A method for preparing a layered manganese dioxide material with large-size cation embedding and a method for preparing an aqueous zinc ion battery positive electrode
By using layered manganese dioxide material embedded with organic ammonium cations in aqueous zinc ion batteries, the layer spacing of δ-MnO2 is expanded, the problem of structural instability is solved, and the cycle stability and specific capacity of the battery are significantly improved. More efficient electrochemical properties are achieved.
Patent Information
- Application Number
- CN202211020116.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-08-24
AI Technical Summary
The existing layered manganese dioxide is unstable in aqueous zinc ion batteries, resulting in severe electrostatic interactions and steric hindrance during the insertion and removal of zinc ions, affecting the electrochemical stability, and the existing modification methods cannot effectively expand the layer. spacing.
By synthesizing δ-MnO2 nanosheet dispersion in aqueous solution, and using the electrostatic effect between organic ammonium cations and δ-MnO2 nanosheets, large-sized cations are embedded between δ-MnO2 layers through aqueous phase layer assembly method. Expand the layer spacing and improve the electrochemical energy storage performance and stability of the material.
The cycling stability and specific capacity of aqueous zinc ion batteries are significantly improved, and the layer spacing of modified materials is more suitable for Zn2+ rapid and reversible embedding, improving the electrochemical performance of the battery.
Smart Images

Figure CN115312729B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aqueous zinc ion batteries. Background Art
[0002] As a new type of secondary battery, aqueous zinc-ion batteries (ZIBs) have the advantages of high energy density, efficient and safe discharge process, non-toxic and cheap battery materials, and simple preparation process. They have high application value and development prospects in emerging large-scale energy storage fields such as energy storage grids. However, due to the large ionic radius and high charge density of divalent zinc ions, zinc ions have strong electrostatic interactions and large steric hindrance during the embedding and extraction process of positive electrode materials, which greatly affects the structural stability of positive electrode materials. Therefore, it is necessary to develop new positive electrode materials for zinc-ion batteries.
[0003] MnO2 is a commonly used positive electrode material for aqueous zinc-ion batteries. It can be divided into tunnel structure (i.e., α, β, γ, R and other crystal forms of MnO2) and layered structure (δ-MnO2) according to its crystal form. Among them, the layered structure of δ-MnO2 has larger spacing channels than other tunnel-type MnO2. Moreover, layered nanomaterials have a large specific surface area. These characteristics are beneficial to Zn 2+ Rapid and reversible (de)embedding. Therefore, δ-MnO2 is considered to be a good energy storage material for rapid charging and discharging of aqueous zinc-ion batteries. However, due to the serious structural transformation problem of δ-MnO2 during the cycle process, the electrochemical stability of the Zn||δ-MnO2 battery system is significantly affected. In order to solve the problem of structural instability of δ-MnO2, interlayer modification is an effective solution. As a positive electrode material for aqueous zinc-ion batteries, the existing interlayer modification methods are mainly achieved by introducing pillar-type metal cations. 0.28 MnO2·0.5H2O as a High Performance Cathode for Aqueous Zinc-Ion Battery (Small, 2020, 16, 2000597) discloses a Ca 2+ Pre-embedded δ-MnO2 material; "Zinc ion stabilized MnO2 nanospheres for high capacity and long lifespan aqueous zinc-ion batteries" (J. Mater. Chem. A, 2019, 7, 13727) discloses a Zn 2+ Pre-embedded δ-MnO2 material. However, none of the above materials can further expand the interlayer spacing of δ-MnO2. Summary of the invention
[0004] The present invention aims to solve the problem that the existing layered manganese dioxide interlayer modification method cannot expand the δ-MnO2 interlayer spacing on a large scale, and further provide a method for preparing a large-size cation-embedded layered manganese dioxide material and a method for preparing an aqueous zinc ion battery positive electrode.
