Preparation process of solid-liquid hybrid capacitor
By forming a porous layer on the positive electrode foil and the negative electrode foil, and forming a dispersed protective layer on the electrolytic paper, combined with the treatment of dispersed liquid and chemical liquid, the problems of short service life and high defect rate of solid-liquid mixed capacitors are solved, and the problem of short service life and high defect rate of solid-liquid mixed capacitors is achieved. The effect of larger capacity, lower loss and lower leakage current is improved, and the high-temperature storage performance of the capacitor is improved.
Patent Information
- Application Number
- CN202411257406.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing solid-liquid mixed capacitor preparation process has problems such as short service life at high temperature, poor storage and high defect rate.
By forming a porous layer on the positive electrode foil and the negative electrode foil and forming a dispersed protective layer on the electrolytic paper, the dispersion liquid and the chemical liquid are used for pressurized impregnation and chemical repair treatment, and combined with the impregnation of the electrolyte, it forms a larger capacity and more Solid-liquid hybrid capacitors with low loss and lower leakage current.
It improves the high-temperature storage performance and service life of the capacitor, reduces the production defect rate, ensures the consistency of the capacity, loss and leakage current of the capacitor, and enhances the high-temperature storage performance of the product.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of capacitors, and in particular to a preparation process of a solid-liquid hybrid capacitor. Background Art
[0002] As the market demand for high-power, small-volume electrical products (including power supplies) increases, this also translates into electrical (including power supply) manufacturers putting forward requirements for smaller volume and larger ripple current for aluminum electrolytic capacitor manufacturers. Under this call, only solid hybrid capacitors can meet the requirements of large ripple, long life, and small volume. Solid hybrid capacitors are solid-liquid hybrid electrolytic capacitors, which combine the advantages of conventional liquid and solid electrolytic capacitors, and are more flexible in use than liquid capacitors. Although hybrid capacitors cannot provide the same voltage and capacity as traditional electrolyte capacitors, they have the ability to generate and repair the oxide film dielectric layer on the surface of the anode aluminum foil compared to traditional solid capacitors, and greatly reduce the equivalent series resistance of the capacitor.
[0003] At present, solid-liquid hybrid capacitors have been deeply used in automotive, 5G, industrial power supplies and other aspects, and their application prospects are very broad. However, since the dispersion of solid-liquid hybrid capacitors is a solid + liquid suspension, rather than a true solution, the impregnation in the preparation process of solid-liquid hybrid capacitors is relatively difficult. Therefore, the main disadvantages of solid-liquid hybrid electrolytic capacitors prepared by existing technologies are: (i) short high-temperature service life. The product after impregnation with additives is extremely easy to absorb moisture in the air, and the high-temperature storage performance is not very good. During use, it will involve a long period of high-temperature no-load state, resulting in poor product characteristics or life; (ii) high leakage current and defective rate. The electrolyte cannot be evenly immersed in the corrosion holes and polymer layers of the positive and negative foils, so it is impossible to effectively repair the defects of the positive and negative foils and the polymer layers, which will lead to an increase in the leakage current and defective rate of the product. Therefore, the existing preparation method of solid-liquid hybrid capacitors has the defects of short high-temperature service life, poor high-temperature storage performance and high defective rate, which makes the use of this technology very limited. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation process of a solid-liquid hybrid capacitor to solve the following technical problems: The existing preparation process of solid-liquid hybrid capacitors has the problems of short high-temperature service life, poor high-temperature storage performance and high defect rate.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A preparation process of a solid-liquid hybrid capacitor comprises at least the following steps: forming a positive electrode porous layer on the positive electrode foil, forming a negative electrode porous layer on the negative electrode foil, and forming a dispersed protective layer on the electrolytic paper; stacking the positive electrode foil, the electrolytic paper and the negative electrode foil together and winding them into a core package; The core package is impregnated with the dispersion liquid under pressure to obtain a core package impregnated with the dispersion liquid; Performing a chemical repair treatment on the core package impregnated with the dispersion liquid by using a chemical liquid to obtain a core package after chemical formation; Impregnating the formed core package with an electrolyte to obtain a core package impregnated with the electrolyte; Assembling the core package impregnated with the electrolyte with the aluminum shell and the leather plug and subjecting them to aging treatment to obtain a solid-liquid hybrid capacitor; Wherein, the pore size of the positive electrode porous layer is 20-400nm and the thickness is 1-3μm; The pore size of the negative electrode porous layer is 20-400 nm, and the thickness is 1-3 μm.
