Compositions containing cerium and zirconium and methods for preparing them using oxalic acid

By preparing cerium and zirconium oxide compositions with small particle sizes and narrow particle size distributions, the problem of structural instability of cerium and zirconium oxide-based materials in high temperatures and hydrothermal environments is solved, and high activity and heat resistance are achieved. , reducing the usage of precious metals and improving the performance of the catalyst.

CN115315313BActive Publication Date: 2024-10-25NEO PERFORMANCE MATERIALS (SINGAPORE) PTE LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180015622.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-21
Filing Date
2021-02-19
Publication Date
2024-10-25
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Existing cerium and zirconium oxide-based materials are difficult to maintain structural integrity under high temperatures and hydrothermal environments, resulting in reduced catalyst activity, and the use of precious metals increases costs, and catalysts need to have sufficiently large specific surface area and oxygen at high temperatures. Buffering capacity.

Method used

Preparing a cerium and zirconium oxide composition having a small particle size, a narrow particle size distribution, a desired mercury injection volume and surface area, by mixing an oxalic acid aqueous solution, a zirconium solution and a cerium solution, adding lauric acid and diethylene glycol mono-n-butyl A precipitate is formed in an alkaline solution of ether and calcined in an oxidizing environment to prepare a catalyst with a stable surface and high redox activity.

Benefits of technology

It achieves the maintenance of catalyst activity under high temperature and hydrothermal conditions, reduces the use of precious metals, improves the heat resistance and activity of the catalyst, reduces mass transfer resistance, and improves dynamic oxygen storage and release characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115315313B_ABST
    Figure CN115315313B_ABST
Patent Text Reader

Abstract

Disclosed herein are compositions comprising zirconium and cerium having surprisingly small particle sizes. The compositions disclosed herein comprise zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium. The compositions exhibit a characteristic D 90 The value is about 20‑45 μm and D 99 The invention discloses a method for producing the compositions using oxalic acid in a process. The compositions can be used as catalysts and / or as part of a catalyst system in an automotive exhaust system.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application relates to compositions comprising cerium and zirconium having small particle size and desired mercury intrusion volume and surface area. These compositions with small particle size can also have a narrow particle size distribution. Methods for preparing these compositions are also disclosed herein. The compositions disclosed herein comprise zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium.

[0002] Introduction

[0003] Cerium and zirconium oxides (CeO 2 -ZrO 2 )-based materials have been used in catalytic applications. The introduction of zirconium into the cerium (IV) oxide lattice or cerium into the zirconium oxide lattice greatly enhances and promotes oxygen migration. This fact has been readily adopted by the automotive pollution control catalyst industry, where cerium and zirconium oxide (CeO 2 -ZrO 2 ) are commonly used as washcoat components. These materials catalyze the oxidation of carbon monoxide and hydrocarbons and the reduction of nitrogen oxides as shown in the following formula:

[0004] 2CO+O 2 →2CO 2

[0005] C x H 2x+2 +[(3x+1) / 2]O 2 →xCO 2 +(x+1)H 2 O

[0006] 2NO+2CO→2CO 2 +N 2

[0007] Cerium and zirconium oxides (CeO 2 -ZrO 2 )-based materials have also been used as carriers for dispersing active metal catalysts in catalytic applications to increase the activity of the catalyst, thereby producing high conversion rates. For this reason, carriers play an important role in maintaining a highly dispersed state of active metal catalysts even under harsh operating conditions such as high temperatures and hydrothermal environments. Carriers that fail to maintain their structural integrity under harsh conditions may result in closure or sintering of active catalyst metal sites, resulting in reduced catalyst activity on a per molecule basis. Since many of these catalysts use expensive precious metals such as platinum, palladium and / or rhodium, the loss of catalyst metal activity directly affects the cost of such catalysts, requiring the use of increased precious metal loadings to maintain the desired catalyst activity. At the same time, the use of structurally stable carriers can reduce the use of precious metals while maintaining or improving catalyst activity.

[0008] These cerium and zirconium catalysts help reduce harmful vehicle exhaust gases. They provide high surface area and oxygen buffering capacity, which is useful in these applications. These materials help improve the ability of catalytic systems to reduce emissions of gases such as hydrocarbons, carbon monoxide and nitrogen oxides.

[0009] Typically, catalytic materials need to have a sufficiently large specific surface area and a high enough oxygen buffering capacity even at high temperatures.