[0005] A method for preparing a large-size cation-embedded layered manganese dioxide material is carried out according to the following steps:
[0006] 1. Dissolve potassium permanganate, concentrated sulfuric acid solution and anhydrous methanol in ultrapure water, stir evenly, and heat to react to obtain a manganese dioxide nanosheet dispersion;
[0007] 2. dissolving the salt containing the pre-embedded cation in ultrapure water to obtain a salt solution;
[0008] The pre-embedded cation in the salt containing pre-embedded cations is an organic ammonium cation;
[0009] 3. Adding the salt solution to the manganese dioxide nanosheet dispersion, stirring at a stirring speed of 200 rpm to 1000 rpm until a precipitate is precipitated, and then filtering, washing and drying to obtain a large-sized cation-embedded layered manganese dioxide material;
[0010] The molar ratio of the salt containing pre-embedded cations in the salt solution to the Mn element in the manganese dioxide nanosheet dispersion is 100:(3-15);
[0011] The interlayer spacing of the layered manganese dioxide material with large-size cation embedding is
[0012] A method for preparing an aqueous zinc ion battery positive electrode from a layered manganese dioxide material with large-sized cations embedded therein, comprising the following steps: mixing the layered manganese dioxide material with large-sized cations embedded therein, a conductive agent, a binder and N-methylpyrrolidone to obtain a homogenate, coating the homogenate on a current collector or pressing the dried homogenate on the current collector to obtain an aqueous zinc ion battery positive electrode;
[0013] The mass ratio of the large-size cation embedded layered manganese dioxide material to the binder is (6-8):1; the mass ratio of the conductive agent to the binder is (3-1):1; the loading amount of the large-size cation embedded layered manganese dioxide material in the positive electrode of the aqueous zinc ion battery is 0.8 mg / cm 2 ~2mg / cm 2 .
[0014] The beneficial effects of the present invention are:
[0015] The present invention discloses a method for preparing a layered manganese dioxide with large-sized cations embedded therein. The method firstly synthesizes a δ-MnO2 nanosheet dispersion in an aqueous solution, and then utilizes the electrostatic interaction between organic ammonium cations and the δ-MnO2 nanosheets to embed large-sized cations into the δ-MnO2 interlayer from bottom to top through a water-phase layer-by-layer assembly method, thereby effectively expanding the interlayer spacing of the δ-MnO2 to 100 nm. Increase its active sites and improve the electrochemical energy storage performance of the material. At the same time, the embedded large-sized organic ammonium cations can also play a certain supporting role and improve the stability of the material in electrochemical tests. The above preparation method is simple in process, easy to operate and repeat, has universality, can be used for large-scale production, and has good application prospects.
[0016] The present invention also discloses the application of the above-mentioned large-size cation-embedded layered manganese dioxide material in the positive electrode of an aqueous zinc ion battery. Due to the supporting effect of the embedded cations in the material, when the material is used as the positive electrode material of an aqueous zinc ion battery, the cycle stability of the battery system is significantly improved (TMA-δ-MnO2 has a first cycle capacity of 61.1 mAh / g at a current density of 1 A / g, and after activation, the capacity can be maintained at 94.7 mAh / g after 800 cycles). The modified δ-MnO2 material has a wider interlayer spacing and is more suitable for Zn 2+ Rapid and reversible (de)embedding and increased active sites can effectively improve the specific capacity of the battery (TMA-δ-MnO2 has a capacity of up to 374.7 mAh / g at a current density of 0.15 A / g, which is a significant improvement over the 193.2 mAh / g of δ-MnO2 prepared in comparative experiment 1). In summary, the electrochemical performance of the above-mentioned large-size cation-embedded layered manganese dioxide materials in aqueous zinc-ion batteries, including specific capacity and cycle stability, has been significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The δ-MnO2 prepared in comparative experiment 1 is used as the positive electrode active material and assembled into a button cell, which is cycled 800 times at a current density of 1A / g. 1 is the coulomb efficiency curve, and 2 is the discharge specific capacity curve;
