A core-shell bio-based polyacrylate emulsion with aromatic odor, preparation method and application thereof

By using the microcapsule structure of core-shell bio-based polyacrylate emulsion on textiles, the problem of fragrance fading of aromatic finishing agents after washing is solved, and the long-lasting release of fragrance and washability are achieved, which is suitable for environmentally friendly water-based printing glue. preparation.

CN115304724BActive Publication Date: 2024-10-25DONGGUAN CTL NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211080785.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-05
Publication Date
2024-10-25
Estimated Expiration
2042-09-05

AI Technical Summary

Technical Problem

In the prior art, aromatic finishing agents and spices are added to textiles and the aroma fades after washing, making it difficult to achieve long-lasting fragrance and resistance to washing.

Method used

Using core-shell bio-based polyacrylate emulsion, by designing the structure of the core layer and shell layer in the emulsion particles, acrylic and hydroxyacrylate monomers are used to form hydrogen bonds, and the cross-linking monomers and post-cross-linking monomers are combined. The body forms a microcapsule structure that releases aromatic scent for a long time and is water-resistant.

Benefits of technology

It achieves long-lasting release of fragrance on textiles and washability. The printing glue can continuously and slowly release fragrance on textiles and the fragrance does not dissipate after multiple washings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003833122740000042
    Figure BDA0003833122740000042
  • Figure BDA0003833122740000051
    Figure BDA0003833122740000051
  • Figure BDA0003833122740000061
    Figure BDA0003833122740000061
Patent Text Reader

Abstract

The invention provides a core-shell type bio-based polyacrylate emulsion with aromatic odor, and a preparation method and application thereof. The emulsion particles of the core-shell type bio-based polyacrylate emulsion are of a core-shell structure, the core-shell structure comprises a core layer and a shell layer, the raw materials for preparing the core layer comprise natural essence, acrylic monomers, hydroxy acrylic ester monomers, bio-based monomers, emulsifier A, emulsifier B and initiator; the raw materials for preparing the shell layer comprise cross-linking monomer A, cross-linking monomer B, post-cross-linking monomer, emulsifier A, bio-based monomer and initiator; by limiting the raw materials for preparing the shell layer and the core layer in the core-shell structure, the obtained core-shell type bio-based polyacrylate emulsion can release aromatic odor for a long time and is resistant to water washing, and also has excellent environmental protection characteristics, so that the printing paste prepared by using the emulsion has environmental protection performance and lasting fragrance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles, and in particular relates to a core-shell bio-based polyacrylate emulsion with aromatic odor, and a preparation method and application thereof. Background Art

[0002] With the improvement of living standards, people not only pay more and more attention to the appearance of textiles, but also begin to pursue the comfort and safety of textiles. Fragrance can not only make people have beautiful reverie, but also has many medical and health effects. Scientific research has proved that many fragrances have sedative, sterilizing, health care and other effects. If the fragrance is sprayed directly on the fabric, the fragrance will last for a short time and will not withstand washing.

[0003] The preparation process of textiles will go through padding, impregnation and printing processes. Adding an appropriate amount of aromatic finishing agent or fragrance during the preparation process of textiles can give the fabric a long-lasting and refreshing fragrance, make the fabric have a better wearing experience, and improve the grade and added value of the fabric products. CN113756091A discloses a textile finishing agent with added fragrance, belonging to the technical field of daily chemical products. The textile finishing agent is prepared by the following steps: a fragrance additive, an antibacterial agent, citric acid, sodium hypophosphite and deionized water are mixed to obtain a textile finishing agent with added fragrance; a homemade antibacterial agent is added to the textile finishing agent with added fragrance prepared by the invention, and the antibacterial agent is based on chitosan, which has antibacterial effect. Isocyanate groups are introduced into the antibacterial agent in the invention, and the isocyanate groups can react with hydroxyl groups on the surface of cotton textile fibers to be grafted with covalent bonds, thereby improving the stable antibacterial property of the antibacterial agent; in addition, ultraviolet absorbers are also introduced into the structure of the antibacterial agent, and after washing and drying clothes, the occurrence of fading of colored clothes and whitening of black clothes is reduced.

[0004] CN109385904A discloses a knitted fabric with three-proof and aromatic functions and a manufacturing method thereof, the method comprising: ① pre-treating and dyeing the knitted fabric; ② dehydrating and drying after leaving the vat, then dipping and rolling the aromatic finishing agent and the three-proof finishing agent in sequence, or dipping and rolling the aromatic finishing agent and the three-proof finishing agent at the same time, or dipping the aromatic finishing agent before leaving the vat, and dipping and rolling the three-proof finishing agent after leaving the vat; ③ drying and shaping. The knitted fabric produced by the invention not only has good three-proof functions, but also utilizes the principle of fragrance microcapsules, through the friction and destruction of the microcapsules during wearing, slowly releases a light fragrance, eliminates odor, refreshes the mind, and makes people feel relaxed and happy.

