Laminated Film
By using the same kind of polyolefin-based resin and electron beam irradiation treatment in the laminated film, combined with the multi-layer resin structure, the problem of insufficient heat resistance of the laminated film during the heat sealing process is solved, and high heat resistance and applicability are achieved. promote.
Patent Information
- Application Number
- CN202180025479.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-03-29
AI Technical Summary
In existing laminated films, the resin film easily adheres to the heating plate during the heat sealing process, has insufficient heat resistance, and is difficult to effectively recycle.
A laminated film structure with the same type of polyolefin resin is used, in which the first resin layer and the second resin layer show that the E'(110)/E'(100) value is 0.2 or more through dynamic viscoelasticity measurement, and the gel fraction is 30 % or more, and is processed under electron beam irradiation with an absorption dose of 20 to 300kGy. The third resin layer is composed of multiple layers to improve heat resistance and recyclability.
The heat resistance and reusability of the laminated film are significantly improved, and the adhesion of the resin film to the heating sealing device is reduced, achieving higher heat resistance and applicability.
Smart Images

Figure CN115335231B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated film.
[0002] This application claims priority based on Japanese Patent Application No. 2020-060062 filed in Japan on March 30, 2020 and Japanese Patent Application No. 2020-209113 filed in Japan on December 17, 2020, and the contents of which are incorporated herein by reference. Background Art
[0003] Laminated films composed of a plurality of laminated resin layers are widely used as materials for packaging. Typical laminated films include laminated films having at least a sealant layer provided for heat-sealing with an object to be sealed and an outer layer provided on the side opposite to the sealant layer.
[0004] On the other hand, such laminated films for packaging are produced and consumed in large quantities around the world every day due to their high convenience, and a large amount of waste is generated after use. From the perspective of improving the global environment, the generation of waste has become an important issue to be solved. In recent years, methods for reducing the amount of waste generated and reusing (regenerating) waste have been actively studied.
[0005] For example, if the main constituent materials of the plurality of resin layers in a laminated film are the same, there is no need to separate the resin layers and reuse them separately, and the entire laminated film can be easily reused, thereby increasing its usefulness.
[0006] As such a laminated film, for example, a polyethylene laminate for packaging materials is disclosed, which comprises at least a stretched polyethylene film, an adhesive layer containing a solvent-free adhesive, and a heat-sealable polyethylene layer (see Patent Document 1).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent document 1: Japanese Patent Application Publication No. 2019-189333. Summary of the invention
[0010] Problems to be solved by the invention
[0011] Generally, when a resin film is heat-sealed, the resin film often tends to adhere to a heating plate in a heat-sealing device. This is because the resin film has insufficient heat resistance. In this regard, it is unclear whether the laminated film described in Patent Document 1 has sufficient heat resistance.
[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminated film having higher heat resistance and higher recycling suitability than conventional films.
[0013] Means for solving problems
[0014] In order to solve the above-mentioned problems, the present invention adopts the following configuration.
[0015] [1] A laminate film, wherein the laminate film comprises a first resin layer and a second resin layer, wherein the first resin layer and the second resin layer contain the same polyolefin resin, and the second resin layer is subjected to dynamic viscoelasticity measurement. When the elastic modulus E'(100) at 100°C and the elastic modulus E'(110) at 110°C are measured at a vibration frequency of 1 Hz, the value of E'(110) / E'(100) is greater than 0.2.
[0016] [2] The laminated film according to [1], wherein the laminated film has a gel fraction of 30% or more.
[0017] [3] The laminated film according to [1] or [2], wherein the laminated film is irradiated with an electron beam at an absorbed radiation dose of 20 to 300 kGy.
[0018] [4] The laminated film according to any one of [1] to [3], wherein a temperature at which a displacement of 2000 μm is shown when the laminated film is subjected to thermomechanical analysis is 120° C. or higher.
[0019] [5] The laminate film according to any one of [1] to [4], wherein the laminate film further comprises a third resin layer between the first resin layer and the second resin layer, and the first resin layer, the second resin layer and the third resin layer contain the same type of polyolefin-based resin.
[0020] [6] The laminated film according to [5], wherein the third resin layer is composed of three or more layers, at least one of which contains the polyolefin-based resin, ethylene-vinyl alcohol copolymer and ethylene-vinyl alcohol-vinyl acetate copolymer, and the polyolefin-based resin is not any of ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer and ethylene-vinyl alcohol-vinyl acetate copolymer.
[0021] [7] The laminated film according to any one of [1] to [6], wherein the polyolefin-based resin is a polyethylene-based resin.
[0022] [8] A laminated film according to any one of [1] to [7], wherein when the front end of a needle having a curvature radius of 0.5 mm is pressed vertically relative to the laminated film at a speed of 500 mm / min, the load applied to the needle becomes greater than 7N at the moment the needle penetrates the laminated film.
[0023] [9] The laminated film according to [1], wherein the value of E'(110) / E'(100) is 0.5 or more.
[0024]
[10] The laminated film according to [1] or [9], wherein the second resin layer comprises high-density polyethylene.
[0025] Effects of the Invention
[0026] According to the present invention, it is possible to provide a laminated film having higher heat resistance and higher recyclability than conventional laminated films.
[0027] Brief description of the attached figure
[0028] Figure 1 It is a cross-sectional view schematically showing an example of a laminated film according to one embodiment of the present invention.
[0029] Figure 2 It is a cross-sectional view schematically showing another example of the laminated film according to one embodiment of the present invention.
[0030] Figure 3 This is a cross-sectional view schematically showing an example of a package body including a laminated film according to an embodiment of the present invention. DETAILED DESCRIPTION
[0031] <<Laminated Film>>
[0032] In one embodiment of the present invention, a laminate film comprises a first resin layer and a second resin layer, wherein the first resin layer and the second resin layer comprise the same polyolefin-based resin, and the second resin layer is subjected to dynamic viscoelasticity measurement (DMA), and when the elastic modulus E'(100) at 100°C and the elastic modulus E'(110) at 110°C are measured at a vibration frequency of 1 Hz, the value of E'(110) / E'(100) (sometimes referred to as "E'(110) / E'(100) value" in this specification) is greater than 0.2.
[0033] In this specification, "elastic modulus" means "storage modulus" unless otherwise specified.
[0034] In the laminated film of the present embodiment, since the first resin layer and the second resin layer contain the same kind of polyolefin-based resin, the laminated film has high recycling suitability.
[0035] Furthermore, in the laminated film of the present embodiment, since the E'(110) / E'(100) value of the second resin layer is 0.2 or more, the heat resistance of the second resin layer is high, and thus the heat resistance is higher than that of a laminated film containing a general polyolefin resin. When such a laminated film having high heat resistance is heat-sealed, the laminated film (particularly the second resin layer) can be prevented from adhering to the heating plate in the heat-sealing device.
[0036] <First resin layer>
[0037] The first resin layer includes a polyolefin-based resin.
[0038] The polyolefin-based resin contained in the first resin layer is not particularly limited as long as it has a structural unit derived from an olefin, and may be a homopolymer of one olefin or a copolymer of two or more olefins.
[0039] Examples of the olefin homopolymer include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), metallocene-catalyzed linear low-density polyethylene (mLLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE); and polypropylene (homopolymer polypropylene).
[0040] Linear low-density polyethylene (LLDPE) and metallocene catalyst linear low-density polyethylene (mLLDPE) are both types of low-density polyethylene (LDPE).
[0041] The classification of each density of polyethylene is defined in, for example, old JIS K 6748: 1995. In this specification, polyethylene is classified according to each density based on this definition.
[0042] That is, in this specification, low-density polyethylene (LDPE) refers to a polyethylene having a density of 0.91 g / cm 3 Above and less than 0.93g / cm 3 of polyethylene.
[0043] And, medium density polyethylene (MDPE) refers to a polyethylene with a density of 0.93 g / cm 3 Above and less than 0.942g / cm 3 of polyethylene.
[0044] And, high-density polyethylene (HDPE) refers to a polyethylene with a density of 0.942 g / cm 3 Polyethylene above.
[0045] Examples of the olefin copolymer include ethylene-based copolymers having at least a constituent unit derived from ethylene and propylene-based copolymers having at least a constituent unit derived from propylene.
[0046] The ethylene-based copolymer has constituent units derived from ethylene and constituent units derived from monomers other than ethylene. However, for convenience, copolymers having constituent units derived from ethylene and constituent units derived from propylene in which the number of constituent units derived from propylene is greater than the number of constituent units derived from ethylene are classified as propylene-based copolymers.
[0047] As ethylene-based copolymers, for example, ethylene-vinyl acetate copolymers (EVA), ethylene-vinyl alcohol copolymers (EVOH), ethylene-vinyl alcohol-vinyl acetate copolymers (another name: partially saponified ethylene-vinyl acetate copolymers, sometimes referred to as "partially saponified EVA" in this specification), ethylene-methyl acrylate copolymers (EMA), ethylene-methyl methacrylate copolymers (EMMA), ethylene-ethyl acrylate copolymers (EEA), ethylene-acrylic acid copolymers (EAA), ethylene-methacrylic acid copolymers (EMAA), ethylene-ethyl acrylate-maleic anhydride copolymers (E-EA-MAH), ionomers (ION), etc. can be cited.
[0048] Examples of the ionomer include a copolymer of ethylene and a small amount of acrylic acid or methacrylic acid, in which a resin has an ion-bridged structure through a salt formed between the acid portion and a metal ion.
[0049] The propylene-based copolymer has a constituent unit derived from propylene and a constituent unit derived from a monomer other than propylene.
[0050] Examples of the propylene-based copolymer include a propylene-ethylene random copolymer (another name: a polypropylene random copolymer (rPP)) and a propylene-ethylene block copolymer (another name: a polypropylene block copolymer (bPP)).
[0051] The polyolefin-based resin contained in the first resin layer may be only one kind or two or more kinds. In the case of two or more kinds, the combination and ratio of these can be arbitrarily selected according to the purpose.
[0052] The polyolefin-based resin contained in the first resin layer is preferably a polyethylene-based resin, and more preferably a low-density polyethylene.
[0053] The first resin layer may contain other components in addition to the polyolefin-based resin as long as the effects of the present invention are not impaired.