[0010] It has also been reported that the production of cerium and zirconium oxides (CeO 2 -ZrO 2 ) based materials.

[0011] One object of the present application is to provide cerium and zirconium based materials with excellent catalyst properties suitable for catalysis and methods for synthesizing these materials, namely, as catalysts / catalyst supports, having high surface areas, stable surfaces under oxidation, reduction, hydrothermal and redox conditions, stable crystallographic properties under severe aging conditions, high and stable mercury intrusion volumes, selective porosity / mercury intrusion volumes, high activity at relatively low temperatures, low mass transfer resistance and high dynamic oxygen storage and release properties.

[0012] Overview

[0013] As disclosed herein, the compositions of the present invention comprise zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium. These compositions have a small particle size characterized by D 90 The value is about 20-45 μm and D 99 The value is about 55-100 μm. These compositions having small particle sizes may also have a narrow particle size distribution and further have a desired mercury intrusion volume and surface area.

[0014] In certain embodiments of the above compositions, the compositions also have a total mercury intrusion volume of about 0.5-4 cc / g after calcination at 1000°C for 10 hours in an oxidizing environment, and a total mercury intrusion volume of about 0.5-3.0 cc / g after calcination at 1100°C for 10 hours in an oxidizing environment.

[0015] In other embodiments of the above composition, the composition further has a relative humidity of about 40-100 m / s after calcination at 1000° C. for 10 hours in an oxidizing environment. 2 / g, and has a surface area of ​​about 20-85 m2 after calcination at 1100°C for 10 hours in an oxidizing environment. 2 / g of surface area.

[0016] Further disclosed herein is a method for producing a composition comprising zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium. The method comprises the following steps: (a) mixing an aqueous oxalic acid solution, a zirconium solution, and a cerium solution to provide a mixture; (b) adding the mixture to an alkaline solution comprising lauric acid and diethylene glycol mono-n-butyl ether to form a precipitate; (c) calcining the precipitate to provide a composition comprising zirconium and cerium. The method further comprises the step of washing the precipitate with water before calcining. The method may also include mixing a rare earth metal solution other than cerium and yttrium in step (a), and further mixing a yttrium solution in step (a) to provide the mixture. The composition prepared by these methods has a small particle size, a narrow particle size distribution, and a desired mercury injection volume and surface area.

[0017] When used together with a noble metal, the disclosed compositions can be used in catalysts or catalyst supports for purifying exhaust gas to improve heat resistance and catalyst activity. 2 -ZrO 2 )-based materials have high surface areas and stable surfaces when subjected to severe aging conditions, such as high temperature air, hydrothermal and redox conditions. They also have stable crystallographic properties under severe aging conditions, high, stable and selective mercury intrusion volumes, high redox activity at lower temperatures, low mass transfer resistance and high dynamic oxygen storage and release properties.

[0018] BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A flow chart illustrating an embodiment of an experimental process for preparing a cerium and zirconium containing composition using an aqueous oxalic acid solution as disclosed herein is shown.

[0020] Figure 2 Shown is a graph comparing the as-produced particle size distribution of a Ce / Zr / La / Nd-containing composition prepared by the methods disclosed herein using oxalic acid and a Ce / Zr / La / Nd-containing composition prepared by a method that does not include the use of oxalic acid.

[0021] Figure 3 A bar graph is provided showing the surface area of ​​oxidative environment aging of a cerium and zirconium containing composition prepared by the methods disclosed herein using oxalic acid versus a Ce / Zr / La / Nd containing composition prepared by a method that does not include the use of oxalic acid. The ratios listed are weight percentages based on oxide equivalents.

[0022] Detailed description

[0023] Before disclosing and describing compositions and methods having small particle size, narrow particle size distribution, and desired mercury intrusion volume and surface area, it should be understood that the present disclosure is not limited to the specific structures, process steps, or materials disclosed herein, but extends to equivalents thereof recognized by ordinary technicians in the relevant art. It should also be understood that the terms used herein are used only for the purpose of describing specific embodiments and are not intended to be limiting. It must be noted that as used in this specification, the singular forms "a", "an", and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "a step" may include multiple steps, reference to "production" or "products" of a reaction or treatment should not be considered to be all reaction / treatment products, and reference to ""treatment"" may include reference to one or more such treatment steps. Thus, a treatment step may include multiple or repeated treatments of similar materials / streams to produce confirmed treatment products.