[0005] However, if the aromatic finishing agents and spices provided in the above-mentioned prior art are directly added to the printing coating, although the fabric can achieve the effect of releasing fragrance, the fragrance on the fabric will disappear once the fabric is washed, indicating that if the aromatic finishing agents and spices are directly added to the printing coating, they are very not resistant to washing.

[0006] Therefore, developing a core-shell bio-based polyacrylate emulsion with a long-lasting fragrance and water-resistant aroma is a technical problem that needs to be solved in the current field. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a core-shell type bio-based polyacrylate emulsion with an aromatic smell, and a preparation method and application thereof. The emulsion particles of the core-shell type bio-based polyacrylate emulsion are a core-shell structure. By limiting the preparation raw materials of the shell layer and the core layer of the core-shell structure, the obtained core-shell type bio-based polyacrylate emulsion can release the aromatic smell for a long time and is resistant to water washing, and also has environmental protection characteristics. Therefore, the printing paste prepared using the emulsion also has excellent environmental protection characteristics and a lasting fragrance.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a core-shell bio-based polyacrylate emulsion with an aromatic odor, wherein the emulsion particles of the core-shell bio-based polyacrylate emulsion are a core-shell structure, and the core-shell structure includes a core layer and a shell layer;

[0010] The raw materials for preparing the core layer include natural essence, acrylic monomer, hydroxy acrylic ester monomer, bio-based monomer, emulsifier A, emulsifier B and initiator;

[0011] The raw materials for preparing the shell layer include a cross-linking monomer A, a cross-linking monomer B, a post-cross-linking monomer, an emulsifier A, a bio-based monomer and an initiator.

[0012] The emulsion particles in the core-shell bio-based polyacrylate emulsion with aromatic odor provided by the present invention are core-shell structures. First, the bio-based monomers in the raw materials for preparing the core layer and the shell layer of the core-shell structure can have good compatibility with natural flavors, thereby making the obtained polyacrylate emulsion have environmental protection characteristics. Secondly, the functional monomers selected for the raw materials for preparing the core layer include acrylic monomers and hydroxy acrylate monomers. The carboxyl group in the acrylic monomer and the hydroxyl group in the hydroxy acrylate monomer can form a strong hydrogen bond force with the natural flavor, thereby helping to slow down the release rate of the flavor, so that the obtained polyacrylate emulsion has a lasting aromatic odor and the fragrance will not dissipate after washing. Finally, the raw materials for preparing the shell layer include two cross-linking monomers and a post-cross-linking monomer, so that the shell of the obtained core-shell structure can contain two cross-linking systems, thereby making the obtained core-shell acrylic emulsion have more excellent water resistance.

[0013] In summary, the core-shell bio-based polyacrylate emulsion provided by the present invention is a microcapsule structure with natural essence as the core and acrylic ester as the wall. It has the advantages of releasing aromatic odor for a long time and being resistant to water washing. It also has excellent environmental protection. After the coating printed on the textile fabric using the printing paste prepared therefrom is completely dried, it can slowly release the fragrance for a long time, and the fragrance will not dissipate after washing.

[0014] Preferably, the natural flavor includes floral natural flavor and / or non-floral natural flavor.

[0015] Preferably, the non-floral natural flavor includes a fruity natural flavor.

[0016] Preferably, the acrylic monomer includes any one of methacrylic acid, acrylic acid or β-acryloxypropionic acid (β-CEA) or a combination of at least two thereof.

[0017] Preferably, the hydroxyacrylate monomer includes any one of hydroxyethyl acrylate, hydroxypropyl acrylate or hydroxybutyl acrylate, or a combination of at least two thereof.

[0018] Preferably, the bio-based monomers in the core layer and the shell layer each independently include any one or a combination of at least two of biomass-derived vinyl monomers or acrylate monomers.

[0019] Preferably, the vinyl monomer includes acrylonitrile.

[0020] Preferably, the acrylic acid ester monomer includes lauric acid acrylate and / or octadecyl acrylate.

[0021] Preferably, the emulsifier A in the core layer and the shell layer includes an ammonium salt polymer emulsifier, for example, the reactive emulsifier ADEKA SR-10 produced by Japan ADEKA Corporation can be selected.

[0022] Preferably, the emulsifier B comprises a sodium salt polymer emulsifier.

[0023] Preferably, the sodium salt polymeric emulsifier includes 3-allyloxy-2-hydroxy-1-propanesulfonic acid sodium salt, for example, the emulsifier produced by Qingxin County Hanke Chemical Technology Co., Ltd. can be selected. HAPS.

[0024] Preferably, the initiators in the core layer and the shell layer each independently include any one of ammonium persulfate, sodium persulfate or potassium persulfate, or a combination of at least two of them.

[0025] Preferably, the cross-linking monomer A includes any one of ethylene glycol dimethacrylate, 1,6-hexanediol diacrylate or 1,4-butanediol diacrylate, or a combination of at least two thereof.

[0026] Preferably, the cross-linking monomer B comprises diacetone acrylamide.

[0027] Preferably, the post-crosslinking monomer comprises adipic acid dihydrazide.