[0054] The other components may be any of resin components (sometimes referred to as “other resin components” in this specification) and non-resin components (sometimes referred to as “other non-resin components” in this specification).
[0055] The other resin components are not particularly limited as long as they are resins other than the polyolefin-based resins.
[0056] Examples of the other non-resin components include additives known in the art.
[0057] Examples of the additives include antifogging agents, antiblocking agents, antioxidants, antistatic agents, crystal nucleating agents, inorganic particles, viscosity reducers, thickeners, heat stabilizers, lubricants, infrared absorbers, and ultraviolet absorbers.
[0058] The other components contained in the first resin layer may be only one kind or two or more kinds. In the case of two or more kinds, the combination and ratio of these components can be arbitrarily selected according to the purpose.
[0059] In the first resin layer, the content of the polyolefin resin (the total content of the polyolefin resin of the same type as the polyolefin resin included in the second resin layer and the polyolefin resin of a different type from the polyolefin resin included in the second resin layer) is preferably 90 to 100% by mass, more preferably 95 to 100% by mass, for example, any one of 97 to 100% by mass and 99 to 100% by mass. When the ratio is equal to or greater than the lower limit, the effect obtained by the first resin layer containing the polyolefin resin can be more significantly obtained.
[0060] The above ratio is usually the same as the ratio of the content of the polyolefin resin (the total content of the polyolefin resin of the same type as the polyolefin resin contained in the second resin layer and the polyolefin resin of a different type from the polyolefin resin contained in the second resin layer) (parts by mass) in the first resin composition described later relative to the total content (parts by mass) of components that do not vaporize at room temperature.
[0061] The first resin layer and the second resin layer contain the same type of polyolefin-based resin.
[0062] In the present embodiment, not limited to the case of polyolefin resins, "resins of the same type" means that when resins having the same constituent units are compared with each other, no matter which resin, the amount (molar) of the same constituent units relative to the total amount (molar) of the constituent units is 20 mol% or more. For example, low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), metallocene catalyst linear low-density polyethylene (mLLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ethylene-methyl acrylate copolymer (EMA resin), ethylene-methyl methacrylate copolymer (EMMA resin), ethylene-vinyl alcohol copolymer (EVOH), ethylene-vinyl acetate copolymer (EVA), ethylene-vinyl alcohol-vinyl acetate copolymer (EVA partial saponification product), etc., all of which have a constituent unit derived from ethylene (molar) relative to the total amount (molar) of the constituent units. The ratio is 20 mol% or more, and therefore they are of the same type. On the other hand, for example, in propylene-ethylene random copolymers and propylene-ethylene block copolymers, the amount (mole) of constituent units derived from ethylene is less than 20 mol% relative to the total amount (mole) of constituent units, which is not the same as the above-mentioned low-density polyethylene.
[0063] In the present embodiment, regardless of the type of resin, the ratio of the amount (mole) of the same constituent unit to the total amount (mole) of the constituent units is preferably 30 mol% or more, more preferably 40 mol% or more, and further preferably 50 mol% or more. For example, it can be any one of 60 mol% or more, 70 mol% or more, and 80 mol% or more.
[0064] In the first resin layer, the content of the same type of polyolefin resin as that contained in the second resin layer is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, and for example, may be any one of 95 to 100% by mass and 99 to 100% by mass relative to the total mass of the first resin layer. When the ratio is equal to or greater than the lower limit, the reuse suitability of the laminated film becomes higher.
[0065] When the first resin layer includes low-density polyethylene, in the first resin layer, the content of the low-density polyethylene is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, and further preferably 90 to 100 mass % relative to the total mass of the first resin layer. When the ratio is above the lower limit, the effect obtained by including the low-density polyethylene in the first resin layer becomes higher.
[0066] In this specification, "normal temperature" means a temperature at which cooling or heating is not particularly performed, that is, a normal temperature, and examples thereof include a temperature of 15 to 25°C.
[0067] The first resin layer can be composed of one layer (monolayer), or can be composed of more than two layers. When the first resin layer is composed of multiple layers, these multiple layers can be the same as or different from each other, and the combination of these multiple layers is not particularly limited as long as the effect of the present invention is not impaired.
[0068] In this specification, not limited to the case of the first resin layer, "multiple layers may be the same or different from each other" means "all layers may be the same, all layers may be different, or only some layers may be the same", and "multiple layers are different from each other" means "at least one of the constituent materials and thicknesses of each layer is different from each other".
[0069] The thickness of the first resin layer can be arbitrarily set according to the application of the laminated film and is not particularly limited.
[0070] The thickness of the first resin layer is usually preferably 5 to 100 μm, more preferably 10 to 80 μm, and further preferably 20 to 60 μm. When the thickness of the first resin layer is above the lower limit, the strength of the first resin layer is further improved, and the effect obtained by the laminate film having the first resin layer can be more significantly obtained. When the thickness of the first resin layer is below the upper limit, it can be suppressed from becoming too thick.
[0071] When the first resin layer is composed of a plurality of layers, the total thickness of the plurality of layers can be set to the above-mentioned preferred thickness of the first resin layer.
[0072] The first resin layer is preferably an unstretched layer (film). When the first resin layer is an unstretched layer, the moldability of the laminated film is improved.
[0073] The first resin layer is suitable as, for example, a sealant layer.
[0074] <Second resin layer>
[0075] The second resin layer includes a polyolefin-based resin of the same kind as the polyolefin-based resin included in the first resin layer.
[0076] The polyolefin-based resin of the same kind contained in the second resin layer may be only one kind or two or more kinds. In the case of two or more kinds, the combination and ratio of these can be arbitrarily selected according to the purpose.
[0077] The polyolefin resin of the same type contained in the second resin layer is preferably a polyethylene resin, more preferably a high-density polyethylene. The second resin layer containing a polyethylene resin (especially a high-density polyethylene) is more likely to have an E'(110) / E'(100) value of 0.2 or more.
[0078] That is, it is preferred that both the first resin layer and the second resin layer contain a polyethylene-based resin, and it is more preferred that the second resin layer contain a high-density polyethylene.
[0079] The second resin layer may contain other components in addition to the same polyolefin-based resin as the polyolefin-based resin contained in the first resin layer, within a range not impairing the effects of the present invention.
[0080] The other components in the second resin layer may be any of resin components (sometimes referred to as “other resin components” in this specification) and non-resin components (sometimes referred to as “other non-resin components” in this specification).
[0081] The other resin component in the second resin layer is not particularly limited as long as it is a resin other than the same type of polyolefin-based resin as the polyolefin-based resin contained in the first resin layer.
[0082] Examples of the other resin component in the second resin layer include a polyolefin-based resin that is different from the polyolefin-based resin contained in the first resin layer and a resin other than the polyolefin-based resin.
[0083] Examples of the polyolefin-based resin that is different from the polyolefin-based resin contained in the first resin layer include the same resins as those exemplified above as the polyolefin-based resin contained in the first resin layer.
[0084] Examples of the non-resin component in the second resin layer include the same ones as those in the first resin layer.
[0085] The other components contained in the second resin layer may be only one kind or two or more kinds. In the case of two or more kinds, the combination and ratio of these components can be arbitrarily selected according to the purpose.
[0086] In the second resin layer, the content of the polyolefin resin (the total content of the polyolefin resin of the same type as the polyolefin resin included in the first resin layer and the polyolefin resin of a different type from the polyolefin resin included in the first resin layer) relative to the total mass of the second resin layer is preferably 90 to 100% by mass, more preferably 95 to 100% by mass, for example, it may be any one of 97 to 100% by mass and 99 to 100% by mass. When the ratio is greater than the lower limit, the effect obtained by the second resin layer containing the polyolefin resin can be more significantly obtained.
[0087] The ratio is usually the same as the ratio of the content of the polyolefin resin in the second resin composition described later (the total content of the polyolefin resin of the same type as the polyolefin resin contained in the first resin layer and the polyolefin resin of a different type from the polyolefin resin contained in the first resin layer) (parts by mass) relative to the total content (parts by mass) of components that do not vaporize at room temperature.
[0088] In the second resin layer, the content of the same type of polyolefin resin as that contained in the first resin layer is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, for example, 95 to 100% by mass and 99 to 100% by mass relative to the total mass of the second resin layer. When the ratio is greater than the lower limit, the reuse applicability of the laminated film becomes higher.
[0089] When the second resin layer includes high-density polyethylene, in the second resin layer, the content of the high-density polyethylene is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, and further preferably 90 to 100 mass % relative to the total mass of the second resin layer. When the ratio is greater than the lower limit, the heat resistance of the second resin layer is significantly improved.
[0090] The second resin layer may be subjected to electron beam irradiation. That is, the laminated film may be subjected to electron beam irradiation, preferably from the second resin layer side. For example, even if the second resin layer does not contain high-density polyethylene, the second resin layer can be subjected to electron beam irradiation to easily make its E'(110) / E'(100) value greater than 0.2. It is speculated that the reason for this is that the crosslinking density of the resin in the second resin layer is increased by electron beam irradiation.
[0091] As a preferred second resin layer in the electron beam irradiated second resin layer, for example, a second resin layer comprising low-density polyethylene that has not been irradiated with an electron beam (in this specification, in order to distinguish the second resin layer at this time from the second resin layer after electron beam irradiation, it is sometimes referred to as "unirradiated second resin layer") after being irradiated with an electron beam.
[0092] That is, as a preferred laminated film among the laminated films irradiated with an electron beam, for example, there can be cited a laminated film having a second resin layer containing low-density polyethylene as the non-irradiated second resin layer (in this specification, in order to distinguish the laminated film at this time from the laminated film after electron beam irradiation, it is sometimes referred to as an "unirradiated laminated film") after electron beam irradiation.
[0093] In the unirradiated second resin layer, the content of the low-density polyethylene is preferably 70 to 100 mass %, more preferably 80 to 100 mass %, and further preferably 90 to 100 mass % relative to the total mass of the unirradiated second resin layer. When the ratio is greater than the lower limit, the effect of electron beam irradiation can be more significantly obtained.
[0094] The electron beam irradiation of the unirradiated second resin layer or the unirradiated laminated film is preferably performed under the condition of an absorbed radiation dose of 20 to 300 kGy. When the absorbed radiation dose is above the lower limit, the effect of the electron beam irradiation can be more significantly obtained. When the absorbed radiation dose is below the upper limit, excessive crosslinking of the resin in the second resin layer can be suppressed.