[0018] Figure 2 The figure is a cycle performance diagram of a button cell assembled with TMA-δ-MnO2 prepared in Example 1 as the positive electrode active material and cycled 800 times at a current density of 1 A / g, wherein 1 is the coulomb efficiency curve and 2 is the discharge specific capacity curve;
[0019] Figure 3The cycle performance diagram of a button cell assembled with NH4-δ-MnO2 prepared in Example 2 as the positive electrode active material and cycled 800 times at a current density of 1 A / g, 1 is the coulomb efficiency curve, and 2 is the discharge specific capacity curve;
[0020] Figure 4 The cycle performance diagram of a button cell assembled with TEA-δ-MnO2 prepared in Example 3 as the positive electrode active material and cycled 800 times at a current density of 1 A / g, 1 is the coulombic efficiency curve, and 2 is the discharge specific capacity curve;
[0021] Figure 5 This is the X-ray diffraction image of δ-MnO2 prepared in comparative experiment 1;
[0022] Figure 6 This is the X-ray diffraction image of TMA-δ-MnO2 prepared in Example 1;
[0023] Figure 7 This is the X-ray diffraction image of NH4-δ-MnO2 prepared in Example 2;
[0024] Figure 8 This is the X-ray diffraction image of TEA-δ-MnO2 prepared in Example 3;
[0025] Fig. 9 The TMA-δ-MnO2 prepared in Example 1 is used as the positive electrode active material and a button cell is assembled. After 10 cycles of activation at a low current density of 0.15 A / g, the charge and discharge curves of the 10th cycle, 1 is the charge curve, and 2 is the discharge curve;
[0026] Fig.10 The δ-MnO2 prepared in comparative experiment 1 is used as the positive electrode active material and assembled into a button cell. After 10 cycles of activation at a low current density of 0.15A / g, the charge and discharge curves of the 10th cycle, 1 is the charge curve, 2 is the discharge curve;
[0027] Fig.11 This is a high-resolution image of δ-MnO2 prepared in the comparative experiment 1 under a transmission electron microscope (TEM);
[0028] Fig.12 This is a high-resolution image of TMA-δ-MnO2 prepared in Example 1 under a transmission electron microscope (TEM);
[0029] Fig.13 This is an image of the manganese dioxide nanosheets in the manganese dioxide nanosheet dispersion prepared in step 1 of Example 1 under a scanning electron microscope (SEM). DETAILED DESCRIPTION
[0030] Specific implementation method 1: This implementation method is a method for preparing a large-size cation-embedded layered manganese dioxide material, which is carried out according to the following steps:
[0031] 1. Dissolve potassium permanganate, concentrated sulfuric acid solution and anhydrous methanol in ultrapure water, stir evenly, and heat to react to obtain a manganese dioxide nanosheet dispersion;
[0032] 2. dissolving the salt containing the pre-embedded cation in ultrapure water to obtain a salt solution;
[0033] The pre-embedded cation in the salt containing pre-embedded cations is an organic ammonium cation;
[0034] 3. Adding the salt solution to the manganese dioxide nanosheet dispersion, stirring at a stirring speed of 200 rpm to 1000 rpm until a precipitate is precipitated, and then filtering, washing and drying to obtain a large-sized cation-embedded layered manganese dioxide material;
[0035] The molar ratio of the salt containing pre-embedded cations in the salt solution to the Mn element in the manganese dioxide nanosheet dispersion is 100:(3-15);
[0036] The interlayer spacing of the layered manganese dioxide material with large-size cation embedding is
[0037] The beneficial effects of this embodiment are:
[0038] This embodiment discloses a method for preparing a layered manganese dioxide with large-sized cations embedded therein. The method first synthesizes a δ-MnO2 nanosheet dispersion in an aqueous solution, and then utilizes the electrostatic interaction between organic ammonium cations and δ-MnO2 nanosheets to embed large-sized cations into the δ-MnO2 interlayer from bottom to top through an aqueous phase layer-by-layer assembly method, thereby effectively expanding the interlayer spacing of δ-MnO2 to Increase its active sites and improve the electrochemical energy storage performance of the material. At the same time, the embedded large-sized organic ammonium cations can also play a certain supporting role and improve the stability of the material in electrochemical tests. The above preparation method is simple in process, easy to operate and repeat, has universality, can be used for large-scale production, and has good application prospects.