[0028] Preferably, the raw materials for preparing the core layer further include a buffer and / or deionized water.

[0029] Preferably, the buffer comprises sodium bicarbonate and / or disodium hydrogen phosphate.

[0030] Preferably, the raw materials for preparing the shell layer also include ionized water.

[0031] Preferably, the raw materials for preparing the core layer include the following components in parts by weight:

[0032]

[0033]

[0034] Among them, the natural flavor can be 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight or 9.5 parts by weight, etc.

[0035] The acrylic monomer may be 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, or 0.95 parts by weight.

[0036] The hydroxy acrylate monomer may be 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight, etc.

[0037] The bio-based monomer may be 20.5 parts by weight, 21 parts by weight, 21.5 parts by weight, 22 parts by weight, 22.5 parts by weight, 23 parts by weight, 23.5 parts by weight, 24 parts by weight, 24.5 parts by weight, etc.

[0038] The emulsifier A may be 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight, etc.

[0039] The emulsifier B may be 0.11 parts by weight, 0.12 parts by weight, 0.13 parts by weight, 0.14 parts by weight, 0.15 parts by weight, 0.16 parts by weight, 0.17 parts by weight, 0.18 parts by weight, or 0.19 parts by weight.

[0040] The buffer may be 0.021 parts by weight, 0.022 parts by weight, 0.023 parts by weight, 0.024 parts by weight, 0.025 parts by weight, 0.026 parts by weight, 0.027 parts by weight, 0.028 parts by weight, or 0.029 parts by weight.

[0041] The initiator may be 0.21 parts by weight, 0.22 parts by weight, 0.23 parts by weight, 0.24 parts by weight, 0.25 parts by weight, 0.26 parts by weight, 0.27 parts by weight, 0.28 parts by weight, or 0.29 parts by weight, etc.

[0042] The deionized water may be 25.5 parts by weight, 26 parts by weight, 26.5 parts by weight, 27 parts by weight, 27.5 parts by weight, 28 parts by weight, 28.5 parts by weight, 29 parts by weight, 29.5 parts by weight, etc.

[0043] Preferably, the raw materials for preparing the shell layer include the following components in parts by weight:

[0044]

[0045] The crosslinking monomer A may be 0.32 parts by weight, 0.34 parts by weight, 0.36 parts by weight, 0.38 parts by weight, 0.4 parts by weight, 0.42 parts by weight, 0.44 parts by weight, 0.46 parts by weight or 0.48 parts by weight.

[0046] The crosslinking monomer B may be 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight, etc.

[0047] The emulsifier A may be 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight or 0.95 parts by weight, etc.

[0048] The bio-based monomer may be 20.5 parts by weight, 21 parts by weight, 21.5 parts by weight, 22 parts by weight, 22.5 parts by weight, 23 parts by weight, 23.5 parts by weight, 24 parts by weight, 24.5 parts by weight, etc.

[0049] The initiator may be 0.11 parts by weight, 0.12 parts by weight, 0.13 parts by weight, 0.14 parts by weight, 0.15 parts by weight, 0.16 parts by weight, 0.17 parts by weight, 0.18 parts by weight, 0.19 parts by weight, etc.

[0050] The post-crosslinking monomer may be 0.55 parts by weight, 0.6 parts by weight, 0.65 parts by weight, 0.7 parts by weight, 0.75 parts by weight, 0.8 parts by weight, 0.85 parts by weight, 0.9 parts by weight, or 0.95 parts by weight, etc.

[0051] The deionized water may be 15.5 parts by weight, 16 parts by weight, 16.5 parts by weight, 17 parts by weight, 17.5 parts by weight, 18 parts by weight, 18.5 parts by weight, 19 parts by weight, 19.5 parts by weight, etc.

[0052] Preferably, the solid content of the core-shell bio-based polyacrylate emulsion is 50-55%, for example, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%, 53.5%, 54% or 54.5%, etc.

[0053] Preferably, the viscosity of the core-shell bio-based polyacrylate emulsion is 1000-2000 cps, for example, 1100 cps, 1200 cps, 1300 cps, 1400 cps, 1500 cps, 1600 cps, 1700 cps, 1800 cps or 1900 cps.

[0054] In a second aspect, the present invention provides a method for preparing the core-shell bio-based polyacrylate emulsion as described in the first aspect, the preparation method comprising the following steps:

[0055] (1) dissolving emulsifier A in deionized water, adding natural flavor, acrylic monomer, hydroxy acrylate monomer and bio-based monomer for pre-emulsification to obtain a core layer pre-emulsion;

[0056] dissolving emulsifier A in deionized water, adding bio-based monomer, cross-linking monomer A and cross-linking monomer B for pre-emulsification to obtain a shell pre-emulsion;

[0057] (2) reacting a portion of the core layer pre-emulsion obtained in step (1), an emulsifier B, a portion of the core layer initiator, and an optional buffer in deionized water to obtain a seed emulsion;

[0058] (3) adding the remaining part of the initiator of the core layer and the remaining part of the core layer pre-emulsion obtained in step (1) to the seed emulsion obtained in step (2) to react and obtain a core layer emulsion;

[0059] (4) adding the shell layer pre-emulsion and the shell layer initiator obtained in step (1) to the core layer emulsion obtained in step (3) to react, cooling, adjusting the pH value, adding a post-crosslinking monomer and mixing to obtain the core-shell type bio-based polyacrylate emulsion.