[0006] As a further embodiment of the present invention: the positive electrode foil is one of aluminum, tantalum, niobium or titanium, and the method for preparing the positive electrode porous layer comprises the following steps: Treating the positive electrode foil with an alkaline solution to remove the surface oxide film and oil stains; The positive electrode foil treated with alkali solution is placed in a nitric acid solution, and oxidized by applying voltage and controlling temperature to generate the positive electrode porous layer.
[0007] As a further solution of the present invention: the negative electrode foil is one of aluminum, tantalum, niobium or titanium, and is the same as the positive electrode foil, and the preparation method of the negative electrode porous layer is the same as the preparation method of the positive electrode porous layer.
[0008] As a further solution of the present invention: the preparation method of the dispersed protective layer comprises the following steps: adding sodium polystyrene sulfonate and a phosphate compound into a dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) to obtain a mixed solution; Soaking or spraying electrolytic paper with the mixed solution to form the dispersed protective layer on the electrolytic paper; The content of the dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) is 10-60wt%, the content of the sodium polystyrene sulfonate is 0.1-5wt%, and the content of the phosphate compound is 0.1-5wt%.
[0009] As a further solution of the present invention: the dispersion liquid is a dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate), and the diameter of the solid material particles in the dispersion liquid is not greater than 200 nm.
[0010] As a further solution of the present invention: the chemical formation liquid is one of aqueous solutions of ammonium adipate, boric acid, phosphoric acid and ammonium dihydrogen phosphate, and the mass concentration of the chemical formation liquid is 5% to 10%.
[0011] As a further solution of the present invention: the voltage used in the chemical formation repair treatment is 12-16V, and the current density is 0.01-0.03mA / pcs.
[0012] As a further embodiment of the present invention: the electrolyte comprises at least one or more of γ-butyrolactone, cyclopentane sulfone, polyethylene glycol, triethylamine phthalate, ethylene glycol, phthalic acid, and adipic acid.
[0013] Beneficial effects of the present invention: (1) In the present invention, by forming a positive electrode porous layer on the positive electrode foil, forming a negative electrode porous layer on the negative electrode, and forming a dispersed protective layer on the electrolytic paper, the solid hybrid capacitor obtained by the preparation method of the solid-liquid hybrid capacitor provided by the present invention has the advantages of larger capacity, smaller loss, smaller leakage current, and lower equivalent series resistance, thereby improving the high-temperature storage performance of the capacitor and the product production yield. Specifically, by forming a positive electrode porous layer on the positive electrode foil and forming a negative electrode porous layer on the negative electrode, even if a dispersion solution is used to form a conductive polymer layer, the tightness between the conductive polymer layer and the porous layer can be improved, so that the consistency of the conductive polymer is high, and the consistency of the product capacity, loss and leakage current is maintained. The porous layer is formed on the foil in advance, so that the particles can enter the pores of the positive electrode foil, so that in the later impregnation process, the molecular material can be more and more evenly attached to the surface of the aluminum foil, which can ensure that the positive electrode foil is fully impregnated, reduce the difficulty of impregnation, and reduce the defective rate of product production. In addition, the formation of the porous layer can increase the surface area of the positive electrode foil and the negative electrode foil, thereby increasing the capacitance. Forming the porous layer on the foil before the winding step can also help remove burrs generated in the foil cutting step, thereby avoiding affecting the performance of the capacitor due to the presence of burrs.
