tubular containers

By using paper-based sheets and hot-melt welding technology, a tubular container containing thermoplastic resin and filler is formed, solving the problem of reduced stiffness of resin tubular containers after reducing the amount of resin, thus achieving efficient resin reduction and stiffness maintenance.

CN115335296BActive Publication Date: 2026-11-17TOPPAN HOLDINGS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180019836.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-01
Filing Date
2021-03-10
Publication Date
2026-11-17
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

Existing resin-bonded tubular containers suffer from reduced rigidity and self-supporting capacity in their main body when the amount of resin is reduced, making it difficult to meet the container's usage requirements.

Method used

The main body is constructed from a sheet material with paper as the primary material, and a material containing thermoplastic resin and filler is used in the injection port. A tubular container is formed by hot-melt welding technology, which reduces the amount of resin used while maintaining rigidity and self-support.

Benefits of technology

It achieves a reduction in resin usage while maintaining or improving the rigidity and self-support of tubular containers, making it suitable for packaging pharmaceuticals, cosmetics, food, etc., and it also has good processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115335296B_ABST
    Figure CN115335296B_ABST
Patent Text Reader

Abstract

A tubular container is provided that reduces resin usage compared to conventional containers and provides the rigidity required for container self-standing. The tubular container comprises: a tubular main body closed at one end and an outlet portion attached to the other end of the main body, the main body being formed of a paper-based material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to tubular containers. Background Technology

[0002] As packaging materials for pharmaceuticals, cosmetics, food, etc., tubular containers made primarily of resin are widely used. For example, Patent Document 1 describes a tubular container consisting of a dispensing unit for removing contents and a main body fused to the dispensing unit for containing the contents.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-199280

[0006] Patent Document 2: Japanese Utility Model Publication No. 7-45311

[0007] Patent Document 3: Japanese Patent Application Publication No. 2012-25471 Summary of the Invention

[0008] The problem to be solved by the present invention

[0009] In recent years, from the perspective of reducing environmental impact and conserving resources, there has been a desire to reduce the amount of resin used in packaging containers. Therefore, in the resinous tubular container described in Patent Document 1, in order to reduce the amount of resin, for example, it is considered to make the film constituting the main body thinner.

[0010] However, when only the membrane constituting the main body is thinned, the rigidity of the main body weakens and the self-supporting ability of the container decreases.

[0011] Therefore, the purpose of this disclosure is to provide a tubular container that reduces the amount of resin used compared to the conventional one, and has the rigidity required for the self-supporting function of the container.

[0012] Methods for solving problems

[0013] The tubular container disclosed herein is a tubular container comprising: a tubular main body closed at one end and an outlet portion installed at the other end of the main body, the main body being formed of a paper-based material.

[0014] Effects of the present invention

[0015] According to this disclosure, a tubular container can be provided that reduces the amount of resin used compared to the conventional one, and has the rigidity required for the container's self-support. Attached Figure Description

[0016] [ Figure 1 ] Figure 1This is a front view showing a schematic configuration of the tubular container according to the first embodiment.

[0017] [ Figure 2 ] Figure 2 yes Figure 1 The diagram shows a three-dimensional view of the injection port.

[0018] [ Figure 3 ] Figure 3 It is along Figure 2 The end view of line III-III is shown.

[0019] [ Figure 4 ] Figure 4 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0020] [ Figure 5 ] Figure 5 This is a perspective view showing a schematic configuration of the paper tubular container according to the embodiment.

[0021] [ Figure 6 ] Figure 6 It is along Figure 5 The enlarged cross-sectional view of line VI-VI shown.

[0022] [ Figure 7 ] Figure 7 This is a diagram showing an example of a sheet material that constitutes the cylindrical and flat sections.

[0023] [ Figure 8 ] Figure 8 This is a diagram showing an example of a sheet material that constitutes the main body.

[0024] [ Figure 9A ] Figure 9A This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0025] [ Figure 9B ] Figure 9B This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0026] [ Figure 9C ] Figure 9C This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0027] [ Figure 9D ] Figure 9D This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0028] [ Figure 9E ] Figure 9E This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0029] [ Figure 9F ] Figure 9F This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0030] [ Figure 9G ] Figure 9G This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0031] [ Figure 9H ] Figure 9H This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0032] [ Figure 9I ] Figure 9I This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container.

[0033] [ Figure 10A ] Figure 10A This is a schematic diagram illustrating an example of a method for manufacturing a cap.

[0034] [ Figure 10B ] Figure 10B This is a schematic diagram illustrating an example of a method for manufacturing a cap.

[0035] [ Figure 10C ] Figure 10C This is a schematic diagram illustrating an example of a method for manufacturing a cap.

[0036] [ Figure 10D ] Figure 10D This is a schematic diagram illustrating an example of a method for manufacturing a cap.

[0037] [ Figure 11 ] Figure 11 This is a perspective view illustrating a schematic configuration of the tubular container according to the embodiment.

[0038] [ Figure 12 ] Figure 12 It is along Figure 11 The cross-sectional view of line XII-XII shown.

[0039] [ Figure 13 ] Figure 13 It is along Figure 11 The cross-sectional view of line XIII-XIII shown.

[0040] [ Figure 14 ] Figure 14 It is along Figure 11 The cross-sectional view of line XIV-XIV shown.

[0041] [ Figure 15 ] Figure 15This is a cross-sectional view showing an example of the layered structure of the sheet material constituting the main body of the tubular container.

[0042] [ Figure 16 ] Figure 16 This is a top view of the sheet material that makes up the main body of the tubular container.

[0043] [ Figure 17A ] Figure 17A It is a cross-sectional view used to illustrate the manufacturing method of the main body of a tubular container.

[0044] [ Figure 17B ] Figure 17B It is a cross-sectional view used to illustrate the manufacturing method of the main body of a tubular container.

[0045] [ Figure 17C ] Figure 17C It is a cross-sectional view used to illustrate the manufacturing method of the main body of a tubular container.

[0046] [ Figure 17D ] Figure 17D It is a cross-sectional view used to illustrate the manufacturing method of the main body of a tubular container.

[0047] [ Figure 18A ] Figure 18A This diagram illustrates the welding method between the main body and the outlet of a tubular container.

[0048] [ Figure 18B ] Figure 18B This diagram illustrates the welding method between the main body and the outlet of a tubular container.

[0049] [ Figure 18C ] Figure 18C This diagram illustrates the welding method between the main body and the outlet of a tubular container.

[0050] [ Figure 19 ] Figure 19 This is a cross-sectional view showing the layered structure of the laminated sheets constituting the main body of the tubular container according to the fourth embodiment.

[0051] [ Figure 20 ] Figure 20 This is a top view showing the blank for forming the main body of the tubular container according to the fourth embodiment.

[0052] [ Figure 21 ] Figure 21 yes Figure 20 Enlarged cross-sectional view of line AA.

[0053] [ Figure 22 ] Figure 22(a) is an enlarged cross-sectional view orthogonal to the height direction of the main body of the tubular container according to the fourth embodiment. (b) is an enlarged cross-sectional view orthogonal to the height direction of the main body of the tubular container according to the modified example.

[0054] [ Figure 23 ] Figure 23 (a) is a front view of the first example of a tubular container using the main body of the tubular container according to the fourth embodiment. (b) is a side view of the first example of a tubular container using the main body of the tubular container according to the fourth embodiment.

[0055] [ Figure 24 ] Figure 24 yes Figure 23 (b) is an enlarged cross-sectional view of the BB line near the injection outlet.

[0056] [ Figure 25 ] Figure 25 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0057] [ Figure 26 ] Figure 26 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0058] [ Figure 27 ] Figure 27 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0059] [ Figure 28 ] Figure 28 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0060] [ Figure 29 ] Figure 29 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0061] [ Figure 30 ] Figure 30 This is a cross-sectional view of the main body of the tubular container.

[0062] [ Figure 31 ] Figure 31 This is a front view showing a schematic configuration of the tubular container according to the sixth embodiment.

[0063] [ Figure 32 ] Figure 32 It is along Figure 31 The end view of line XXXII-XXXII shown.

[0064] [ Figure 33 ] Figure 33This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0065] [ Figure 34 ] Figure 34 This diagram illustrates the state before the strip is attached to the main body.

[0066] [ Figure 35 ] Figure 35 This diagram illustrates the state before the strip is attached to the main body.

[0067] [ Figure 36 ] Figure 36 This diagram illustrates the state after the strip has been attached to the main body.

[0068] [ Figure 37 ] Figure 37 (a) is a front perspective view of the area near the other end of the main body and the injection port of the tubular container according to the seventh embodiment before the main body and the injection port are installed. (b) is a front perspective view of the area near the other end of the main body and the injection port of the tubular container according to the seventh embodiment with the other end of the main body folded at the periphery of the flange and welded.

[0069] [ Figure 38 ] Figure 38 (a) is a front view of the tubular container according to the seventh embodiment. (b) is a side view of the tubular container according to the seventh embodiment.

[0070] [ Figure 39 ] Figure 39 yes Figure 38 (b) is an enlarged cross-sectional view of the GG line near the injection outlet.

[0071] [ Figure 40 ] Figure 40 (a) is a top view of the tubular container according to the seventh embodiment. (b) is... Figure 40 (a) Enlarged cross-sectional view of the HH line.

[0072] [ Figure 41 ] Figure 41 (a) is Figure 37 (a) is a magnified front view near the other end of the main body of the tubular container. (b) is a view of... Figure 37 (a) is a magnified front view of the tubular container with the main body folded at the periphery of the flange, near the other end of the main body. (c) is... Figure 37 (b) A magnified front view of the other end of the main body of the tubular container.

[0073] [ Figure 42 ] Figure 42This is a cross-sectional view of the laminated sheets constituting the main body of the tubular container according to the seventh embodiment.

[0074] [ Figure 43 ] Figure 43 This is a front perspective view of an example of a mold used to form the first grid line and the second grid line in the main body of the tubular container according to the seventh embodiment.

[0075] [ Figure 44 ] Figure 44 This is a front view showing a schematic configuration of the tubular container according to the eighth embodiment.

[0076] [ Figure 45 ] Figure 45 It is along Figure 44 The cross-sectional view of the XLV-XLV line shown.

[0077] [ Figure 46 ] Figure 46 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container. Detailed Implementation

[0078] <First Implementation>

[0079] Figure 1 This is a front view illustrating a schematic configuration of the tubular container according to the first embodiment. Figure 2 yes Figure 1 The perspective view of the injection outlet shown. Figure 3 It is along Figure 2 The end view of line III-III shown. Figure 2 and Figure 3 The image shows the state before the main body is sealed to the injection port.

[0080] The tubular container 1100 includes a tubular main body 101 and an outlet 102 installed on the main body 101.

[0081] The main body 101 is a component for containing contents, formed by shaping a sheet having a pair of generally parallel end edges into a cylindrical shape. The main body 101 is formed into a cylindrical shape, for example, by joining and welding the inner surfaces of strip-shaped portions comprising a pair of end edges of the sheet together in a palm-like manner. One end 105a of the main body 101 ( Figure 1 The lower end of the main body 101 is sealed and closed. On the other hand, the other end 105b of the main body 101 ( Figure 1The portion near the upper end of the membrane is sealed to the outside 108 of the flange 104 (described later) in a folded state. Multiple pleats 112, formed by folding the sheet constituting the main body 101, are formed at the weld between the main body 101 and the flange 104. The adhesive portion (backing portion) formed on the main body 101 by adhering the end edge of the membrane can be bent and adhered to the main body 101 along the outside of the main body 101. There is no particular limitation on the method of adhering the adhesive portion 107 to the main body 101, but the two can be welded together by a heat-sealing resin provided on the entire surface or a portion of the membrane constituting the main body 101, or by an adhesive such as hot melt adhesive. It should be noted that... Figure 1 The method of pasting the main body 101 shown is exemplary. Alternatively, the outer surface of a strip region containing one edge of the membrane constituting the main body 101 can be pasted together with the inner surface of a strip region containing the other edge of the membrane.

[0082] Figure 4 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0083] The main body 101 of the tubular container 1100 is composed of a sheet 141 primarily made of paper. The sheet 141 is a multilayer sheet, with a substrate film layer 133, a barrier layer 134, and a sealant layer 135 sequentially laminated on one side of the paper layer 132. A paper protective layer 137 is laminated on the other side of the paper layer 132, and further, an ink layer 138 and an outer varnish layer 139 are laminated on the paper protective layer 137. The details of each layer will be described below.

[0084] (Paper layer)

[0085] Paper layer 132 is a structural layer that imparts strength and rigidity to the tubular container 1100. There are no particular limitations on the type of paper constituting paper layer 132, but single-sided or double-sided kraft paper is preferred in terms of strength, flexural strength, and printability. Alternatively, water-resistant paper, oil-resistant paper, or paper cup base paper can be used as the paper constituting paper layer 132, depending on the requirements. Furthermore, paper layer 132 can be paper containing 50% or more pulp fibers (cellulose fibers), or it can be a blended paper containing resin fibers other than pulp fibers.

[0086] The weight per unit area of ​​the paper used for paper layer 132 is 30–300 g / m². 2 The preferred value is 50-120 g / m³. 2 The weight per unit area of ​​the paper used for paper layer 132 is less than 30 g / m². 2In this case, the rigidity of the main body 101 is insufficient. To compensate for the lack of rigidity, for example, it would be necessary to thicken the resin film disposed inside the paper layer 132, but this would lead to an increase in the resin content, which is undesirable in terms of reducing environmental impact. Furthermore, the weight per unit area of ​​the paper used for the paper layer 132 exceeds 300 g / m². 2 In such cases, the paper's rigidity and thermal insulation properties deteriorate, resulting in poor tube-making (bag-making), formability, and weldability, and manufacturing costs also increase, making it an undesirable option.

[0087] (Substrate film layer)

[0088] The substrate film layer 133 imparts physical strengths such as heat resistance and toughness to the sheet 141. The substrate film layer 133 also serves as the substrate for the barrier layer 134. There are no particular limitations on the material of the film constituting the substrate film layer 133, but from the viewpoint of heat resistance and physical strength, stretched films such as polypropylene, polyester, and polyamide are preferred. However, the substrate film layer 133 may also be made of paper.

[0089] (Barrier layer)

[0090] Barrier layer 134 is a functional layer that blocks oxygen and water vapor to improve the preservation of the contents. Barrier layer 134 can be composed of one or more of the following: an inorganic compound vapor-deposited film such as silica or alumina; a metal vapor-deposited film such as aluminum; a metal foil such as aluminum; or a coating containing a barrier coating agent comprising plate-like minerals and / or a barrier resin. The barrier resin used in the barrier coating agent can be ethylene-vinyl alcohol copolymer (EVOH) or polyvinylidene chloride (PVDC), and an adhesive resin other than the barrier resin can be appropriately incorporated into the barrier coating agent. Barrier layer 134 can be pre-laminated on substrate film layer 133 to form a barrier film, or it can be configured as a single-layer film.

[0091] (Sealant layer)

[0092] The material of the sealant layer 135 is not particularly limited, but thermoplastic resins such as polypropylene, polyethylene, cyclic polyolefins, and polyester are preferred. The sealant layer 135 uses a resin whose softening temperature is at least 20°C lower than that of the substrate film layer 133. If the softening temperature of the sealant layer 135 is not at least 20°C lower than that of the substrate film layer 133, the substrate film layer 133 is more likely to soften and develop pinholes during sealing, which is therefore undesirable. The softening temperature of the sealant layer 135 is preferably at least 40°C lower than that of the substrate film layer 133.

[0093] The thermoplastic resin used for the sealant layer 135 only needs to be adhesive to the thermoplastic resin constituting the injection port portion 102 described later, but it is preferably the same material as the thermoplastic resin used for the injection port portion 102. By using the same thermoplastic resin for the sealant layer 135 and the thermoplastic resin used for the injection port portion 102, the sealing strength between the main body portion 101 and the injection port portion 102 can be improved.

[0094] (Paper protective layer)

[0095] The paper protective layer 137 is a layer used to protect the paper layer 132 constituting the sheet 141 from the adhesion of contents and dirt. There are no particular limitations on the material and formation method of the paper protective layer 137; it can be laminated by extrusion coating of a thermoplastic resin, coating with a water-resistant agent, or an oil-resistant agent. The thickness of the paper protective layer 137 is preferably 0.2 to 50 μm, more preferably 1 to 20 μm. If the thickness of the paper protective layer 137 is less than 0.2 μm, pinholes may occur in the paper protective layer 137, and the protection of the paper layer 132 may become insufficient. Furthermore, if the thickness of the paper protective layer 137 exceeds 50 μm, it is not preferable from the perspective of resin usage and manufacturing cost.

[0096] (Ink layer, outer varnish layer)

[0097] The ink layer 138 is a layer applied by printing for various displays, and the outer varnish layer 139 is a layer used to impart abrasion resistance, etc. The stacking order of the ink layer 138 and the outer varnish layer can be... Figure 4 The opposite of the above. In addition, the outer varnish layer 139 can also serve as a paper protective layer 137.

[0098] The thickness (total thickness) of the sheet 141 constituting the main body 101 is not particularly limited, but is preferably 30 to 300 μm. If the thickness of the film constituting the main body 101 is within this range, the main body 101 can be easily processed into a cylindrical shape using a bag-making machine, a pillow / core packaging machine, or the like. In addition, since the paper layer 132 imparts strength and rigidity, it can be thinner than a typical laminated tube (thickness 300 to 500 μm), and the amount of resin used can also be reduced.

[0099] In order to reduce the resin content of the sheet 141 constituting the main body 101, the proportion of the paper layer 132 in the mass of the sheet 141 is preferably 50% or more. From the viewpoint of reducing the amount of resin used, the higher the proportion of the paper layer 132, the more preferred.

[0100] It should be noted that the sheet constituting the main body 101 may be a sheet in which a sealant layer 135 is laminated on at least one surface side of the paper layer 132 (the surface side that serves as the inner side of the tubular container 1100), or one or more of the aforementioned substrate film layer 133, barrier layer 134, paper protective layer 137, ink layer 138, and outer coating varnish layer 139 may be omitted.

[0101] Refer again Figures 1-3 The outlet portion 102 is a nozzle for removing the contents contained in the main body portion 101 to the outside, and includes a cylindrical outlet portion 103 and a flange portion 104. The flange portion 104 is connected to one end 106a of the outlet portion 103. Figure 1 The flange 104 is a flat plate-shaped portion that connects to and extends outside the dispensing cylinder 103 from the lower end of the flange. In this embodiment, the flange 104 is positioned in a direction orthogonal to the axial direction of the dispensing cylinder 103. Figure 1 It is formed by extending in the left-right direction. In this embodiment, the flange portion 104 is formed in a ring shape, but as long as it can be joined with the main body portion 101, the shape of the flange portion 104 is not limited, and it can be elliptical, oblong, track-shaped, polygonal, etc.

[0102] The injection port 102 is molded from a material comprising a thermoplastic resin and fillers other than the resin. The thermoplastic resin used as the material for the injection port 102 can be, for example, any one of polyethylene, polypropylene, polyester, polyamide, and cyclic polyolefins, or a combination of two or more. The filler can be any one of talc, kaolin, paper flour, and cellulose fibers, or a combination of two or more. By using a mixture of thermoplastic resin and fillers other than the resin as the material for the injection port 102, the amount of resin used can be reduced while maintaining moldability and heat-welding properties to the sheet of the main body 101. There are no particular limitations on the molding method for the injection port 102; existing molding methods such as extrusion molding, vacuum forming / hot plate pressurized air forming, and compression molding can be used.