[0060] Preferably, the pre-emulsification time in step (1) is independently 15 to 30 min, for example, 17 min, 19 min, 21 min, 23 min, 25 min, 27 min or 29 min.

[0061] Preferably, the pre-emulsification in step (1) is carried out under stirring conditions, and more preferably, is carried out under stirring conditions at a rotation speed of 80 to 150 rpm (e.g., 85 rpm, 90 rpm, 95 rpm, 100 rpm, 110 rpm, 120 rpm, 130 rpm or 140 rpm, etc.).

[0062] Preferably, the reaction temperature in step (2) is 80-82°C, for example, 80.2°C, 80.4°C, 80.6°C, 80.8°C, 81°C, 81.2°C, 81.4°C, 81.6°C or 81.8°C, etc.

[0063] Preferably, the reaction time of step (2) is 10 to 20 min, for example, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min or 19 min.

[0064] Preferably, the adding in step (3) is performed dropwise.

[0065] Preferably, the dropping time in step (3) is 1 to 1.5 h, for example, 1.05 h, 1.1 h, 1.15 h, 1.2 h, 1.25 h, 1.3 h, 1.35 h, 1.4 h or 1.45 h.

[0066] Preferably, the temperature of the dropping in step (3) is 80-82°C, for example, 80.2°C, 80.4°C, 80.6°C, 80.8°C, 81°C, 81.2°C, 81.4°C, 81.6°C or 81.8°C, etc.

[0067] Preferably, the adding in step (4) is performed dropwise.

[0068] Preferably, the dripping time in step (4) is 2 to 3 h, for example, 2.1 h, 2.2 h, 2.3 h, 2.4 h, 2.5 h, 2.6 h, 2.7 h, 2.8 h or 2.9 h.

[0069] Preferably, the temperature of the dropping in step (4) is 80-82°C, for example, 80.2°C, 80.4°C, 80.6°C, 80.8°C, 81°C, 81.2°C, 81.4°C, 81.6°C or 81.8°C, etc.

[0070] Preferably, the temperature of the system after cooling in step (4) is 50-55°C, for example, 50.5°C, 51°C, 51.5°C, 52°C, 52.5°C, 53°C, 53.5°C, 54°C or 54.5°C, etc.

[0071] Preferably, the pH value of the system after adjusting the pH value in step (4) is 7.5-8.5, for example, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3 or 8.4.

[0072] In a third aspect, the present invention provides an environmentally friendly water-based printing paste with fragrance, which comprises the following components in parts by weight: 25 to 30 parts by weight of the core-shell bio-based polyacrylate emulsion as described in the first aspect, 25 to 30 parts by weight of filler, 0.5 to 1 part by weight of dispersant, 3 to 4 parts by weight of wax emulsion, 0.5 to 1 part by weight of thickener and 5 to 7 parts by weight of water.

[0073] Wherein, the core-shell bio-based polyacrylate emulsion can be 25.5 parts by weight, 26 parts by weight, 26.5 parts by weight, 27 parts by weight, 27.5 parts by weight, 28 parts by weight, 28.5 parts by weight, 29 parts by weight or 29.5 parts by weight, etc.

[0074] The filler may be 25.5 parts by weight, 26 parts by weight, 26.5 parts by weight, 27 parts by weight, 27.5 parts by weight, 28 parts by weight, 28.5 parts by weight, 29 parts by weight, 29.5 parts by weight, etc.

[0075] The dispersant may be 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, etc.

[0076] The wax emulsion may be 3.1 parts by weight, 3.2 parts by weight, 3.3 parts by weight, 3.4 parts by weight, 3.5 parts by weight, 3.6 parts by weight, 3.7 parts by weight, 3.8 parts by weight, 3.9 parts by weight, etc.

[0077] The thickener may be 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, etc.

[0078] The water may be 5.2 parts by weight, 5.4 parts by weight, 5.6 parts by weight, 5.8 parts by weight, 6 parts by weight, 6.2 parts by weight, 6.4 parts by weight, 6.6 parts by weight, 6.8 parts by weight, etc.

[0079] In a fourth aspect, the present invention provides a method for preparing the environmentally friendly water-based printing paste as described in the third aspect, the preparation method comprising: mixing a core-shell bio-based polyacrylate emulsion, a filler, a dispersant, a wax emulsion, a thickener and water to obtain the environmentally friendly water-based printing paste.

[0080] In a fifth aspect, the present invention provides a use of the environmentally friendly water-based printing paste as described in the fourth aspect in textiles.