[0095] That is, a preferred laminated film among the laminated films irradiated with electron beams is a laminated film irradiated with electron beams under the condition of an absorbed radiation dose of 20 to 300 kGy.
[0096] The acceleration voltage when the unirradiated second resin layer or the unirradiated laminated film is subjected to electron beam irradiation is preferably 100 to 300 kV, more preferably 120 to 280 kV, and further preferably 140 to 260 kV. When the acceleration voltage is above the lower limit, the effect of electron beam irradiation can be more significantly obtained. When the acceleration voltage is below the upper limit, excessive crosslinking of the resin in the second resin layer can be suppressed.
[0097] For example, the gel fraction of the laminated film increases by electron beam irradiation, that is, the gel fraction of the laminated film is larger than the gel fraction of the non-irradiated laminated film.
[0098] The gel fraction of the laminated film is preferably 30% or more, for example, 30 to 90%, 32 to 78%, and 34 to 76%. Such a laminated film has more preferable heat resistance as a laminated film having a second resin layer having the above-mentioned E'(110) / E'(100) value.
[0099] The gel fraction of the laminated film can be measured in accordance with JIS K 6769. That is, the laminated film can be immersed in an organic solvent such as xylene, and the mass of the insoluble matter that does not dissolve and remains can be obtained after drying, and the gel fraction can be calculated based on the mass of the laminated film before dissolution and the mass of the insoluble matter from the laminated film after drying. More specifically, for example, a laminated film of Xg is wrapped with a stainless steel wire mesh of Yg and immersed in a heated organic solvent, and the insoluble matter from the laminated film is taken out from the organic solvent together with the stainless steel wire mesh. Then, the stainless steel wire mesh wrapped with the insoluble matter is vacuum dried, and the total mass (Zg) of the insoluble matter and the stainless steel wire mesh after drying is measured. The gel fraction of the laminated film is calculated according to the following formula (1).
[0100] Gel fraction of laminated film (mass %) = (ZY) / X×100 (1)
[0101] The laminated film changes its characteristics, for example, when subjected to thermomechanical analysis, by electron beam irradiation.
[0102] For example, when the laminated film is subjected to thermomechanical analysis, the temperature showing a displacement of 2000 μm (sometimes referred to as "2000 μm displacement temperature" in this specification) is preferably 120° C. or higher, for example, 125 to 200° C. and 130 to 195° C. Such a laminated film has more preferred heat resistance as a laminated film having a second resin layer having the above-mentioned E'(110) / E'(100) value.
[0103] For example, when the laminated film is subjected to thermomechanical analysis, the displacement at a temperature of 100° C. is preferably 500 μm or less, for example, 50 to 490 μm or 100 to 480 μm or less. Such a laminated film has more preferable heat resistance as a laminated film having a second resin layer having the above-mentioned E'(110) / E'(100) value.
[0104] Thermomechanical analysis of the laminated film can be performed, for example, by measuring the thermal expansion amount of a sample based on the difference in thermal expansion amounts when a standard sample and a target sample are heated at a constant rate in accordance with JIS K 7196.
[0105] The second resin layer can be composed of one layer (monolayer), or can be composed of more than two layers. When the second resin layer is composed of multiple layers, these multiple layers can be the same as each other, or they can be different from each other. As long as the effect of the present invention is not damaged, the combination of these multiple layers is not particularly limited.
[0106] The thickness of the second resin layer can be arbitrarily set according to the application of the laminated film and is not particularly limited.
[0107] The thickness of the second resin layer is usually preferably 5 to 100 μm, more preferably 10 to 80 μm, and further preferably 20 to 60 μm. When the thickness of the second resin layer is above the lower limit, the strength of the second resin layer is further improved, and the effect obtained by the laminate film having the second resin layer can be more significantly obtained. When the thickness of the second resin layer is below the upper limit, it can be suppressed from becoming too thick.
[0108] When the second resin layer is composed of a plurality of layers, the total thickness of the plurality of layers can be set to the above-mentioned preferred thickness of the second resin layer.
[0109] In the laminated film, the ratio (thickness ratio) of [thickness of the first resin layer] / [thickness of the second resin layer] is not particularly limited, but is preferably 0.7 to 1.3 regardless of the presence or absence of the third resin layer described later. When the thickness ratio is within such a range, the effects obtained by the laminated film having the first resin layer and the effects obtained by the laminated film having the second resin layer can be obtained in a more balanced manner.
[0110] The second resin layer was subjected to dynamic viscoelasticity measurement (DMA: Dynamic Mechanical Analysis), and when the elastic modulus E'(100) at 100°C with a vibration frequency of 1 Hz and the elastic modulus E'(110) at 110°C with a vibration frequency of 1 Hz were measured, the value of E'(110) / E'(100) was greater than 0.2.
[0111] At this time, as the second resin layer for dynamic viscoelasticity measurement, i.e., the test piece of the second resin layer, a test piece with a width of 1 cm and a length of 5 cm or more can be cited. It is preferred to use such a test piece, set the test piece in such a way that the length of the measurement object part for dynamic viscoelasticity measurement becomes 2 cm, heat the test piece at a heating rate of 5°C / min, and perform the dynamic viscoelasticity measurement. By setting such conditions, the elastic modulus E'(100) and the elastic modulus E'(110) can be measured with higher accuracy.
[0112] From the viewpoint of further improving the heat resistance of the second resin layer and the laminated film, the E'(110) / E'(100) value of the second resin layer is preferably 0.24 or more, for example, 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more.
[0113] The upper limit of the E'(110) / E'(100) value of the second resin layer is not particularly limited. For example, a second resin layer having an E'(110) / E'(100) value of 0.9 or less can be more easily realized.
[0114] The E'(110) / E'(100) value of the second resin layer can be appropriately adjusted within a range set by arbitrarily combining any of the above lower limit values and upper limit values. For example, in one embodiment, the E'(110) / E'(100) value of the second resin layer is preferably 0.2 to 0.9, more preferably 0.24 to 0.9, for example, any one of 0.3 to 0.9, 0.4 to 0.9, 0.5 to 0.9, and 0.6 to 0.9.
[0115] The E'(110) / E'(100) value of the second resin layer containing high-density polyethylene tends to become larger.
[0116] For example, a second resin layer having a value of E'(110) / E'(100) of 0.5 or more can be more easily realized by a second resin layer containing high-density polyethylene.
[0117] The E'(100) of the second resin layer is not particularly limited as long as the above-mentioned E'(110) / E'(100) value is satisfied. For example, the E'(100) of the second resin layer may be 1.6×10 7 ~2×10 8 Pa.
[0118] The E'(110) of the second resin layer is not particularly limited as long as the above-mentioned E'(110) / E'(100) value is satisfied. For example, the E'(110) of the second resin layer may be 1.5×10 7 ~2.2×10 8 Pa.
[0119] The second resin layer is preferably an unstretched layer (film). When the second resin layer is an unstretched layer, the moldability of the laminated film is improved.
[0120] The second resin layer has heat resistance and is therefore suitable as, for example, an outer layer (an outermost layer on the side opposite to the sealant layer side).
[0121] <Third resin layer>
[0122] The laminated film may further include a third resin layer between the first resin layer and the second resin layer.
[0123] The third resin layer contains the same polyolefin resin as the polyolefin resin contained in the first resin layer and the second resin layer. That is, in the laminated film having the third resin layer, the first resin layer, the second resin layer and the third resin layer contain the same polyolefin resin.
[0124] In the present embodiment, not limited to the case of polyolefin resins, "resins of the same type" means that when resins having the same constituent units are compared with each other, no matter which resin, the amount (molar) of the same constituent units relative to the total amount (molar) of the constituent units is 20 mol% or more. For example, low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), metallocene catalyst linear low-density polyethylene (mLLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ethylene-methyl acrylate copolymer (EMA resin), ethylene-methyl methacrylate copolymer (EMMA resin), ethylene-vinyl alcohol copolymer (EVOH), ethylene-vinyl acetate copolymer (EVA), ethylene-vinyl alcohol-vinyl acetate copolymer (EVA partial saponification product), etc., all of which have a constituent unit derived from ethylene (molar) relative to the total amount (molar) of the constituent units. The ratio is 20 mol% or more, and therefore they are of the same type. On the other hand, for example, in propylene-ethylene random copolymers and propylene-ethylene block copolymers, the amount (mole) of constituent units derived from ethylene is less than 20 mol% relative to the total amount (mole) of constituent units, which is not the same as the above-mentioned low-density polyethylene.
[0125] In the present embodiment, regardless of the type of resin, the ratio of the amount (mole) of the same constituent unit to the total amount (mole) of the constituent units is preferably 30 mol% or more, more preferably 40 mol% or more, and further preferably 50 mol% or more. For example, it can be any one of 60 mol% or more, 70 mol% or more, and 80 mol% or more.
[0126] The laminated film including the third resin layer has the effects obtained by including the third resin layer and has high recyclability.
[0127] The polyolefin-based resin of the same kind contained in the third resin layer may be only one kind or two or more kinds. In the case of two or more kinds, the combination and ratio of these can be arbitrarily selected according to the purpose.
[0128] The polyolefin-based resin of the same kind contained in the third resin layer is preferably a polyethylene-based resin.
[0129] That is, it is preferred that the first resin layer, the second resin layer, and the third resin layer all contain a polyethylene-based resin.
[0130] The third resin layer may contain other components in addition to the same polyolefin-based resin as the polyolefin-based resin contained in the first resin layer and the second resin layer, within a range not impairing the effects of the present invention.
[0131] The other components in the third resin layer may be any of resin components (sometimes referred to as “other resin components” in this specification) and non-resin components (sometimes referred to as “other non-resin components” in this specification).
[0132] The other resin component in the third resin layer is not particularly limited as long as it is a resin other than the same type of polyolefin-based resin as the polyolefin-based resin contained in the first resin layer and the second resin layer.
[0133] Examples of the other resin component in the third resin layer include polyolefin-based resins that are different from the polyolefin-based resins contained in the first resin layer and the second resin layer and resins other than polyolefin-based resins.