[0024] Numerical values ​​with "about" include typical experimental variances. As used herein, the term "about" refers to values ​​with statistically significant ranges, such as the particle diameter, concentration range, time range, molecular weight, temperature or pH. Such ranges may be within an order of magnitude of the indicated value or range, typically within 10%, or even more typically within 5%. Sometimes, such ranges may be within the typical experimental error of the standard method for measuring and / or determining a given value or range. The permitted variations included in the term "about" will depend on the particular system being studied, and can be easily understood by one of ordinary skill in the art. When a range is described in this application, each integer within the range is also considered to be an embodiment of the present invention.

[0025] The present application relates to compositions with small particle size, narrow particle size distribution and desired mercury intrusion volume and surface area. The present application further relates to methods for preparing these compositions. Compositions disclosed herein comprise zirconium, cerium, optionally yttrium and optionally one or more rare earth metals other than cerium and yttrium. These compositions have advantageous properties for catalysis as a catalyst and / or catalyst system part.

[0026] As disclosed herein, the compositions include zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium.

[0027] In one embodiment, the composition further comprises lanthanum, praseodymium, neodymium, or mixtures thereof. In additional embodiments of any of the foregoing compositions, the composition further comprises yttrium.

[0028] These compositions have a particle size D 90 Values ​​of about 20-45 μm and D 99 In some embodiments, these compositions have a particle size D 90Values ​​of about 25-40 μm and D 99 In some of these embodiments as defined above, the composition has a D 50 The value is about 1.5-10 μm, and in certain embodiments, about 2-5 μm. In certain of these embodiments, the composition has D 10 The value is about 0.05-1μm.

[0029] In some embodiments, these compositions have a particle size D 90 Values ​​of about 25-35 μm and D 99 In some of these embodiments, the composition further has a D 50 In some of these embodiments, the composition has a D 10 The value is about 0.1-0.8μm.

[0030] In some embodiments, these compositions have D 50 Values ​​of about 2-5 μm and D 99 Features with values ​​of about 20-30μm.

[0031] In a specific embodiment, the composition has a particle size D 90 Value about 30μm, D 50 Values ​​of about 3 μm and D 10 In these embodiments, the composition may also have a D 25 Value about 1.5μm, D 75 Values ​​of about 8 μm and D 99 Features with a value of about 62μm.

[0032] In some embodiments, the compositions disclosed herein can exhibit D compared to similar compositions prepared according to similar methods but without the use of oxalic acid. 50 The percentage reduction is ≥ 80%, and compared with a similar composition prepared according to a similar method but without using oxalic acid, D 90 The percentage reduction is ≥45%.

[0033] Particle size analysis was performed using a Microtrac S3500 particle size analyzer. A typical measurement is to use approximately 0.2 g of powder sample to which 20 ml of a 2% sodium hexametaphosphate solution is added. The sample + solution is then sonicated for approximately 3 minutes. A few drops of the sonicated solution are then added to the instrument's sample container. The sample is sonicated again in the machine for 3 minutes. The machine is run three consecutive times according to the instrument manufacturer's instruction manual. The three runs are averaged and the results recorded.

[0034] For narrow particle size distribution, the particle size distribution defined in this paper is (D90 -D 10 ) / D 50 Therefore, as used herein, a narrow particle size distribution is (D 90 -D 10 ) / D 50 Less than about 10. In certain embodiments, the particle size distribution may be less than about 8. In some embodiments of the compositions disclosed herein, a narrow particle size distribution may be exhibited that is about half (about 50% less) smaller than the particle size distribution of a similar composition prepared according to a similar method but without the use of oxalic acid.

[0035] The compositions disclosed herein having a small particle size may also exhibit a total mercury intrusion volume of about 0.5-4.0 cc / g after calcination at 1000° C. for 10 hours in an oxidizing environment, and in certain embodiments, a total mercury intrusion volume of about 0.5-3.5 cc / g after calcination at 1000° C. for 10 hours in an oxidizing environment. The compositions having a small particle size may also exhibit a total mercury intrusion volume of about 0.5-3.0 cc / g after calcination at 1100° C. for 10 hours in an oxidizing environment, and in certain embodiments, a total mercury intrusion volume of about 0.5-2.0 cc / g after calcination at 1100° C. for 10 hours in an oxidizing environment.

[0036] In specific embodiments, the composition may exhibit a total mercury intrusion volume of about 0.62 cc / g after calcination at 1000°C for 10 hours in an oxidizing environment and a total mercury intrusion volume of about 0.6-1 cc / g after calcination at 1100°C for 10 hours in an oxidizing environment.