[0103] like Figure 2 and Figure 3As shown, an annular protrusion 109 and a recess 110 are provided on the outer surface 108 of the flange portion 104 (the surface on the side of the end 106b of the injection cylinder portion 103). When the main body portion 101 is fused to the flange portion 104 of the injection outlet portion 102, the protrusion 109 melts first, and the molten resin spreads between the inner surface of the main body portion 101 and the flange portion 104. In addition, a portion of the molten resin flows into the recess 110. As a result, the resin molten through the protrusion 109 can fuse the inner surface of the main body portion 101 to the outer surface 108 of the flange portion 104 in a surface manner, thereby improving the weld strength. The injection outlet portion 102 according to this embodiment contains fillers other than resin, and the weld strength between the main body portion 101 and the injection outlet portion 102 is prone to decrease, but by providing the protrusion 109 and the recess 110, the necessary weld strength can be ensured. There is no particular limitation on the number of protrusions 109 and recesses 110, and there can be more than two. Furthermore, the number of protrusions 109 and recesses can be different; for example, two recesses 110 can be provided on the inner and outer sides of one protrusion 109. Alternatively, recesses 110 may not be provided.

[0104] The height of the protrusion 109 (the height from the outer surface 108 of the flange portion 104) is set to 0.05 to 2 mm, more preferably 0.1 to 1 mm. When the height of the protrusion 109 is less than 0.05 mm, the effect of improving the weld strength cannot be obtained. On the other hand, when the height of the protrusion 109 exceeds 2 mm, the protrusion 109 does not melt when welding the main body portion 101, and remains on the outer surface 108 of the flange portion 104 as a height difference, resulting in leakage of contents.

[0105] The depth of the recess 110 (the depth from the outer surface 108 of the flange portion 104) is set to 0-2 mm, preferably 0-1 mm. If the protrusion 109 is low, the recess 110 may not be present. Furthermore, if the depth of the recess 110 exceeds 2 mm, the strength of the flange portion 104 decreases, and the appearance after welding the main body portion 101 deteriorates, therefore this is not preferred.

[0106] As a method for welding the main body 101 and the outlet 102 when manufacturing the tubular container 1100, ultrasonic welding, high-frequency welding, heat sealing welding, hot air welding, and pressing of the main body insert can be used. However, in terms of being less affected by the thermal insulation properties of the paper, ultrasonic welding is preferred.

[0107] When the length of the tubular container 1100 is set to L and the diameter to D, the L / D ratio is preferably set in the range of 1 to 10, and more preferably in the range of 1.5 to 8. Here, for example... Figure 1As shown, the pipe length L is the axial length from the point where it is welded to the flange 104 to the end 105a. Regarding the pipe diameter D, when the flange 104 is circular, it is the diameter of the flange 104; when the flange 104 is elliptical, it is (A+B) / 2 (where A is the major axis of the ellipse and B is the minor axis). When the value of L / D is less than 1, the pipe length L is too short relative to the pipe diameter D, and the shape of the tubular container 1100 is unsuitable for packaging. On the other hand, when the value of L / D exceeds 10, the pipe length L is too long relative to the pipe diameter D, thus deteriorating the appearance of the tubular container 1100, and its shape is unsuitable for packaging.

[0108] like Figure 1 As shown, the tubular container 1100 may further include a screw cap 111, which can be attached to and removed from the dispensing cylinder 103 of the dispensing port 102 via threads. With the screw cap 111, the tubular container 1100 can be easily resealed after being opened.

[0109] Alternatively, the tubular container 1100 can also have a hinged cap instead of the screw cap 111. With a hinged cap, it can be connected via a threaded connection. Figure 1 The hinge cover is mounted on the injection outlet portion 102 on the injection cylinder portion 103 shown. Alternatively, ribs can be provided on the outside of the injection cylinder portion 103 instead of screw threads, and the hinge cover can be mounted on the injection outlet portion 102 by embedding the ribs.

[0110] In addition, the end 106b of the dispensing tube 103 can be sealed with a membrane, which seals the dispensing tube 103 when the tubular container 1100 is unopened.

[0111] Furthermore, in order to keep the interior of the tubular container 1100 sealed when unopened, the interior of the dispensing cylinder 103 can be sealed by a partition wall. When a partition wall is provided, it is preferable to have a circular half-cut along the inner circumference of the dispensing cylinder 103, and a pull ring connected to the portion surrounded by the half-cut. With this configuration, when the tubular container 1100 is opened, the user pulls the pull ring to break off a portion of the half-cut 127 of the partition wall, thereby removing a portion of the partition wall surrounded by the half-cut, thus forming an opening for dispensing the contents from the main body 101 into the dispensing cylinder 103.

[0112] As described above, in this embodiment, the main body 101 is composed of a sheet containing paper and a sealant, and the injection port 102 is molded from a material containing thermoplastic resin and fillers other than resin. The paper constitutes the largest proportion of the total mass of the materials constituting the main body 101 and the injection port 102. In conventional resin-based tubular containers, simply thinning the resin layer of the sheet constituting the main body results in insufficient rigidity of the main body, reducing the self-standing and operability of the tubular container. In contrast, in this embodiment, by using paper as the structural material of the main body 101, the amount of resin used can be reduced, and the main body 101 can be given rigidity. Furthermore, by incorporating fillers other than resin into the molding material of the injection port 102, the amount of resin used in the tubular container 1100 can also be reduced. Therefore, according to this embodiment, a tubular container 1100 that reduces the amount of resin used compared to the conventional method and possesses the rigidity required for container self-standing and operability can be achieved. Additionally, the paper used for the main body 101 has a unit area weight of 300 g / m². 2 Therefore, the following operations can be performed without problems: rolling during the formation of the main body 101, welding of the adhesive portion 107, folding near the end 105b of the main body 101 when the main body 101 is installed on the injection outlet portion 102, welding of the end 105b of the main body 101 to the flange portion 104, and the formability of the processing device is good.

[0113] Furthermore, in the tubular container 1100 of this embodiment, the flange 104 has a flat plate shape orthogonal to the central axis of the dispensing cylinder 103. Since the main body 101 is fused to the outer surface 108 of the flange 104, when the contents of the tubular container 1100 are small, the contents can be easily squeezed out by folding the main body 101 along the outer periphery of the flange 104. In addition, since the flange 104 is flat, it does not form a space for residual contents. Therefore, by bending the main body 101 along the outer periphery of the flange 104, the flange 104 and the main body 101 become almost flat, thereby allowing the contents to be squeezed out without residue.

[0114] The tubular container involved in this embodiment is described below.

[0115] [1] A tubular container, comprising:

[0116] A tubular main body consisting of a sheet of paper and sealant, closed at one end; and

[0117] The injection port is made of a material comprising thermoplastic resin and filler composed of materials other than resin, and is installed at the other end of the main body.

[0118] The paper has a unit area weight of 30-300 g / m². 2 ,

[0119] Of the total mass of the materials constituting the main body and the injection port, paper accounts for the highest proportion by mass.

[0120] [2] The tubular container described in Project [1]

[0121] The thermoplastic resin constituting the injection port is selected from at least one of polyethylene, polypropylene, polyester, polyamide, and cyclic polyolefins.

[0122] The filler is selected from at least one of calcium carbonate, talc, kaolin, paper flour, and cellulose fiber.

[0123] [3] The tubular container as described in item [1] or [2]

[0124] The thermoplastic resin constituting the main body and the sealant of the sheet constituting the main body are the same material.

[0125] [4] The tubular container according to any one of items [1] to [3],

[0126] The injection outlet section has:

[0127] The cylindrical injection tube and

[0128] A flat flange portion is connected to one end of the injection cylinder portion and extends outside the injection cylinder portion in a direction orthogonal to the axial direction of the injection cylinder portion.

[0129] The inner surface near the other end of the main body is joined to the other end side of the injection cylinder, one of the two sides of the flange.

[0130] <Second Implementation Method>

[0131] To date, tubular containers using paper as a material have not been adequately studied. For example, since the main body of a tubular container is made of sheet material, it can be considered to be made of sheet material mainly composed of paper. However, when the shoulder (nozzle part) is made of plastic, the proportion of plastic shown in the tubular container increases, and it is discarded in the form of plastic, making it difficult to reuse as a paper resource.

[0132] This embodiment provides a paper tubular container formed from a paper-based sheet, which reduces the amount of resin used compared to the past.

[0133] Figure 5 This is a perspective view illustrating a schematic configuration of the paper tubular container according to the embodiment. Figure 6 It is along Figure 5 The enlarged cross-sectional view of line VI-VI shown.

[0134] The paper tubular container 2100 includes a cylindrical portion 201, a flat portion 202, and a main body portion 203. The cylindrical portion 201, the flat portion 202, and the main body portion 203 are all formed from a sheet of paper.

[0135] The cylindrical portion 201 is a component used to dispense the contents contained in the main body portion 203 to the outside, and has a cylindrical shape. For example... Figure 6 As shown, in the axial direction of the cylindrical section 201 ( Figure 6 A flange 206 is provided at one end 205a (vertical direction) and an outer peripheral portion 207 is provided at the other end 205b. Details will be described later, but the flange 206 can be formed by rolling a blank for forming the cylindrical portion 201 into a cylindrical shape, rolling it outwards from one open end (end edge) within a predetermined range, and then flattening the formed rolled portion along the vertical direction. The flange 206 is used to seal the flat plate portion 202. The outer peripheral portion 207 can be formed by rolling the blank for forming the cylindrical portion 201 outwards from the other open end (end edge) within a predetermined range, and then flattening the formed rolled portion along the outer peripheral surface of the cylindrical portion 201. The outer peripheral portion 207 is used to protect the end face of the blank (sheet) forming the cylindrical portion 201 and to provide strength to the end 205b of the cylindrical portion 201. Additionally, as... Figure 5 As shown, an adhesive portion 208 is formed in the cylindrical portion 201, which is formed by overlapping and sealing near a pair of end edges of the blank after rolling during the formation of the cylindrical portion 201. The shape of the cylindrical portion 201 is not particularly limited, and can be circular, elliptical, oblong, track-shaped, polygonal, etc.

[0136] If the contents of the paper tubular container 2100 do not easily permeate the paper, the outer peripheral portion 207 may not be provided at the end 205b of the cylindrical portion 201. Alternatively, depending on the type and shape of the contents, instead of providing the outer peripheral portion 207 at the end 205b of the cylindrical portion 201, the blank used to form the cylindrical portion 201 can be rolled inward within a predetermined range from the open end (end edge) of the blank, and then the rolled portion can be flattened along the inner peripheral surface of the cylindrical portion 201.

[0137] The flat plate portion 202 is a flat plate-shaped component used to connect the cylindrical portion 201 and the main body portion 203. The flat plate portion 202 has an opening 210 with a cross-sectional shape approximately the same as that of the cylindrical portion 201, and the flat plate portion 202 is generally annular. The opening 210 of the flat plate portion 202 is inserted in such a way that the cylindrical portion 201 passes through it, and one surface 211a of the flat plate portion 202 facing the flange 206 is sealed by the flange 206 of the cylindrical portion 201. Furthermore, by folding back the annular portion including the entire outer periphery of the blank used to form the flat plate portion 202 towards the surface 211b, a folded-back portion 212 is formed on the outer periphery of the flat plate portion 202. The shape of the flat plate portion 202 is not particularly limited, as long as it can seal the main body portion 203; it can be circular, elliptical, oblong, track-shaped, polygonal, etc.

[0138] The nozzle is formed by integrating the cylindrical part 201 and the flat part 202 via the flange 206. By forming both the cylindrical part 201 and the flat part 202 from a sheet material mainly composed of paper, the amount of resin used can be reduced compared to conventional resin-based nozzles.

[0139] The main body 203 is a component for containing contents and can be formed by shaping a sheet having a pair of generally parallel end edges into a cylindrical shape. The main body 203 is formed into a cylindrical shape, for example, by joining and welding the inner surfaces of strip-shaped portions comprising a pair of end edges of a long strip of sheet together in a palm-like manner. One end 214a of the main body 203 ( Figure 5 The lower end of the main body 203 is sealed and closed. On the other hand, the other end 214b of the main body 203 ( Figure 5 The portion near the upper end of the main body 201 is sealed to the outside of the flat plate 202 in a folded state (i.e., the surface 211b on the side of the end 205b of the main body 201, which is one of the two sides of the flat plate 202). Multiple pleats 216 formed by folding the sheet constituting the main body 203 are formed on the outside of the flat plate 202. In addition, the main body 203 is formed with an adhesive portion 215, which is formed by overlapping and bonding the portions near the end edges of the sheet when it is processed into a cylindrical shape. The adhesive portion 215 is bent along the outside of the main body 203 and bonded to the main body 203. There is no particular limitation on the method of bonding the adhesive portion 215 to the main body 203. The two can be fused together by a heat-sealing resin provided on the entire surface or a part of the film constituting the main body 203, or by an adhesive such as hot melt adhesive.

[0140] like Figure 5 and Figure 6 As shown, the paper tubular container 2100 may further include a cover 204 that can be installed on and removed from the cylindrical portion 201. When the paper tubular container 2100 is equipped with the cover 204, it is easy to reseal the paper tubular container 2100 after it has been opened.

[0141] The cover 204 according to this embodiment includes a cylindrical portion 220 and a cover portion 221. Both the cylindrical portion 220 and the cover portion 221 are formed of a sheet material mainly composed of paper.

[0142] The cylindrical portion 220 is a component forming the peripheral wall of the cover 204 and has a cylindrical shape. In the axial direction of the cylindrical portion 220 ( Figure 5 and Figure 6 The cylindrical portion 220 has a connecting portion 223 at one end 222a (vertical direction) and an inner peripheral portion 224 at the other end 222b. Details will be described later, but the connecting portion 223 can be formed by rolling the blank for forming the cylindrical portion 220 into a cylindrical shape, curling it inward from one open end (end edge) within a predetermined range, and then flattening the formed curled portion along the vertical direction. The connecting portion 223 is used to seal the cover portion 221. The inner peripheral portion 224 can be formed by rolling the blank for forming the cylindrical portion 220 into a cylindrical shape, curling it inward from the other open end (end edge) within a predetermined range, and then flattening the formed curled portion along the inner peripheral surface of the cylindrical portion 220. The inner peripheral portion 224 is used to protect the end face of the blank (sheet) for forming the cylindrical portion 220 and to provide strength to the end 222b of the cylindrical portion 220. As described in this embodiment, when an outer peripheral portion 207 is formed at the end 205b of the cylindrical portion 220, by making the inner diameter of the inner peripheral portion 224 smaller than the outermost diameter of the outer peripheral portion 207, a locking mechanism that prevents the cover 204 from falling off at the inner peripheral portion 224 and the outer peripheral portion 207 can be functioned. Furthermore, as... Figure 5 As shown, an adhesive portion 225 is formed in the cylindrical portion 220, which is formed by overlapping and sealing a pair of end edges of the rolled blank during the formation of the cylindrical portion 220. The shape of the cylindrical portion 220 is not particularly limited and can be circular, elliptical, oblong, track-shaped, polygonal, etc. The cylindrical portion 220 is formed in a shape corresponding to the cylindrical portion 201.

[0143] If the contents of the paper tubular container 2100 are not easily permeable to the paper, the inner periphery 224 may not be provided at the end 222b of the lid 204. Alternatively, depending on the type and shape of the contents, instead of providing the inner periphery 224 on the inner periphery 224 of the lid 204, the blank used to form the cylindrical portion 220 can be rolled outward from the open end (end edge) within a predetermined range, and then the rolled portion can be flattened along the outer periphery of the cylindrical portion 220.

[0144] The cover 221 is a flat plate that is embedded inside the cylindrical portion 220 and closes the end 222a of the cylindrical portion 220. The cover 221 is sealed by a connecting portion 223 provided at the end 222a of the cylindrical portion 220.

[0145] It should be noted that the cap 204 is arbitrary; the paper tubular container 2100 may not have a cap 204. Furthermore, when the paper tubular container 2100 is unopened, the top sealing material of the closed cylindrical portion 201 can also be sealed by the end 205b of the cylindrical portion 201. The composition of the top sealing material is not particularly limited, but it is preferable to have at least a barrier layer and a sealant layer. The sealant layer of the top sealing material preferably has easy-peel properties, allowing the top sealing material to be easily peeled off from the end 205b of the cylindrical portion 201.

[0146] Figure 7 This is a diagram showing an example of a sheet material that constitutes the cylindrical and flat sections. Figure 8 This is a diagram showing an example of a sheet material that constitutes the main body.

[0147] As an example, the cylindrical portion 201 and the flat portion 202 involved in this embodiment are composed of Figure 7 The sheet 231 shown is formed, and the main body 203 is made of Figure 8 The sheet 241 shown is formed.

[0148] Sheet 231 is a multilayer sheet, wherein a substrate film layer 233, a barrier layer 234, and a sealant layer 235 are sequentially laminated on one side of paper layer 232, and a thermoplastic resin layer 236 is laminated on the other side of paper layer 232. Sheet 241 is also a multilayer sheet, wherein a substrate film layer 233, a barrier layer 234, and a sealant layer 235 are sequentially laminated on one side of paper layer 232, a paper protective layer 237 is laminated on the other side of paper layer 232, and further, an ink layer 238 and an outer varnish layer 239 are laminated on the paper protective layer 237. The details of each layer are described below.

[0149] (Paper layer)

[0150] Paper layer 232 is a structural layer that provides strength to the paper tubular container 2100. There are no particular limitations on the type of paper constituting paper layer 232, but single-sided or double-sided kraft paper is preferred in terms of strength, flexural strength, and printability. Furthermore, water-resistant or oil-resistant paper can be used as the paper constituting paper layer 232, depending on the requirements.

[0151] The weight per unit area of ​​the paper used to form the sheet of tube 201 is 50 to 500 g / m². 2 The preferred concentration is 100–300 g / m³. 2 The weight per unit area of ​​the paper used for forming the sheet of tube 201 is less than 50 g / m². 2 In such cases, the curled portion described later cannot be formed, and the strength of the formed tube 201 is insufficient. Furthermore, if the weight per unit area of ​​the paper used for forming the tube 201 exceeds 500 g / m²...2 In such cases, the curled portion described later is difficult to form, which is also undesirable in terms of saving resources and manufacturing costs.

[0152] The weight per unit area of ​​the paper used to form the sheet material constituting the flat section 202 is 50 to 1000 g / m². 2 The preferred concentration is 100–300 g / m³. 2 The weight per unit area of ​​the paper used for forming the sheet in the flat section 202 is less than 50 g / m². 2 In such cases, the paper tubular container 2100 lacks sufficient strength. The weight per unit area of ​​the paper used for forming the sheet of the flat section 202 exceeds 1000 g / m². 2 In some cases, the vibrations during ultrasonic sealing are absorbed by the paper, preventing proper welding, which is undesirable in terms of resource conservation and manufacturing costs.

[0153] The weight per unit area of ​​the paper used to form the sheet of the main body 203 is 30 to 200 g / m². 2 The preferred value is 50-120 g / m³. 2 The weight per unit area of ​​the paper used for forming the sheet of the main body 203 is less than 30 g / m². 2 In this case, the rigidity of the main body 203 is insufficient. To compensate for the lack of rigidity, for example, it would be necessary to thicken the resin film disposed inside the paper layer 232, but this would lead to an increase in the resin content, which is undesirable in terms of reducing environmental impact. Furthermore, the weight per unit area of ​​the paper used in the sheet for forming the main body 203 exceeds 200 g / m². 2 In such cases, the paper's rigidity and thermal insulation properties, as well as its tube-making (bag-making), formability, and weldability, deteriorate, making it unsuitable for use.

[0154] The substrate film layer 233 imparts physical strength, such as heat resistance and toughness during heating, to the sheets 231 and 232. The substrate film layer 233 also serves as the substrate for the barrier layer 234. There are no particular limitations on the material of the film constituting the substrate film layer 233, but from the viewpoint of heat resistance and physical strength, stretched films such as polypropylene, polyester, and polyamide are preferred. However, the substrate film layer 233 may also be made of paper.