[0134] Examples of the polyolefin resin used in the third resin layer (the third resin layer contains) include elastomer components such as α-olefin copolymers; ethylene-vinyl alcohol copolymers (EVOH); and ethylene-vinyl alcohol-vinyl acetate copolymers (EVA partial saponification product). Even if the laminated film having the third resin layer containing an elastomer does not contain polyamide such as nylon, it has high pinhole resistance and high strength. The laminated film having the third resin layer containing EVOH has oxygen barrier properties.
[0135] Examples of the polyolefin resin that is different from the polyolefin resin contained in the first resin layer and the second resin layer include the same resins as those exemplified above as the polyolefin resin contained in the first resin layer; and elastomers such as α-olefin copolymers.
[0136] The laminated film including the third resin layer containing the elastomer has high pinhole resistance and high strength even if it does not contain polyamide such as nylon.
[0137] Examples of the resin other than the polyolefin-based resin in the third resin layer include elastomers such as styrene-ethylene / butylene-ethylene block copolymers.
[0138] The laminated film including the third resin layer containing the elastomer has high pinhole resistance and high strength even if it does not contain polyamide such as nylon.
[0139] Examples of the non-resin component in the third resin layer include the same ones as those in the first resin layer.
[0140] The other components contained in the third resin layer may be only one kind or two or more kinds. In the case of two or more kinds, the combination and ratio of these components can be arbitrarily selected according to the purpose.
[0141] In the third resin layer, the content of the polyolefin resin (the total content of the polyolefin resin of the same type as the polyolefin resin included in the first resin layer and the second resin layer and the polyolefin resin of a different type from the polyolefin resin included in the first resin layer and the second resin layer) relative to the total mass of the third resin layer is preferably 90 to 100% by mass, more preferably 95 to 100% by mass, for example, it may be any one of 97 to 100% by mass and 99 to 100% by mass. When the ratio is above the lower limit, the effect obtained by the third resin layer containing the polyolefin resin can be more significantly obtained.
[0142] The above ratio is usually the same as the ratio of the content of the polyolefin resin in the third resin composition described later (the total content of the polyolefin resin of the same type as the polyolefin resin contained in the first resin layer and the second resin layer and the polyolefin resin of a different type from the polyolefin resin contained in the first resin layer and the second resin layer) (parts by mass) relative to the total content (parts by mass) of components that do not vaporize at room temperature.
[0143] In the third resin layer, the content of the same polyolefin resin as the polyolefin resin contained in the first resin layer and the second resin layer is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, for example, 95 to 100% by mass and 99 to 100% by mass relative to the total mass of the third resin layer. When the ratio is greater than the lower limit, the reuse applicability of the laminated film becomes higher.
[0144] The 3rd resin layer can be composed of one layer (monolayer), or can be composed of more than two layers. When the 3rd resin layer is composed of multiple layers, these multiple layers can be the same as each other, or they can be different from each other. As long as the effect of the present invention is not damaged, the combination of these multiple layers is not particularly limited.
[0145] In the third resin layer composed of a plurality of layers, all the layers contain the same kind of polyolefin-based resin as the polyolefin-based resin contained in the first resin layer and the second resin layer.
[0146] The thickness of the third resin layer can be arbitrarily set according to the application of the laminated film and is not particularly limited.
[0147] The thickness of the third resin layer is usually preferably 15 to 200 μm, more preferably 30 to 160 μm, and further preferably 50 to 120 μm. When the thickness of the third resin layer is greater than the lower limit, the strength of the third resin layer is further improved, and the effect obtained by the laminate film having the third resin layer can be more significantly obtained. When the thickness of the third resin layer is less than the upper limit, it can be suppressed from becoming too thick.
[0148] When the third resin layer is composed of a plurality of layers, the total thickness of the plurality of layers can be set to the above-mentioned preferred thickness of the third resin layer.
[0149] When the laminate film includes a third resin layer, the ratio of the thickness of the third resin layer to the thickness of the laminate film is not particularly limited, but is preferably 50 to 70%.
[0150] When the ratio is equal to or greater than the lower limit, the effect obtained by the laminate film including the third resin layer is further enhanced. When the ratio is equal to or less than the upper limit, the effect obtained by the laminate film including the first resin layer and the second resin layer is further enhanced.
[0151] When the laminate film includes a third resin layer, the ratio of the total thickness of the first resin layer and the second resin layer to the thickness of the laminate film is not particularly limited, but is preferably 30 to 50%. When the ratio is above the lower limit, the effect obtained by the laminate film including the first resin layer and the second resin layer becomes higher. When the ratio is below the upper limit, the effect obtained by the laminate film including the third resin layer becomes higher.
[0152] The third resin layer is preferably an unstretched layer (film). When the third resin layer is an unstretched layer, the moldability of the laminated film is improved.
[0153] The third resin layer is suitable as an intermediate layer such as a pinhole-proof layer or an oxygen-barrier layer, for example.
[0154] The laminated film has high pinhole resistance and high strength even if it does not contain polyamide such as nylon.
[0155] For example, when the front end of a needle with a curvature radius of 0.5 mm is pressed vertically relative to the laminated film at a speed of 500 mm / min, and the load applied to the needle at the moment the needle penetrates the laminated film is taken as the puncture strength (N), it can be said that the higher the puncture strength, the higher the pinhole resistance of the laminated film.
[0156] As the needle, for example, a stainless steel needle can be mentioned.
[0157] The puncture strength of the laminated film is preferably 7N or more, and may be, for example, 8N or more or 10N or more.
[0158] The upper limit of the puncture strength is not particularly limited, but, for example, a laminated film having a puncture strength of 12 N or less can be more easily achieved.
[0159] The laminate film having high puncture strength as described above can be more easily realized by including a third resin layer, for example. The puncture strength of the laminate film can be adjusted by adjusting the type and content of the resin contained in the first resin layer, the second resin layer, and the third resin layer as appropriate.
[0160] The resin layer containing ethylene-vinyl alcohol copolymer (EVOH) has high oxygen barrier properties. Therefore, for example, the laminated film including the third resin layer containing ethylene-vinyl alcohol copolymer has oxygen barrier properties.
[0161] On the other hand, ethylene-vinyl alcohol copolymers generally have low compatibility with polyolefin resins that are not ethylene-vinyl acetate copolymers and ethylene-vinyl alcohol-vinyl acetate copolymers (in other words, ethylene-vinyl acetate copolymers and their partial saponification products). Ethylene-vinyl alcohol-vinyl acetate copolymers (ethylene-vinyl acetate copolymer partial saponification products) generally have compatibility with ethylene-vinyl alcohol copolymers, and have compatibility with polyolefin resins that are not ethylene-vinyl alcohol copolymers, ethylene-vinyl acetate copolymers, and ethylene-vinyl alcohol-vinyl acetate copolymers (sometimes referred to as "non-ethylene polyolefin resins" in this specification). Therefore, in the case where the third resin layer contains the non-ethylene polyolefin resin and ethylene-vinyl alcohol copolymer, the third resin layer is preferably a resin layer (sometimes referred to as "resin layer (I)" in this specification) that also contains ethylene-vinyl alcohol-vinyl acetate copolymer in addition to these resins. The third resin layer as the resin layer (I) has high oxygen barrier properties.
[0162] In the resin layer (I), the non-ethylene polyolefin resin is a polyolefin resin of the same kind as the polyolefin resin contained in the first resin layer and the second resin layer, and is preferably a polyethylene resin.
[0163] In the resin layer (I), the ethylene-vinyl alcohol copolymer and the ethylene-vinyl alcohol-vinyl acetate copolymer are preferably polyolefin resins of the same type as the polyolefin resins contained in the first resin layer and the second resin layer.
[0164] In the resin layer (I) (the third resin layer comprising the ethylene-vinyl alcohol copolymer, the non-ethylene polyolefin resin and the ethylene-vinyl alcohol-vinyl acetate copolymer), the ratio of the amount (mole) of the constituent units derived from ethylene to the total amount (mole) of the constituent units is preferably 20 mol% or more, more preferably 20 to 80 mol%, for example, it can be any one of 20 to 70 mol%, 20 to 60 mol% and 20 to 50 mol%, or any one of 30 to 80 mol%, 40 to 80 mol% and 50 to 80 mol%, or any one of 30 to 70 mol% and 40 to 60 mol%.
[0165] In the resin layer (I), the content of the ethylene-vinyl alcohol copolymer relative to the total mass of the resin layer (I) may be, for example, 25 to 70% by mass. However, from the viewpoint of achieving higher uniformity and oxygen barrier properties of the resin layer (I), the content of the ethylene-vinyl alcohol copolymer is preferably 40 to 70% by mass, more preferably 50 to 70% by mass, and for example, 55 to 65% by mass.
[0166] The above ratio is usually the same as the ratio of the content (mass parts) of the ethylene-vinyl alcohol copolymer to the total content (mass parts) of components that do not vaporize at room temperature in the resin composition (the third resin composition described later) for forming the resin layer (I).
[0167] In the resin layer (I), the content of the non-ethylene polyolefin resin relative to the total mass of the resin layer (I) may be, for example, 5 to 50% by mass. However, from the viewpoint of achieving higher uniformity and oxygen barrier properties of the resin layer (I), the content is preferably 5 to 35% by mass, more preferably 5 to 20% by mass, and for example, 5 to 15% by mass.
[0168] The ratio is usually the same as the ratio of the content (mass parts) of the non-ethylene polyolefin resin in the resin composition (the third resin composition described later) used to form the resin layer (I) relative to the total content (mass parts) of components that do not vaporize at room temperature.
[0169] In the resin layer (I), the content of the ethylene-vinyl alcohol-vinyl acetate copolymer is preferably 20 to 40% by mass, for example, 25 to 35% by mass, relative to the total mass of the resin layer (I). When the content of the ethylene-vinyl alcohol-vinyl acetate copolymer is within such a range, the effect obtained by using the ethylene-vinyl alcohol-vinyl acetate copolymer can be more significantly obtained.
[0170] The above ratio is usually the same as the ratio of the content (parts by mass) of the ethylene-vinyl alcohol-vinyl acetate copolymer in the resin composition (the third resin composition described later) for forming the resin layer (I) to the total content (parts by mass) of components that do not vaporize at room temperature.