[0039] This embodiment also discloses the use of the above-mentioned large-size cation-embedded layered manganese dioxide material in the positive electrode of an aqueous zinc ion battery. Due to the pillar effect of the embedded cations in the material, when the material is used as the positive electrode material of an aqueous zinc ion battery, the cycle stability of the battery system is significantly improved (TMA-δ-MnO2 has a first cycle capacity of 61.1 mAh / g at a current density of 1 A / g, and after activation, the capacity can be maintained at 94.7 mAh / g after 800 cycles). The modified δ-MnO2 material has a wider interlayer spacing and is more suitable for Zn 2+ Rapid and reversible (de)embedding and increased active sites can effectively improve the specific capacity of the battery (TMA-δ-MnO2 has a capacity of up to 374.7 mAh / g at a current density of 0.15 A / g, which is a significant improvement over the 193.2 mAh / g of δ-MnO2 prepared in comparative experiment 1). In summary, the electrochemical performance of the above-mentioned large-size cation-embedded layered manganese dioxide materials in aqueous zinc-ion batteries, including specific capacity and cycle stability, has been significantly improved.
[0040] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the molar ratio of potassium permanganate to sulfuric acid in the concentrated sulfuric acid solution in step 1 is 1:(0.5-2); the molar ratio of potassium permanganate to anhydrous methanol in step 1 is 1:(10-20); the mass percentage of the concentrated sulfuric acid solution in step 1 is 80%-98.3%. Others are the same as specific implementation method 1.
[0041] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the heating reaction described in step 1 is carried out in an air atmosphere at a temperature of 60°C to 95°C for 0.5h to 2h. The rest is the same as specific embodiment 1 or 2.
[0042] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the molar concentration of the Mn element in the manganese dioxide nanosheet dispersion in step 1 is 0.5 mmol / L to 1.5 mmol / L. Other aspects are the same as specific embodiments 1 to 3.
[0043] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the salt containing pre-embedded cations in step 2 is one or more of ammonium chloride, tetramethylammonium chloride, tetraethylammonium chloride and tetrabutylammonium chloride; the diameter of the organic ammonium cation in step 2 is The rest is the same as Specific Embodiments 1 to 4.
[0044] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the concentration of the salt solution in step 2 is 0.1 mol / L to 1 mol / L. The rest is the same as specific implementation methods 1 to 5.
[0045] Specific embodiment 7: This embodiment is different from Specific embodiments 1 to 6 in that: the stirring time in step 3 is 5 min to 240 min; the washing in step 3 is high-speed centrifugal washing; the drying in step 3 is specifically vacuum drying at a temperature of 50°C to 80°C for 6h to 24h. The rest is the same as Specific embodiments 1 to 6.
[0046] Specific embodiment eight: This embodiment is a method for preparing a positive electrode of an aqueous zinc ion battery using a layered manganese dioxide material with large-sized cations embedded therein, which is carried out according to the following steps: mixing a layered manganese dioxide material with large-sized cations embedded therein, a conductive agent, a binder and N-methylpyrrolidone to obtain a homogenate, coating the homogenate on a current collector or pressing the dried homogenate on a current collector to obtain a positive electrode of an aqueous zinc ion battery;
[0047] The mass ratio of the large-size cation embedded layered manganese dioxide material to the binder is (6-8):1; the mass ratio of the conductive agent to the binder is (3-1):1; the loading amount of the large-size cation embedded layered manganese dioxide material in the positive electrode of the aqueous zinc ion battery is 0.8 mg / cm 2 ~2mg / cm 2 .
[0048] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that the current collector is titanium foil, stainless steel foil, titanium mesh or stainless steel mesh. Other aspects are the same as specific embodiment 8.
[0049] Specific embodiment 10: This embodiment is different from specific embodiment 8 or 9 in that: the conductive agent is one of Super P, carbon nanotubes, Ketjen black, acetylene black and graphene or a mixture of several thereof; the binder is one of polyvinylidene fluoride, sodium carboxymethyl cellulose and polyvinyl alcohol or a mixture of several thereof. The rest is the same as specific embodiment 8 or 9.