[0155] (Barrier layer)

[0156] Barrier layer 234 is a functional layer that blocks oxygen and water vapor to improve the preservation of the contents. Barrier layer 234 can be composed of one or more of the following: an inorganic compound vapor-deposited film such as silica or alumina; a metal vapor-deposited film such as aluminum; a metal foil such as aluminum; or a coating containing a barrier coating agent comprising plate-like minerals and / or a barrier resin. The barrier resin used in the barrier coating agent can be ethylene-vinyl alcohol copolymer (EVOH) or polyvinylidene chloride (PVDC), and an adhesive resin other than the barrier resin can be appropriately incorporated into the barrier coating agent. Barrier layer 234 can be pre-laminated on substrate film layer 233 to form a barrier film, or it can be configured as a single-layer film.

[0157] (Sealant layer)

[0158] The material of the sealant layer 235 is not particularly limited, but thermoplastic resins such as polypropylene, polyethylene, cyclic polyolefins, and polyester are preferred. The sealant layer 235 uses a resin whose softening temperature is at least 20°C higher than that of the substrate film layer 233. If the softening temperature of the sealant layer 235 is not at least 20°C higher than that of the substrate film layer 233, the substrate film layer 233 is more likely to soften and develop pinholes during sealing, which is therefore undesirable. The softening temperature of the sealant layer 235 is preferably at least 40°C higher than that of the substrate film layer 233.

[0159] (Thermoplastic resin layer)

[0160] The thermoplastic resin layer 236 is formed by laminating or coating a thermoplastic resin that can fuse with the resin constituting the sealant layer 235. The thermoplastic resin layer 236 can be laminated over the entire surface of the paper layer 232 or partially laminated over the surface of the paper layer 232. By laminating the thermoplastic resin layer 236, the welding of the curled portion during the curling process described later can be strengthened, the welding of the surface 211b of the flat portion 202 and the main body portion 203 can be strengthened, or the folded portion 212 of the flat portion 202 can be welded.

[0161] (Paper protective layer)

[0162] The paper protective layer 237 is a layer used to protect the paper layer 232 constituting the sheet 241 from the adhesion of contents and dirt. There are no particular limitations on the material and formation method of the paper protective layer 237, but it can be laminated by extrusion coating of a thermoplastic resin, coating with a water-resistant agent, or an oil-resistant agent. The thickness of the paper protective layer 237 is preferably 0.2 to 50 μm, more preferably 1 to 20 μm. If the thickness of the paper protective layer 237 is less than 0.2 μm, pinholes may occur in the paper protective layer 237, and sufficient paper protection may not be obtained. Furthermore, if the thickness of the paper protective layer 237 exceeds 50 μm, it is not preferable from the perspective of resin usage and manufacturing cost.

[0163] (Ink layer, outer varnish layer)

[0164] The ink layer 238 is a layer applied by printing to achieve various displays, and the outer varnish layer 239 is a layer used to impart abrasion resistance, etc. The stacking order of the ink layer 238 and the outer varnish layer can be... Figure 8 The opposite of the above. In addition, the outer varnish layer 239 can also serve as a paper protective layer 237.

[0165] To reduce the resin content of the sheets constituting the cylindrical section 201, the flat section 202, and the main body section 203, the proportion of paper layer 232 in the mass of each sheet is preferably 50% or more. From the viewpoint of reducing the amount of resin used, a higher proportion of paper layer 232 is preferred. However, if paper accounts for 50% or more of the total mass of paper and resin constituting the paper tubular container 2100, the proportion of paper layer 232 in any sheet constituting the cylindrical section 201, the flat section 202, and the main body section 203 can be less than 50%.

[0166] It should be noted that the sheets constituting the cylindrical portion 201 and the flat portion 202 may be sheets in which a sealant layer 235 is laminated on at least one side of the paper layer 232 (the side that serves as the inner side of the paper tubular container 2100), or one or more of the aforementioned substrate film layer 233, barrier layer 234, and thermoplastic resin layer 236 may be omitted. Furthermore, the sheets constituting the cylindrical portion 201 and the flat portion 202 may also be appropriately coated with a coating agent for imparting water or oil resistance, for display printing, or for applying an external varnish for printing protection.

[0167] Hereinafter, an example of a method for manufacturing the paper tubular container 2100 according to this embodiment will be described.

[0168] Figures 9A to 9I This is a schematic diagram illustrating an example of a method for manufacturing a paper tubular container. It should be noted that... Figure 9E In the following attached figures, through comparison with... Figure 6 The corresponding cross-section shows the container during the manufacturing process.

[0169] Figures 9A-9G The manufacturing process of a nozzle consisting of a cylindrical portion 201 and a flat portion 202 is shown.

[0170] like Figure 9A As shown, a blank 243 is prepared for forming the cylinder section 201. The blank 243 is, for example, formed by... Figure 7The sheet shown is cut into a rectangle. The portion within a predetermined range from a pair of end edges 244a and 244b of the blank 243 corresponds to the portion overlapped and glued while the blank 243 is rolled into a cylindrical shape. Additionally, the portion within a predetermined range from one end edge 245a of the blank 243 corresponds to the portion rolled for forming the flange 206, and the portion within a predetermined range from the other end edge 245b of the blank 243 corresponds to the portion rolled for forming the flange 206. It should be noted that... Figure 9A The side closest to itself becomes the outer side of the tube 201.

[0171] Next, as Figure 9B As shown, the strip portion 246a including the end edge 244a of the blank 243 and the strip portion 246b including the end edge 244b are folded back in opposite directions (edge ​​folding process).

[0172] Next, as Figure 9C As shown, the blank that has undergone edge folding is rolled into a cylindrical shape, and the folded-back strip portions 246a and 46b are engaged, such that portions (i.e., strip portions 246a and 46b) located within a predetermined range from a pair of end edges 244a and 244b overlap and seal. This forms... Figure 9D The cylindrical intermediate body 247 is shown. The intermediate body 247 has an adhesive portion 208 formed by overlapping and sealing the strip portions 246a and 46b. In this example, in the adhesive portion 208, the blank 243's " "It is formed by stacking and sealing four layers. However, the adhesive portion 208 can also be formed by sealing the overlapping portion without overlapping the strip portions 246a and 46b, i.e., by rolling up the blank 243 so that the end edges 244a and 244b are joined together, or by separating the end edges 244a and 244b. In this case, the sheet of blank 243 is stacked in three layers. Regardless of which method is used to form the adhesive portion 208, the end edges 244a and 244b of blank 243 are folded in and sealed inside the adhesive portion, thereby protecting the end faces of the sheet of end edges 244a and 244b."

[0173] Next, by curling both the portion of the intermediate body 247 from one end edge 245a within a predetermined range and the portion from the other end edge 245b within a predetermined range outwards, a shape is formed as shown below. Figure 9E The intermediate body 249 shown has curled portions 248a and 48b. In this process, the end edges 245a and 245b of the intermediate body 247 are rolled into the interior of the curled portions 248a and 48b. It should be noted that the curled portions 248a and 48b can be formed by a known processing method using a mold.

[0174] Next, by curling the intermediate 249 along the axial direction ( Figure 9E Flatten the coiled portion 248b along the outer periphery of the intermediate body 247 (in the vertical direction), and flatten the coiled portion 248b along the outer periphery of the intermediate body 247 to form a shape like... Figure 9F The cylindrical portion 201 shown has a flange 206 and an outer peripheral portion 207. The flattening of the curled portions 248a and 48b can be performed, for example, by applying pressure while simultaneously applying ultrasonic waves using an ultrasonic welding head. Figure 9F In the process shown, when the curled portions 248a and 48b are flattened, Figure 9F The end edges 245a and 245b of the intermediate body 247 shown are respectively rolled into the interior of the flange 206 and the outer peripheral portion 207 and sealed, thereby protecting the end faces of the sheet material of the end edges 245a and 245b. It should be noted that, without affecting the processability of subsequent processes, the process of flattening one or both of the rolled portions 248a and 248b can be omitted, and can be incorporated into the embedding process described later. Figure 9G In the sealing process of the flat plate portion 202 shown, or in a subsequent process, one or both of the curled portions 248a and 48b can be flattened.

[0175] On the other hand, apart from the tube section 201, the manufacturing... Figure 9G The flat plate portion 202 is represented by a dashed line. The flat plate portion 202 can be, for example, made by... Figure 7 The sheet material is punched into a predetermined shape, and the annular portion, including the entire outer periphery, is folded back towards surface 211b to form a folded-back portion 212. It should be noted that an opening 210, with a cross-sectional shape approximately the same as that of the intermediate body 250 (cylindrical portion 201), is formed on the punched sheet during the punching process or through other steps. Furthermore, the overall dimensions of the punched sheet are set such that the cross-sectional dimensions of the main body 203 are just larger than the folded-back portion 212.

[0176] Next, the cylindrical portion 201 is inserted into the opening 210 of the flat portion 202, as follows. Figure 9G As shown, the flange 206 of the cylindrical portion 201 is brought into contact with the surface 211a of the flat portion 202, and the flange 206 and the surface 211a of the flat portion 202 are sealed. Through this process, a nozzle integrating the cylindrical portion 201 and the flat portion 202 can be obtained.

[0177] Since both the cylindrical section 201 and the flat section 202 are formed bodies of sheet material mainly composed of paper, therefore... Figure 9G In the illustrated process, the portion near the end 205b of the cylindrical portion 201 and / or the portion near the opening 210 of the flat plate portion 202 can be deformed, allowing the cylindrical portion 201 to be inserted into the opening 210 of the flat plate portion 202. However, to facilitate the insertion of the cylindrical portion 201 into the flat plate portion 202, this process can be omitted. Figure 9E The formation of the curled portion 248b shown and Figure 9F The flattening of the curled portion 248b shown is not performed by sealing the flat portion 202 to the flange 206. Instead, the curled portion 248b is formed and flattened afterward.

[0178] Figure 9H and 9I The manufacturing process of a paper tubular container 2100 formed by sealing the main body 203 to the flat plate 202 is shown.

[0179] Main body 203, for example, by using Figure 8 The sheet shown is formed by joining and welding the inner surfaces of strip-shaped portions, each including a pair of end edges of the sheet, together in a palm-like manner. In this embodiment, a sheet with a thickness (total thickness) of 30 to 300 μm is used as the sheet for forming the main body 203, so it can be processed into a cylindrical shape using a bag-making machine, pillow / core packaging machine, etc.

[0180] like Figure 9H As shown, after the flat plate portion 202 is inserted from end 214b into the cylindrical main body portion 203, as... Figure 9I As shown, a portion of the main body 203 from its end 214b within a predetermined range is folded and sealed onto the surface 211b of the flat plate 202. At this time, the portion from the end 214b of the main body 203 is sealed along the entire inner circumference of the folded-back portion 212 and the surface 211b of the flat plate 202. Thus, the end face of the sheet forming the flat plate 202 is protected by being sealed inside the adhesive portion between the main body 203 and the flat plate 202. The main body 203 does not necessarily have to be sealed to the inner circumferential portion of the folded-back portion 212 of the flat plate 202; it may only be sealed to the folded-back portion 212. However, as shown in this embodiment, by sealing the main body 203 across the folded-back portion 212 and its inner circumferential portion, the weld between the main body 203 and the flat plate 202 can be strengthened.

[0181] Through the above processes, paper tubular containers 2100 can be manufactured.

[0182] Figures 10A to 10D This is a schematic diagram illustrating an example of a method for manufacturing a lid.

[0183] First, cut the paper-based sheet into rectangles to prepare the blank for forming the tube 220. For example, the blank for forming the tube 220 can be... Figure 7 The sheet shown. It is formed using a blank prepared for forming the cylindrical portion 220. Figures 9A-9C The process described herein forms and Figure 9C The same cylindrical intermediate body 250 shown (refer to) Figure 10AAn adhesive portion 225 is formed on the intermediate body 250 by overlapping and sealing portions of a pair of end edges of the blank within a predetermined range.

[0184] Next, by curling both the portion of the intermediate body 250 from a predetermined range at one end edge 251a and the portion from a predetermined range at the other end edge 251b inwards, the following is obtained: Figure 10B The intermediate body 253 shown has curled portions 252a and 52b. The curled portions 252a and 52b can be formed by a known processing method using a mold.

[0185] Next, as Figure 10C As shown, a separately manufactured cover 221 is embedded into the cylindrical portion of the intermediate body 253. The cover 221 can be, for example, made by... Figure 7 The sheet shown is formed by punching holes in a shape corresponding to the cover 204.

[0186] Next, the curled portion 252a is flattened axially and sealed to the cover portion 221, and the curled portion 252b is flattened along the inner circumferential surface of the intermediate body 253. Thus, as... Figure 10D As shown, the connecting portion 223, which is flattened by the curled portion 252a, integrates the cylindrical portion 220 and the cover portion 221, thereby obtaining a cover 204 with an inner circumference portion 224. When the curled portions 252a and 252b are flattened, Figure 10A The end edges 251a and 251b of the intermediate body 250 shown are respectively rolled into and sealed inside the connecting portion 223 and the inner peripheral portion 224, thereby protecting the end faces of the sheet material at the end edges 251a and 251b. It should be noted that before sealing the cover portion 221 into the intermediate body 253, the end edges 251a and 251b can be pre-loaded with... Figure 10C The curled portions 252a and 52b of the intermediate shown are flattened.

[0187] In the example above, Figure 10A The intermediate body 250 shown has its end edge 251b curled inward to form a curled portion 252b. However, the curled portion formed by curling the end edge 251b outward can also be flattened along the outer peripheral surface of the intermediate body. In this case, the curling is performed only near the end edge that serves as the inner side of the adhesive portion 225 during manufacturing. Figure 10A The folding process at intermediate body 250 can protect the end face of the sheet forming the cylindrical part 220.

[0188] In the above-mentioned method for manufacturing paper tubular container 2100, ultrasonic welding, high-frequency welding, heat sealing welding, hot air welding, and pressing of the main body insert can be used as welding methods for each part. However, in terms of being less affected by the thermal insulation properties of paper, ultrasonic welding is preferred.

[0189] In the paper tubular container 2100 of this embodiment, the cylindrical portion 201, the flat portion 202, and the main body portion 203 are all formed from sheets of paper, thus reducing the amount of resin used compared to conventional resin-made tubular containers. Furthermore, by providing a barrier layer on the sheets constituting the cylindrical portion 201 and the flat portion 202, it is easy to impart barrier properties to the nozzle portion.

[0190] Furthermore, as described above, in the forming process of the cylindrical section 201, by performing... Figure 9B The described edge folding process and Figure 9E The described curling process seals and protects the entire end face of the sheet constituting the cylindrical portion 201. Furthermore, the entire outer periphery of the flat portion 202 is folded back towards the outer surface of the container (surface 211b side) and sealed and protected at the adhesive portion between the main body portion 203 and the flat portion 202. Moreover, the sheet constituting the main body portion 203 is also adhered in a clasped shape when processed into a cylindrical form. With this configuration, the end faces of the sheets constituting each part inside the paper tubular container 2100 are not exposed, thus preventing liquids or other contents from permeating into the paper layer from the end faces of the sheets. Therefore, according to this embodiment, a paper tubular container 2100 capable of accommodating contents permeable to the paper layer can be constructed.

[0191] It should be noted that, for applications accommodating contents that do not permeate the paper layer, one or more of the following processes can be omitted: edge folding of end 244a, edge folding of end 244b, curling of end 245a, and curling of end 245b. Furthermore, if the end face of the sheet at end 244a or 244b is protected by a protective tape, this process can be omitted. Figure 9B The folding process is shown. Similarly, for the main body 203, as long as it accommodates a content that does not permeate the paper layer, the method of bonding the sheet constituting the main body 203 is not limited; the outer surface of the strip-shaped area containing one edge of the sheet can be bonded to the inner surface of the strip-shaped area containing the other edge of the sheet. The end faces of the sheet constituting the main body 203 can be protected using protective tape.

[0192] Similarly, like the cylindrical portion 201, the cylindrical portion 220 constituting the cover 204 is also constructed by folding and curling so that the end face of the sheet does not protrude from the inside. Therefore, when the paper tubular container 2100 is resealed by the cover 204, even if liquid or other contents adhere to the inner surface of the cover 204, it is possible to prevent the contents from penetrating into the paper layer from the end face of the sheet constituting the cylindrical portion 220. It should be noted that, in order to reliably prevent the contents from penetrating into the paper layer of the sheet constituting the cover 221, a large-sized blank for forming the cover 221 can be pre-formed and sealed to the connecting portion 223 of the cylindrical portion 220 with the annular portion within a predetermined range from the outer periphery folded back outward. However, for applications that contain contents that are not permeable to the paper layer, one or both of the folding process and the processing of the curled portion 252b (inner periphery 224) during the formation of the cylindrical portion 220 can be omitted.

[0193] Furthermore, in the paper tubular container 2100 according to this embodiment, a nozzle is formed by sealing the cylindrical portion 201 with the flat plate portion 202, and the inner surface of the sheet constituting the main body portion 203 is sealed to the outside of the flat plate portion 202. The sheet constituting the main body portion 203 is mainly paper and has a total thickness of 30 to 300 μm, so it is easy to bend. By folding the main body portion 203 along the outer periphery of the flat plate portion 202, the contents can be easily extruded. In addition, since the flat plate portion 202 does not have space for residual contents, residual contents can be reduced when extruding the contents by folding the main body portion 203 along the outer periphery of the flat plate portion 202.

[0194] <Third Implementation Method>

[0195] Since tubular containers are typically used to package contents containing liquids, a resin layer needs to be applied to one side of the paper (the side that serves as the inner side of the main body) to prevent liquid from seeping into the paper when the sheet constituting the main body is made of paper, in order to prevent liquid from seeping into the paper. Additionally, it is necessary to prevent liquid from seeping through the end faces of the sheet. One method involves overlapping sheets of different materials (e.g., the innermost layer is polyethylene, and the outermost layer is paper) in a tubular shape and bonding the innermost and outermost layers of the overlapping portion together. However, this method uses a strip material in the overlapping portion, which increases manufacturing costs. Furthermore, considering that adhesive components may leach from the exposed end faces of the strip material, this is not a preferred configuration for tubular containers. The main body needs to have a structure where the end faces of the sheet do not contact the contents; therefore, a method similar to a pillow-type packaging bag, where the inner faces of the sheets are joined together in a palm-like shape and sealed with a backing, is suitable.

[0196] However, when two sheets containing paper are overlapped and backed together for sealing, the increased rigidity of the backing seal may cause it to bounce off the main body, damaging the appearance of the packaging container.

[0197] This embodiment provides an aesthetically pleasing tubular container in which paper is used on the surface of the main body.

[0198] Figure 11 This is a perspective view illustrating a schematic configuration of the tubular container according to the embodiment. Figure 12 It is along Figure 11 The cross-sectional view of line XII-XII shown. Figure 13 It is along Figure 11 The cross-sectional view of line XIII-XIII shown. Figure 14 It is along Figure 11 The cross-sectional view of line XIV-XIV shown.

[0199] The tubular container 3100 has a tubular main body 301 and an outlet 302 installed on the main body 301.

[0200] The main body 301 is a component for containing contents and is formed from a sheet containing paper and a sealant. The main body 301 is formed by rolling up a sheet having a pair of substantially parallel end edges, and then joining and welding the inner surfaces of the strip-shaped portions each containing a pair of end edges together in a palm-like shape. The main body 301 can be manufactured using a bag-making machine, a pillow / core packaging machine, or the like.

[0201] The injection outlet 302 is a nozzle for removing the contents contained in the main body 301 to the outside, and is molded from a material containing thermoplastic resin. The injection outlet 302 includes an injection cylinder 303 and a flange 304. The flange 304 is connected to one end 306a of the injection cylinder 303. Figure 12 The flange 304 is a flat plate-shaped portion that connects to and extends to the outer side of the dispensing cylinder 303 from the lower end of the flange. In this embodiment, the flange 304 is positioned in a direction orthogonal to the axial direction of the dispensing cylinder 303. Figure 12 It is formed by extending in the left and right direction. In this embodiment, the flange portion 304 is formed in a ring shape, but as long as it can be joined with the main body portion 301, the shape of the flange portion 304 is not limited, and it can be elliptical, oblong, track-shaped, polygonal, etc.