[0037] The mercury intrusion volume was determined using a Micromeritics Auto Pore IV mercury intrusion instrument using the following procedure: The powder sample was accurately weighed to 4 significant figures and then evacuated to 50 μmHg in the machine sample holder. It was then mercury intruded (through the machine) with a filling pressure step of 0.5 psia. The dwell time for each step was 10 seconds. For the required pressure conversion to the inlet pore size, a mercury surface tension value of 485 dyn / cm was used and a contact angle of 130° was used. The mercury intrusion volume is the accumulation of the mercury intrusion volume entering the sample in each pressure step.

[0038] The composition with a small particle size disclosed herein can exhibit a particle size of about 40-100 m after calcination at 1000° C. for 10 hours in an oxidizing environment. 2 / g surface area, and in certain embodiments, after calcination at 1000°C for 10 hours in an oxidizing environment, the surface area is about 40-75 m 2 / g, in other embodiments, after calcination at 1000°C for 10 hours in an oxidizing environment, the surface area is about 40m 2 / g to about 65m2 / g.

[0039] The composition with a small particle size disclosed herein can also exhibit a particle size of about 20-85 μm after calcination at 1100° C. for 10 hours in an oxidizing environment. 2 / g surface area, and in certain embodiments, after calcination at 1100°C in an oxidizing environment for 10 hours, the surface area is about 20-50 m 2 / g.

[0040] In a specific embodiment, the composition disclosed herein having a small particle size exhibits a particle size of about 40-50 m / s after calcination at 1000° C. for 10 hours in an oxidizing environment. 2 The surface area of ​​​​the sample is about 20-30m / g after calcination at 1100 ° C in an oxidizing environment for 10 hours. 2 / g.

[0041] The apparent surface area of ​​the compositions was determined using a Micromeritics ASAP 2000 system and nitrogen at approximately 77 K. The procedure outlined in ASTM International Test Method D 3663-03 (Reapproved 2008) was used with one important exception. It is well known that the "BET surface area" determination is not feasible for materials containing micropores. Recognizing that the surface area is an approximation, the reported values ​​are labeled "apparent surface area" values ​​rather than "BET surface area" values. Following the recognized procedure for determining apparent surface area, the application of the BET equation is limited to the term na(lP / P 0 )With P / P 0 Continuously increasing pressure range. The samples were degassed under nitrogen at about 300°C for about 2 hours.

[0042] Mercury injection volume is related to the porosity and pore structure of the catalyst / catalyst carrier containing cerium and zirconium. Regardless of the activity of the catalyst site, it is very important to facilitate the molecular transport of reactants to the active site and the transport of reaction products away from the active site so that they can be used for further reaction. Without considering the catalyst selectivity, a carrier with a wide and open pore structure is desired. In the case of desired reaction molecules or product selectivity, the porosity required to be designed only allows the desired reactants to reach the active site and only allows the desired product to leave the active site. For example, this type of function is known and is utilized in zeolite materials. Therefore, depending on the type of desired reaction, a material with a specific mercury injection volume is beneficial.

[0043] The particle size of the catalytic material may directly affect the surface area of ​​the composition in units of volume / mass, thereby affecting the number of catalytic conversion active sites. Generally, the surface area (specific surface area) in units of volume / mass increases with the decrease of particle size. Small particle size can also allow more catalytic cerium and zirconium oxide materials to be used in the carrier coating component without blocking the channels of the carrier block in the catalytic converter. In this way, the catalytic converter tends to have better performance while minimizing the exhaust back pressure caused by the clogging of the carrier block.

[0044] In the compositions disclosed and described herein, the above-mentioned particle sizes can be combined in any combination with any of the above-mentioned mercury intrusion volumes after calcination at 1000 and 1100°C for 10 hours in an oxidizing environment, and can further be combined in any combination with the above-mentioned surface areas after calcination at 1000 and 1100°C for 10 hours in an oxidizing environment. The above-mentioned mercury intrusion volumes after calcination at 1000 and 1100°C for 10 hours in an oxidizing environment can be combined in any combination, and can further be combined in any combination with the above-mentioned surface areas after calcination at 1000 and 1100°C for 10 hours in an oxidizing environment. The above-mentioned surface areas after calcination at 1000 and 1100°C for 10 hours in an oxidizing environment can be combined in any combination, and can further be combined in any combination with the above-mentioned mercury intrusion volumes after calcination at 1000 and 1100°C for 10 hours in an oxidizing environment.