[0014] (2) This application forms a dispersed protective layer on the electrolytic paper before the electrolytic paper core is rolled. The dispersed protective layer contains sodium polystyrene sulfonate, phosphate compounds, poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate). After the core package is made, the positive electrode foil, electrolytic paper and negative electrode foil are in close contact. The dispersed protective layer is filled between the positive electrode foil and the electrolytic paper, and between the negative electrode foil and the electrolytic paper to prevent air from entering during the impregnation step, thereby improving the high-temperature storage performance of the solid-liquid hybrid capacitor and the high-temperature service life of subsequent products. At the same time, the particles in the dispersed protective layer can be filled into the positive electrode porous layer and the negative electrode porous layer, so that the conductive polymer material in the dispersion can be more easily attached to the surface of the foil during the impregnation process, and the addition of phosphate compounds can improve the uniformity of the distribution of the conductive polymer material on the electrolytic paper and the foil, thereby ensuring that the entire core package is completely impregnated, improving the impregnation effect, and improving the formation effect. The defects of the positive and negative electrode foils and the polymer layer are effectively repaired, thereby reducing the leakage current and defect rate of the product. DETAILED DESCRIPTION
[0015] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Example 1 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: The cut positive and negative electrode foils were treated with a 2% by mass NaOH solution at room temperature for 10 minutes to remove the oxide film and oil stains on the surface, and then the aluminum foil sample treated with alkali solution was immersed in a nitric acid solution with a volume fraction of 5% and a temperature of 20°C, connected to the circuit, the power cabinet voltage was set to 15V, the current was set to 75mA, and the treatment was carried out for 10 minutes to form a positive electrode porous layer with a thickness of 1.4μm on the positive electrode foil, and a negative electrode porous layer with a thickness of 1.4μm on the negative electrode foil; The cut electrolytic paper is immersed in a dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) containing sodium polystyrene sulfonate and a phosphate compound for 10 minutes to form a dispersed protective layer on the electrolytic paper, wherein the content of the (3,4-ethylenedioxythiophene):poly(styrene sulfonate) aqueous dispersion is 50wt%, the content of sodium polystyrene sulfonate is 1wt%, and the content of the phosphate compound is 1wt%. The positive electrode foil, the negative electrode foil and the electrolytic paper are then wound into a core package by a core package winding machine, wherein the electrolytic paper is between the positive electrode foil and the negative electrode foil, and the length of the electrolytic paper is longer than the length of the overlapping portion of the positive and negative electrode foils, to obtain a core package; The core package is placed in a sealed container and impregnated with a dispersion liquid under pressure, wherein the dispersion liquid is a dispersed aqueous solution of a conductive polymer poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate), wherein the diameter of the solid matter particles in the dispersion liquid is not greater than 100 nm, the pressure of the pressurized impregnation is 8 KG, the time of the pressurized impregnation is 10 minutes, and then the core package is placed at a temperature of 180° C. and dried for 90 minutes to obtain a core package impregnated with the dispersion liquid; The core package impregnated with the dispersion liquid is immersed in a 5% mass concentration of adipic acid amine forming liquid, and voltage is applied to the positive and negative electrodes of the core package at the same time, and the forming repair treatment is performed for 20 minutes, wherein the voltage used is 12-16V, the current density is 0.01-0.03mA / pcs, and the voltage value applied to the positive and negative electrodes of the core package is 0.9 times the withstand voltage value of the positive electrode foil. After the core package is subjected to the forming repair treatment, the core package is placed at a temperature of 125° C. and dried for 40 minutes to obtain a formed core package; The core package after the chemical formation is immersed in an electrolyte containing triethylamine, phthalic acid and adipic acid, and voltage is applied to the positive and negative electrodes of the core package at the same time, and a vacuum pressure impregnation treatment is performed for 15 minutes, wherein the voltage value applied to the positive and negative electrodes of the core package is 0.8 times the withstand voltage value of the positive electrode foil, and then the core package is placed at a temperature of 125° C. and dried for 50 minutes to obtain a core package impregnated with electrolyte; The core package impregnated with electrolyte is assembled with an aluminum shell and a leather plug to obtain a semi-finished capacitor, and the semi-finished capacitor is charged and aged. Voltages are applied at 0.5 times, 1 times and 1.2 times the rated voltage respectively for segmented aging treatment. The aging temperature is 125°C and the aging time is 120 minutes to obtain a solid-liquid hybrid capacitor.
[0017] Example 2 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: The cut positive and negative electrode foils were treated with a 2% by mass NaOH solution at room temperature for 15 minutes to remove the oxide film and oil stains on the surface, and then the aluminum foil sample treated with alkali solution was immersed in a nitric acid solution with a volume fraction of 5% and a temperature of 20°C, connected to the circuit, the power cabinet voltage was set to 15V, the current was set to 75mA, and the treatment was carried out for 10 minutes to form a positive electrode porous layer with a thickness of 1.8μm on the positive electrode foil, and a negative electrode porous layer with a thickness of 1.8μm on the negative electrode foil; The remaining components and preparation method are exactly the same as those in Example 1.