[0202] The thermoplastic resin used as the material for the injection port 302 can be, for example, any one of polyethylene, polypropylene, polyester, polyamide, and cyclic polyolefins, or a combination of two or more. The injection port 302 can also be molded from a material containing a thermoplastic resin and fillers other than the resin. As fillers, any one of talc, kaolin, paper flour, and cellulose fibers, or a combination of two or more, can be used. By using a mixture of thermoplastic resin and fillers other than the resin as the material for the injection port 302, the amount of resin used can be reduced while maintaining moldability and heat-welding properties to the sheet of the main body 301. There are no particular limitations on the molding method for the injection port 302; existing molding methods such as extrusion molding, vacuum forming / hot plate pressurized air forming, and compression molding can be used.

[0203] like Figure 11 and Figure 12 As shown, one end 305a of the main body 301 is sealed and closed. On the other hand, a portion of the main body 301 within a predetermined range from the other end 305b is folded and sealed to the outside 308 of the flange 304 of the outlet portion 302. Figure 11 and Figure 14 As shown, the flange portion 304 has multiple pleats 312 formed by folding the sheet that constitutes the main body portion 301.

[0204] The main body 301 has a backing sealing portion 307 formed by joining and welding the inner surfaces of the sheets together in a palm-like shape. For example... Figure 13 As shown, the backing seal 307 formed on the main body 301 is bent and sealed to the main body 301 in a manner that runs along the outside of the main body 301. The outside of the backing seal 307 and the outside of the main body 301 are sealed with a material that has heat-welding properties.

[0205] In addition, such as Figure 14 As shown, at the flange portion 304 of the injection outlet portion 302, at least a portion of the portion within a predetermined range from the end portion 305b of the main body portion 301 can be folded to form an overlap portion 313 between the sheets. In the overlap portion 313, the outer surfaces of the overlapping sheets are in contact with each other, and the outer surfaces of the sheets in contact with each other are sealed to each other by using a material with heat-welding properties.

[0206] Figure 15 This is a cross-sectional view showing an example of the layered structure of the sheet material constituting the main body of the tubular container.

[0207] The main body 301 of the tubular container 3100 is composed of a sheet 341 primarily made of paper. The sheet 341 is a multilayer sheet, wherein a substrate film layer 133, a barrier layer 134, and a sealant layer 135 are sequentially stacked on one side of the paper layer 132; a paper protective layer 137 is stacked on the other side of the paper layer 132; and an ink layer 138 and an external varnish layer 139 are stacked on the paper protective layer 137. A patterned hot-melt coating 340 is then applied. It should be noted that the paper layer 132, substrate film layer 133, barrier layer 134, sealant layer 135, paper protective layer 137, ink layer 138, and external varnish layer 139 can utilize the layer configurations described in the first embodiment. Furthermore, the total thickness of the sheet 341 constituting the main body 301 and the proportion of paper (pulp fiber) can be set within the same range as in the first embodiment. More than one layer other than the paper layer 132 and the sealant layer 135 can be omitted from the sheet 341.

[0208] (Thermo-weldable coating)

[0209] The heat-fusible coating 340 is a layer used to impart heat-fusibility to the outer surface of the sheet 341. In this embodiment, as described later, the outer surface of the backing seal 307 is sealed to the outer surface of the main body 301 by the heat-fusible coating 340 patterned and applied to the outer surface of the sheet 341 (see reference). Figure 13 Meanwhile, the outer surface of the overlapping sheet is sealed by the overlapping portion 313 formed on the flange portion 304 of the injection port portion 302 (see reference). Figure 14 ).

[0210] The heat-melting coating 340 can be formed by applying a coating agent containing a thermoplastic resin with a melting point below 200°C, such as an acrylic polymer, polyolefin, polyvinyl acetate, or polyester, and then allowing it to dry. In addition to thermoplastic resins, the coating agent can also contain inorganic substances used to prevent adhesion.

[0211] The coating amount of the coating agent used to form the hot-melt coating 340 is 0.2~40 g / m². 2 The preferred concentration is 3.0~30g / m³. 2 When the coating amount of the coating agent is less than 0.2 g / m² 2 In this case, the adhesive strength between the outer surfaces of sheet 341 is insufficient, and the sheets of backing seal 307 and overlapping portion 313 exhibit a bounce-up phenomenon (hereinafter referred to as "paper bounce"). On the other hand, when the coating amount of the coating agent exceeds 40 g / m²... 2 In such cases, the coefficient of friction increases, reducing the mechanical adaptability to processing devices such as bag making machines, or the sheets 341 are prone to sticking together.

[0212] The heat-weldable coating 340 can be applied to the entire surface of the sheet 341, but because the surface of the sheet 341 has a high coefficient of friction, the mechanical adaptability in the processing of the main body 301 and subsequent processes may be reduced. Therefore, from the perspective of mechanical adaptability, it is more preferable to apply the heat-weldable coating 340 to a portion of the surface of the sheet 341 by patterning (partial coating) the coating agent.

[0213] When the heat-fusion coating 340 is applied to a portion of the surface of the sheet 341, the heat-fusion coating 340 can be applied to the sealing target area, i.e., the portion where the outer side of the backing seal 307 contacts the outer side of the main body 301, and the portion where the outer sides of the overlapping sheets in the overlapping portion 313 contact each other. However, the heat-fusion coating 340 may also be applied to only one of the contact surfaces of the sealing target area.

[0214] The thickness (total thickness) of the sheet 341 constituting the main body 301 is not particularly limited, but is preferably 30 to 300 μm. If the thickness of the film constituting the main body 301 is within this range, the main body 301 can be easily processed into a cylindrical shape using a bag-making machine, a pillow / core packaging machine, or the like. In addition, since the paper layer 132 imparts strength and rigidity, it can be thinner than a typical laminated tube (thickness 300 to 500 μm), and the amount of resin used can also be reduced.

[0215] In order to reduce the resin content of the sheet 341 constituting the main body 301, the proportion of paper layer 132 in the mass of sheet 341 is preferably 50% or more. From the viewpoint of reducing the amount of resin used, the higher the proportion of paper layer 132, the better.

[0216] It should be noted that, in Figure 15 In the layer composition of the sheet 341 shown, one or more of the following layers may be omitted: substrate film layer 133, barrier layer 134, paper protective layer 137, ink layer 138, and outer coating varnish layer 139.

[0217] like Figure 11 As shown, the tubular container 3100 may further include a screw cap 311, which is threadedly connected to the dispensing cylinder 303 of the dispensing outlet 302 and is removable. With the screw cap 311, the tubular container 3100 can be easily resealed after being opened.

[0218] Alternatively, the tubular container 3100 can also have a hinged cap instead of the screw cap 311. When a hinged cap is provided, it can be connected by a threaded connection. Figure 11The dispensing cylinder portion 303 shown is installed on the dispensing outlet portion 302. Alternatively, ribs can be provided on the outside of the dispensing cylinder portion 303 instead of threads, and the hinge cover can be installed on the dispensing outlet portion 302 by inserting the ribs.

[0219] In addition, the end 306b of the dispensing cylinder 303 can be sealed with a membrane that closes the dispensing cylinder 303 when the tubular container 3100 is unopened.

[0220] Furthermore, in order to keep the interior of the tubular container 3100 sealed when unopened, the interior of the dispensing cylinder 303 can be sealed by a partition wall. When a partition wall is provided, it is preferable to have a circular half-cut along the inner circumference of the dispensing cylinder 303, and a pull ring connected to the portion surrounded by the half-cut. With this configuration, when the tubular container 100 is opened, the user pulls the pull ring to break off a portion of the half-cut 327 of the partition wall, thereby removing a portion of the partition wall surrounded by the half-cut, thus forming an opening for dispensing the contents from the main body 301 into the dispensing cylinder 303.

[0221] The manufacturing method of the tubular container 3100 according to this embodiment will be described below.

[0222] Figure 16 This is a top view of the sheet material that makes up the main body of the tubular container.

[0223] Figure 16 The sheet 320 shown has Figure 15 The sheet material with the layered structure described herein corresponds to one main body part 301. Figure 16 The area near the upper edge 324 corresponds to the part that is fused with the injection outlet 302. Figure 16 The lower edge of the tube corresponds to the closed end portion. Furthermore, the central region 321, enclosed by two dashed lines, forms the front of the tubular container 3100, and the regions 322 adjacent to both sides of region 321 form the back of the tubular container 3100. Additionally, Figure 16 The side of the paper closest to itself becomes the outer surface of the main body 301.

[0224] On the outer surface of sheet 320, a heat-welding coating is formed in a patterned coating of a heat-welding agent in a strip region 325 along end edge 323a and a strip region 326 including end edge 324 adjacent to end edge 323a. Sheet 320 is rolled into a cylindrical shape, and the inner surfaces of the strip regions along opposing parallel end edges 323a and 323b are joined together in a palm-like manner to form a backing seal 307. When the backing seal 307 is bent along the main body 301, region 325 corresponds to the portion where the outer surface of the backing seal 307 contacts the outer surface of the main body 301. Furthermore, when the cylindrical sheet 320 is joined to the flange 304 of the injection port 302, region 326 is the portion welded to the flange 304, corresponding to the portion folded and forming a pleat 312.

[0225] Figures 17A to 17D This is a cross-sectional view used to illustrate the manufacturing method of the main body of a tubular container. Figures 17A to 17D In the diagram, the direction orthogonal to the paper surface is the conveying direction of sheet 320, which is processed sequentially while being conveyed by a conveying device (not shown).

[0226] First, such as Figure 17A As shown, sheet 320 is wound onto a plate-shaped clamp 351 such that a predetermined area including one end edge 323a overlaps with a predetermined area including the other end edge 323b. Figure 16 As described, a heat-weldable coating is provided in region 325 along the end edge 323a.

[0227] Next, as Figure 17B As shown, using a guide 352 with an inverted T-shaped cross section, the strip-shaped portion along the end edge 323a and the strip-shaped portion along the end edge 323b are erected and clamped with the guide 352 so that their inner surfaces are facing each other in a palm-like shape.

[0228] Next, as Figure 17C As shown, using a flat guide 353, the inner surfaces of sheet 320, which are joined together in a palm-like shape, are bent at approximately 90 degrees to obtain a state where three sheets overlap.

[0229] In this state, such as Figure 17D As shown, by using a sealing strip 354 to seal, the inner surfaces of the sheet 320 are fused together to form a backing seal 307. At the same time, by using a heat-fusible coating provided in region 325, a main body 301 can be formed by fusing the backing seal 307 to the outside of the main body 301.

[0230] Figures 18A-18C This diagram illustrates the welding method between the main body and the outlet of a tubular container.

[0231] First, such as Figure 18A and Figure 18B As shown, a cylindrical main body 301 and a separately formed injection outlet 302 are prepared, and the flange 304 of the injection outlet 302 is inserted from the end 305b of the main body 301. Preferably, a separately formed screw cap 311 is screwed into the injection outlet 302 for integral integration. Figure 16 As described, a heat-weldable coating is provided in region 326, which includes end edge 324.

[0232] Next, as Figure 18B As shown, the inner surface of the flange is supported by a clamp 356 inserted from the other end of the main body 301, and a claw (not shown) is used to clamp the portion within a predetermined range from the end edge 324 (end 305b) of the main body 301. Figure 18B The white arrow indicates the direction to fold back and press. Multiple grippers for folding back the main body 301 can be provided at predetermined intervals along the circumferential direction of the injection outlet 302.

[0233] Next, as Figure 18C As shown, a portion of the body portion 301 within a predetermined range from the end edge 324 is clamped between the welding device 357 (such as an ultrasonic welding head) and the clamp 356. By using multiple spaced-apart grippers to press the portion within the predetermined range from the end edge 324 of the body portion 301 and pressing it with the welding device 357, and folding the portion within the predetermined range from the end edge 324 of the body portion 301, it is welded to the flange portion 304. Thus, the body portion 301 and the injection port portion 302 can be joined together.

[0234] Then, by filling the contents into the interior of the main body 301 and closing the end of the main body 301, a package using the tubular container 3100 can be obtained.

[0235] As a method for welding the main body 301 and the outlet 302 when manufacturing the tubular container 3100, ultrasonic welding, high-frequency welding, heat sealing welding, hot air welding, and pressing of the main body insert can be used. However, in terms of being less affected by the thermal insulation properties of the paper, ultrasonic welding is preferred.

[0236] As described above, in the tubular container of this embodiment, since the main body 301 is made of a sheet containing paper and sealant, the amount of resin used can be reduced, and the paper imparts rigidity to the main body 301, resulting in excellent self-standing and operability of the container. Since the backing seal 307 formed on the main body 301 is fused to the outside of the main body 301, and the overlapping portions 313 of the sheet formed on the flange 304 are fused to each other, a tubular container 3100 with excellent aesthetics can be provided where the backing seal 307 and the overlapping portions 313 do not spring back.

[0237] Furthermore, in the tubular container 3100 of this embodiment, the flange portion 304 has a flat plate shape orthogonal to the central axis of the dispensing cylinder portion 303, and the main body portion 301 is fused to the outer surface 308 of the flange portion 304. Therefore, when the contents of the tubular container 3100 are small, the contents can be easily squeezed out by folding the main body portion 301 along the outer periphery of the flange portion 304. In addition, since the flange portion 304 is flat, no space for residual contents is formed in the flange portion 304. Therefore, by bending the main body portion 301 along the outer periphery of the flange portion 304, the flange portion 304 and the main body portion 301 become almost flat, and the contents can be squeezed out without residue.

[0238] (Modified example)

[0239] In the above embodiments, it is explained that in Figure 16 The example shown illustrates the layered heat-fusion coating 340 in regions 325 and 26. However, depending on the shape of the flange 304 and the folding method of the body 301 towards the welded portion of the flange 304, the heat-fusion coating 340 in region 326 (overlapping portion 313) can be omitted, and the heat-fusion coating 340 can be provided only in region 325, where the number and overlap area of ​​the overlapping portions 313 can be reduced. In this case, by bending and sealing the backing seal 307 along the outside of the body 301, an aesthetically pleasing tubular container that prevents the paper of the backing seal 307 from springing up can be obtained.

[0240] In addition, in the above embodiment, an example of laminating the heat-welding coating 340 by patterning the coating agent was described. However, the heat-welding coating 340 can also be formed by coating the entire surface of the sheet constituting the main body 301 with the coating agent.

[0241] Furthermore, in the above embodiment, an example was described in which the backing seal portion 307 and the overlapping portion 313 were welded by providing a heat-welding coating 340. However, it is also possible to form the heat-welding coating 340 on the entire surface of the paper layer 132 without laminating the heat-welding coating 340. Figure 16The paper protective layer 137 shown allows the backing seal 307 to be welded to the outside of the main body 301. Furthermore, in addition to the backing seal 307, the overlapping sheets at the overlapping portion 313 on the flange 304 can also be welded together using the paper protective layer 137. When the paper protective layer 137 is formed using a thermoplastic material, thermoplastic resins such as acrylic polymers, polyolefins, polyvinyl acetate, and polyesters can be extruded and coated onto the paper layer 132. Alternatively, a coating agent containing these thermoplastic resins and, if necessary, inorganic compounds can be added to the paper layer 132. When the thermoplastic paper protective layer 137 is formed by resin extrusion coating, the thickness is preferably 5 to 30 μm; when the thermoplastic paper protective layer 137 is formed by a coating agent, the thickness is preferably 0.2 to 20 μm.

[0242] The tubular container involved in this embodiment is described below.

[0243] [1] A tubular container, comprising:

[0244] The inlet port has a cylindrical inlet section and a flange section connected to one end of the inlet section and extending to the outside of the inlet section; and

[0245] The tubular main body is constructed of a sheet of paper with a sealant on one side, closed at one end, and sealed to the flange portion at a predetermined distance from the other end.

[0246] The main body has a backing sealing portion that allows the rolled-up cylindrical sheet to be joined and sealed in a palm-like shape.

[0247] The backing seal is curved along the outside of the main body and seals the main body.

[0248] [2] The tubular container described in Project [1]

[0249] By folding at least a portion of the predetermined range of the main body, an overlap is formed between the sheets.

[0250] The overlapping sheets at the overlapping portion are sealed to each other.

[0251] [3] The tubular container as described in Project [2]

[0252] The backing seal is sealed to the outside of the main body by partially coating the other side of the paper sheet constituting the main body with a heat-welding material, while the overlapping sheets at the overlapping portion seal each other.

[0253] [4] The tubular container as described in Project [3]

[0254] The coating amount of the coating agent is 0.2–40 g / m². 2 .

[0255] [5] The tubular container as described in Project [2]

[0256] The backing seal is sealed to the outside of the main body by layering a thermally bondable material on the entire surface of the other side of the sheet of paper constituting the main body, while the sheets overlapping at the overlap seal each other.

[0257] <Fourth Implementation>

[0258] In the main body of the tubular container described in Japanese Utility Model Publication No. 7-45311, the paper's end face is exposed inside the tubular container, leading to problems such as the contents coming into contact with the paper, dissolving through the paper, and precipitating out. Therefore, as in the main body of the tubular container described in Japanese Patent Application Publication No. 2012-25471, by overlapping and folding back the innermost layers of the two ends of the blank, which consists of a laminated body containing an intermediate layer of paper, and then heat-sealing (folding and bonding), the paper's end face is not exposed inside the tubular container. However, this results in a thicker sealing portion of the main body containing the paper, and a deterioration in the appearance of the tubular container.

[0259] This embodiment provides a tubular container body that has a good appearance, where the end face of the paper is not exposed inside the body of the tubular container.

[0260] <Main body of the tubular container in the fourth embodiment>

[0261] Figure 19 This is a cross-sectional view showing the layered structure of the laminated sheet 410 constituting the main body 4100 of the tubular container according to the fourth embodiment. For example, a paper layer 420 is laminated between an inner laminated film 411 and an outer laminated film 415. The inner laminated film 411 sequentially comprises a first sealant layer 412, a barrier layer 413, and a first substrate film layer 414, while the outer laminated film 415 sequentially comprises a second substrate film layer 416 and a second sealant layer 417. The paper layer 420 is sandwiched between a first adhesive layer 418 and a second adhesive layer 419, wherein the first adhesive layer 418 is laminated on the side of the first substrate film layer 414 opposite to the barrier layer 413, and the second adhesive layer 419 is laminated on the side of the second substrate film layer 416 opposite to the second sealant layer 417. In addition, an ink layer 421 is partially laminated on the side of the second substrate film layer 416 of the paper layer 420.

[0262] Next, each layer constituting the laminated sheet 410 will be described in detail.

[0263] (First sealant layer)

[0264] The first sealant layer 412 is the innermost layer of the laminated sheet 410 and the innermost layer of the inner laminated film 411, and is a thermoplastic resin layer. The first sealant layer 412 is the layer that seals the innermost second sealant layer 417 when the laminated sheet 410 is formed into a cylindrical shape. Furthermore, when the cylindrical body portion 4100 is used in the tubular container 4300 described later, the first sealant layer 412 is the layer that adheres to the injection port portion 450; therefore, a tight seal with the injection port portion 450 is preferable.

[0265] The material used for the first sealant layer 412 can be any thermoplastic resin and is not particularly limited, such as polypropylene, polyethylene, cyclic polyolefin, polyester, etc. Furthermore, the softening temperature of the first sealant layer 412 needs to be at least 20°C lower than the softening temperature of the first substrate film layer 414, more preferably at least 40°C lower. When the temperature obtained by subtracting the softening temperature of the first sealant layer 412 from the softening temperature of the first substrate film layer 414 is less than 20°C, the first substrate film layer 414 and the second substrate film layer 416 soften during sealing of the cylindrical main body portion used to form the laminated sheet 410, increasing the likelihood of micropores (pinholes) forming in the main body portion 4100.