[0045] In these compositions, the molecular ratio of Zr / Ce is greater than 50%. The ratio of Zr to Ce (Zr:Ce) in the composition is about 1:1-4:1, and in certain embodiments, about 1:1-2:1. In certain embodiments of these compositions, any additional components (e.g., yttrium and rare earth metals other than cerium) are present in an amount of 0-30 wt% based on the oxide.

[0046] In certain compositions, the equivalent ratio of cerium to zirconium oxide (CeO 2 / ZrO 2 ) may be about 15-60 wt% / 40-75 wt%. All compositions are based on oxide equivalents.

[0047] In a specific embodiment of the composition, CeO 2 / ZrO 2 / La 2 O 3 / Nd 2 O 3 The ratio of CeO may be about 18-55wt% / 40-75wt% / 1-8wt% / 1-8wt%. In an exemplary embodiment of these compositions, CeO 2 / ZrO 2 / La 2 O3 / Nd 2 O 3 The ratio of may be about 20.8 wt% / 72.2 wt% / 1.7 wt% / 5.3 wt%. All compositions are based on oxide equivalents.

[0048] In other embodiments, CeO 2 / ZrO 2 / La 2 O 3 / Y 2 O 3 The ratio of CeO may be about 20-55wt% / 40-75wt% / 1-8wt% / 1-8wt%. In an exemplary embodiment of these compositions, CeO 2 / ZrO 2 / La 2 O 3 / Y 2 O 3 The ratio may be about 45wt% / 45wt% / 5wt% / 5wt%.

[0049] In further embodiments of these compositions, CeO 2 / ZrO 2 / La 2 O 3 / Nd 2 O 3 / Pr 6 O 11 The ratio of CeO can be about 30-55wt% / 40-75wt% / 1-8wt% / 1-8wt% / 1-8wt%. In some of these compositions, CeO 2 / ZrO 2 / La 2 O 3 / Nd 2 O 3 / Pr 6 O 11 The ratios may be 40 / 50 / 2 / 4 / 4. All compositions are based on oxide equivalents.

[0050] The composition disclosed herein is prepared by the following method: (a) mixing an aqueous oxalic acid solution, a zirconium solution, and a cerium solution to provide a mixture; (b) adding the mixture to an alkaline solution containing lauric acid and diethylene glycol mono-n-butyl ether to form a precipitate; (c) calcining the precipitate to provide a composition containing zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium.

[0051] Thus, step (a) of the method may further comprise mixing rare earth metal solutions other than cerium and yttrium to provide a mixture. Such rare earths include, for example, lanthanum, praseodymium, neodymium, or mixtures thereof. Step (a) may further comprise mixing yttrium solutions to provide a mixture.

[0052] Zirconium, cerium, optionally yttrium and optionally other rare earth metal solutions can be made from any soluble salt form of these elements. The starting rare earth metal salt is water soluble and can be dissolved in water in the methods disclosed herein. The rare earth metal salt can be a nitrate, chloride, etc. The cerium salt can be Ce(III) or Ce(IV) oxidation state.

[0053] Preferably, oxalic acid is first combined with zirconium and cerium solutions and optionally other rare earth solutions and yttrium solutions. This mixture is then added to the alkaline solution containing lauric acid and diethylene glycol mono-n-butyl ether solution. The rate of addition of the reactants is not critical.

[0054] The composition prepared by the present method may have D as described above. 90 Value and D 99 The composition prepared by the present method may also exhibit a narrow particle size distribution as described above. It is important to note that these small particle sizes are achieved without an active pulverization step. As described above, small particle sizes can lead to a larger specific surface area and more active sites. In addition, when the composition exhibits a small particle size, more catalytic material can be used without generating further exhaust back pressure. Furthermore, if the product can be obtained as is without an additional pulverization step as a well-controlled small particle size cerium and zirconium oxide (CeO 2 -ZrO 2 )-based materials, the production workload and cost can be significantly reduced.

[0055] The addition of oxalic acid during the process is a distinctive feature of the present method, and by this addition a composition having a surprisingly small size and narrow particle size distribution is obtained, even without a pulverization step. In the method disclosed herein, the amount of oxalic acid added may be about 25-100 wt % relative to the equivalent oxide.

[0056] Furthermore, in the methods disclosed herein, the alkaline solution may have an alkali concentration of about 3-6 N, and in one embodiment about 4.5 N. The alkaline solution may be ammonia, ammonium hydroxide, sodium hydroxide, etc. The alkaline solution comprises lauric acid and diethylene glycol mono-n-butyl ether.