[0171] In the resin layer (I), the total content of the ethylene-vinyl alcohol copolymer, the non-ethylene polyolefin resin and the ethylene-vinyl alcohol-vinyl acetate copolymer is preferably 90 to 100% by mass, more preferably 95 to 100% by mass, for example, 97 to 100% by mass and 99 to 100% by mass relative to the total mass of the resin layer (I). When the ratio is equal to or greater than the lower limit, the oxygen barrier property of the resin layer (I) becomes higher.
[0172] The ratio is usually the same as the ratio of the total content (parts by mass) of the ethylene-vinyl alcohol copolymer, the non-ethylene polyolefin resin and the ethylene-vinyl alcohol-vinyl acetate copolymer to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition (the third resin composition described later) used to form the resin layer (I).
[0173] When the laminated film comprises a resin layer (I) as the third resin layer, it may comprise only one resin layer (I) or may comprise two or more resin layers (I). When the laminated film comprises two or more resin layers (I), these two or more resin layers (I) may be the same as or different from each other, and the combination of these resin layers (I) is not particularly limited as long as the effect of the present invention is not impaired.
[0174] As the laminated film having a resin layer (I) as a third resin layer, for example, there can be cited a laminated film having a single resin layer (I) and a single or two layers of a third resin layer other than the resin layer (I) on either or both sides of the first resin layer side and the second resin layer side of the resin layer (I).
[0175] As such a laminated film, more specifically, for example, there can be mentioned: a laminated film in which a first resin layer, a layer of resin layer (I) (third resin layer), one or two layers of a third resin layer other than the resin layer (I), and a second resin layer are laminated in sequence in their thickness direction, and the third resin layer has two or three layers in total; a laminated film in which a first resin layer, a layer of resin layer (I) (third resin layer) and a second resin layer are laminated in sequence in their thickness direction, and the third resin layer has two or three layers in total; a laminated film in which a first resin layer, a layer of resin layer (I) (third resin layer) and a second resin layer are laminated in sequence in their thickness direction, and the third resin layer has three to five layers in total.
[0176] In the laminated film exemplified here, the first resin layer, the resin layer (I), the third resin layer other than the resin layer (I), and the second resin layer all contain the same kind of polyolefin-based resin.
[0177] In the laminated film exemplified here, the first resin layer and the second resin layer may each be a single layer or two or more layers.
[0178] As a preferred laminated film among the laminated films, for example, from the viewpoint of having oxygen barrier properties, there can be cited a laminated film in which the third resin layer is composed of three or more layers, at least one layer of which contains the non-ethylene polyolefin resin, ethylene-vinyl alcohol copolymer and ethylene-vinyl alcohol-vinyl acetate copolymer (that is, the resin layer (I)).
[0179] In the third resin layer serving as the resin layer (I), it is sufficient that one or more polyolefin resins selected from the group comprising the non-ethylene polyolefin resins, ethylene-vinyl alcohol copolymers and ethylene-vinyl alcohol-vinyl acetate copolymers are the same as the polyolefin resins contained in the first resin layer and the second resin layer.
[0180] For example, when the non-ethylene polyolefin resin is the same type of polyolefin resin, either or both of the ethylene-vinyl alcohol copolymer and the ethylene-vinyl alcohol-vinyl acetate copolymer may be the same type of polyolefin resin, or both of the ethylene-vinyl alcohol copolymer and the ethylene-vinyl alcohol-vinyl acetate copolymer may not be the same type of polyolefin resin.
[0181] In the laminated film having the resin layer (I) as the third resin layer, the ratio of the thickness of the resin layer (I) to the thickness of the laminated film is not particularly limited, but is preferably 4 to 15%. The uniformity of the thickness of the resin layer (I) is higher when the ratio is above the lower limit. When the ratio is below the upper limit, the reuse applicability of the laminated film becomes higher.
[0182] When the laminate film includes the resin layer (I) as the third resin layer, the oxygen permeability of the laminate film measured in accordance with JIS K7126-2:2006 at a temperature of 23° C. and a relative humidity (RH) of 50% may be 500 ml / (m 2 ·24h·atm) or less, but preferably 100ml / (m 2 ·24h·atm) or less, more preferably 50ml / (m 2 ·24h·atm) or less, more preferably 25ml / (m 2 ·24h·atm) or less, for example, it can be 10ml / (m 2 On the other hand, the oxygen permeability of the laminated film is 0 ml / (m 2 ·24h·atm) or more.
[0183] When the laminate film includes a resin layer (I) as the third resin layer, the haze of the laminate film measured from the outside of the second resin layer side may be 35% or less and 30% or less, but is preferably 20% or less. The laminate film having a haze of less than or equal to the upper limit has higher oxygen barrier properties. This is because the resin layer (I) has high uniformity and high oxygen barrier properties.
[0184] In this specification, "haze" means a value measured in accordance with JIS K 7136:2000.
[0185] In the laminated film, each layer (the first resin layer and the second resin layer, and the third resin layer according to the case) constituting the laminated film comprises the same polyolefin resin, so that not only is the reuse applicability high, but also the layers can be made to adhere to each other without an adhesive layer. That is, even if the laminated film does not have an adhesive layer, the adhesion of each layer is high. Moreover, the laminated film without an adhesive layer can be manufactured at a low cost.
[0186] In the laminated film, the content of the same polyolefin resin relative to the total mass of the laminated film is preferably 90% or more, more preferably 92% or more, and further preferably 95% or more. When the ratio is above the lower limit, the laminated film can be made of a single material and the entire laminated film can be easily reused.
[0187] Figure 1 It is a cross-sectional view schematically showing an example of the laminated film according to the present embodiment.
[0188] The laminated film 1 shown here is configured to include a first resin layer 11 and a second resin layer 12, and further include a third resin layer 13 between the first resin layer 11 and the second resin layer 12. That is, the laminated film 1 is configured by laminating the first resin layer 11, the third resin layer 13, and the second resin layer 12 in this order in their thickness directions.
[0189] The first resin layer 11 , the second resin layer 12 , and the third resin layer 13 have been described above.
[0190] The third resin layer 13 is an optional structure, and the laminated film 1 does not need to include the third resin layer 13 .
[0191] One surface 11 b of the first resin layer 11 (the surface on the side opposite to the second resin layer 12 side, sometimes referred to as “second surface” in this specification) is an exposed surface.
[0192] One surface 12 a of the second resin layer 12 (the surface on the side opposite to the first resin layer 11 side, sometimes referred to as “first surface” in this specification) is an exposed surface.
[0193] As described above, the ratio of the thickness of the third resin layer 13 to the thickness of the laminated film 1 is not particularly limited, but is preferably 50 to 70%.
[0194] As described above, the ratio of the total thickness of the first resin layer 11 and the second resin layer 12 to the thickness of the laminated film 1 is not particularly limited, but is preferably 30 to 50%.
[0195] In the laminated film 1 , as described above, the ratio (thickness ratio) of [the thickness of the first resin layer 11 ] / [the thickness of the second resin layer 12 ] is not particularly limited, but is preferably 0.7 to 1.3.
[0196] Figure 2 It is a cross-sectional view schematically showing another example of the laminated film according to the present embodiment.
[0197] The laminated film 2 shown here has a five-layer structure of laminated resin layers as the third resin layer 23, and the five-layer structure of the laminated resin layers is formed by stacking the 3-1 resin layer 231, the 3-2 resin layer 232, the 3-3 resin layer 233, the 3-4 resin layer 234 and the 3-5 resin layer 235 in sequence in their thickness direction from the 1st resin layer 11 side to the 2nd resin layer 12 side.
[0198] That is, the laminated film 2 is formed by laminating the first resin layer 11, the 3-1 resin layer 231, the 3-2 resin layer 232, the 3-3 resin layer 233, the 3-4 resin layer 234, the 3-5 resin layer 235 and the second resin layer 12 in this order in their thickness directions.
[0199] The laminated film 2 is the same as the laminated film 1 except that the laminated film 2 includes a third resin layer 23 instead of the third resin layer 13 .
[0200] In the third resin layer 23, the 3-1 resin layer 231 and the 3-5 resin layer 235 are preferably resin layers other than the resin layer (I). It is preferred that any one or two or more of the 3-2 resin layer 232, the 3-3 resin layer 233 and the 3-4 resin layer 234 are the resin layer (I), i.e., resin layers having oxygen barrier properties.
[0201] As a more preferred third resin layer in this third resin layer 23, for example, a 3-1 resin layer 231, a 3-2 resin layer 232, a 3-4 resin layer 234 and a 3-5 resin layer 235 are all resin layers other than the resin layer (I), and the 3-3 resin layer 233 is the third resin layer of the resin layer (I) having oxygen-barrier properties.
[0202] In the laminated film 2 having the resin layer (I) as the third resin layer, as described above, the ratio of the thickness of the resin layer (I) to the thickness of the laminated film 2 is not particularly limited, but is preferably 4 to 15%. For example, when the 3-3 resin layer 233 in the third resin layer 23 is the resin layer (I), in the laminated film 2, the ratio of the thickness of the 3-3 resin layer 233 to the thickness of the laminated film 2 is preferably 4 to 15%.
[0203] As described above, the ratio of the thickness of the third resin layer 23 to the thickness of the laminated film 2 is not particularly limited, but is preferably 50 to 70%.
[0204] As described above, the ratio of the total thickness of the first resin layer 11 and the second resin layer 12 to the thickness of the laminated film 2 is not particularly limited, but is preferably 30 to 50%.
[0205] In the laminated film 2 , as described above, the ratio (thickness ratio) of [the thickness of the first resin layer 11 ] / [the thickness of the second resin layer 12 ] is not particularly limited, but is preferably 0.7 to 1.3.
[0206] In the laminated film 2 , the third resin layer 23 may be a laminated resin layer other than a five-layer structure.
[0207] For example, the third resin layer 23 may have a three-layer structure without the 3-1 resin layer 231 and the 3-2 resin layer 232, and the 3-3 resin layer 233 is the resin layer (I).
[0208] For example, the third resin layer 23 may have a double-layer structure without the 3-1 resin layer 231, the 3-2 resin layer 232, and the 3-4 resin layer 234, and the 3-3 resin layer 233 is the resin layer (I).