[0266] (Barrier layer)

[0267] The barrier layer 413 is the intermediate layer of the inner laminated film 411, and is laminated for the purpose of ensuring the quality of the contents and extending the shelf life.

[0268] The barrier layer 413 comprises a barrier coating material consisting of metal vapor deposition such as aluminum, inorganic compounds such as silica or alumina vapor deposition, plate-like minerals, and binder resins, including one or more barrier resin films such as ethylene-vinyl alcohol copolymer (EVOH) and polyvinylidene chloride (PVDC) as components. Alternatively, these materials can be used in combination. It should be noted that when the barrier layer 413 is transparent, it helps to make the main body 4100 of the tubular container transparent, thereby improving the visibility of the contents and making it easier to confirm the remaining amount, etc. Therefore, the barrier layer 413 is preferably transparent.

[0269] (First substrate film layer)

[0270] The first substrate film layer 414 is the innermost layer of the inner laminated film 411 and also serves as the substrate layer of the aforementioned barrier layer 413.

[0271] There are no particular limitations on the material used for the first substrate film layer 414. From the viewpoints of heat resistance, toughness during heating, and physical strength, stretched films such as polyolefins, polyesters, and polyamides are preferred. Alternatively, paper can also be used for the first substrate film layer 414.

[0272] It should be noted that if the outer laminate 415 contains the second substrate film layer 416 (described later), the inner laminate 411 may not contain the first substrate film layer 414.

[0273] (First adhesive layer)

[0274] The first adhesive layer 418 is used to sandwich the paper layer 420 together with the second adhesive layer 419 (described later) and is integrated with the outer laminate 415.

[0275] The first adhesive layer 418 is composed of a thermoplastic resin, such as a substance containing one or more polyolefins, polyacrylic acid, PE-based materials, PP-based materials, or other hot-melt materials. The composition is not particularly limited as long as the second adhesive layer 419 can be hot-melted, but it is preferable to use the same material as the second adhesive layer 419 described later, as this can result in higher adhesive strength.

[0276] The thickness of the first adhesive layer 418 is, for example, 5 μm to 100 μm, and particularly preferably 10 μm to 50 μm. When the thickness of the first adhesive layer 418 is less than 5 μm, sufficient strength cannot be obtained when bonding the paper layer 420 to the outer laminate 415. When the thickness of the first adhesive layer 418 is greater than 100 μm, the processing adaptability and processing speed when bonding the paper layer 420 to the outer laminate 415 deteriorate, and the amount of resin used increases, which is uneconomical.

[0277] (Paper layer)

[0278] The paper layer 420 is the middle layer of the laminated sheet 410, and is such a layer that it imparts strength to the body portion 4100 of the tubular container by being sandwiched between the first adhesive layer 418 and the second adhesive layer 419 (described later), and by being bonded to these films between the outer laminated film 415 and the inner laminated film 411.

[0279] There are no particular limitations on the materials used for paper layer 420, but for aesthetic purposes, flowing paper can be used, and for rigidity, thick kraft paper can be used. In addition, paper layer 420 is distinguished from synthetic paper made from resin fiber paper by containing more than 5% cellulose fibers.

[0280] The preferred weight per unit area of ​​paper layer 420 is 3 g / m². 2 Above 300g / m 2 Below. Additionally, if the unit area weight of paper layer 420 is 10 g / m²... 2 Above 150g / m 2 The following operations are then easily performed, such as forming the main body, and the main body 4100 exhibits good rigidity when used in a tubular container 4300 employing this main body 4100. When the weight per unit area of ​​the paper layer 420 is less than 3 g / m²...2 When bonding the outer laminate 415 to the inner laminate 411, paper breaks occur, hindering the proper forming of the main body 4100. Furthermore, when the weight per unit area of ​​the paper layer 420 exceeds 300 g / m²... 2 When the total thickness of the laminated sheet 410 increases, it cannot be properly welded when formed into a cylindrical shape.

[0281] (Second adhesive layer)

[0282] The second adhesive layer 419 is used to sandwich the paper layer 420 together with the aforementioned first adhesive layer 418 and is integrated with the inner laminated film 411.

[0283] The second adhesive layer 419 is composed of a thermoplastic resin, such as a substance containing one or more polyolefins, polyacrylic acid, PE-based materials, PP-based materials, or other hot-melt materials. The composition is not particularly limited as long as the first adhesive layer 418 can be hot-melted, but it is preferable to use the same material as the first adhesive layer 418 to obtain higher adhesive strength.

[0284] The thickness of the second adhesive layer 419 is the same as that of the first adhesive layer 418, for example, 5 μm to 100 μm, and particularly preferably 10 μm to 50 μm. When the thickness of the second adhesive layer 419 is less than 5 μm, sufficient strength cannot be obtained when bonding the paper layer 420 to the inner laminate 411. When the thickness of the second adhesive layer 419 is greater than 100 μm, the processing adaptability and processing speed when bonding the paper layer 420 to the inner laminate 411 deteriorate, and the amount of resin used increases, which is uneconomical.

[0285] (Second substrate film layer)

[0286] The second substrate film layer 416 is the innermost layer of the inner laminated film 411 and is mainly used to impart toughness. The material used for the second substrate film layer 416 is the same as that used for the first substrate film layer 414 described above.

[0287] It should be noted that if the first substrate film layer 414 is laminated in the inner laminated film 411, the second substrate film layer 416 may not be laminated in the outer laminated film 415.

[0288] (Second sealant layer)

[0289] The second sealant layer 417 is the outermost layer of the laminated sheet 410 and the outermost layer of the outer laminated film 415, and is a thermoplastic resin layer.

[0290] The second sealant layer 417 imparts heat-welding properties to the first sealant layer 412 and serves to protect the paper layer 420.

[0291] The second sealant layer 417 can be any thermoplastic resin without particular limitation. For example, it can be formed by extruding a substance containing one or more low-melting-point polyethylene, polypropylene, polyethylene terephthalate, and polymethacrylic acid, or by coating a liquefied substance. In addition, in order to form the laminated sheet 410 into a cylindrical shape, patterned coating can be applied only to the sealing portion.

[0292] The thickness of the second sealant layer 417 is preferably 3 μm to 200 μm, more preferably 8 μm to 30 μm. When the thickness of the second sealant layer 417 is less than 3 μm, it cannot maintain sufficient strength when heat-fused with the first sealant layer 412, and problems such as bag rupture may occur when the laminated sheet 410 is used in the tubular container 4300. On the other hand, when the thickness of the second sealant layer 417 is greater than 200 μm, the laminated sheet 410 becomes too thick, which is uneconomical.

[0293] (Ink layer)

[0294] exist Figure 19 In this process, the ink layer 421 is only partially laminated on the outer side of the paper layer 420 on the laminated film 415 side, but the position of the laminated ink layer 421 is not particularly limited.

[0295] In addition to the outer side of the paper layer 420, the ink layer 421 may be laminated on the side of the second sealant layer 417 opposite to the second substrate film layer, the side of the first substrate film layer 414 opposite to or on the side of the barrier layer 413, the side of the second substrate film layer 416 on the side of the second sealant layer, or the side opposite to the second sealant layer 417.

[0296] There are no particular limitations on the type of ink used for ink layer 421, but inks suitable for the printing method and printing substrate are preferred. There are no particular limitations on the printing method for ink layer 421; for example, general printing methods such as gravure printing, offset printing, and flexographic printing can be used.

[0297] The fabrication of the laminated sheet 410 using the above-mentioned layers is as follows.

[0298] Ink layer 421 is laminated (printed) onto one side of paper layer 420. First sealant layer 412, barrier layer 413, and first substrate film layer 414 are sequentially laminated and dry-laminated using a dry lamination adhesive to create inner laminate film 411. Additionally, second sealant layer 417 is formed on one side of second substrate film layer 416 by extrusion lamination to create outer laminate film 415.

[0299] A first adhesive layer 418 is laminated on the side of the first substrate film layer 414 opposite to the barrier layer 413. On the side of the first adhesive layer 418 opposite to the first substrate film layer 414, a printed paper layer 420 is supplied and laminated with the printed side facing upwards and forming multiple stripes. A second adhesive layer 419 and an outer laminated film 415 with the second sealant layer 417 facing upwards are sequentially laminated on the side of the paper layer 420 opposite to the first adhesive layer 418. Using the first adhesive layer 418 and the second adhesive layer 419, the inner laminated film 411, the outer laminated film 415, and the paper layer 420 between them are bonded by extrusion lamination, thereby completing the laminated sheet 410.

[0300] The thickness of the laminated sheet 410 is preferably 30 μm to 300 μm. With this thickness, in a tubular container 4300 formed using a tubular container body 4100 made of the laminated sheet 410, the contents can be easily extruded with a slight force. Furthermore, when the contents are extruded, the body portion 4100 can be uniformly flattened to its end, thereby reducing the radius of curvature at the width-direction end of the body portion 4100 and suppressing content residue.

[0301] Figure 20 This is a top view showing the blank 4200 for forming the main body portion 4100 of the tubular container according to the fourth embodiment. Figure 21 yes Figure 20 Enlarged cross-sectional view along line AA. The blank 4200 for forming the main body is composed of the aforementioned laminated sheet 410. The blank 4200 for forming the main body is formed by the following method: in the laminated sheet 410 formed by multiple striped laminated paper layers 420 in the height direction of the main body, such as... Figure 20 As shown, when viewed from above in the height direction of the main body, it is cut in such a way that portions 431 and 432, which are only film portions with the paper layer 420 portion as the center and the portions on both sides of the paper layer 420 not stacked, are formed. Furthermore, it is cut to a predetermined length in a direction orthogonal to the height direction of the main body. Here, the height direction of the main body refers to the height direction of the cylinder when the main body 4100 is formed into a cylindrical shape (for example).

[0302] like Figure 20 As shown, the blank 4200 used for forming the main body portion 4100 of the tubular container according to the fourth embodiment is, for example, generally rectangular. Figure 21As shown, the end face 441 of the paper layer 420 is not exposed at least on the two opposite end edges of the blank 4200 forming the main body portion. The paper layer 420 is sandwiched between the inner laminate 411 and the outer laminate 415, and the end faces 441 of the paper layer 420 on the two opposite end edges of the blank 4200 forming the main body portion are protected. It should be noted that the inner laminate 411, the paper layer 420, and the outer laminate 415 are connected by... Figure 19 The first adhesive layer 418 and the second adhesive layer 419 shown ( Figure 21 (Not shown in the diagram) Integration.

[0303] Figure 22 (a) is an enlarged cross-sectional view orthogonal to the height direction of the main body 4100 of the tubular container according to the fourth embodiment.

[0304] like Figure 22 As shown in (a), the main body 4100 of the tubular container is formed by overlapping and heat-melting the outermost surface 410A and the innermost surface 410B, which are thermoplastic resins, with opposite ends of the main body forming blank 4200 forming a cylindrical shape. That is, by overlapping and heat-melting the opposite ends of the main body forming blank 4200 with one end inside the main body 4100 of the tubular container and the other end outside the main body 4100 of the tubular container, a so-called sealing bonding is achieved.

[0305] exist Figure 22 In the main body 4100 of the tubular container according to the fourth embodiment shown in (a), when the two opposite ends of the main body forming blank 4200 are overlapped, the portion with the stacked paper layer 420 is wound until it overlaps and then heat-fused. For example, the portion with the stacked paper layer 420 is wound onto a mandrel or plate until it overlaps, and after the two opposite ends of the main body forming blank 4200 are overlapped, a heat sealing rod or hot plate is applied from one or both sides, so that the two opposite ends of the main body forming blank 4200 are heat-fused. Alternatively, for example, by heating one or both ends of the main body forming blank 4200, while the surface resin melts, the portion with the stacked paper layer 420 is wound until it overlaps, so that the main body forming blank 4200 overlaps and is cooled, thereby achieving a seal.

[0306] As a method for forming the aforementioned main body forming blank 4200 into a cylindrical shape, the following methods can be listed: using a general tube making machine, bag making machine, pillow / core packaging machine, etc., the innermost and outermost layers of the two opposite end edges of the main body forming blank 4200 are overlapped and heat-fused together. For example, when using a bag making machine, the following methods can be listed: the laminated sheet 410 cut into strips is folded into a cylindrical shape in a direction orthogonal to the height direction of the main body using a sheet folding guide, such that the innermost and outermost layers of the two end edges of the laminated sheet 410 overlap, and heat-fused together from above the overlap using a heat sealing bar.

[0307] <The main body of the tubular container in the modified example>

[0308] The main body 4101 of the modified tubular container can be formed from the same main body forming blank 4200 as the main body forming blank 4200 constituting the main body 4100 of the tubular container of the first embodiment, but the structure of the heat-welded portion when formed into a cylindrical shape is different.

[0309] Figure 22 (b) is an enlarged cross-sectional view orthogonal to the height direction of the main body 4101 of the tubular container involved in the modified example.

[0310] With Figure 22 In the same manner as the main body 4100 of the tubular container according to the fourth embodiment shown in (a), the main body 4101 of the tubular container is formed by overlapping and heat-melting the outermost surface 410A and the innermost surface 410B, which are thermoplastic resins, so that the two opposing end edges of the main body forming blank 4200 are formed into a cylindrical shape, thereby completing the main body 4101 of the tubular container. That is, the two opposing end edges of the main body forming blank 4200 are overlapped and heat-melted with each other such that one end edge is inside the main body 4101 of the tubular container and the other end edge is outside the main body 4101 of the tubular container.

[0311] However, unlike the main body 4100 of the tubular container in the fourth embodiment, in Figure 22In the modified example shown in (b), in the main body 4101 of the tubular container, when the two opposite ends of the main body forming blank 4200 are overlapped, a portion of the laminated paper layer 420 is wound until just overlapped and then heat-fused. For example, a portion of the laminated paper layer 420 is wound onto a mandrel and a plate until just overlapped, and after the two opposite ends of the main body forming blank 4200 are overlapped, a heat-sealing rod or hot plate is applied from one or both sides, causing the two opposite ends of the main body forming blank 4200 to be heat-fused together. Alternatively, for example, by heating one or both ends of the main body forming blank 4200, while the surface resin melts, a portion of the laminated paper layer 420 is wound until just overlapped, causing the main body forming blank 4200 to overlap and then cool, thereby achieving a seal.

[0312] It should be noted that when the laminated sheet 410 is rolled and heat-fused together with only the film portions 431 and 432 overlapping each other (excluding the unlaminated paper layers 420), the paper layers 420 are not provided in a portion of the entire circumference of the cross-section orthogonal to the height direction of the main body. This is not preferable from the perspective of protecting the contents. Therefore, as Figure 22 (a) Figure 22 As shown in (b), it is preferable to provide a paper layer 420 on the entire circumference of a cross section orthogonal to the height direction of the main body.

[0313] As in the tubular container body 4101 of the modified example, the method of forming the body part blank 4200 into a cylindrical shape is similar to that of the tubular container body 4100 according to the fourth embodiment. The following methods can be listed: using a general tube-making machine, bag-making machine, pillow / core packaging machine, etc., the innermost and outermost layers of the two opposing end edges of the body part forming blank 4200 are overlapped and heat-fused. For example, when using a bag-making machine, the following method can be listed: a laminated sheet 410 cut into strips is folded into a cylindrical shape in a direction orthogonal to the height direction of the body part using a sheet folding guide, such that the innermost and outermost layers of the two end edges of the laminated sheet 410 overlap, and heat-fused from above the overlapping portion using a heat-sealing bar.

[0314] <An example of a tubular container that uses the main body of the tubular container according to the fourth embodiment>

[0315] Figure 23 (a) is a front view of a first example of a tubular container using the main body 4100 of the tubular container according to the fourth embodiment. Figure 23 (b) is a side view of a first example of a tubular container using the main body 4100 of the tubular container according to the fourth embodiment.

[0316] The tubular container 4300 includes the aforementioned tubular container body 4100 and inlet outlet 450. One end of the tubular container body 4100 is closed, and the inlet outlet 450 is installed at the other end of the body 4100. Additionally, as an example, the tubular container 4300 further includes a hinged cap (not shown) installed to the inlet outlet 450. It should be noted that, for convenience, Figure 23 The hinge cover (not shown) is shown not installed on the inlet 450.

[0317] In the main body 4100 of the tubular container, the bottom 462 at one end is closed and contains contents (not shown). As an example, the main body is formed by forming a cylindrical blank 4200, which is composed of the aforementioned laminated sheets 410, and then bonding the bottom 462 and the end edges of the laminated sheets 410, which are end edges along the height direction of the main body, to each other. The method of bonding the laminated sheets 410 in the bottom 462 to each other is not particularly limited; for example, a method can be used where an adhesive layer containing polyethylene is provided between the innermost layers of the opposing laminated sheets 410, and they are thermally fused together. The method of bonding the laminated sheets 410 in the main body 4100 of the tubular container to each other can be the same as described above. Figure 22 The tubular forming method of the main body 4100 of the tubular container shown in the fourth embodiment is the same. Therefore, in the tubular main body sealing part and bottom 462 used to form the main body 4100, the contents will not come into contact with the end face 441 of the paper layer 420.

[0318] Figure 24 It is along Figure 23 An enlarged cross-sectional view of the BB line near the inlet outlet 450. The inlet outlet 450 is a component installed at the top 461 of the main body 4100 of the tubular container and capable of closing the top 461 of the main body 4100. The inlet outlet 450 has a flat plate-shaped closing portion 451 orthogonal to the height direction of the main body 4100 of the tubular container. Figure 23 , Figure 24 In this context, the height direction of the main body refers to the axial direction of the main body 4100, which connects the bottom 462 located at one end of the main body 4100 to the injection outlet 450 installed at the other end of the main body 4100.

[0319] As an example, the closure portion 451 is circular, but any flat plate shape is acceptable; its shape is not limited and can also be elliptical, oblong, polygonal, etc. The material of the injection outlet portion 450 is not particularly limited, but resin materials such as low-density polyethylene are preferred. Furthermore, by using a material that imparts a barrier function to the injection outlet portion 450 in conjunction with the main body portion 4100, the overall barrier function of the tubular container 4300 can be improved, thereby further protecting the quality of the contents. Compared to the conical injection outlet portion 450 of the prior art, the flat plate shape of the closure portion 451 reduces the amount of material used.

[0320] As an example, the closure 451 has an annular half-cut 452 at approximately its center, and a pull ring 453 is provided inside the half-cut 452. By providing the half-cut 452 and the pull ring 453, the user of the tubular container 4300 pulls the pull ring 453 and removes a portion of the closure 451 along the half-cut 452, thereby forming an opening in the closure 451 for removing the contents. It should be noted that the half-cut 452 and pull ring 453 may also be omitted, and the opening for removing the contents may be pre-formed in the closure 451.

[0321] In the periphery of the inlet 450, the top 461 of the main body 4100 of the tubular container is mounted on the surface of the inlet 450 opposite to the bottom 462 of the main body 4100 of the tubular container. Figure 24 In the closure portion 451, at the end edge (peripheral portion), the top 461 of the main body portion 4100 of the tubular container is bonded to the surface of the closure portion 451 opposite to the bottom 462 side of the main body portion 4100. Therefore, in the mounting positions of the tubular main body sealing portion, bottom 462, and outlet portion 450 of the main body portion 4100, the contents will not contact the end face 441 of the paper layer 420. As a whole, the contents of the tubular container 4300 using the main body portion 4100 will not contact the end face 441 of the paper layer 420.

[0322] There is no particular limitation on the bonding method between the main body 4100 and the closure 451 of the tubular container. For example, the following method can be used: a second sealant layer containing polyethylene is provided on the innermost layer of the laminated sheet 410, and the injection outlet 450 is formed using a material containing polyethylene, and then they are heat-fused together.

[0323] The hinge cover (not shown) is a component that is installed on the injection outlet 450 and enables the opening formed in the injection outlet 450 to be closed and opened.