[0057] The amount of lauric acid added may be about 50-200 wt% of the oxide equivalent. The amount of diethylene glycol mono-n-butyl ether added may be about 50-150 wt% of the oxide equivalent.

[0058] In the methods disclosed herein, supercritical drying is optional. If employed, it can be carried out at about 250-350°C and about 130-140 bar.

[0059] The method may further include a step of washing the precipitate with water after the precipitation step. The precipitate is washed with water to obtain a selected conductivity. In some embodiments, this desired conductivity is about 6-8 mS / cm.

[0060] The precipitate may be separated from the liquid by decantation, vacuum filtration, a combination of both, or any other suitable method.

[0061] In the methods disclosed herein, calcination may be performed at a temperature of about 400-1100° C. for about 0.25-24 hours, and in certain embodiments, calcination may be performed at a temperature range of about 700-900° C. for about 3-7 hours, and in a specific embodiment, calcination is performed at a temperature of about 750° C. for about 5 hours. The temperature and time of calcination should be sufficient to remove non-rare earth metals and non-zirconium materials and ensure that oxides are obtained.

[0062] Calcination can be carried out in any suitable furnace and environment, including but not limited to oxidative, reductive, hydrothermal or inert environments. In some embodiments, oxidative environments are preferred. Tube furnaces can be used. With their tubular design, tube furnaces allow better gas flow for more thorough treatment.

[0063] Figure 1 is a flow chart of one embodiment of a method of making a composition disclosed herein.

[0064] The compositions disclosed herein were prepared and tested for particle size, mercury intrusion volume, and surface area and compared to similar compositions prepared according to similar methods but without the use of oxalic acid. The compositions disclosed herein and prepared by the methods disclosed herein exhibit surprisingly small particle size ( Figure 2 ), good mercury intrusion volume and similar surface area ( Figure 3 ).

[0065] The compositions disclosed herein and prepared by the methods disclosed herein also exhibit surprisingly narrow particle size distributions compared to similar compositions prepared according to similar methods but without the use of oxalic acid. Thus, in some embodiments, the compositions disclosed herein exhibit a particle size distribution that is about half the particle size distribution of similar compositions prepared according to similar methods but without the use of oxalic acid.

[0066] Below, the process of the invention and its more detailed features for preparing a composition comprising zirconium, cerium oxide, optionally one or more rare earths other than cerium and optionally yttrium are illustrated by way of example, although the scope of the invention is by no means limited thereby. Example

[0067] Example 1: Synthesis of CeO 2 / ZrO 2 / La 2 O 3 / Nd 2 O 3 (20.8wt% / 72.2wt% / 1.7wt% / 5.3wt%)

[0068] according to Figure 1 The illustrated steps are as follows:

[0069] 1) preparing an aqueous oxalic acid solution (50 wt %, based on metal oxide equivalent);

[0070] 2) Based on equivalent ZrO 2 Prepare about 300 g / L zirconium oxynitrate solution;

[0071] 3) preparing a Ce / La / Nd nitrate solution (100 g / L, based on equivalent oxides), wherein the cerium salt used was ammonium cerium nitrate;

[0072] 4) Preparation of aqueous ammonium hydroxide solution NH 4 OH (4.5M, NH 4 OH / M + =10.1);

[0073] 5) Mix 30 g of rare earth nitrate solution Ce / Zr / La / Nd based on oxide equivalent with NH 4 OH, lauric acid (50 wt %, based on metal oxide equivalent), diethylene glycol mono-n-butyl combination ether (150 wt %, based on metal oxide equivalent) are combined to provide a precipitate;

[0074] 4) washing the precipitate with deionized water until the conductivity reaches 6-8 mS / cm, and separating it by vacuum filtration;

[0075] 5) The precipitate was calcined at 750°C for 5 hours.