[0209] For example, the third resin layer 23 may have a three-layer structure without the third-fourth resin layer 234 and the third-fifth resin layer 235, and the third-third resin layer 233 is the resin layer (I).
[0210] For example, the third resin layer 23 may have a double-layer structure without the 3-2 resin layer 232, the 3-4 resin layer 234, and the 3-5 resin layer 235, and the 3-3 resin layer 233 is the resin layer (I).
[0211] For example, the 3rd resin layer 23 may have a four-layer structure without the 3-2nd resin layer 232, and the 3-3rd resin layer 233 is the resin layer (I).
[0212] For example, the third resin layer 23 may have a four-layer structure without the third-fourth resin layer 234, and the third-third resin layer 233 is the resin layer (I).
[0213] For example, the third resin layer 23 may have a three-layer structure without the 3-2 resin layer 232 and the 3-4 resin layer 234, and the 3-3 resin layer 233 is the resin layer (I).
[0214] The laminated film may include other layers that are not included in any of the first resin layer, the second resin layer, and the third resin layer within a range not impairing the effects of the present invention, but preferably does not include such other layers.
[0215] The other layer is a layer not containing a polyolefin-based resin. By not having such an other layer, the laminated film has higher recycling suitability.
[0216] The thickness of the entire laminated film is not particularly limited, but is preferably 100 to 200 μm, for example.
[0217] In the laminated film, all the layers constituting the laminated film (for example, the first to third resin layers) are preferably unstretched layers (films). Such an unstretched laminated film has particularly excellent formability and is suitable for, for example, forming a deep-drawn package.
[0218] <<Method for producing laminated film>>
[0219] The laminated film can be produced, for example, by a feed block method in which resins or resin compositions serving as materials for forming each layer are melt-extruded using several extruders, a coextrusion T-die method such as a multi-manifold method, or an air-cooled or water-cooled coextrusion inflation method.
[0220] Furthermore, the laminated film can also be manufactured by pre-preparing two or more films for constituting any two or more layers, laminating and stacking them by thermal lamination or the like without using an adhesive, and further stacking layers other than these as needed to achieve a target configuration.
[0221] The resin composition that is the material for forming any layer in the laminated film can be manufactured by adjusting the types and contents of the components so that the formed layer contains the target components at the target content. For example, the ratio of the contents of the components that do not vaporize at room temperature in the resin composition is usually the same as the ratio of the contents of the components in the layer formed by the resin composition.
[0222] As a material for forming the first resin layer (in Figure 1 The laminated film 1 and Figure 2The resin composition (sometimes referred to as "first resin composition" in this specification) of the first resin layer 11 in the laminated film 2 shown may include, for example, a resin composition containing the polyolefin resin and other components as required. The other components are the components described above.
[0223] As a material for forming the second resin layer (in Figure 1 The laminated film 1 and Figure 2 The resin composition (in this specification, sometimes referred to as "second resin composition") of the laminated film 2 shown as the second resin layer 12) may include, for example, a resin composition containing the polyolefin resin and other components as required. The other components are the components described above.
[0224] As a material for forming the third resin layer (in Figure 1 The laminated film 1 shown is the third resin layer 13; Figure 2 The resin composition (sometimes referred to as "the third resin composition" in this specification) of the laminated film 2 shown as the 3-1 resin layer 231, the 3-2 resin layer 232, the 3-3 resin layer 233, the 3-4 resin layer 234 and the 3-5 resin layer 235) can be, for example, a resin composition containing the polyolefin resin and other components as required. The other components are the components described above. In particular, as the third resin composition for forming the resin layer as the resin layer (I) in the 3-1 resin layer 231 to the 3-5 resin layer 235, a resin composition containing an ethylene-vinyl alcohol copolymer, the non-ethylene polyolefin resin, an ethylene-vinyl alcohol-vinyl acetate copolymer and other components as required can be mentioned.
[0225] <<Packaging>>
[0226] The laminated film is suitable as a material for packaging.
[0227] That is, a preferred package body is a package body including the above-mentioned laminated film.
[0228] The packaging body of the present embodiment can be manufactured by packaging an object to be packaged using the laminate film. When manufacturing the packaging body, it is preferred that the first resin layer in the laminate film is disposed on the packaging object side, and the second resin layer is disposed on the side opposite to the packaging object side, and the packaging object is packaged.
[0229] For example, the laminated film is also suitable for forming any of the cover material and the base material of the deep-drawn package. In particular, the laminated film having good formability is particularly suitable for forming a base material having a recessed portion for forming a housing portion.
[0230] Figure 3 It is a cross-sectional view schematically showing an example of a package body including the laminated film according to the present embodiment.
[0231] The package body 101 shown here includes a lid member 8 and a bottom member 10 and is a deep-drawn package body obtained by deep-drawing a resin film.
[0232] Either or both of the cover material 8 and the base material 10 are used. Figure 1 The laminated film 1 or the laminated film 2 shown is constituted.
[0233] exist Figure 3 In the cover material 8 or the base material 10, the distinction between the layers in the laminated film 1 or the laminated film 2 constituting the cover material 8 or the base material 10 is omitted.
[0234] A recess 100 is formed on the base material 10 .
[0235] A surface 10b of the base material 10 excluding the recess 100 (sometimes referred to as the "second surface" in this specification) and a surface 8b of the cover material 8 (sometimes referred to as the "second surface" in this specification) are both sealing surfaces and are opposite to each other.
[0236] The package 101 is formed by sealing the cover material 8 and the base material 10. More specifically, the second surface 10b of the base material 10 in the area other than the recessed portion 100 overlaps with the second surface 8b of the cover material 8, and they are sealed in the area near their peripheral portions. As a result, a receiving portion 101a is formed between the second surface 10b of the base material 10 and the second surface 8b of the cover material 8 in the area of the recessed portion 100 of the base material 10. The contents 9 are received in the receiving portion 101a.
[0237] When the substrate 10 is formed using the laminate film 1 or the laminate film 2, one surface (second surface) 10b of the substrate 10 is preferably the same as the second surface 11b of the first resin layer 11 in the laminate film 1 or the laminate film 2. The other surface (sometimes referred to as the "first surface" in this specification) 10a of the substrate 10 is preferably the same as the first surface 12a of the second resin layer 12 in the laminate film 1 or the laminate film 2.
[0238] When the cover material 8 is formed using the laminate film 1, one surface (second surface) 8b of the cover material 8 is preferably the same as the second surface 11b of the first resin layer 11 in the laminate film 1 or the laminate film 2. The other surface (sometimes referred to as the "first surface" in this specification) 8a of the cover material 8 is preferably the same as the first surface 12a of the second resin layer 12 in the laminate film 1 or the laminate film 2.
[0239] exist Figure 3In the embodiment, some gaps are observed between the contents 9 and the base material 10, and between the contents 9 and the cover material 8, in the containing portion 101a of the package 101. However, the existence of these gaps is not necessary in the package 101 containing the contents 9.
[0240] The thickness of the base material 10 at its flat portion and the thickness of the cover material 8 may be the same as the thickness of the laminated film 1 or the laminated film 2 described above.
[0241] Hereinafter, the deep-drawn package body has been described as an example of a package body including the laminated film. However, the package body including the laminated film is not limited to the deep-drawn package body, and may be other package bodies.
[0242] <<Method for manufacturing packaging body>>
[0243] The packaging body can be manufactured, for example, by forming a receiving portion for receiving a packaging object (in other words, a received object) by the laminated films or the laminated films and other resin films other than the laminated films, receiving the packaging object, and heat-sealing the regions of the films other than the receiving portion. In this case, the laminated films (particularly the second resin layer) can be prevented from adhering to the heating plate in the heat-sealing device.
[0244] Example
[0245] Hereinafter, the present invention will be described in further detail based on specific examples, but the present invention is not limited to the following examples.
[0246] [Example 1]
[0247] <<Manufacturing of laminated films>>
[0248] Through the following steps, a Figure 1 The structure of the laminated film is shown.
[0249] That is, as the resin constituting the first resin layer, a low-density polyethylene (LDPE) ("UBE POLYETHYLENE (registered trademark) F222NH" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) having a density of 0.922 g / cm 3 ).
[0250] As the resin constituting the second resin layer, high-density polyethylene (HDPE) ("Nipolon Hard (registered trademark) 4010 manufactured by Tosoh Corporation) with a density of 0.964 g / cm 3, melt mass flow rate: 5.4 g / 10 min). In this specification, this HDPE is sometimes referred to as "HDPE (1)".
[0251] As the resin constituting the third resin layer, metallocene catalyst linear low-density polyethylene (mLLDPE) ("UMERIT (registered trademark) 1520F" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) with a density of 0.913 g / cm 3 ).
[0252] By co-extruding the LDPE, the mLLDPE and the HDPE (1) in sequence, a laminated film (150 μm thick) was obtained in which the first resin layer (30 μm thick), the third resin layer (90 μm thick) and the second resin layer (30 μm thick) were laminated in sequence in their thickness direction.
[0253] <<Evaluation of laminated films>>
[0254] <Calculation of E'(110) / E'(100) value of second resin layer>
[0255] The HDPE (1) was extruded to obtain a test resin film (thickness: 30 μm).
[0256] A test piece (1) having a size of 7 cm×1 cm was cut out from the test resin film, and the test piece (1) was set in a sample holder so that the length of the measurement target portion became 2 cm.
[0257] Next, using a dynamic viscoelasticity measuring device ("DMS6100" manufactured by Seiko Instruments Inc.), in the tensile mode, in the temperature range of 20°C to 130°C, under the conditions of displacement of 5 μm, vibration frequency of 1 Hz, and heating rate of 5°C / min, E'(100) and E'(110) were measured, and the E'(110) / E'(100) value was calculated. The results are shown in Table 1.
[0258] <Measurement of puncture strength of laminated film>
[0259] The front end of a needle having a curvature radius of 0.5 mm was inserted into the laminated film obtained above from the second resin layer side thereof and pressed vertically into the laminated film at a speed of 500 mm / min. At the moment when the needle penetrated the laminated film, the load applied to the needle was read, and the read value was used as the puncture strength of the laminated film. The results are shown in Table 1.