[0324] It should be noted that the method of closing and opening the opening formed in the injection outlet 450 is not limited to a hinged cover. For example, it may also include a cylindrical portion having an external thread provided in the injection outlet 450 and a cover having an internal thread that can be screwed into the external thread.

[0325] In the tubular container 4300, the dispensing outlet 450 has a flat, closed portion 451 orthogonal to the height direction of the main body 4100 of the tubular container. Simultaneously, at the end edge of the closed portion 451, the top 461 of the main body 4100 of the tubular container is adhered to the surface of the closed portion 451 opposite to the bottom 462 side of the main body 4100. Therefore, by bending the main body 4100 at the end edge of the closed portion 451 with a finger or the like, the contents slightly remaining in the main body 4100 can be squeezed out towards the periphery of the opening of the dispensing outlet 450 through the plane clamped between the inner side of the closed portion 451 and the inner surface of the main body 4100.

[0326] Furthermore, since the closing portion 451 of the dispensing outlet 450 is flat, unlike the conical dispensing outlet 450 in the prior art, there is no space on the inner side for contents to remain. Therefore, the contents squeezed out to the periphery of the opening of the dispensing outlet 450 do not remain inside the main body 4100 and the dispensing outlet 450, but are squeezed out from the opening. As a result, the retention of contents inside the container can be suppressed.

[0327] It should be noted that, in the tubular container 4300, as described above, by extruding the contents while bending the main body 4100, the residue of the contents can be suppressed. Therefore, it is preferable to use a laminated sheet 410 with low rigidity (not strong) that is easy to bend to form the main body.

[0328] As described above, by setting the thickness of the laminated sheet 410 constituting the main body 4100 of the tubular container to 30 μm or more and 300 μm or less, the contents can be easily squeezed out with a slight force in the tubular container 4300 using the main body 4100 of the tubular container made of the laminated sheet 410, thereby suppressing the residue of the contents. In addition, the main body 4100 of the tubular container can be easily bent.

[0329] Furthermore, when the hinged cover is provided as a cover, compared with the case where the cover is provided and the closing part 451 is screwed and rotated to open, the rigidity relative to the torsion required to hold the main body by hand when opening can be reduced, so it is easier to use a laminated sheet 410 with low rigidity, which is therefore preferred.

[0330] <Fifth Implementation>

[0331] In the case of tubular containers that use resin and paper in the main body, from the viewpoint of resource recycling, it is preferable to be able to separate the membrane and paper for disposal. However, in tubular containers that have been studied in the past and which use paper as part of the material constituting the main body, it is not possible to separate the membrane and paper.

[0332] This embodiment provides a tubular container capable of separating the membrane and paper constituting the main body.

[0333] The tubular container involved in this embodiment has the same... Figure 11 and Figure 12 The tubular main body and the inlet port mounted on the main body are the same as those in the tubular container shown in the third embodiment. However, the sheet material constituting the main body is different from the sheet material constituting the main body in the third embodiment.

[0334] Figures 25-29 This is a cross-sectional view showing an example of the sheet material that constitutes the main body of the tubular container. Figure 30 This is a cross-sectional view of the main body of the tubular container.

[0335] The main body of the tubular container is composed of sheet 541. Sheet 541 is a multilayer sheet, wherein a substrate film layer 133, a barrier layer 134, and a sealant layer 135 are sequentially laminated on one side of paper layer 132, and a paper protective layer 137 is laminated on the other side of paper layer 132, and an ink layer 138 and an outer coating varnish layer 139 are further laminated on the paper protective layer 137. An adhesive can be used to bond the layers together.

[0336] The paper layer 132 and the substrate film layer 133 are easily peelable. That is, the peel strength between the paper layer 132 and the substrate film layer 133 is designed to be weaker than the peel strength between other layers, thus allowing the paper layer 132 to be peeled off from the substrate film layer 133. By peeling the paper layer 132 from the substrate film layer 133, the paper layer 132 and the layers stacked on top of the paper layer 132 can be easily separated. Figures 25-29 The paper protective layer 137, ink layer 138, and outer varnish layer 139 are separated from the sheet 541. The peel strength between the paper layer 132 and the substrate film layer 133 is 0.5 N / 15 mm or more and 10 N / 15 mm or less, more preferably 1 N / 15 mm or more and 3 N / 15 mm or less. When the peel strength is less than 0.5 N / 15 mm, the adhesive strength is weak, and the paper layer 132 may be unintentionally peeled off during the use of the tubular container 5100. When the peel strength exceeds 10 N / 15 mm, the peel strength is strong, and the paper layer 132 is difficult to separate from the substrate film layer 133.

[0337] It should be noted that the paper layer 132, substrate film layer 133, barrier layer 134, sealant layer 135, paper protective layer 137, ink layer 138, and outer varnish layer 139 can be used in the same configuration as those described in the first embodiment. Furthermore, the total thickness of the sheet 541 constituting the main body and the proportion of paper (pulp fiber) can be set within the same range as in the first embodiment. One or more layers other than the paper layer 132 and sealant layer 135 can be omitted from the sheet 541.

[0338] In this embodiment, the area weight of the paper used for paper layer 132 is 30 to 300 g / m². 2 The preferred value is 50–170 g / m³. 2 Furthermore, in this embodiment, the sealant layer 135 is a layer provided for welding the adhesive portion 507 and the injection port portion to the main body portion. In this embodiment, the thickness of the paper protective layer 137 is preferably 0.2 to 50 μm, more preferably 0.5 to 20 μm.

[0339] Next, a method for imparting easy peelability between the paper layer 132 and the substrate film layer 133 will be described. As an example of imparting easy peelability, such as... Figure 25 The method shown describes a method of laminating an easy-peel layer 536a between a paper layer 132 and a substrate film layer 133. The easy-peel layer 536a is, for example, a layer containing an easy-peel material, a pseudo-adhesive, etc., and is provided to weaken the peel strength between the paper layer 132 and the substrate film layer 133. The following describes the case where an easy-peel material and a pseudo-adhesive are used as the easy-peel layer 536a.

[0340] (Method using EP material)

[0341] As the easy-peel layer 536a laminated between the paper layer 132 and the substrate film layer 133, an EP layer made of an easy-peel (EP) material can be laminated. By using an EP material with a peel strength of 0.5 N / 15 mm or more and 10 N / 15 mm or less, the peel strength between the paper layer 132 and the substrate film layer 133 can be set to 0.5 N / 15 mm or more and 10 N / 15 mm or less, allowing the paper layer 132 and the substrate film layer 133 to be peeled off. It should be noted that the peel strength between the paper layer 132 and the substrate film layer 133 is essentially equal to the peel strength of the EP material. Therefore, by adjusting the peel strength of the EP material, the peel strength between the paper layer 132 and the substrate film layer 133 can be appropriately set. Examples of EP materials include easy-peel films and hot-melt materials with weak cohesion.

[0342] (Using a pseudo-adhesive)

[0343] In the bonding of paper layer 132 and substrate film layer 133, a pseudo-adhesive such as a pressure-sensitive adhesive or a re-peelable adhesive can be used. In this case, the applied pseudo-adhesive acts as a re-peelable layer 536a. The material and application amount of these pseudo-adhesives can be appropriately selected and adjusted so that the peel strength between paper layer 132 and substrate film layer 133 is between 0.5 N / 15 mm and 10 N / 15 mm. Therefore, the peel strength between paper layer 132 and substrate film layer 133 can be appropriately set, and the paper layer 132 and substrate film layer 133 can be peeled off.

[0344] In addition, as another method to impart easy peelability between the paper layer 132 and the substrate film layer 133, for example, Figures 26-28 As shown, the peel strength between the paper layer 132 and the substrate film layer 133 is weakened by patterned application of a release varnish or an easy-to-adhere varnish. The following will describe the case of patterned application of a release varnish or an easy-to-adhere varnish.

[0345] (A method for applying patterned stripping varnish)

[0346] like Figure 26 As shown, by patterning a peelable varnish (peelable varnish) 536b onto at least one of the surfaces of the paper layer 132 on the side of the substrate film layer 133 and the surface of the substrate film layer 133 on the side of the paper layer 132, the paper layer 132 and the substrate film layer 133 can be bonded together by an adhesive. The amount and pattern of the peelable varnish 536b are appropriately adjusted so that the peel strength between the paper layer 132 and the substrate film layer 133 is between 0.5 N / 15 mm and 10 N / 15 mm. Thus, the peel strength between the paper layer 132 and the substrate film layer 133 can be appropriately set, and the paper layer 132 and the substrate film layer 133 can be peeled off. When laminating the substrate film layer 133 and the paper layer 132, a thermoplastic resin can be extruded using an extruder, which strongly adheres to the substrate film layer 133 and the paper layer 132 but not strongly adheres to the peelable varnish.

[0347] (A method for applying patterned, easily adhesive clear varnish)

[0348] like Figure 27 and Figure 28As shown, a film layer 536c made of the same material as the substrate film layer 133 is laminated on the surface of the paper layer 132 on the side of the substrate film layer 133. A patterned varnish (easy-to-adhere varnish) 536d with easy-to-adhere properties is applied to at least one of the surfaces of the substrate film layer 133 on the paper layer 132 side and the surface of the film layer 536c on the substrate film layer 133 side. Further, a resin layer 536f is laminated adjacent to the easy-to-adhere varnish 536d. The resin layer 536f is made of a material that has the property of strongly adhering to the easy-to-adhere varnish 536d without fusing to the substrate film layer 133 (film layer 536c), and has a peel strength of 0.5 N / 15 mm or more and 10 N / 15 mm or less with the substrate film layer 133 (film layer 536c). Therefore, the paper layer 132 and the substrate film layer 133 can be peeled off by peeling the film layer 536c from the resin layer 536f, or by peeling the resin layer 536f from the substrate film layer 133. It should be noted that the peel strength between the paper layer 132 and the substrate film layer 133 is approximately equal to the peel strength between the resin layer 536f and the substrate film layer 133 (film layer 536c). Therefore, by appropriately selecting the materials of the resin layer 536f and the substrate film layer 133 (film layer 536c), the peel strength between the paper layer 132 and the substrate film layer 133 can be appropriately set.

[0349] Alternatively, as another method to impart easy peelability between the paper layer 132 and the substrate film layer 133, for example, a paper with specific properties can be used as the paper layer 132. In this case, a general adhesive 536e, which is also used for bonding other layers, can be used to bond the paper layer 132 and the substrate film layer 133. Hereinafter, using Figure 29 The use of paper with specific properties in paper layer 132 is explained.

[0350] (A method for adjusting the surface smoothness of the paper layer)

[0351] As the paper layer 132, paper with a surface smoothness of 20 to 300 seconds in the Becker smoothness specification as specified in JISP 8119 is used. The surface of the paper layer 132 with this smoothness has a finely textured surface, and the paper layer 132 contacts the substrate film layer 133 or the adhesive 536e coated on the substrate film layer 133 in a point-like manner, thus reducing the bonding area and peel strength. Therefore, by using paper with a surface smoothness of 20 to 300 seconds, the peel strength between the paper layer 132 and the substrate film layer 133 can be set to 0.5 N / 15 mm or more and 10 N / 15 mm or less, thereby enabling the paper layer 132 and the substrate film layer 133 to peel off. As the adhesive 536e used to bond the paper layer 132 and the substrate film layer 133 together, examples include polyolefin resins, with a thickness preferably of 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. When the thickness is less than 10 μm, the peel strength between the paper layer 132 and the substrate film layer 133 is weak; when it exceeds 100 μm, the peel strength is too strong and cannot be easily peeled off. Therefore, the peel strength between the paper layer 132 and the substrate film layer 133 can be appropriately set by adjusting the surface smoothness of the paper and the material and thickness of the adhesive.

[0352] The method described above for imparting easy peelability between the paper layer 132 and the substrate film layer 133 is one example. It is not limited to the method described above, as long as the peel strength between the paper layer 132 and the substrate film layer 133 is between 0.5 N / 15 mm and 10 N / 15 mm. Alternatively, the peel strength between the paper layer 132 and the substrate film layer 133 can be adjusted by appropriately combining the above methods.

[0353] use Figure 30 The method for separating the paper layer 132 from the main body 501 of the tubular container 5100 will be described. Figure 30 In this context, A refers to paper layer 132 and the layer stacked on top of paper layer 132, which is a layer separate from the main body 501. Figure 30 (a) shows the state before separation. From this state, the paper layer 132 is peeled off from the main body 501, starting from the adhesive portion 507. Figure 30 (b)), and peeled off intact along the outer periphery of the film in the main body 501, finally separating the paper layer 132 and the layers stacked on the paper layer 132 from the main body 501. Figure 30 (c) Additionally, a cut can be formed in a portion of the adhesive portion 507. By forming the cut, it can serve as the starting point for separating the paper layer 132 from the substrate film layer 133, further facilitating the separation of the paper layer 132 from the substrate film layer 133. The cut can be provided only in the paper layer 132 and the layers stacked on the paper layer 132, or it can be provided in all the layers constituting the sheet 541.

[0354] As described above, in this embodiment, since the peel strength between the paper layer 132 and the substrate film layer 133 is 0.5 N / 15 mm or more and 10 N / 15 mm or less, the paper layer 132 can be separated from the main body 501 starting from the adhesive portion 507, and the paper layer 132 will not be unintentionally peeled off during the use of the tubular container 5100. Therefore, according to this embodiment, a tubular container 5100 capable of separating the film and paper constituting the main body 501 can be provided.

[0355] In addition, if the peel strength between the paper layer 132 and the substrate film layer 133 is more than 1N / 15mm and less than 3N / 15mm, the paper layer 132 can be more easily separated from the main body 501.

[0356] The tubular container of this embodiment is described below.

[0357] [1] A tubular container, comprising:

[0358] A tubular main body, closed at one end, is formed of a sheet material having, in sequence, a paper layer, a substrate film layer, and a sealant layer, with a thickness of 30 μm to 300 μm; and

[0359] The injection port is installed at the other end of the main body.

[0360] The peel strength when peeling the paper layer from the substrate film layer is 0.5 N / 15 mm or more and 10 N / 15 mm or less.

[0361] [2] The tubular container described in Project [1]

[0362] The peel strength is above 1N / 15mm and below 3N / 15mm.

[0363] [3] The tubular container as described in item [1] or [2]

[0364] An easily peelable material is laminated between the paper layer and the substrate film layer.

[0365] [4] The tubular container as described in item [1] or [2]

[0366] A peelable varnish is patterned and coated on at least one of the substrate film side surface of the paper layer and the paper side surface of the substrate film layer.

[0367] [5] The tubular container as described in item [1] or [2],

[0368] A film layer made of the same material as the substrate film layer is laminated on the surface of the paper layer on the side of the substrate film layer.

[0369] A patterned, easily adhesive varnish is applied to at least one of the paper-side surface of the substrate film layer and the substrate-side surface of the film layer.

[0370] A resin layer is laminated at the location in contact with the easily adhesive varnish, the resin layer having the characteristic of strong bonding with the easily adhesive varnish but not bonding with the substrate film layer.

[0371] [6] The tubular container as described in item [1] or [2],

[0372] The paper layer and the substrate film layer are bonded together by a pressure-sensitive adhesive or a peelable adhesive.

[0373] [7] The tubular container as described in item [1] or [2],

[0374] The Beck smoothness of the surface of the paper layer is between 20 seconds and 300 seconds.

[0375] [8] The tubular container according to any one of items [1] to [7],

[0376] After peeling the paper layer from the substrate film layer, the mass of the paper layer remaining on the substrate film layer side is less than 5% of the mass of the paper layer, or the mass of the substrate film layer remaining on the paper layer side after peeling the paper layer from the substrate film layer is less than 5% of the mass of the substrate film layer.

[0377] <Sixth Implementation>

[0378] The main body of the tubular container is formed by making a sheet constituting the main body into a cylindrical shape and gluing the two ends together. Methods of gluing the sheet include: "clasp-together gluing" (where the inner surfaces of the sheets are glued together and fused together); "butt-sealing gluing" (where the butt joints of the two ends of the sheets are sealed with a strip); and "sealing tape gluing" (where the inner and outer surfaces of the sheets are overlapped and sealed with a strip). However, clasp-together gluing causes the glued part to protrude from the main body, which can lead to the glued part touching the hand during use and reducing operability.

[0379] Compared to adhesive tape, the adhesive portion does not protrude from the main body in butt-joint adhesive tape and sealing tape adhesive tape, which is preferable for ease of operation. In the tape used to adhesively attach the main body, in addition to the resin layer that can be fused to the main body, a barrier layer can also be provided to ensure the barrier properties of the adhesive portion. In the case of such a multi-layered structure, the adhesive disposed between the layers is exposed from the ends of the tape, and the adhesive may dissolve from the contents side. Furthermore, the interfaces between the layers of the tape are exposed, so interlayer peeling of the tape constituting the main body may occur.

[0380] This embodiment provides a tubular container with excellent operability that can suppress adhesive leaching from the ends of the strip and interlayer delamination of the strip.

[0381] Figure 31 This is a front view illustrating a schematic configuration of the tubular container according to this embodiment. Figure 32 It is along Figure 31 The end view of line XXXII-XXXII shown in the figure. Figure 33 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0382] The tubular container 6100 has a tubular main body 601 and an outlet 602 installed on the main body 601.

[0383] The main body 601 is a component for accommodating contents, and a sheet 641 having a pair of generally parallel opposing end edges is formed into a cylindrical shape. As a method for attaching the two ends of the sheet 641, methods such as... Figure 32 As shown in (a), the strip 620 is used to seal the butt joint formed by joining the two ends of the sheet 641, starting from the inner surface of the sheet 641; as shown in (a), the butt joint is sealed by bonding the strip 620 to the butt joint formed by joining the two ends of the sheet 641. Figure 32 As shown in (b), the sealing tape is attached to the inner and outer surfaces of the sheet 641 using tape 620, starting from the inner surface. One end 605a of the main body 601 ( Figure 31 The lower end of the main body 601 is sealed and closed. On the other hand, the other end 605b of the main body 601 ( Figure 31 The portion near the upper end of the body portion 601 is sealed to the outside 608 of the flange portion 604 (described later) in a folded state. Multiple pleats 612, formed by folding the sheet 641 constituting the body portion 601, are formed at the weld between the body portion 601 and the flange portion 604. Additionally, an adhesive portion 607 (backing portion) is formed on the body portion 601. The body portion 601... Figure 31 The length in the vertical direction can be set to, for example, 50 to 250 mm.

[0384] like Figure 33 As shown, the sheet 641 constituting the main body 601 of the tubular container 6100 is a multilayer sheet, wherein a substrate film layer 133, a barrier layer 134, and a sealant layer 135 are sequentially stacked on one side of the paper layer 132, and a paper protective layer 137 is stacked on the other side of the paper layer 132.

[0385] It should be noted that the paper layer 132, substrate film layer 133, barrier layer 134, sealant layer 135, and paper protective layer 137 can be constructed using the configurations of the layers described in the first embodiment. Furthermore, the total thickness of the sheet 641 constituting the main body 601 and the proportion of paper (pulp fiber) can be set within the same range as in the first embodiment. One or more layers other than the paper layer 132 and sealant layer 135 can be omitted from the sheet 541.

[0386] In this embodiment, the weight per unit area of ​​the paper used for paper layer 132 is preferably 50 to 200 g / m². 2 More preferably 70–150 g / m 2 The barrier layer 134 can be, for example, GL-RD (manufactured by Toppan Printing Co., Ltd.) as a barrier film. The substrate film layer 133 can be, for example, ONBC (manufactured by Unitika Co., Ltd.). In this embodiment, the sealant layer 135 is provided for welding the tape 620 to the main body 601 in the adhesive portion 607, and for welding the injection port 602 to the main body 601. In this embodiment, the thickness of the paper protective layer 137 is preferably 0.2 to 50 μm, more preferably 0.5 to 20 μm. An ink layer can be provided between the paper layer 132 and the paper protective layer 137. Furthermore, the stacking order of the paper protective layer 137 and the ink layer can be reversed; in this case, to impart abrasion resistance, etc., an external varnish layer as described in the first embodiment can be stacked on the ink layer. Additionally, an adhesive can be used to bond the layers together.