[0081] Compared with the prior art, the present invention has the following beneficial effects:

[0082] (1) The emulsion particles of the core-shell type bio-based polyacrylate emulsion with aromatic odor provided by the present invention are of a core-shell structure, wherein the core-shell structure comprises a core layer and a shell layer, wherein the raw materials for preparing the core layer comprise natural essence, acrylic monomers, hydroxy acrylic ester monomers, bio-based monomers, emulsifier A, emulsifier B and initiator; the raw materials for preparing the shell layer comprise cross-linking monomer A, cross-linking monomer B, post-cross-linking monomer, emulsifier A, bio-based monomer and initiator; and by limiting the raw materials for preparing the shell layer and the core layer of the core-shell structure, the obtained core-shell type bio-based polyacrylate emulsion can release aromatic odor for a long time and is resistant to water washing, and also has excellent environmental protection characteristics.

[0083] (2) After the coating of the printing paste containing the above emulsion is completely dried on the textile fabric, it can continue to slowly release fragrance for more than 3 to 6 months, and after at least 10 washings, the printing does not fall off or crack, and still has a faint fragrance.

[0084] (3) The printing paste provided by the present invention does not need to be overheated at high temperature during use, which can avoid accelerating the volatilization of flavors during high-temperature baking. DETAILED DESCRIPTION

[0085] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0086] Examples 1 to 3

[0087] A core-shell bio-based polyacrylate emulsion with an aromatic odor, wherein the emulsion particles are a core-shell structure, and the raw materials for preparing the shell layer and the core layer are shown in Table 1, wherein the units of each component are "parts by weight";

[0088] Table 1

[0089]

[0090]

[0091] The preparation method of the core-shell bio-based polyacrylate emulsion provided in Examples 1 to 3 comprises the following steps:

[0092] (1) Dissolve core layer emulsifier A (reactive emulsifier ADEKA SR-10 produced by Japan ADEKA Co., Ltd.) in part of core layer deionized water (accounting for 50% of the mass percentage of core layer deionized water), add floral natural flavor (Firmenich, FIR0112), acrylic acid, hydroxyethyl acrylate, core layer biomass-derived acrylonitrile (Solvay) and biomass-derived lauric acid ester, and pre-emulsify in a pre-emulsification kettle at a speed of 100 rpm for 20 minutes to obtain a core layer pre-emulsion;

[0093] Shell emulsifier A (reactive emulsifier ADEKA SR-10 produced by Japan ADEKA Co., Ltd.) was dissolved in deionized water, and acrylonitrile (Solvay) derived from biomass and lauric acid ester, 1,6-hexanediol diacrylate and diacetone acrylamide derived from biomass were added to the shell, and pre-emulsified for 20 minutes in a pre-emulsification kettle at a rotation speed of 100 rpm to obtain a shell pre-emulsion;

[0094] (2) a portion of the core layer pre-emulsion obtained in step (1) (accounting for 10% of the mass percentage of the core layer pre-emulsion obtained in step (1)) and emulsifier B (emulsifier A produced by Qingxin County Hanke Chemical Technology Co., Ltd.) were added to the mixture. HAPS), sodium bicarbonate and the remaining deionized water of the core layer are mixed at 65°C, and ammonium persulfate of a part of the core layer (accounting for 50% of the amount of ammonium persulfate in the core layer) is added, and the mixture is reacted at 80°C for 15 minutes to obtain a seed emulsion;

[0095] (3) at 80° C., slowly dropwise adding the remaining ammonium persulfate of the core layer and the remaining core layer pre-emulsion obtained in step (1) to the seed emulsion obtained in step (2) for 1.5 h to obtain a core layer emulsion;

[0096] (4) at 80° C., slowly dropping the shell pre-emulsion and the ammonium persulfate of the shell into the core emulsion obtained in step (3) for 2.5 h, cooling to 50° C., adjusting the pH value to 8, adding adipic acid dihydrazide, and obtaining the core-shell bio-based polyacrylate emulsion;

[0097] Example 4

[0098] A core-shell bio-based polyacrylate emulsion with an aromatic odor, which differs from Example 1 only in that a fruity natural flavor (Firmenich, FIR0101) is used to replace the floral flavor, and other components, amounts and preparation methods are the same as those in Example 1.

[0099] Example 5

[0100] A core-shell bio-based polyacrylate emulsion with an aromatic odor, which differs from Example 1 only in that methacrylic acid is used to replace acrylic acid in the core layer, and other components, amounts and preparation methods are the same as those in Example 1.

[0101] Example 6

[0102] A core-shell bio-based polyacrylate emulsion with an aromatic odor, which differs from Example 1 only in that hydroxybutyl acrylate is used to replace hydroxyethyl acrylate in the core layer, and other components, amounts and preparation methods are the same as those in Example 1.