[0260] [Example 2]
[0261] <<Manufacturing of laminated films>>
[0262] When forming the second resin layer, HDPE (1) (Nipolon Hard (registered trademark) 4010 manufactured by Tosoh Corporation, with a density of 0.964 g / cm 3 , melt mass flow rate of 5.4 g / 10 min), while a different type of HDPE ("Nipolon Hard (registered trademark) 1000" manufactured by TOSOH CORPORATION, density of 0.964 g / cm 3 , melt mass flow rate of 20 g / 10 min), except for this point, a laminated film was produced by the same method as in Example 1. In this specification, the HDPE used in this example may be referred to as "HDPE (2)".
[0263] <<Evaluation of laminated films>>
[0264] The laminated film obtained above was evaluated by the same method as in Example 1. Table 1 shows the results.
[0265] In Table 1, the entry “-” in the “Evaluation Result” column means that the item was not evaluated.
[0266] [Example 3]
[0267] A laminated film was produced by the same method as in Example 1 except that a third resin composition was used instead of mLLDPE ("UMERIT (registered trademark) 1520F" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) when forming the third resin layer. The third resin composition was obtained by kneading mLLDPE ("UMERIT (registered trademark) 1520F" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) (90 parts by mass) and an elastomer ("TAFMER (registered trademark) BL3450M" manufactured by Mitsui Chemicals, Inc.) (10 parts by mass) at 200°C for 10 minutes.
[0268] <<Evaluation of laminated films>>
[0269] The laminated film obtained above was evaluated by the same method as in Example 1. Table 1 shows the results.
[0270] [Example 4]
[0271] When forming the second resin layer, HDPE (1) (Nipolon Hard (registered trademark) 4010 manufactured by Tosoh Corporation, with a density of 0.964 g / cm 3 ), and a second resin composition was used, and a laminated film was produced by the same method as in Example 1 except that the second resin composition was used. The second resin composition was obtained by kneading HDPE (1) ("Nipolon Hard (registered trademark) 4010" manufactured by TOSOH CORPORATION) (60 parts by mass) and LDPE ("UBEPOLYETHYLENE (registered trademark) F222NH" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) (40 parts by mass) at 200° C. for 10 minutes.
[0272] <<Evaluation of laminated films>>
[0273] The laminated film obtained above was evaluated by the same method as in Example 1. Table 2 shows the results.
[0274] [Example 5]
[0275] <<Manufacturing of laminated films>>
[0276] When forming the second resin layer, HDPE (1) (Nipolon Hard (registered trademark) 4010 manufactured by Tosoh Corporation, with a density of 0.964 g / cm 3 ), a laminated film (the non-irradiated laminated film) was manufactured by the same method as in Example 1, except that mLLDPE ("UMERIT (registered trademark) 1520F" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) was used.
[0277] Next, the laminated film was irradiated with electron beam (EB) from the second resin layer side. At this time, the absorbed radiation dose was 50 kGy and the acceleration voltage was 150 kV. The laminated film obtained in this way was used as the laminated film of this example.
[0278] <<Evaluation of laminated films>>
[0279] <Calculation of E'(110) / E'(100) value of second resin layer>
[0280] The laminated film obtained above was measured for E'(100) and E'(110) by the same method as in Example 1, and the value of E'(110) / E'(100) was calculated.
[0281] <Measurement of puncture strength of laminated film>
[0282] The puncture strength of the laminated film obtained above was measured by the same method as in Example 1. Table 2 shows the results.
[0283] <Measurement of gel fraction of laminated film>
[0284] The gel fraction of the laminated film obtained above was measured in accordance with JIS K 6769.
[0285] Specifically, a test piece (2) of 3 cm×3 cm was cut out from the laminated film, and the test piece (2) was wrapped with a 400-mesh stainless steel wire mesh (100 g). The test piece (2) wrapped with the stainless steel wire mesh was immersed in xylene (18 mL) at 110° C. for 24 hours.
[0286] Next, the immersed test piece (2) and the stainless steel wire mesh were taken out of the xylene and vacuum dried at 110°C and 1.7 kPa for 24 hours. The mass of the obtained dried product was determined and the gel fraction was calculated. The results are shown in Table 2.
[0287] <Measurement of 2000 μm displacement temperature of laminated film>
[0288] The laminated film obtained above was subjected to thermomechanical analysis using a thermal analyzer ("EXSTAR6000" manufactured by Seiko Instruments Inc.) in accordance with JIS K 7196, and the 2000 μm displacement temperature was determined from the obtained thermomechanical analysis curve.
[0289] [Comparative Example 1]
[0290] <<Manufacturing of laminated films>>
[0291] As the resin constituting the sealant layer, a low-density polyethylene (LDPE) ("UBE POLYETHYLENE (registered trademark) F222NH" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) having a density of 0.922 g / cm 3 ).
[0292] As a resin constituting the intermediate layer, metallocene catalyst linear low-density polyethylene (mLLDPE) ("UMERIT (registered trademark) 1520F" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) was prepared.
[0293] As a resin constituting the adhesive layer, a modified polyolefin resin ("NF536" manufactured by Mitsui Chemicals, Inc.) was prepared.
[0294] As the resin constituting the strength-retaining layer and the outer layer, 6-nylon (Ny) ("1022B" manufactured by Ube Industries, Ltd.) was prepared.
[0295] By co-extruding the LDPE, the mLLDPE, the modified polyolefin resin, the Ny, the modified polyolefin resin and the Ny in sequence, a laminated film (150 μm thick) was obtained in which a sealant layer (20 μm thick), an intermediate layer (60 μm thick), an adhesive layer (15 μm thick), a strength retaining layer (30 μm thick), an adhesive layer (15 μm thick) and an outer layer (10 μm thick) were laminated in sequence in their thickness direction.
[0296] <<Evaluation of laminated films>>
[0297] <Calculation of E'(110) / E'(100) value of outer layer>
[0298] The E'(100) and E'(110) of the outer layer of the laminated film obtained above were measured by the same method as in Example 1, and the value of E'(110) / E'(100) was calculated.
[0299] <Measurement of puncture strength of laminated film>
[0300] The puncture strength of the laminated film obtained above was measured by the same method as in Example 1. Table 3 shows the results.
[0301] [Table 1]
[0302]
[0303] [Table 2]
[0304]
[0305] [Table 3]
[0306]
[0307] It is clear from the above results that in Examples 1 to 5, the E'(110) / E'(100) value of the second resin layer is 0.25 or more (0.25 to 0.7), which is large enough to be recognized as a sufficiently high heat resistance of the second resin layer. Among them, in Examples 1 to 4, the E'(110) / E'(100) value of the second resin layer is particularly large, 0.66 to 0.7, and the effect of the second resin layer containing HDPE is high.
[0308] In the laminated films of Examples 1 to 5, the first to third resin layers all contain PE, mainly contain the same type of polyolefin-based resin, and have high recyclability.
[0309] A resin layer (resin film) identical to the second resin layer in Example 5 was prepared except that EB irradiation was not performed, and its E'(100) and E'(110) were measured, and the E'(110) / E'(100) value was calculated. The result was 0.11. As described above, in Example 5, the E'(110) / E'(100) value of the second resin layer increased due to the effect of EB irradiation.
[0310] Furthermore, in Example 5, the gel fraction of the laminated film was 42%, and the 2000 μm displacement temperature of the laminated film was 125° C., and the effect of the EB irradiation of the second resin layer was also confirmed here.
[0311] In Examples 1 to 5, the puncture strength of the laminated film was sufficiently high, not less than 7.4 N (7.4 to 10.8 N). As described above, the laminated films of Examples 1 to 5 had sufficiently high pinhole resistance and high strength even without using polyamide such as Ny.
[0312] In Examples 1 to 5, all of the first to third resin layers are unstretched layers (films), and the laminated films of these Examples are excellent in formability.
[0313] In the laminated film of Comparative Example 1, since the outer layer contains Ny, it has sufficient heat resistance, and since the strength-retaining layer contains Ny, the strength is sufficiently high. However, the sealant layer and the intermediate layer contain PE, and the adhesive layer contains a modified polyolefin resin. As described above, the laminated film of Comparative Example 1 has layers mainly containing resins of different types, and has low recyclability.
[0314] [Example 6]
[0315] <<Manufacturing of laminated films>>
[0316] Through the following steps, a Figure 2 The structure of the laminated film is shown.
[0317] That is, as the resin constituting the first resin layer, a low-density polyethylene (LDPE) ("UBE POLYETHYLENE (registered trademark) F222NH" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) having a density of 0.922 g / cm 3 ).
[0318] As the resin constituting the second resin layer, high-density polyethylene (HDPE) ("Nipolon Hard (registered trademark) 4010 manufactured by Tosoh Corporation) with a density of 0.964 g / cm 3 , melt mass flow rate is 5.4 g / 10 min, HDPE (1)).
[0319] As the resin constituting the 3-1 resin layer, the 3-2 resin layer, the 3-3 resin layer, the 3-4 resin layer and the 3-5 resin layer, metallocene catalyst linear low-density polyethylene (mLLDPE) ("UMERIT (registered trademark) 1520F" manufactured by Ube-Maruzen Polyethylene Co., Ltd.) with a density of 0.913 g / cm 3 ).
[0320] As resins constituting the 3-3 resin layer, ethylene-vinyl alcohol-vinyl acetate copolymer (EVA partially saponified product) ("melthene (registered trademark)-H3051R" manufactured by TOSOH CORPORATION) and ethylene-vinyl alcohol copolymer (EVOH) ("EVAL (registered trademark) E105B" manufactured by KURARAY CO., LTD.) were prepared.
[0321] The mLLDPE (40 parts by mass), the partially saponified EVA (30 parts by mass), and the EVOH (30 parts by mass) were kneaded at 200° C. for 10 minutes to produce a third resin composition.
[0322] The LDPE, the mLLDPE, the mLLDPE, the third resin composition, the mLLDPE, the mLLDPE and the HDPE (1) are sequentially co-extruded to obtain a laminated film (150 μm thick) in which the first resin layer (30 μm thick), the 3-1 resin layer (15 μm thick), the 3-2 resin layer (30 μm thick), the 3-3 resin layer (15 μm thick), the 3-4 resin layer (15 μm thick), the 3-5 resin layer (15 μm thick) and the second resin layer (30 μm thick) are sequentially laminated in their thickness direction.