[0018] Example 3 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: The cut positive and negative electrode foils were treated with a 2% by mass NaOH solution at room temperature for 20 minutes to remove the oxide film and oil stains on the surface, and then the aluminum foil sample treated with alkali solution was immersed in a nitric acid solution with a volume fraction of 5% and a temperature of 20°C, connected to the circuit, the power cabinet voltage was set to 15V, the current was set to 75mA, and the treatment was carried out for 10 minutes to form a positive electrode porous layer with a thickness of 2.0μm on the positive electrode foil, and a negative electrode porous layer with a thickness of 2.0μm on the negative electrode foil; The remaining components and preparation method are exactly the same as those in Example 1.
[0019] Example 4 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: The cut electrolytic paper is immersed in a dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) containing sodium polystyrene sulfonate and a phosphate compound for 10 minutes to form a dispersed protective layer on the electrolytic paper, wherein the amount of PEDOT:PSS aqueous dispersion is 50wt%, the amount of sodium polystyrene sulfonate is 2wt%, and the content of the phosphate compound is 2wt%. The positive electrode foil, the negative electrode foil and the electrolytic paper are then wound into a core package by a core package winding machine, wherein the electrolytic paper is between the positive electrode foil and the negative electrode foil, and the length of the electrolytic paper is longer than the length of the overlapping part of the positive and negative electrode foils, to obtain a core package; The remaining components and preparation method are exactly the same as those in Example 1.
[0020] Comparative Example 1 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: After forming a dispersed protective layer on the electrolytic paper, the positive electrode foil, the negative electrode foil and the electrolytic paper are wound into a core package by a core package winding machine, the electrolytic paper is between the positive electrode foil and the negative electrode foil, and the length of the electrolytic paper is longer than the length of the overlapping part of the positive and negative electrode foils, to obtain a core package, and the steps of forming a positive electrode porous layer on the positive electrode foil and forming a negative electrode porous layer on the negative electrode foil are omitted The remaining components and preparation method are exactly the same as those in Example 1.
[0021] Comparative Example 2 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: After forming a positive electrode porous layer on the positive electrode foil and a negative electrode porous layer on the negative electrode foil, the positive electrode foil, the negative electrode foil and the electrolytic paper are wound into a core package by a core package winding machine, wherein the electrolytic paper is interposed between the positive electrode foil and the negative electrode foil, and the length of the electrolytic paper is longer than the length of the overlapping part of the positive and negative electrode foils, to obtain a core package, and the step of forming a dispersed protective layer on the electrolytic paper is omitted; The remaining components and preparation method are exactly the same as those in Example 1.
[0022] Comparative Example 3 The preparation method of the solid-liquid hybrid capacitor comprises the following steps: The positive electrode foil, the negative electrode foil and the electrolytic paper are directly wound into a core package by a core package winding machine, the electrolytic paper is between the positive electrode foil and the negative electrode foil, and the length of the electrolytic paper is longer than the length of the overlapping part of the positive and negative electrode foils, to obtain the core package, and the steps of forming a positive electrode porous layer on the positive electrode foil, forming a negative electrode porous layer on the negative electrode foil, and forming a dispersed protective layer on the electrolytic paper are omitted; The remaining components and preparation method are exactly the same as those in Example 1.
[0023] Performance Testing Ten solid-liquid hybrid electrolytic capacitors of Examples 1-4 and Comparative Examples 1-3 were prepared, with capacitor specifications of 68 μF / 35 V and sizes of Φ6.3*7 mm. The seven groups of products were tested for capacitance (CAP), dissipation factor (DF), and equivalent series resistance (ESR) at a frequency of 120 Hz, and then tested for leakage current (LC) at a voltage of 35 V. The test results are shown in Table 1. The capacitance, dissipation factor, ESR, leakage current, and capacity decay measured at 125° C. after 4000 hours of load are shown in Table 2. Table 1 Performance test results of products in Examples 1-4 and Comparative Examples 1-3
[0024] Table 2 Performance test results of products after high temperature load in Examples 1-4 and Comparative Examples 1-3
[0025] As can be seen from Table 1, the capacitor prepared by the method of the present invention has a large capacity, small loss, small leakage current, and low equivalent series resistance. Compared with the capacitors prepared by the methods of Comparative Examples 1, 2, and 3, the capacitor prepared by the method of the present invention has a larger capacity, smaller loss, smaller leakage current, and lower equivalent series resistance, and the consistency of the capacitor's capacity, equivalent series resistance, and leakage current is better, which shows that the present invention can improve the consistency of the product's electrical performance. As can be seen from Table 2, the solid-liquid hybrid capacitor obtained by the preparation method of the present invention still has a larger capacitance, smaller loss, smaller leakage current, and lower equivalent series resistance after being loaded for 4000 hours at 125°C, and compared with Comparative Examples 1-3, △C / C, that is, the capacity decay, is greatly reduced. It can be seen that the process of the present invention improves the high-temperature storage performance of the product and enables the product to obtain a longer service life.