[0103] Comparative Example 1

[0104] A bio-based polyacrylate emulsion with aromatic odor, wherein the raw materials for preparing the emulsion include the following components in parts by weight: 7 parts by weight of floral natural flavor, 0.75 parts by weight of acrylic acid, 1.5 parts by weight of hydroxyethyl acrylate, 4.5 parts by weight of acrylonitrile derived from biomass, 17.5 parts by weight of lauric acid ester derived from biomass, 1.5 parts by weight of emulsifier A, 0.15 parts by weight of emulsifier B, 0.02 parts by weight of sodium bicarbonate, 0.25 parts by weight of ammonium persulfate and 27 parts by weight of deionized water;

[0105] The preparation method of the bio-based polyacrylate emulsion provided in this comparative example comprises the following steps:

[0106] (1) Dissolve core layer emulsifier A (reactive emulsifier ADEKA SR-10 produced by Japan ADEKA Co., Ltd.) in part of core layer deionized water (accounting for 50% of the mass percentage of core layer deionized water), add floral fragrance (Firmenich, FIR0112), acrylic acid, hydroxyethyl acrylate, biomass-derived acrylonitrile (Solvay) and biomass-derived lauric acid ester, and pre-emulsify for 20 minutes in a pre-emulsification kettle at a rotation speed of 100 rpm to obtain a pre-emulsion;

[0107] (2) a portion of the pre-emulsion obtained in step (1) (accounting for 10% by weight of the pre-emulsion obtained in step (1)) and emulsifier B (emulsifier A produced by Qingxin County Hanke Chemical Technology Co., Ltd.) were added to the mixture. HAPS), sodium bicarbonate and the remaining deionized water were mixed at 65° C., and part of ammonium persulfate (accounting for 50% of the mass percentage of ammonium persulfate) was added and reacted at 80° C. for 15 minutes to obtain a seed emulsion;

[0108] (3) slowly adding the remaining part of the ammonium persulfate and the remaining part of the pre-emulsion obtained in step (1) to the seed emulsion obtained in step (2), the dropping time is 1 hour, and reacting at 80° C. for 30 minutes to obtain the bio-based polyacrylate emulsion with aromatic odor.

[0109] Comparative Example 2

[0110] A bio-based polyacrylate emulsion with aromatic odor, which is different from Example 1 only in that no acrylic acid or hydroxyethyl acrylate is added to the preparation raw materials, and other components, amounts and preparation methods are the same as those in Example 1.

[0111] Comparative Example 3

[0112] A bio-based polyacrylate emulsion with an aromatic odor, which differs from Example 1 in that 1,6-hexanediol diacrylate is not added to the raw materials for preparing the shell layer, the added amount of diacetone acrylamide is 1.9 parts by weight, and other components, amounts and preparation methods are the same as those in Example 1.

[0113] Comparative Example 4

[0114] A bio-based polyacrylate emulsion with an aromatic odor, which differs from Example 1 in that diacetone acrylamide is not added to the raw materials for preparing the shell layer, the added amount of 1,6-hexanediol diacrylate is 1.9 parts by weight, and other components, amounts and preparation methods are the same as those in Example 1.

[0115] Application Example 1

[0116] A fragrant environmentally friendly water-based printing paste, which comprises the following components in parts by weight: 30 parts by weight of core-shell bio-based polyacrylate emulsion (Example 1), 30 parts by weight of titanium dioxide, 0.75 parts by weight of dispersant (San Nopco, 5040), 3.5 parts by weight of wax emulsion (Ding Hengxin, DHX-50503), 0.75 parts by weight of thickener (Aison, PTF) and 6 parts by weight of water;

[0117] The preparation method of the environmentally friendly water-based printing paste provided in this application example comprises: mixing a core-shell bio-based polyacrylate emulsion, a filler, a dispersant, a wax solution, a thickener and water to obtain the environmentally friendly water-based printing paste.

[0118] Application Examples 2 to 6

[0119] A fragrant and environmentally friendly water-based printing paste, which differs from Application Example 1 only in that the core-shell bio-based polyacrylate emulsions obtained in Examples 2 to 6 are used to replace the core-shell bio-based polyacrylate emulsion obtained in Example 1, and other components, dosages and preparation methods are the same as those in Application Example 1.

[0120] Comparative Application Examples 1 to 4

[0121] A fragrant and environmentally friendly water-based printing paste, which differs from Application Example 1 only in that the bio-based polyacrylate emulsions obtained in Comparative Examples 1 to 4 are used to replace the core-shell bio-based polyacrylate emulsion obtained in Example 1, and other components, dosages and preparation methods are the same as those in Application Example 1.

[0122] Performance Test:

[0123] (1) Fragrance persistence: The test was conducted with reference to GB / T14454.2-2008 Fragrance Fragrance Evaluation Method. The evaluation room and evaluators selected in the standard were used. Three evaluators evaluated the printed cloth with fragrance in the evaluation room. After each evaluation, the cloth was placed in a 60°C oven and taken out every 24 hours for the next evaluation. The above operation was repeated until more than two evaluators determined that there was no fragrance. The number of days was recorded, which was the evaluation of the durability of the print. The longer the number of days, the better the durability.