[0323] <<Evaluation of laminated films>>
[0324] <Measurement of puncture strength of laminated film>
[0325] The laminated film obtained above was evaluated by the same method as in Example 1. Table 4 shows the results.
[0326] <Measurement of haze of laminated film>
[0327] The haze of the laminated film obtained above was measured from the outside on the second resin layer side in accordance with JIS K 7136: 2000. The results are shown in Table 4.
[0328] <Measurement of oxygen permeation rate of laminated film>
[0329] The oxygen permeation rate of the laminated film obtained above was measured under the conditions of a temperature of 23° C. and a relative humidity of 50% in accordance with JIS K 7126-2: 2006. Table 4 shows the results.
[0330] [Example 7]
[0331] <<Manufacturing of laminated films>>
[0332] When manufacturing the third resin composition, instead of kneading the mLLDPE (40 parts by mass), the partially saponified EVA (30 parts by mass) and the EVOH (30 parts by mass) at 200°C for 10 minutes, the mLLDPE (25 parts by mass), the partially saponified EVA (30 parts by mass) and the EVOH (45 parts by mass) were kneaded at 200°C for 10 minutes. Except for this point, a laminated film was manufactured by the same method as in Example 6.
[0333] The laminated film is a laminated film (150 μm thick) formed by stacking the 1st resin layer (30 μm thick), the 3-1st resin layer (15 μm thick), the 3-2nd resin layer (30 μm thick), the 3-3rd resin layer (15 μm thick), the 3-4th resin layer (15 μm thick), the 3-5th resin layer (15 μm thick) and the 2nd resin layer (30 μm thick) in sequence in their thickness direction.
[0334] <<Evaluation of laminated films>>
[0335] The laminated film obtained above was evaluated by the same method as in Example 6. Table 4 shows the results.
[0336] [Example 8]
[0337] <<Manufacturing of laminated films>>
[0338] When manufacturing the third resin composition, instead of kneading the mLLDPE (40 parts by mass), the partially saponified EVA (30 parts by mass) and the EVOH (30 parts by mass) at 200°C for 10 minutes, the mLLDPE (10 parts by mass), the partially saponified EVA (30 parts by mass) and the EVOH (60 parts by mass) were kneaded at 200°C for 10 minutes. A laminated film was manufactured by the same method as in Example 6, except that this point was not mixed.
[0339] The laminated film is a laminated film (150 μm thick) formed by stacking the 1st resin layer (30 μm thick), the 3-1st resin layer (15 μm thick), the 3-2nd resin layer (30 μm thick), the 3-3rd resin layer (15 μm thick), the 3-4th resin layer (15 μm thick), the 3-5th resin layer (15 μm thick) and the 2nd resin layer (30 μm thick) in sequence in their thickness direction.
[0340] <<Evaluation of laminated films>>
[0341] The laminated film obtained above was evaluated by the same method as in Example 6. The results are shown in FIG4 .
[0342] [Example 9]
[0343] <<Manufacturing of laminated films>>
[0344] When manufacturing the third resin composition, instead of kneading the mLLDPE (40 parts by mass), the partially saponified EVA (30 parts by mass) and the EVOH (30 parts by mass) at 200°C for 10 minutes, the LDPE (10 parts by mass), the partially saponified EVA (30 parts by mass) and the EVOH (60 parts by mass) were kneaded at 200°C for 10 minutes. Except for this point, a laminated film was manufactured by the same method as in Example 6.
[0345] The laminated film is a laminated film (150 μm thick) formed by stacking the 1st resin layer (30 μm thick), the 3-1st resin layer (15 μm thick), the 3-2nd resin layer (30 μm thick), the 3-3rd resin layer (15 μm thick), the 3-4th resin layer (15 μm thick), the 3-5th resin layer (15 μm thick) and the 2nd resin layer (30 μm thick) in sequence in their thickness direction.
[0346] <<Evaluation of laminated films>>
[0347] The laminated film obtained above was evaluated by the same method as in Example 6. Table 5 shows the results.
[0348] [Example 10]
[0349] <<Manufacturing of laminated films>>
[0350] A laminated film was produced by the same method as in Example 9 except that the extrusion amount of the mLLDPE was increased and the extrusion amount of the third resin composition was decreased.
[0351] The laminated film is a laminated film (thickness 150 μm) formed by stacking the 1st resin layer (thickness 37.5 μm), the 3-1st resin layer (thickness 15 μm), the 3-2nd resin layer (thickness 30 μm), the 3-3rd resin layer (thickness 7.5 μm), the 3-4th resin layer (thickness 15 μm), the 3-5th resin layer (thickness 15 μm) and the 2nd resin layer (thickness 30 μm) in sequence in their thickness direction.
[0352] <<Evaluation of laminated films>>
[0353] The laminated film obtained above was evaluated by the same method as in Example 6. Table 5 shows the results.
[0354] [Example 11]
[0355] <<Manufacturing of laminated films>>
[0356] A laminated film was produced by the same method as in Example 6 except that the mLLDPE was used instead of the third resin composition.
[0357] The laminated film is a laminated film (150 μm thick) formed by stacking the 1st resin layer (30 μm thick), the 3-1st resin layer (15 μm thick), the 3-2nd resin layer (30 μm thick), the 3-3rd resin layer (15 μm thick), the 3-4th resin layer (15 μm thick), the 3-5th resin layer (15 μm thick) and the 2nd resin layer (30 μm thick) in sequence in their thickness direction.
[0358] <<Evaluation of laminated films>>
[0359] The laminated film obtained above was evaluated by the same method as in Example 6. Table 5 shows the results.
[0360] [Table 4]
[0361]
[0362] [Table 5]
[0363]
[0364] As is clear from the above results, in Examples 6 to 11, the E'(110) / E'(100) value of the second resin layer was 0.7, which was large enough to indicate that the heat resistance of the second resin layer was sufficiently high.
[0365] In the laminated films of Examples 6 to 11, the first to third resin layers all contain PE, mainly contain the same type of polyolefin-based resin, and have high recyclability.
[0366] In Examples 6 to 11, the puncture strength of the laminated films was sufficiently high, not less than 7.5 N (7.5 to 8.5 N). As described above, the laminated films of Examples 6 to 11 had sufficiently high pinhole resistance and high strength even without using polyamide such as Ny.
[0367] In Examples 6 to 10 of Examples 6 to 11, the oxygen permeability of the laminated film was 452.2 ml / (m 2 ·24h·atm) or less (9.4~452.2ml / (m 2 ·24h·atm)), the laminated films of Examples 6 to 10 have oxygen barrier properties. This is because the 3-3 resin layer in these laminated films is the resin layer (I).
[0368] Among them, the oxygen permeation rate of the laminated films of Examples 7 to 10 was 21.3 ml / (m 2 ·24h·atm) or less (9.4~21.3ml / (m 2 ·24h·atm)), the laminated films of Examples 7 to 10 have high oxygen barrier properties. This is because the 3-3 resin layer in these laminated films has high uniformity and oxygen barrier properties.
[0369] In Examples 6 to 11, the haze of the laminated film was 25.7% or less (16.5 to 25.7%). In Examples 8 to 10, the haze of the laminated film was 18.9% or less (16.5 to 18.9%), which was low, but this was because the uniformity of the 3-3 resin layer in these laminated films was high, which was consistent with the high oxygen barrier properties of these laminated films.
[0370] In Examples 6 to 11, all of the first to third resin layers are unstretched layers (films), and the laminated films of these Examples are excellent in formability.
[0371] Industrial Applicability
[0372] The present invention can be used to manufacture various packaging bodies that can be reused after use.
[0373] Description of Reference Numerals
[0374] 1, 2: laminated film; 11: first resin layer; 11b: second surface of first resin layer 11; 12: second resin layer; 12a: first surface of second resin layer 12; 13, 23: third resin layer; 231: third-1 resin layer; 232: third-2 resin layer; 233: third-3 resin layer; 234: third-4 resin layer; 235: third-5 resin layer; 100: recess; 101: packaging body (deep-drawn packaging body); 101a: containing portion; 8: cover material; 8a: first surface of cover material 8; 8b: second surface of cover material 8; 9: content; 10: base material; 10a: first surface of base material 10; 10b: second surface of base material 10.
Claims
1. A laminated film, in, The laminated film comprises a first resin layer and a second resin layer. The first resin layer and the second resin layer include the same type of polyolefin resin. The second resin layer is subjected to dynamic viscoelasticity measurement. When the elastic modulus E'(100) at 100° C. and the elastic modulus E'(110) at 110° C. are measured at a vibration frequency of 1 Hz, the value of E'(110) / E'(100) is greater than 0.
69. The first resin layer and the second resin layer are composed only of the polyolefin-based resin.
2. The laminated film according to claim 1, in, The gel fraction of the laminated film is 30% or more.
3. The laminated film according to claim 1 or 2, in, The laminated film is irradiated with an electron beam under the condition of an absorbed radiation dose of 20 to 300 kGy.
4. The laminated film according to claim 1 or 2, in, When the laminated film was subjected to thermomechanical analysis, the temperature at which a displacement of 2000 μm was observed was 120° C. or higher.
5. The laminated film according to claim 1 or 2, in, The laminated film further comprises a third resin layer between the first resin layer and the second resin layer. The first resin layer, the second resin layer, and the third resin layer include the same type of polyolefin-based resin.
6. The laminated film according to claim 5, in, The third resin layer is composed of three or more layers, at least one of which contains the polyolefin resin, ethylene-vinyl alcohol copolymer, and ethylene-vinyl alcohol-vinyl acetate copolymer. The polyolefin-based resin is not any of ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol-vinyl acetate copolymer.
7. The laminated film according to claim 1 or 2, in, The polyolefin resin is a polyethylene resin.
8. The laminated film according to claim 1 or 2, in, When the tip of a needle having a tip curvature radius of 0.5 mm was pushed vertically into the laminated film at a speed of 500 mm / min, the load applied to the needle became 7N or more at the moment when the needle penetrated the laminated film.
9. The laminated film according to claim 1, in, The second resin layer includes high-density polyethylene.
Citation Information
Patent Citations
Polyethylene laminate for packaging material and packaging material including the laminate
JP2019189333A
Toilet bowl device and accessory member
JP2020060062A
Polyethylene co-extrusion film and packaging material prepared therewith
JP2018202617A