[0026] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A process for preparing a solid-liquid hybrid capacitor, characterized in that: At least the following steps are included: forming a positive electrode porous layer on the positive electrode foil, forming a negative electrode porous layer on the negative electrode foil, and forming a dispersed protective layer on the electrolytic paper; stacking the positive electrode foil, the electrolytic paper and the negative electrode foil together and winding them into a core package; The core package is impregnated with the dispersion liquid under pressure to obtain a core package impregnated with the dispersion liquid; Performing a chemical repair treatment on the core package impregnated with the dispersion liquid by using a chemical liquid to obtain a core package after chemical formation; Impregnating the formed core package with an electrolyte to obtain a core package impregnated with the electrolyte; Assembling the core package impregnated with the electrolyte with the aluminum shell and the leather plug and subjecting them to aging treatment to obtain a solid-liquid hybrid capacitor; Wherein, the pore size of the positive electrode porous layer is 20-400nm and the thickness is 1-3μm; The pore size of the negative electrode porous layer is 20-400 nm, and the thickness is 1-3 μm.
2. The process for preparing a solid-liquid hybrid capacitor according to claim 1, characterized in that: The positive electrode foil is one of aluminum, tantalum, niobium or titanium, and the preparation method of the positive electrode porous layer comprises the following steps: Treating the positive electrode foil with an alkaline solution to remove the surface oxide film and oil stains; The positive electrode foil treated with alkali solution is placed in a nitric acid solution, and oxidized by applying voltage and controlling temperature to generate the positive electrode porous layer.
3. The process for preparing a solid-liquid hybrid capacitor according to claim 2, characterized in that: The negative electrode foil is one of aluminum, tantalum, niobium or titanium and is the same as the positive electrode foil. The preparation method of the negative electrode porous layer is the same as the preparation method of the positive electrode porous layer.
4. The process for preparing a solid-liquid hybrid capacitor according to claim 1, characterized in that: The preparation method of the dispersion protective layer comprises the following steps: adding sodium polystyrene sulfonate and a phosphate compound into a dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) to obtain a mixed solution; Soaking or spraying electrolytic paper with the mixed solution to form the dispersed protective layer on the electrolytic paper; The content of the dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) is 10-60wt%, the content of the sodium polystyrene sulfonate is 0.1-5wt%, and the content of the phosphate compound is 0.1-5wt%.
5. The process for preparing a solid-liquid hybrid capacitor according to claim 1, characterized in that: The dispersion liquid is a dispersed aqueous solution of poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate), and the diameter of solid material particles in the dispersion liquid is not greater than 200 nm.
6. The process for preparing a solid-liquid hybrid capacitor according to claim 1, characterized in that: The chemical formation liquid is one of aqueous solutions of ammonium adipate, boric acid, phosphoric acid and ammonium dihydrogen phosphate, and the mass concentration of the chemical formation liquid is 5% to 10%.
7. The process for preparing a solid-liquid hybrid capacitor according to claim 1, characterized in that: The voltage used in the chemical formation repair treatment is 12-16V, and the current density is 0.01-0.03mA / pcs.
8. The process for preparing a solid-liquid hybrid capacitor according to claim 1, characterized in that: The electrolyte includes at least one or more of γ-butyrolactone, cyclopentane sulfone, polyethylene glycol, triethylamine phthalate, ethylene glycol, phthalic acid, and adipic acid.
Citation Information
Patent Citations
Preparation process of solid-liquid hybrid capacitor and solid-liquid hybrid capacitor
CN110379627A
Solid-liquid hybrid capacitor and preparation method thereof
CN113593909A
Solid-state electrolytic capacitor and manufacturing method thereof
JP2001135551A
Electrolytic capacitor
JP2017045868A