[0050] The following examples are used to verify the beneficial effects of the present invention:
[0051] Embodiment 1:
[0052] A method for preparing a large-size cation-embedded layered manganese dioxide material is carried out according to the following steps:
[0053] 1. Dissolve 0.75mmol potassium permanganate, concentrated sulfuric acid solution and 15mmol anhydrous methanol in 500mL ultrapure water, stir evenly, and heat to react for 1h in an air atmosphere at 95°C to obtain a manganese dioxide nanosheet dispersion;
[0054] The molar ratio of potassium permanganate to sulfuric acid in the concentrated sulfuric acid solution is 1:1; the molar concentration of Mn element in the manganese dioxide nanosheet dispersion is 1.5 mmol / L; the mass percentage of the concentrated sulfuric acid solution is 98.3%;
[0055] 2. Dissolve 25 mmol of tetramethylammonium chloride (TMA) in 50 mL of ultrapure water to obtain a salt solution;
[0056] The concentration of the salt solution is 0.5 mol / L;
[0057] 3. Adding the salt solution to the manganese dioxide nanosheet dispersion, stirring for 30 min at a stirring speed of 600 rpm, precipitating the precipitate, and then filtering, washing and drying to obtain a TMA-embedded layered manganese dioxide material (TMA-δ-MnO2);
[0058] The molar ratio of tetramethylammonium chloride in the salt solution to the Mn element in the manganese dioxide nanosheet dispersion is 100:3;
[0059] The washing described in step three is high-speed centrifugal washing; the drying described in step three is specifically vacuum drying at a temperature of 60° C. for 12 hours.
[0060] The method for preparing an aqueous zinc ion battery positive electrode from a layered manganese dioxide material with large-size cation embedding is carried out according to the following steps: mixing a layered manganese dioxide material embedded with TMA, a conductive agent, a binder and N-methylpyrrolidone to obtain a homogenate, and coating the homogenate on a current collector to obtain an aqueous zinc ion battery positive electrode;
[0061] The mass ratio of the TMA-embedded layered manganese dioxide material to the adhesive is 6:1; the mass ratio of the conductive agent to the adhesive is 3:1; the loading amount of the TMA-embedded layered manganese dioxide material in the positive electrode of the aqueous zinc ion battery is 1 mg / cm 2 .
[0062] The current collector is titanium foil; the conductive agent is Super P; and the binder is polyvinylidene fluoride.
[0063] Example 2: This example is different from Example 1 in that the tetramethylammonium chloride in step 2 is replaced with ammonium chloride (NH4Cl); and in step 3, an ammonium chloride-embedded layered manganese dioxide material (NH4-δ-MnO2) is obtained. Others are the same as Example 1.
[0064] Example 3: This example is different from Example 1 in that tetramethylammonium chloride in step 2 is replaced with tetraethylammonium chloride (TEA); and in step 3, a TEA-embedded layered manganese dioxide material (TEA-δ-MnO2) is obtained. Others are the same as Example 1.
[0065] Comparative Experiment 1: This comparative experiment is different from Example 1 in that the embedding process of Step 2 and Step 3 is eliminated, and the manganese dioxide nanosheet dispersion is directly filtered, washed and dried to obtain a manganese dioxide material (δ-MnO2). The rest is the same as Example 1.
[0066] Assembly of button cell: In an air atmosphere, a battery shell, a positive electrode sheet, a separator, an electrolyte and a negative electrode sheet are assembled in sequence to obtain an aqueous zinc ion button cell. The positive electrode sheet is the positive electrode of the aqueous zinc ion battery prepared in Examples 1 to 3 or Comparative Experiment 1, the separator is a glass fiber separator, the electrolyte is ZnSO4+MnSO4, and the concentration of ZnSO4 in the electrolyte is 2 mol / L, the concentration of MnSO4 in the electrolyte is 0.1 mol / L, and the negative electrode sheet is a zinc sheet.
[0067] Figure 1 The δ-MnO2 prepared in comparative experiment 1 is used as the positive electrode active material and assembled into a button cell, and the cycle performance diagram is cycled 800 times at a current density of 1A / g. 1 is the coulomb efficiency curve, and 2 is the discharge specific capacity curve. It can be seen from the figure that manganese dioxide (δ-MnO2) without embedded cations has a significant capacity decay problem during the cycle process. The initial discharge capacity is 116.8mAh / g, and the discharge capacity after 800 cycles is only 33.9mAh / g.