[0076] Example 2: Comparative Example Synthesis of CeO 2 / ZrO 2 / La 2 O 3 / Nd 2 O 3 (20.8wt% / 72.2wt% / 1.7wt% / 5.3wt%)

[0077] Do the following:

[0078] 1) Based on equivalent ZrO 2 Prepare 300 g / L zirconium oxynitrate solution;

[0079] 3) preparing a Ce / La / Nd nitrate solution (100 g / L, based on equivalent oxides), wherein the cerium salt used was ammonium cerium nitrate;

[0080] 4) Preparation of aqueous ammonium hydroxide solution (NH 4 OH=4.5M,NH 4 OH / M + =10.1);

[0081] 5) Mix 30 g of rare earth nitrate solution Ce / Zr / La / Nd based on oxide equivalent with NH 4 OH, lauric acid (50 wt %, based on metal oxide equivalent), diethylene glycol mono-n-butyl combination ether (150 wt %, based on metal oxide equivalent) are combined to provide a precipitate;

[0082] 4) washing the precipitate with deionized water until the conductivity reaches 6-8 mS / cm, and separating it by vacuum filtration;

[0083] 5) The precipitate was calcined at 750°C for 5 hours.

[0084] Example 3: The composition of the example CeO 2 / ZrO 2 / La 2 O 3 / Nd 2 O 3 (20.8wt% / 72.2wt% / 1.7wt% / 5.3wt%) incorporated into the catalyst or catalyst carrier

[0085] The mixed oxide materials comprising cerium and zirconium as described herein can be used as the main component in a catalyst or catalyst support for incorporation into an automotive exhaust system. The introduction of zirconium into the cerium (IV) oxide lattice or cerium into the zirconium oxide lattice greatly enhances and promotes the migration of oxygen. In addition, the introduction of these cerium and zirconium oxides (CeO 2 -ZrO 2 ) solid solution with other rare earth metal elements such as La, Nd, Pr and Y doping further improves catalytic activity and heat resistance. These mixed oxide materials as disclosed herein have high surface area and are thermally stable when subjected to severe aging conditions such as high temperature air, hydrothermal and redox conditions. They also have stable crystallographic characteristics under severe aging conditions, high and stable porosity, highly selective mercury injection volume, high redox activity at lower temperatures, low mass transfer resistance and high dynamic oxygen storage and release characteristics.

[0086] To prepare a catalyst or catalyst support, these cerium and zirconium mixed oxide powders are mixed with a high temperature resistant inorganic oxide such as alumina, silicon oxide or titanium oxide in water to form a powder slurry. Subsequently, a noble metal such as palladium, rhodium or platinum and other additives such as stabilizers, promoters and binders are added to the oxide slurry to obtain a carrier coating. This carrier coating slurry can then be applied to a support such as a ceramic monolithic honeycomb structure to prepare a catalyst for automobile exhaust purification.

[0087] Unless otherwise indicated, all numbers expressing quantities of ingredients, properties such as molecular weight, reaction conditions, and the like used in the specification and claims are to be understood as being modified in all instances by the term "about." Accordingly, unless indicated to the contrary, the numerical parameters set forth in the following specification and attached claims are approximations that may vary depending upon the desired properties sought to be obtained.

[0088] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the technology are approximations, the numerical values ​​set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.

[0089] It is apparent that the compositions and methods described herein are well suited for achieving the objects and advantages mentioned and inherent therein. Those skilled in the art will recognize that the methods and systems of the present specification may be implemented in a variety of ways and are therefore not limited by the foregoing exemplary embodiments and examples. In this regard, any number of features of the various embodiments described herein may be combined into a single embodiment, and alternative embodiments having less than or more than all of the features described herein are possible.

[0090] Although various embodiments have been described for the purpose of the present invention, various changes and modifications can be made that are well within the scope of the present invention. Many other changes can be made that are easy for those skilled in the art to suggest and are included in the spirit of the present invention.

Claims

1. A composition comprising zirconium, cerium, optionally one or more rare earth metals other than cerium and optionally yttrium, characterized in that D 10 The value is 0.05-1μm, D 90 The value is 20-45μm and D 99 The particle size of the present invention is 55-100 μm, and the composition is produced by a method comprising the following steps: mixing an aqueous oxalic acid solution, a zirconium solution, a cerium solution, optionally a yttrium solution, and optionally one or more rare earth metal solutions other than the cerium and yttrium solutions to provide a mixture, and adding the mixture to an alkaline solution containing lauric acid and diethylene glycol mono-n-butyl ether to form a precipitate.

2. The composition of claim 1, characterized in that D 90 The value is 25-40μm and D 99 The value is 60-85μm particle size.

3. The composition of claim 1, wherein D 50 The value is 1.5-10μm.

4. The composition of claim 1, wherein D 50 The value is 2-5μm.

5. The composition of any one of claims 1 to 4, wherein the composition comprises one or more other rare earth metals, wherein the other rare earth metals are selected from lanthanum, praseodymium, neodymium or mixtures thereof.