[0124] (2) Washing fastness: Wash the printed fabric in 60°C water for 1 hour, cycle 5 times, and observe whether the printed part has cracking or falling off. Test instrument: According to GB / T8629-2017 Type A washing machine 4N procedure;

[0125] (3) Fragrance durability in washing: The test was conducted with reference to GB / T14454.2-2008 Fragrance Fragrance Evaluation Method. The evaluation room and evaluators selected in this standard were used. Three evaluators evaluated the printed cloth with a fragrant smell in the evaluation room. After each evaluation, the cloth was washed in water at 40°C for 1 hour and dried before the next evaluation. The above operation was repeated until more than two evaluators determined that there was no fragrant smell. The number of washes was recorded, which was the durability evaluation of the print. The longer the number of washes, the better the durability of the print.

[0126] According to the above test method, the environmentally friendly water-based printing paste with fragrance provided by Examples 1 to 6 and Comparative Application Examples 1 to 4 was tested, and the test results are shown in Table 2:

[0127] Table 2

[0128]

[0129]

[0130] It can be seen from the data in Table 2 that the printing paste prepared by using the core-shell bio-based polyacrylate emulsion provided by the present invention has excellent fragrance persistence, water washing resistance and water washing fragrance persistence.

[0131] Specifically, according to the data of Application Examples 1 to 6, it can be seen that the fragrance of the environmentally friendly water-based printing paste provided in Application Examples 1 to 6 lasts for 8 to 15 days, the water absorption fastness tests all show that it is intact, and the fragrance washing durability can be washed 15 to 20 times; and according to the data of Application Examples 1 to 6, it can also be seen that within a specific range, the more the amount of fragrance added, the greater the amount of cross-linking agent used, and the more outstanding the performance.

[0132] It can be seen from the data of Comparative Application Example 1 and Comparative Application Example 1 that the printing paste provided in Comparative Application Example 1 adopts a conventional bio-based polyacrylate emulsion of non-core-shell type. Because there is no shell layer coating, the flavor evaporates quickly, so the fragrance persistence and fragrance water washing resistance are poor.

[0133] By comparing the data of Application Example 1 and Comparative Application Example 2, it can be found that the bio-based emulsion obtained without adding functional monomers will also cause the flavor to volatilize quickly due to the lack of hydrogen bonding, which in turn makes the fragrance persistence and fragrance water washing resistance of the prepared printing paste poor.

[0134] Further comparison of Application Example 1 and Comparative Application Examples 3-4 also shows that Comparative Application Example 3 uses the bio-based polyacrylate emulsion prepared by Comparative Example 3 without adding an internal cross-linking monomer, which will affect the washing fastness and water-resistant fragrance persistence of the obtained printing paste due to the lack of a network structure in the shell layer; and Comparative Application Example 4 uses the bio-based polyacrylate emulsion prepared by Comparative Example 4 without adding diacetone acrylamide, which will also affect the washing fastness of the obtained printing paste.

[0135] The applicant declares that the present invention illustrates a core-shell bio-based polyacrylate emulsion with aromatic odor and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A core-shell bio-based polyacrylate emulsion with aromatic odor, It is characterized in that The emulsion particles of the core-shell bio-based polyacrylate emulsion are of a core-shell structure, and the core-shell structure comprises a core layer and a shell layer; The raw materials for preparing the core layer include natural essence, acrylic monomer, hydroxy acrylic ester monomer, bio-based monomer, emulsifier A, emulsifier B and initiator; The raw materials for preparing the shell layer include cross-linking monomer A, cross-linking monomer B, post-cross-linking monomer, emulsifier A, bio-based monomer and initiator; The hydroxy acrylate monomer includes any one of hydroxyethyl acrylate, hydroxypropyl acrylate or hydroxybutyl acrylate, or a combination of at least two thereof; The emulsifier A in the core layer and the shell layer both include ammonium salt polymer emulsifiers; The emulsifier B includes a sodium salt polymer emulsifier; The crosslinking monomer A includes any one or a combination of at least two of ethylene glycol dimethacrylate, 1,6-hexanediol diacrylate or 1,4-butanediol diacrylate; The post-crosslinking monomer includes adipic acid dihydrazide; The bio-based monomers in the core layer and the shell layer each independently include any one or a combination of at least two of acrylonitrile or acrylate monomers derived from biomass; The cross-linking monomer B includes diacetone acrylamide.

2. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The natural flavors include floral natural flavors and / or non-floral natural flavors.

3. The core-shell bio-based polyacrylate emulsion according to claim 2, It is characterized in that The non-floral natural flavor includes fruity natural flavor.

4. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The acrylic monomer includes any one of methacrylic acid, acrylic acid or β-acryloxypropionic acid or a combination of at least two thereof.

5. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The acrylic acid ester monomers include lauric acid acrylate and / or octadecyl acrylate.

6. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The sodium salt polymer emulsifier includes 3-allyloxy-2-hydroxy-1-propanesulfonic acid sodium salt.

7. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The initiators in the core layer and the shell layer independently include any one of ammonium persulfate, sodium persulfate or potassium persulfate, or a combination of at least two of them.

8. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The raw materials for preparing the core layer also include a buffer and / or deionized water.

9. The core-shell bio-based polyacrylate emulsion according to claim 8, It is characterized in that The buffer includes sodium bicarbonate and / or disodium hydrogen phosphate.

