacturing a thin-walled composite product according to claim 15, wherein: The support (34) is selected from a support (34) of woven material or a support (34) of non-woven material from the following list: a unidirectional fiber web; a superposition of unidirectional fiber webs, ie a multidirectional web; and a randomly distributed fiber mat.
19. The method of manufacturing a thin-walled composite product according to claim 15, wherein: The support member (34) is a pad.
20. The method of manufacturing a thin-walled composite product according to claim 16, wherein: The assembly line is polyester.
21. A method for manufacturing a thin-walled composite product, comprising the steps of: - Manufacturing of impregnated yarn (10d) according to the method of claim 1; 10e), - providing a base yarn having a smaller size than said impregnated yarn (10d; 10e), - weaving or knitting said base yarn with said impregnated yarn (10d; 10e) to form a preform, - compression moulding of the preform, thereby forming a composite product having a ribbed surface, the ribs being at least partially produced by the impregnated yarns (10d; 10e).
22. A method of manufacturing an article comprising a thin-walled portion, wherein: The thin-walled portion is formed by or comprises a thin-walled composite material product manufactured according to the method of claim 15, the article belonging to the group comprising: Auto body parts, including doors, roofs, hoods, fenders, spoilers, front and rear bumpers, aerodynamic kits; or Auto interior parts, including door caps, instrument panels, center consoles, pillar trims, trunk trims, roofs; or Sporting goods, including canoe hulls, kayak or light boat hulls, bicycle frames; or furniture parts; or aircraft interior parts, including side panels, roof panels, luggage compartments; or light aircraft aerodynamic parts, including engine covers, wheel covers; or Aerodynamic fairing for any movable machine; or suitcase shell.
23. An impregnated yarn (10d; 10e) having at least two continuous strands (10a; 10b) comprising vegetable fibers (11), said strands (10a; 10b) being impregnated with a thermoplastic polymer material (12a) in at least 60% of their volume, each of said strands (10a; 10b) being individually twisted with a twist (T1) in a first orientation, and all of said strands (10a; 10b) being also twisted into a configuration held by the thermoplastic polymer material (12a) according to a total twist (T2) in a second orientation different from the first orientation, wherein: The outer vegetable fibers (11) of one or more strands (10a; 10b) form an angle (δ) between -20° and +20° with the longitudinal direction or main direction of the impregnated yarn; The impregnated yarn further comprises at least one binding thread (13) which is spirally wound around all the strands (10a; 10b) to form an impregnated and bound yarn; Wherein, the dipped yarn is manufactured by the method for manufacturing a dipped yarn according to any one of claims 1-14.
24. The impregnated yarn (10d; 10e) according to claim 23, wherein The outer vegetable fibers (11) of the strands (10a; 10b) form an angle (δ) between +10° and -10° with the longitudinal direction or main direction (P) of the impregnated yarn (10d; 10e).
25. The impregnated yarn (10d; 10e) according to claim 23, wherein The strands (10a; 10b) have an individual twist (T1) between 50 and 300 tpm.
26. The impregnated yarn (10d; 10e) according to claim 23, comprising between three and six strands (10a; 10b), each strand having a weight between 200 and 800 tex.
27. The impregnated yarn (10d; 10e) according to claim 23, wherein The outer vegetable fibers (11) of the strands (10a; 10b) form an angle (δ) between +5° and -5° with the longitudinal direction or main direction (P) of the impregnated yarn (10d; 10e).
28. The impregnated yarn (10d; 10e) according to claim 23, wherein The strands (10a; 10b) have an individual twist (T1) between 100 and 200 tpm.
29. The impregnated yarn (10d; 10e) according to claim 23, comprising between three and six strands (10a; 10b), each strand having a weight between 300 and 600 tex.
30. A thin-walled composite product comprising an impregnated yarn (10d; 10e) according to claim 23, said composite product having a ribbed surface, said ribs being at least partially produced by said impregnated yarn (10d; 10e).
Citation Information
Patent Citations
Stiffened thin-walled fibre composite products and method of making same
EP2648890A1
Impregnated-yarn cloth and process for producing impregnated-yarn cloth
EP2813607A1
Composite grid structure
WO2017099585A1
Composite product comprising a treillis and a polymer
WO2019087141A1
Injection moldings of natural-fiber reinforced thermoplastic resin
CN102317050A