6. The composition of claim 1, wherein the composition comprises yttrium.

7. The composition of claim 5, wherein the composition further comprises yttrium.

8. The composition of claim 1 having a total mercury intrusion volume of 0.5-4.0 cc / g after calcination at 1000°C for 10 hours in an oxidizing environment and a total mercury intrusion volume of 0.5-3.0 cc / g after calcination at 1100°C for 10 hours in an oxidizing environment.

9. The composition of claim 1 having a total mercury intrusion volume of 0.5-3.5 cc / g after calcination at 1000°C for 10 hours in an oxidizing environment and a total mercury intrusion volume of 0.5-2.0 cc / g after calcination at 1100°C for 10 hours in an oxidizing environment.

10. The composition of claim 1 having a total mercury intrusion volume of 0.6-2 cc / g after calcination at 1000°C for 10 hours in an oxidizing environment and a total mercury intrusion volume of 0.6-1.0 cc / g after calcination at 1100°C for 10 hours in an oxidizing environment.

11. The composition of claim 1, having a surface area of ​​40 to 100 m after calcination at 1000°C for 10 hours in an oxidizing environment. 2 / g and a surface area of ​​20-85 m2 after calcination at 1100 °C for 10 h in an oxidizing environment. 2 / g of surface area.

12. The composition of claim 1, having a carbon content of 40-75 m / s after calcination at 1000°C for 10 hours in an oxidizing environment. 2 / g and a surface area of ​​20-50 m2 after calcination at 1100 °C for 10 h in an oxidizing environment. 2 / g of surface area.

13. The composition of claim 1, having a carbon content of 40-50 m after calcination at 1000°C for 10 hours in an oxidizing environment. 2 / g and a surface area of ​​20-30 m2 after calcination at 1100 °C for 10 h in an oxidizing environment. 2 / g of surface area.

14. The composition of claim 1, comprising cerium and zirconium in a ratio of 15-60 wt% / 40-75 wt% based on oxide equivalent weight.

15. A process for producing a composition comprising zirconium, cerium, optionally yttrium, optionally one or more rare earth metals other than cerium and yttrium, The following steps are involved: (a) mixing an aqueous oxalic acid solution, a zirconium solution, a cerium solution, optionally a yttrium solution, and optionally one or more rare earth metal solutions other than the cerium and yttrium solutions to provide a mixture, wherein the amount of oxalic acid added is 25-100 wt % relative to the equivalent oxide content; (b) adding the mixture to an alkaline solution comprising lauric acid and diethylene glycol mono-n-butyl ether to form a precipitate; and (c) calcining the precipitate to provide a composition comprising zirconium, cerium, optionally yttrium, and optionally one or more rare earth metals other than cerium and yttrium.

16. The method of claim 15, wherein in step (a) an aqueous oxalic acid solution, a zirconium solution, a cerium solution and a solution of one or more rare earth metals selected from the group consisting of lanthanum, praseodymium, neodymium and mixtures thereof are mixed to provide the mixture.

17. The method of claim 15 or 16, wherein in step (a) yttrium solutions are mixed to provide the mixture.

18. The method of claim 15, further comprising washing the precipitate with water after precipitation.

19. The method of claim 15, wherein the alkaline solution is 4.5M; the amount of lauric acid is 50-200 wt% relative to the amount of oxide; and the amount of diethylene glycol mono-n-butyl ether is 50-150 wt% relative to the oxide equivalent content.

20. The method of claim 15, wherein the calcination is carried out at a temperature of 400-1100°C for 0.25-24 hours.

21. The method of claim 20, wherein the calcination is carried out at a temperature of 700-900°C for 3-7 hours.

22. The method of claim 21, wherein the calcination is carried out at a temperature of 750°C for 5 hours.

23. The method of claim 15, wherein the method further comprises supercritical drying.

24. The method of claim 15, wherein the method does not include an active comminution step.

25. A composition prepared by the method of claim 15, wherein the composition has a characteristic that D 90 The value is 20-45μm and D 99 The particle size of 55-100 μm and less than 10 is defined as (D 90 -D 10 ) / D 50 wherein the composition has a particle size distribution characterized by D 10 The value is 0.05-1µm and D 50 The value is 1.5-10µm particle size.

26. The composition of claim 25, wherein the composition has a smaller particle size than a composition prepared by a process without oxalic acid.

27. A catalyst or catalyst composition comprising the composition of claim 1 or 25.