10. The core-shell bio-based polyacrylate emulsion according to claim 8, It is characterized in that The raw materials for preparing the shell layer also include deionized water.

11. The core-shell bio-based polyacrylate emulsion according to claim 8, It is characterized in that The raw materials for preparing the core layer include the following components in parts by weight: Natural flavor 5-10 parts by weight Acrylic acid monomer 0.5~1 weight part 1-2 parts by weight of hydroxy acrylate monomer Bio-based monomer 20-25 parts by weight Emulsifier A 1~2 parts by weight Emulsifier B 0.1~0.2 parts by weight Buffer 0.02~0.03 parts by weight Initiator 0.2~0.3 parts by weight Deionized water 25-30 parts by weight.

12. The core-shell bio-based polyacrylate emulsion according to claim 10, It is characterized in that The raw materials for preparing the shell layer include the following components in parts by weight: Crosslinking monomer A 0.3~0.5 parts by weight Crosslinking monomer B 1~2 parts by weight Emulsifier A 0.5~1 weight part Bio-based monomer 20-25 parts by weight Initiator 0.1~0.2 parts by weight Post-crosslinking monomer 0.5~1 weight part 15-20 parts by weight of deionized water.

13. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The solid content of the core-shell bio-based polyacrylate emulsion is 50-55%.

14. The core-shell bio-based polyacrylate emulsion according to claim 1, It is characterized in that The viscosity of the core-shell bio-based polyacrylate emulsion is 1000-2000 cps.

15. A method for preparing the core-shell bio-based polyacrylate emulsion according to any one of claims 1 to 14, It is characterized in that The preparation method comprises the following steps: (1) dissolving emulsifier A in water, adding natural flavor, acrylic monomer, hydroxy acrylate monomer and bio-based monomer for pre-emulsification to obtain a core layer pre-emulsion; dissolving emulsifier A in deionized water, adding bio-based monomer, cross-linking monomer A and cross-linking monomer B for pre-emulsification to obtain a shell pre-emulsion; (2) reacting a portion of the core layer pre-emulsion obtained in step (1), emulsifier B, a portion of the core layer initiator, and optionally a buffer in deionized water to obtain a seed emulsion; (3) adding the remaining part of the initiator of the core layer and the remaining part of the core layer pre-emulsion obtained in step (1) to the seed emulsion obtained in step (2) to react and obtain a core layer emulsion; (4) adding the shell pre-emulsion and the shell initiator obtained in step (1) to the core emulsion obtained in step (3) to react, cooling, adjusting the pH value, adding a post-crosslinking monomer and mixing to obtain the core-shell bio-based polyacrylate emulsion.

16. The preparation method according to claim 15, It is characterized in that The pre-emulsification time in step (1) is independently 15 to 30 minutes.

17. The preparation method according to claim 15, It is characterized in that The pre-emulsification in step (1) is carried out under stirring conditions.

18. The preparation method according to claim 17, It is characterized in that The pre-emulsification in step (1) is carried out under stirring conditions at a rotation speed of 80 to 150 rpm.

19. The preparation method according to claim 15, It is characterized in that The reaction temperature in step (2) is 80-82°C.

20. The preparation method according to claim 15, It is characterized in that The reaction time of step (2) is 10 to 20 minutes.

21. The preparation method according to claim 15, It is characterized in that The method of adding in step (3) is dropwise addition.

22. The preparation method according to claim 21, It is characterized in that The dripping time in step (3) is 1 to 1.5 hours.

23. The preparation method according to claim 21, It is characterized in that The temperature of the dropping in step (3) is 80-82°C.

24. The preparation method according to claim 15, It is characterized in that The method of adding in step (4) is dropwise addition.

25. The preparation method according to claim 24, It is characterized in that The dripping time in step (4) is 2 to 3 hours.

26. The preparation method according to claim 24, It is characterized in that The temperature of the dropwise addition in step (4) is 80-82°C.

27. The preparation method according to claim 15, It is characterized in that After the cooling in step (4), the temperature of the system is 50-55°C.

28. The preparation method according to claim 15, It is characterized in that After the pH value is adjusted in step (4), the pH value of the system is 7.5-8.

5.

29. A scented environmentally friendly water-based printing paste. It is characterized in that The environmentally friendly water-based printing paste comprises the following components in parts by weight: 25 to 30 parts by weight of the core-shell bio-based polyacrylate emulsion as described in any one of claims 1 to 14, 25 to 30 parts by weight of filler, 0.5 to 1 part by weight of dispersant, 3 to 4 parts by weight of wax emulsion, 0.5 to 1 part by weight of thickener and 5 to 7 parts by weight of water.

30. A method for preparing the environmentally friendly water-based printing paste as claimed in claim 29, It is characterized in that The preparation method comprises: mixing core-shell bio-based polyacrylate emulsion, filler, dispersant, wax emulsion, thickener and water to obtain the environmentally friendly water-based printing paste.

31. Use of the environmentally friendly water-based printing paste as claimed in claim 29 in textiles.