[0387] use Figures 34-36 The application of the strip 620 to both ends of the sheet 641 is explained. Figure 34 and Figure 35 This diagram illustrates the state before the strip is attached to the main body. Figure 36 This diagram illustrates the state after the strip has been attached to the main body.

[0388] The strip 620 includes a first resin layer 621, a second resin layer 622, and a substrate 623. A main body 601 is formed by fusing the strip 620 to the sealant layer 135, including a pair of end edges of a sheet 641 and / or their vicinity. The substrate 623 has a strip-like shape, with one side covered by the first resin layer 621 and the other side covered by the second resin layer 622. When the strip 620 is fusing to the main body 601, the first resin layer 621 is laminated on one side of the substrate 623 relative to the main body 601, and the second resin layer 622 is laminated on the opposite side.

[0389] The first resin layer 621 is a layer that can be fused to the sealant layer 135 of the main body 601. Before fusion, the thickness of the first resin layer 621 is 10 μm to 70 μm, more preferably 20 μm to 50 μm. The material of the first resin layer 621 is not particularly limited as long as it can be fused to the sealant layer 135 of the main body 601; for example, thermoplastic resins such as polypropylene, polyethylene, cyclic polyolefins, and polyester can be used. In particular, it is preferable to use the same material as the thermoplastic resin used for the sealant layer 135. By using the same thermoplastic resin for the first resin layer 621 as the thermoplastic resin layer used for the sealant layer 135, the sealing strength between the main body 601 and the strip 620 can be improved.

[0390] Before welding, the thickness of the second resin layer 622 is 10 μm to 70 μm, more preferably 20 μm to 50 μm. The material of the second resin layer 622 can be, for example, thermoplastic resins such as polypropylene, polyethylene, cyclic polyolefins, and polyester. In particular, it is preferable to use the same material as the thermoplastic resin used for the first resin layer 621.

[0391] The substrate 623 is a functional layer with barrier and light-shielding properties. It can be appropriately selected from stretch films such as polypropylene, metal vapor-deposited films such as aluminum, and metal foils such as aluminum, depending on the desired function. The substrate 623 can be a single layer or multiple layers, and its thickness can be, for example, 9–40 μm. When using a transparent barrier film as the substrate 623, GL-RD, GL-ARH, GL-AE, GL-AN, and GX (manufactured by Toppan Printing Co., Ltd.) can be appropriately selected, for example.

[0392] The strip 620 and the sheet 641 are fused together by heat sealing using a sealing strip. The sealing strip is wider than the strip 620, i.e., it has a heating section capable of being heated in a manner that covers the strip 620. Therefore, as... Figure 34 As shown in the strip 620, even if the substrate 623 is exposed from the end face of the strip 620, it can be welded as shown in the figure. Figure 35 In this way, the end face of the strip 620 is covered (protected) by the resin of the first resin layer 621 or the second resin layer 622, which has melted during welding. Therefore, the interlayer adhesive can be prevented from dissolving from the end of the strip into the tubular container, thereby preventing the deterioration of the taste and color of the contents of the tubular container 6100. In addition, interlayer delamination of the strip 620 can be prevented.

[0393] It should be noted that, as Figure 36As shown in the strip 620, the end faces can be covered by end-face resin 624 in the state before welding. Even in this case, in the state before welding, the thickness of the first resin layer 621 is 10μm to 70μm, more preferably 30μm to 50μm, and the thickness of the second resin layer 622 is 10μm to 70μm, more preferably 30μm to 50μm. At this time, the sealing strip used for welding can be narrower than the width of the strip 620. Even when using a narrow sealing strip, since the end faces of the strip 620 are pre-covered by the end-face resin 624, it remains as... Figure 35 That way, the end face of strip 620 is covered (protected). Figure 36 The strip 620 shown can be fabricated, for example, by ultrasonic slits, in which case the end-face resin 624 is made of the same material as the first resin layer 621 or the second resin layer 622.

[0394] As described above, in the tubular container 6100 of this embodiment, the end face of the strip 620 adhered to the main body 601 is covered by the first resin layer 621 or the second resin layer 622 that melted during the welding of the strip 620. Therefore, even if the strip has a multilayer structure, it is possible to prevent the adhesive between the layers from dissolving from the end of the strip, and in addition, it is possible to suppress interlayer peeling of the strip.

[0395] In addition, the substrate 623 of the strip 620 has barrier properties. As a result, the barrier properties of the joint of the sheet 641 of the tubular container 6100 are improved.

[0396] Furthermore, in the state before welding, the thickness of both the first resin layer 621 and the second resin layer 622 of the strip 620 is more than 10 μm and less than 70 μm, and the strip 620 is welded using a sealing strip that is wider than the strip 620. Therefore, the end face of the strip 620 can be covered (protected) by the resin of the first resin layer 621 or the second resin layer 622 that has melted during welding.

[0397] Furthermore, in the state before welding, the end face of the strip 620 can also be covered by the end face resin 624. Thus, even when welding is performed using a sealing strip narrower than the width of the strip 620, the end face of the strip 620 can be covered by the resin from the first resin layer 621 or the second resin layer 622 that melted during the welding of the strip 620.

[0398] The method for manufacturing the tubular container involved in this embodiment is as follows.

[0399] [1] A method for manufacturing a tubular container, the tubular container comprising: a main body formed by forming a sheet having a pair of opposing end edges into a cylindrical shape, and attaching strips to portions of the pair of end edges along the inner surface of the sheet; and an outlet portion mounted to one end of the main body.

[0400] The strip material has the following features:

[0401] Barrier strip-shaped substrate,

[0402] The first resin laminated on one side of the main body portion of the substrate, and

[0403] A second resin is laminated on the side of the substrate opposite to the main body.

[0404] The first resin layer has a thickness of 10 μm or more, or 70 μm or more.

[0405] The second resin layer has a thickness of 10μm to 70μm.

[0406] The strip is heat-sealed to the body using a sealing strip that is wider than the strip itself.

[0407] [2] A method for manufacturing a tubular container, the tubular container comprising: a main body formed by forming a sheet having a pair of opposing end edges into a cylindrical shape, and attaching strips to portions of the pair of end edges along the inner surface of the sheet; and an outlet portion mounted to one end of the main body.

[0408] The strip material has the following features:

[0409] Barrier strip-shaped substrate,

[0410] The first resin laminated on one side of the main body portion of the substrate, and

[0411] A second resin is laminated on the side of the substrate opposite to the main body.

[0412] The first resin layer has a thickness of 10 μm or more, or 70 μm or more.

[0413] The second resin layer has a thickness of 10μm to 70μm.

[0414] The end face of the strip is coated with the same resin as the first resin or the second resin.

[0415] The strip is heat-sealed to the main body using a sealing strip.

[0416] <Seventh Implementation>

[0417] The paper-containing body cannot be aesthetically pleasingly formed on the flat periphery of the injection port, resulting in a poor appearance and unstable sealing of the mounting part.

[0418] This embodiment provides a tubular container in which a paper-containing main body with pleats can be formed on the flat periphery of the inlet, resulting in a good appearance and easy and stable sealing of the mounting part.

[0419] Figure 37 (a) is a front perspective view of the area near the other end 721 of the main body 720 and the inlet 710 of the tubular container 7100 according to the seventh embodiment before the main body 720 and the inlet 710 are installed. Figure 37 (b) is a front perspective view of the other end 721 of the main body 720 and the outlet 710 of the tubular container 7100 according to the seventh embodiment after the other end of the main body 720 is folded at the periphery 713 of the flange 712 and welded. Figure 38 (a) is a front view of the tubular container 7100 according to the seventh embodiment. Figure 38 (b) is a side view of the tubular container 7100 according to the seventh embodiment. Figure 39 It is along Figure 38 (b) An enlarged cross-sectional view of the GG line near the injection outlet 710. Figure 40 (a) is a top view of the tubular container 7100 according to the seventh embodiment. Figure 40 (b) is along Figure 40 (a) Enlarged cross-sectional view of the HH line.

[0420] like Figure 38 As shown, the tubular container 7100 includes a main body 720 closed at one end and an outlet 710 installed at the other end 721 of the main body 720, which contains contents (not shown). Figure 38 In the above-mentioned main body 720, one end is the bottom 727 of the tubular container 7100.

[0421] The main body 720 consists of components with a weight per unit area greater than 30g / m². 2 And less than 300g / m 2 A laminated sheet 750 of paper is formed. In the main body 720, for example, the laminated sheet 750 having a pair of substantially parallel end edges is formed into a cylindrical shape with a substantially circular cross-sectional shape, and a backing seal 726 is formed by joining and fusing the inner surfaces of the strip-shaped portions that respectively contain a pair of end edges of the laminated sheet 750 together in a palm-like shape. Figure 37 and Figure 38(Not shown in the diagram). The main body 720 can be manufactured using a bag-making machine, pillow / core packaging machine, etc. Here, "cross-sectional shape" refers to... Figure 38 The cross-sectional shape of the main body 720 in a plane (cross section) orthogonal to the central axis X of the tubular container 7100.

[0422] There is no particular limitation on the method of bonding the laminated sheets 750 in the bottom 727 to each other. For example, the following method can be used: an adhesive layer containing polyethylene is provided between the innermost layers of the opposing laminated sheets 750, and they are thermally fused together.

[0423] like Figure 37 , Figure 38 As shown, the injection outlet 710 has a cylindrical injection cylinder 711 and a flat flange 712 connected to one end of the injection cylinder 711 and orthogonal to the height direction of the main body 720. The flange 712 is a portion extending outward from one end of the injection cylinder 711. When viewed from the height direction of the main body 720, the peripheral edge 713 of the flange 712 is approximately circular in shape. Furthermore, in the peripheral edge 713 of the flange 712, the other end 721 of the main body 720 is mounted on the surface of the flange 712 opposite to the end side of the main body 720. Here, "height direction" refers to... Figure 38 The direction of the central axis X of the tubular container 7100.

[0424] The material of the outlet portion 710 is not particularly limited, but resin materials such as low-density polyethylene are preferred. Furthermore, by using a material that also provides a barrier function to the outlet portion 710 along with the main body portion 720, the overall barrier function of the tubular container 7100 can be improved, thereby further protecting the quality of the contents. Compared to the conical outlet portion 710 of the prior art, the flat-plate outlet portion 710 of the flange portion 712 reduces the amount of material used.

[0425] Because the flange 712 is flat, unlike the conical flange 712 in the prior art, there is no space on the inner side for contents to remain. Therefore, by bending the main body 720 at the edge of the flange 712 with a finger or the like, any contents that remain slightly in the main body 720 can be squeezed out towards the periphery of the opening of the dispensing outlet 710 through the plane clamped between the inner side of the flange 712 and the inner surface of the main body 720. Furthermore, the contents squeezed out towards the periphery of the opening of the dispensing outlet 710 do not remain inside the main body 720 and the dispensing outlet 710, but are squeezed out from the opening. As a result, the retention of contents inside the container can be suppressed.

[0426] It should be noted that, as described above, by extruding the contents while bending the main body 720, the residue of the contents can be suppressed. Therefore, it is preferable to form the main body 720 using a laminated sheet 750 with low rigidity that is easy to bend.

[0427] By setting the thickness of the laminated sheet 750 constituting the main body 720 to 30 μm or more and 300 μm or less, the main body 720 of the tubular container 7100 can be easily bent, thus it can be easily molded, and the contents can be easily squeezed out with a slight force, thus suppressing the residue of the contents.

[0428] like Figure 39 As shown, in the peripheral portion 713 of the flat flange portion 712 orthogonal to the height direction of the main body portion 720, the other end 721 of the main body portion 720 is mounted on the surface of the flange portion 712 opposite to one end of the main body portion 720. Additionally, as... Figure 40 As shown in (b), the other end 721 of the main body 720 is folded back to form a pleat 723, with the inner surfaces of the stacked sheets 750 contacting each other, and is installed on the peripheral portion 713. This pleat 723 is folded in one direction (right or left) on the outside of the other end 721 of the main body 720 on the peripheral portion of the flange 712, and is sealed together on the outside of the other end 721 of the main body 720 on the peripheral portion of the flange 712. By folding the pleat 723 in one direction, a more stable and aesthetically pleasing pleat 723 can be formed. Here, "on the peripheral portion" refers to the side of the peripheral portion 713 opposite to one end of the main body 720. Additionally, "the outside of the other end of the main body" refers to the side of the other end 721 of the main body 720 opposite to the contents.

[0429] In addition, such as Figure 37 As shown, the other end 721 of the main body 720 has a first grid line 724 and a second grid line 725, and bends along the first grid line 724 and the second grid line 725. A fold 723 is formed on the outside of the other end 721 of the main body 720 on the periphery of the flange 712, and is mounted on the periphery 713.

[0430] Figure 37 (a) shows the main body 720, on which the first grid line 724 and the second grid line 725 are formed, separated from the outlet section 710. However, as will be described later, according to the manufacturing method of the tubular container 7100, the first grid line 724 and the second grid line 725 are formed on the main body 720, which is formed by inserting a mandrel on which the outlet section 710 is mounted.

[0431] like Figure 37As shown in (a), the first grid line 724 is a bend line, which is formed in the circumferential direction of the main body 720 so as to bend at the center side of the main body 720 and be installed on the peripheral part 713 of the flange part 712. For example, it is formed in a straight line in the circumferential direction of the main body 720.

[0432] The second grid line 725 is configured such that one mountain fold line 7251 and two valley fold lines 2521 and 2522 are grouped together, and two or more groups are evenly formed along the circumferential direction of the periphery 713 of the flange portion 712.

[0433] Figure 41 (a) is Figure 37 (a) A front enlarged view of the vicinity of the other end 721 of the main body 720 of the tubular container 7100. That is, a front enlarged view of the vicinity of the other end 721 of the main body 720 in the state before the main body 720 and the outlet 710 of the tubular container 7100 according to the seventh embodiment are installed. Figure 41 (b) is Figure 37 (a) A top enlarged view of the tubular container 7100 near the other end 721 of the tubular container 720 after the main body 720 has been folded back on the periphery 713 of the flange 712. Figure 41 (c) is Figure 37 (b) A top enlarged view of the vicinity of the other end 721 of the main body 720 of the tubular container 7100. That is, a top enlarged view of the vicinity of the other end 721 of the main body 720 of the tubular container 7100 according to the seventh embodiment after the other end 721 of the main body 720 has been folded and welded on the periphery 713 of the flange 712.

[0434] Figure 41 The inner circumferential surface of the main body 720 is shown. Figure 41 The outlet section is not intentionally shown in the text.

[0435] like Figure 41 As shown in (a), a mountain zigzag line 7251 extends approximately at a right angle to the first grid line 724 from the edge 722 on the other side of the main body 720 toward a point on the first grid line 724. Two valley zigzag lines 2521 and 2522 extend symmetrically to the mountain zigzag line 7251 from the aforementioned point on the first grid line 724, in an oblique direction from the edge 722 on the other side of the main body 720 toward the vertex of the first grid line 724, forming an isosceles triangle with the edge 722 on the other side of the main body 720 as its base. Figure 41In this configuration, the line extending diagonally upwards and to the left from the aforementioned point on the first grid line 724 relative to a mountain fold line 7251 becomes the first valley fold line 2521; the line extending diagonally upwards and to the right from the aforementioned point on the first grid line 724 relative to a mountain fold line 7251 becomes the second valley fold line 2522. The mountain fold line 7251 becomes the line that bisectes the isosceles triangle formed by the first valley fold line 2521 and the second valley fold line 2522, with the edge 722 on the other side of the main body 720 as its base.

[0436] Let A be the length of the outer periphery of the main body 720 near the peripheral edge 713 of the flange 712, let B be the diameter of the outer periphery of the main body 720 near the peripheral edge 713 of the flange 712, and let C be the length of the line extending approximately perpendicularly to the first grid line 724 from the edge 722 on the other side of the main body 720 (the amount of bending of the main body 720 toward the peripheral edge of the flange 712) (refer to...). Figure 41 (a) Furthermore, let D be the length of the base of the isosceles triangle of the edge 722 on the other end side of the main body 720, and let E be the number of sets of one mountain fold line 7251 and the two valley fold lines 2521 and 2522. In addition, when F is set as the circumference of the circle with a diameter of (BC×2) (the circumference of the circle formed by bending the edge 722 of the other end 721 of the main body 720 on the periphery of the flange 712), the relationship (AF) / E=D is satisfied.

[0437] For example, the length (A) of the outer periphery of the main body 720 near the peripheral edge 713 of the flange 712 is set to approximately 110 mm, the diameter (B) of the outer periphery of the main body 720 near the peripheral edge 713 of the flange 712 is set to 35 mm, and the length (C) of the line extending approximately perpendicularly to the first grid line 724 from the edge 722 on the other side of the main body 720 is set to 5 mm. In this case, the length of (BC×2) is 25 mm, and the circumference (F) of the circle with a diameter of 25 mm is approximately 78.5 mm. The length of (AF) is approximately 31.5 mm. When the number (E) of the group of one mountain fold line 7251 and the first valley fold line 2521 and the second valley fold line 2522 on the left and right of the mountain fold line 7251 is set to 10, the length (D) of the base of the isosceles triangle of the edge 722 on the other side of the main body 720, i.e. (AF) / E, is approximately 31.5 / 10, approximately 3.2 mm.

[0438] The main body 720 has a unit area weight greater than 30g / m². 2 And less than 300g / m 2As described above, the first grid line 724 and the second grid line 725 are formed on the other end 721 of the main body 720. The other end 721 of the main body 720 is bent along the first grid line 724 and the second grid line 725, and a folded 723 is formed on the outside of the other end 721 of the main body 720 on the periphery of the flange 712, and is installed on the periphery 713 of the flange 712.

[0439] Thus, pleats 723 are uniformly formed along the circumferential direction of the main body 720 on the flat flange 712 of the injection port 710, forming the main body 720 in an aesthetically pleasing manner with a good appearance, and the sealing performance of the mounting part with the flange 712 is easily and stably maintained.

[0440] In addition, such as Figure 28 and Figure 39 As shown, as an example, the dispensing outlet 710 has a closing portion 714 with an annular half-cut 715 at approximately the center, and a pull ring 716 is provided inside the half-cut 715. By providing the half-cut 715 and the pull ring 716, the user of the tubular container 7100 can pull the pull ring 716 and remove a portion of the closing portion 714 along the half-cut 751, thus forming an opening in the closing portion 714 for removing the contents. It should be noted that the half-cut 715 and pull ring 716 may also be omitted, and the opening for removing the contents may be pre-formed in the dispensing outlet 710.

[0441] The tubular container 7100 may include a cap (not shown) that can be installed on and is removable from the dispensing cylinder 711 of the dispensing outlet 710. Examples of removable caps include hinged caps installed on the dispensing outlet 7100 and screw caps that can be installed and removed via threads. When the tubular container 7100 has a removable cap, it is easy to reseal it after opening.

[0442] When a hinged cover is provided as a cover, compared with a cover that is screwed and rotated to open the dispensing cylinder 711, the rigidity of the torsion required to hold the main body 720 by hand when opening the cover can be reduced, and it is easier to use a laminated sheet 750 with low rigidity, so it is preferred.

[0443] Figure 42 This is a cross-sectional view showing the layered structure of the laminated sheet 750 that constitutes the main body 720 of the tubular container 7100 according to this embodiment.

[0444] The main body 720 is composed of a laminated sheet 750, which is mainly composed of paper. The total thickness of the laminated sheet 750 is preferably 30 μm or more and 300 μm or less.