[0068] Figure 2 The cycle performance diagram of button-type battery with TMA-δ-MnO2 prepared in Example 1 as positive electrode active material and 800 cycles at a current density of 1A / g is shown in Figure 1, where 1 is the coulomb efficiency curve and 2 is the discharge specific capacity curve. As can be seen from the figure, the first cycle capacity is 61.1mAh / g, and after activation, the TMA-δ-MnO2 material can still maintain a discharge specific capacity of 94.7mAh / g after 800 cycles, which is significantly improved compared to the stability of δ-MnO2 without embedded cations.
[0069] Figure 3The cycle performance diagram of the button cell assembled with NH4-δ-MnO2 prepared in Example 2 as the positive electrode active material and cycled 800 times at a current density of 1A / g, 1 is the coulomb efficiency curve, and 2 is the discharge specific capacity curve. It can be seen that after the NH4-δ-MnO2 material is activated, it can still maintain a discharge specific capacity of 65.9mAh / g after 800 cycles, which is significantly improved compared to the stability of δ-MnO2 without embedded cations.
[0070] Figure 4 The cycle performance diagram of the button cell assembled with TEA-δ-MnO2 prepared in Example 3 as the positive electrode active material and cycled 800 times at a current density of 1A / g, 1 is the coulomb efficiency curve, and 2 is the discharge specific capacity curve. It can be seen that the TEA-δ-MnO2 material can still maintain a discharge specific capacity of 58.5mAh / g after 800 cycles, and the stability is significantly improved compared to the δ-MnO2 without embedded cations.
[0071] Figure 5 The X-ray diffraction image of δ-MnO2 prepared in the first experiment is compared; it can be seen from the figure that it is consistent with the standard δ-MnO2 (JCPDS: 01-080-1098), and the 2θ corresponding to the (001) plane diffraction peak is 12.35° (basically consistent with the standard value of 12.54°), and the corresponding interlayer spacing is
[0072] Figure 6 The X-ray diffraction image of TMA-δ-MnO2 prepared in Example 1 is shown in the figure. Compared with the δ-MnO2 prepared in Comparative Experiment 1, the 2θ corresponding to the (001) diffraction peak shifts from 12.35° to 9.59°, corresponding to the interlayer spacing shifting from Expand to
[0073] Figure 7 The X-ray diffraction image of NH4-δ-MnO2 prepared in Example 2 is shown in the figure. Compared with the δ-MnO2 prepared in Comparative Experiment 1, the 2θ corresponding to the (001) diffraction peak shifts from 12.35° to 12.03°, corresponding to the interlayer spacing shifting from Expand to
[0074] Figure 8 The X-ray diffraction image of TEA-δ-MnO2 prepared in Example 3 is shown in the figure. Compared with the δ-MnO2 prepared in Comparative Experiment 1, the 2θ corresponding to the (001) diffraction peak shifts from 12.35° to 9.43°, corresponding to the interlayer spacing shifting from Expand to
[0075] Fig. 9 The TMA-δ-MnO2 prepared in Example 1 is used as the positive electrode active material and a button cell is assembled. After 10 cycles of activation at a small current density of 0.15 A / g, the charge and discharge curves of the 10th cycle are shown in Figure 1, where 1 is the charge curve and 2 is the discharge curve. It can be seen from the figure that the capacity of TMA-δ-MnO2 is as high as 374.7 mAh / g at a current density of 0.15 A / g.
[0076] Fig.10 The δ-MnO2 prepared in comparative experiment 1 is used as the positive electrode active material and assembled into a button cell. After 10 cycles of activation at a low current density of 0.15A / g, the charge and discharge curves of the 10th cycle are shown in Figure 1, where 1 is the charge curve and 2 is the discharge curve. Fig. 9 By comparison, we can see that the capacity of TMA-δ-MnO2 is as high as 374.7 mAh / g at a current density of 0.15 A / g, which is a significant improvement compared to 193.2 mAh / g of δ-MnO2.
[0077] Fig.11 This is a high-resolution image of δ-MnO2 prepared in the first experiment under a transmission electron microscope (TEM); as can be seen from the figure, the interlayer spacing of the δ-MnO2 (001) crystal plane in the control group is measured to be It is consistent with the XRD test results very well.
[0078] Fig.12 This is a high-resolution image of TMA-δ-MnO2 prepared in Example 1 under a transmission electron microscope (TEM); as can be seen from the figure, the interlayer spacing of the TMA-δ-MnO2 (001) crystal plane is measured to be This is basically consistent with the XRD test results. It also directly proves that the interlayer spacing of δ-MnO2 is successfully widened by embedding TMA.
[0079] Fig.13 This is an image of the manganese dioxide nanosheets in the manganese dioxide nanosheet dispersion prepared in step 1 of Example 1 under a scanning electron microscope (SEM); as can be seen from the figure, it presents a dispersed nanosheet structure, which is also the main reason why large cations can be embedded into the δ-MnO2 interlayer without being restricted by the δ-MnO2 interlayer spacing.
Claims
1. A method for preparing a layered manganese dioxide material with large-size cation embedding, characterized in that It is carried out in the following steps:
1. Dissolve 0.75mmol potassium permanganate, concentrated sulfuric acid solution and 15mmol anhydrous methanol in 500mL ultrapure water, stir evenly, and heat to react for 1h in an air atmosphere at 95°C to obtain a manganese dioxide nanosheet dispersion; The molar ratio of potassium permanganate to sulfuric acid in the concentrated sulfuric acid solution is 1:1; the molar concentration of Mn element in the manganese dioxide nanosheet dispersion is 1.5 mmol / L; the mass percentage of the concentrated sulfuric acid solution is 80% to 98.3%; 2. dissolving the salt containing the pre-embedded cation in ultrapure water to obtain a salt solution; The pre-embedded cation in the salt containing pre-embedded cations is an organic ammonium cation; the salt containing pre-embedded cations is one or more of ammonium chloride, tetramethylammonium chloride, tetraethylammonium chloride and tetrabutylammonium chloride; the concentration of the salt solution is 0.1 mol / L to 1 mol / L; 3. Adding the salt solution to the manganese dioxide nanosheet dispersion, stirring at a stirring speed of 200 rpm to 1000 rpm until a precipitate is precipitated, and then filtering, washing and drying to obtain a large-sized cation-embedded layered manganese dioxide material; The molar ratio of the salt containing pre-embedded cations in the salt solution to the Mn element in the manganese dioxide nanosheet dispersion is 100:(3-15); The interlayer spacing of the layered manganese dioxide material with large-size cation embedding is 2. The method for preparing a large-size cation-embedded layered manganese dioxide material according to claim 1, characterized in that The diameter of the organic ammonium cation described in step 2> 3. The method for preparing a large-size cation-embedded layered manganese dioxide material according to claim 1, characterized in that The stirring time in step 3 is 5 min to 240 min; the washing in step 3 is high-speed centrifugal washing; the drying in step 3 is specifically vacuum drying at a temperature of 50° C. to 80° C. for 6 h to 24 h.
4. A method for preparing a positive electrode for an aqueous zinc ion battery using a large-size cation-embedded layered manganese dioxide material as prepared in claim 1, characterized in that The method is carried out according to the following steps: mixing a layered manganese dioxide material with large-size cations embedded therein, a conductive agent, a binder and N-methylpyrrolidone to obtain a homogenate, coating the homogenate on a current collector or pressing the dried homogenate on the current collector to obtain a positive electrode for an aqueous zinc ion battery; The mass ratio of the large-size cation embedded layered manganese dioxide material to the binder is (6-8):1; the mass ratio of the conductive agent to the binder is (3-1):1; the loading amount of the large-size cation embedded layered manganese dioxide material in the positive electrode of the aqueous zinc ion battery is 0.8 mg / cm 2 ~2mg / cm 2 .
5. The method for preparing an aqueous zinc ion battery positive electrode from a layered manganese dioxide material with large-size cation embedding according to claim 4, characterized in that The current collector is titanium foil, stainless steel foil, titanium mesh or stainless steel mesh.
6. The method for preparing an aqueous zinc ion battery positive electrode from a layered manganese dioxide material with large-size cation embedding according to claim 4, characterized in that The conductive agent is one of Super P, carbon nanotubes, Ketjen black, acetylene black and graphene or a mixture of several thereof; the binder is one of polyvinylidene fluoride, sodium carboxymethyl cellulose and polyvinyl alcohol or a mixture of several thereof.