[0445] The laminated sheet 750 is a multi-layer sheet, wherein a substrate film layer 752, a barrier layer 753, and a sealant layer 754 are sequentially laminated on one side of the paper layer 751, a paper protective layer 755 is laminated on the other side of the paper layer 751, an ink layer 756 and an external varnish layer 757 are further laminated on the paper protective layer 755, and a patterned hot-melt coating 758 is applied. The details of each layer are described below.

[0446] (Paper layer)

[0447] Paper layer 751 is a structural layer that imparts strength and rigidity to the tubular container 7100. There are no particular limitations on the type of paper used to constitute paper layer 751, but single-sided or double-sided kraft paper is preferred in terms of strength, bending resistance, and printability. Furthermore, water-resistant or oil-resistant paper can be used as the paper constituting paper layer 751, depending on the requirements. Additionally, paper layer 751 can be paper containing 50% or more cellulose fibers, or it can be a blended paper containing resin fibers other than cellulose fibers.

[0448] The weight per unit area of ​​the paper used for paper layer 751 is greater than 30 g / m². 2 And less than 300g / m 2 More preferably 50g / m 2 Above 250g / m 2 The following is an example: The weight per unit area of ​​the paper used for paper layer 751 is 30 g / m². 2 In the following situations, it is impossible to aesthetically form the first grid line 724 and the second grid line 725 on the main body 720, at 300g / m 2 In the above situations, when the main body 720 is sealed to the periphery 713 of the flange 712, the height difference is difficult to fill, resulting in leakage.

[0449] (Substrate film layer)

[0450] The substrate film layer 752 imparts heat resistance and physical strength to the laminated sheet 750. The substrate film layer 752 also serves as the substrate for the barrier layer 753. There are no particular limitations on the material constituting the substrate film layer 752; from the viewpoint of heat resistance and physical strength, stretched films such as polypropylene, polyester, and polyamide are preferred. However, the substrate film layer 752 may also be made of paper.

[0451] (Barrier layer)

[0452] Barrier layer 753 is a functional layer that blocks oxygen and water vapor to improve the preservation of contents. Barrier layer 753 can be composed of one or more of the following: vapor-deposited films of inorganic compounds such as nylon, silica, or alumina; vapor-deposited films of metals such as aluminum; metal foils such as aluminum; or coatings containing plate-like minerals and / or barrier resins. The barrier resin used in the barrier coating can be ethylene-vinyl alcohol copolymer (EVOH) or polyvinylidene chloride (PVDC), and an adhesive resin other than the barrier resin can be appropriately incorporated into the barrier coating. Barrier layer 753 can be pre-laminated on substrate film layer 752 to form a barrier film, or it can be configured as a single-layer film.

[0453] (Sealant layer)

[0454] The material of the sealant layer 754 is not particularly limited, but thermoplastic resins such as polypropylene, polyethylene, cyclic polyolefins, and polyester are preferred. The sealant layer 754 uses a resin whose softening temperature is at least 20°C lower than that of the substrate film layer 752. If the softening temperature of the sealant layer 754 is not at least 20°C lower than that of the substrate film layer 752, the substrate film layer 752 is more likely to soften and develop pinholes during sealing, which is therefore undesirable. The softening temperature of the sealant layer 754 is preferably at least 40°C lower than that of the substrate film layer 752.

[0455] The thermoplastic resin used for the sealant layer 754 only needs to be adhesive to the thermoplastic resin constituting the injection port portion 710, but it is preferably the same material as the thermoplastic resin used for the injection port portion 710. By using the same thermoplastic resin for the sealant layer 754 and the thermoplastic resin layer for the injection port portion 710, the sealing strength between the main body portion 720 and the injection port portion 710 can be improved.

[0456] (Paper protective layer)

[0457] The paper protective layer 755 is a layer used to protect the paper layer 751 constituting the laminated sheet 750 from the adhesion of contents and dirt. There are no particular limitations on the material and formation method of the paper protective layer 755; it can be laminated by extrusion coating of a thermoplastic resin, coating with a water-resistant agent, or an oil-resistant agent. The thickness of the paper protective layer 755 is preferably 0.2 to 50 μm, more preferably 1 to 20 μm. If the thickness of the paper protective layer 755 is less than 0.2 μm, pinholes may occur in the paper protective layer 755, and the protection of the paper layer 751 may become insufficient. Furthermore, if the thickness of the paper protective layer 755 exceeds 50 μm, it is not preferable from the perspective of resin usage and manufacturing cost.

[0458] (Ink layer, outer varnish layer)

[0459] The ink layer 756 is a layer applied by printing to achieve various displays, and the outer varnish layer 757 is a layer used to impart abrasion resistance, etc. The stacking order of the ink layer 756 and the outer varnish layer 757 can be... Figure 42 The opposite of the above. In addition, the outer varnish layer 757 can also serve as a paper protective layer 755.

[0460] (Thermo-weldable coating)

[0461] The heat-weldable coating 758 is a layer used to impart heat-weldability to the outside of the laminated sheet 750. In this embodiment, the heat-weldable coating 758, which is patterned and applied (partially applied) to the outside of the laminated sheet 750, seals the outside of the backing seal 726 to the outside of the main body 720. At the same time, the pleats 723 formed at the other end 721 of the main body 720 are folded, so that the outside of the other end 721 of the main body 720 on the periphery of the flange 712 is sealed to each other.

[0462] When the heat-welding coating 758 is applied to a portion of the surface of the laminated sheet 750, the heat-welding coating 758 can be applied to the portion where the outer side of the sealing target area (i.e., the backing seal portion 726) contacts the outer side of the main body portion 720, and to the portion where the outer side of the other end 721 of the main body portion 720 on the periphery of the flange portion 712 contacts each other due to the fold 723 formed at the other end 721 of the main body portion 720 being folded. However, the heat-welding coating 758 may also be applied to only one of the contact surfaces of the sealing target area.

[0463] The heat-melting coating 758 can be formed by applying a coating agent containing thermoplastic resins such as acrylic polymers, polyolefins, polyvinyl acetate, and polyesters and then allowing it to dry. In addition to thermoplastic resins, inorganic substances for preventing adhesion may also be incorporated into the coating agent.

[0464] The coating amount of the coating agent used to form the hot-melt coating 758 is 0.2~40 g / m². 2 The preferred concentration is 3.0~30g / m³. 2 When the coating amount of the coating agent is less than 0.2 g / m² 2 In this case, the adhesive strength between the outer surfaces of the laminated sheets 750 is insufficient, and the laminated sheets 750 at the welded portions of the backing seal 726 and pleats 723 to the other end 721 of the main body 720 exhibit a spring-like phenomenon. On the other hand, when the coating amount exceeds 40 g / m²... 2 In such cases, the coefficient of friction increases, reducing the mechanical adaptability to processing devices such as bag making machines, or causing adhesion to easily occur between the stacked sheets at 750°.

[0465] The heat-weldable coating 758 can be applied to the entire surface of the laminated sheet 750, but because the surface of the laminated sheet 750 has a high coefficient of friction, the mechanical adaptability in the processing of the main body 720 and subsequent processes may be reduced. Therefore, from the perspective of mechanical adaptability, it is more preferable to apply the heat-weldable coating 758 to a portion of the surface of the laminated sheet 750 by patterning the coating agent.

[0466] It should be noted that, in Figure 42 In the layered structure of the laminated sheet 750 shown, one or more of the following layers may be omitted: substrate film layer 752, barrier layer 753, paper protective layer 755, ink layer 756, and outer coating varnish layer 757.

[0467] The manufacturing method of the tubular container 7100 includes a process of forming a main body 720 of the tubular container 7100 and a process of installing the main body 720 onto the outlet 710.

[0468] Next, the method for forming the main body 720 of the tubular container 7100 will be described.

[0469] For example, the main body 720 is processed sequentially while being conveyed by a conveying device via laminated sheets 750. The laminated sheets 750 are wound onto a plate-shaped jig with a generally circular cross-section, so that the strip-shaped portions, each containing a pair of end edges, overlap each other. Next, using a guide with an inverted T-shaped cross-section, the strip-shaped portions, each containing a pair of end edges, are stood upright, and their inner surfaces are brought together in a clasped-together position, clamping the guide. Then, using a flat guide, the portion where the inner surfaces of the laminated sheets 750 are joined together in a clasped-together position is bent at approximately 90 degrees to obtain a state where three laminated sheets 750 overlap. In this state, a sealing strip is used to seal the inner surfaces of the laminated sheets 750, fusing them together to form a backing seal 726. Simultaneously, a heat-weldable coating 758 is used to fuse the backing seal 726 to the outside of the main body 720, thereby forming the main body 720.

[0470] The method of installing the main body 720 onto the injection outlet 710 will be described next.

[0471] The method of mounting the main body 720 to the injection outlet 710 may include: mounting the injection outlet 710 to the upper part of the mandrel; inserting the main body 720, whose length in the height direction is longer than the length in the height direction of the mandrel, into the mandrel; fixing the main body 720 at a position protruding from the mandrel by a length C; and forming a first grid line 724 and a second grid line 725 on the main body 720.

[0472] For example, after the injection port 710 is installed onto the upper part of the mandrel, the main body 720, whose length in the height direction is longer than that in the height direction of the mandrel, is inserted into the mandrel, and the main body 720 is fixed at a position where the length C protrudes from the mandrel. Then, the first grid line 724 and the second grid line 725 are formed on the main body 720 using a female mold.

[0473] Regarding the formation of the first grid line 724 and the second grid line 725 on the main body 720, the first grid line 724 and the second grid line 725 can be formed on the main body 720 by heating and pressurizing at a temperature below the melting point of the main body 720. In this method, it is also effective to use a material with low dead angle and high rigidity for the main body 720.

[0474] Furthermore, when the outermost layer of the laminated sheet 750 constituting the main body 720 uses a heat-softened resin, a male mold is not used in the aforementioned heating and pressurization process. Instead, the first grid line 724 and the second grid line 725 are formed by contacting the main body 720 with a female mold and causing the contact portion of the main body 720 to undergo thermal shrinkage. This allows the production of a tubular container 7100 where pleats 723 are uniformly formed along the circumferential direction of the peripheral portion 713, resulting in an aesthetically pleasing main body and easily stable sealing at the mounting portion with the flange portion 712.

[0475] Figure 43 This is a front perspective view showing an example of a mold used to form the first grid line 724 and the second grid line 725 on the main body 720 of the tubular container 7100 according to the seventh embodiment.

[0476] For example, the other end 721 of the main body 720 is shaped like a male mold, and a mold corresponding to this male mold is used. Figure 43 The female mold 770, which has a star-shaped frustum-shaped cross-section, can form the first grid line 724 and the second grid line 725 at the other end 721 of the main body 720.

[0477] Furthermore, regarding the formation of the first grid line 724 and the second grid line 725, in addition to being formed before the welding of the main body portion 720 and the peripheral portion 713 as described above, they can also be formed in the state of the rolled raw material of the laminated sheet 750 or in the state of the sleeve. When the first grid line 724 and the second grid line 725 are formed in the state of the rolled raw material of the laminated sheet 750, the grid lines can also be formed by using a male die and a female die.

[0478] After forming the first grid line 724 and the second grid line 725 as described above, the other end 721 of the main body 720 is bent along the first grid line 724 toward the center side of the main body 720, and as shown... Figure 41As shown in (b), along the mountain fold line 7251 and valley fold lines 2521, 2522 of the second grid line 725, a fold 723 is formed by folding back the laminated sheets 750 in the peripheral portion 713 of the flange portion 712 in such a way that the inner surfaces of the laminated sheets 750 come into contact with each other, and as shown in (b). Figure 41 As shown in (c), for example, the other end 721 of the main body 720 is folded in one direction along the second valley fold line 2522 on the periphery portion 713. Then, an annular heating and pressing device is used to heat and pressurize the entire other end 721 of the main body 720 from above, so as to weld the fold 723 to the periphery portion 713. It should be noted that, as a specific method for welding using a heating and pressing device, hot plate pressing, ultrasonic sealing, high-frequency sealing, pulse sealing, etc., can be used. Furthermore, the other end 721 of the main body 720 and the periphery portion 713 of the flange portion 712 can be sealed between their contacting outer surfaces by using a material with heat-welding properties. For example, a method can be used where a polyethylene-containing sealant layer 754 is provided in the innermost layer of the laminated sheet 750 constituting the main body 720, and an injection port 710 is formed using a polyethylene-containing material, so as to heat-weld them together.

[0479] When the main body 720 is formed by a backing seal 726 formed by joining and welding in a palm-like shape, the backing seal 726 has high rigidity, making it difficult to form folds 723, and the sealing performance is also poor. Therefore, as Figure 40 As shown in (a) and (b), the backing seal 726 preferably does not form folds 723. Since the left and right portions of the backing seal 726, which are formed by butt-jointing and welding in a palm-like manner, have a large difference in wall thickness, folds 723 can be intentionally formed to avoid a large difference in wall thickness.

[0480] The tubular container and its manufacturing method involved in this embodiment are described below.

[0481] [1] A tubular container comprising a main body closed at one end and an outlet portion mounted at the other end of the main body, characterized in that,

[0482] The injection port has a flat flange that is orthogonal to the height direction of the main body. When viewed from the height direction of the main body, the periphery of the flange is approximately circular.

[0483] The main body has a weight per unit area greater than 30g / m². 2 And less than 300g / m 2 The paper,

[0484] In the peripheral portion of the flange, the other end of the main body is mounted on the surface of the flange opposite to one end of the main body, having a first grid line and a second grid line, and bending along the first grid line and the second grid line. A fold is formed on the outside of the other end of the main body on the peripheral portion of the flange, and is mounted on the peripheral portion of the flange.

[0485] The first grid line is a zigzag line, which is formed in the circumferential direction of the main body so as to bend towards the center of the main body for installation on the periphery of the flange.

[0486] The second grid line is constructed by forming a group of one mountain fold line and two valley fold lines, and two or more such groups are evenly formed along the circumferential direction of the flange portion.

[0487] The mountain-shaped zigzag line is a line that extends approximately at a right angle to the first grid line from the edge of the other end of the main body towards a point on the first grid line.

[0488] The two valley zigzag lines are lines that extend symmetrically to the left and right relative to the one mountain zigzag line, with the point of the first grid line as the vertex and sloping from the edge of the other end of the main body towards the vertex of the first grid line, forming an isosceles triangle with the edge of the other end of the main body as the base.

[0489] When the length of the outer perimeter of the main body near the periphery of the flange is set as A, the diameter of the outer perimeter of the main body near the periphery of the flange is set as B, the length of the line extending approximately at a right angle to the first grid line from the edge of the other end of the main body is set as C, the length of the base of the isosceles triangle at the edge of the other end of the main body is set as D, the number of sets of the one mountain zigzag line and the two valley zigzag lines is set as E, and the circumference of the circle with a diameter of (BC×2) is set as F, the relationship (AF) / E=D is satisfied.

[0490] [2] The tubular container according to item [1] is characterized in that,

[0491] The fold is folded in one direction on the outside of the other end of the main body portion on the periphery of the flange portion.

[0492] [3] The method for manufacturing the tubular container described in item [1] or [2] is characterized in that it includes:

[0493] The process of installing the injection port onto the upper part of the mandrel;

[0494] The process of inserting a main body portion whose height direction is longer than the height direction of the mandrel into the mandrel;

[0495] The process of fixing the main body at the position where the mandrel protrudes beyond length C; and

[0496] The process of forming the first grid line and the second grid line in the main body.

[0497] [4] The method for manufacturing the tubular container according to item [3] is characterized in that it includes:

[0498] The process of forming the first grid line and the second grid line on the main body by heating and pressurizing at a temperature below the melting point of the main body.

[0499] [5] The method for manufacturing the tubular container according to item [4] includes:

[0500] The main body is made of a laminated sheet of resin that is softened by heat as the outermost layer. In the process of heating and pressurizing, the first grid line and the second grid line are formed by contacting the main body with the female mold and causing the contact portion of the main body to shrink thermally.

[0501] <Eighth Implementation>

[0502] The main body is formed by making the sheet constituting the main body into a cylindrical shape and then bonding the two ends together. Methods of bonding the sheet include: * **clasp bonding:** bonding the inner surfaces of the sheets together and fusing them; * **butt-band bonding:** sealing the butt joint formed by joining the two ends of the sheets with a strip; * **seal bonding:** fusing the inner and outer surfaces of the sheets together. However, in clasp bonding, the bonded portion protrudes from the main body, damaging the appearance of the tubular container.

[0503] During the bonding process, the strength of the joint weakens, potentially leading to paper peeling during the use of tubular containers, thus affecting durability. Furthermore, in addition to the sealant layer used for welding to the innermost sheet forming the main body, a barrier layer is also needed to ensure the barrier properties of the tubular container. There is a concern that components of the adhesive used to bond the barrier layer between the layers may leach from the end face of the strip into the interior of the main body.

[0504] In addition, while the strength of the bonded portion can be ensured in the sealing process of welding the inner and outer surfaces of the sheet together, the adhesive contained in the sheet may dissolve from the end face of the sheet inside the main body into the tubular container. Furthermore, the contents may permeate into the paper layer from the end face of the sheet inside the main body, thereby leaking the contents out of the tubular container.

[0505] This embodiment provides a tubular container that is aesthetically pleasing, durable, and has excellent barrier properties, and does not have a barrier layer or adhesive on the strip, thus inhibiting the leaching of adhesive components from the strip and sheet.

[0506] Figure 44 This is a front view illustrating a schematic configuration of the tubular container according to the embodiment. Figure 45 It is along Figure 44 The cross-sectional view of the XLV-XLV line shown in the figure. Figure 46 This is a cross-sectional view showing an example of a sheet that constitutes the main body of a tubular container.

[0507] The tubular container 8100 includes: a tubular main body 801, an outlet 802 installed on the main body 801, and a strip 820.

[0508] The main body 801 is a component for containing contents, and is formed by rolling a sheet 841 having a pair of generally parallel opposing end edges into a cylindrical shape. As a method of bonding the two ends of the laminated sheet 841, a sealing sleeve is used to bond the inner and outer surfaces of the sheet 841 with a strip 820. One end 805a of the main body 801 ( Figure 1 The lower end of the main body 801 is sealed and closed. On the other hand, the other end 805b of the main body 801 ( Figure 1 The portion near the upper end of the body portion 801 is sealed to the outside 808 of the flange portion 804 (described later) in a folded state. Multiple folds 812 are formed at the weld between the body portion 801 and the flange portion 804 by folding the sheet 841 constituting the body portion 801. Additionally, an overlapping portion 807 (backing portion) is formed on the body portion 801.

[0509] The overlapping portion 807 is a portion formed by sealing the outermost layer of a part within a predetermined range from one end edge of the sheet 841 with the innermost layer of a part within a predetermined range from the other end edge. The width W of the overlapping portion 807 in the circumferential direction of the main body 801 is 1.0 to 8.0 mm, preferably 1.0 to 3.0 mm. If the width of the overlapping portion exceeds 8.0 mm, the rigidity of the overlapping portion is too strong, and the pleats 812 may protrude from the main body 801, resulting in damage to the appearance. If the width of the overlapping portion 807 is less than 1.0 mm, the inner and outer surfaces of the sheet 841 will not overlap due to offset during bag making, and the barrier properties and durability of the tubular container 8100 may be compromised.

[0510] like Figure 46As shown, the sheet 841 constituting the main body 801 of the tubular container 8100 is a multilayer sheet, wherein a substrate film layer 133, a barrier layer 134, and a sealant layer 135 are sequentially laminated on one side of the paper layer 132, and an ink layer 138 and a paper protective layer 137 are laminated on the other side of the paper layer 132. The lamination order of the ink layer 138 and the paper protective layer 137 can be... Figure 3 Conversely, adhesives can be used between layers to bond them together.

[0511] It should be noted that the paper layer 132, substrate film layer 133, barrier layer 134, sealant layer 135, paper protective layer 137, and ink layer 138 can be constructed using the structures of the layers described in the first embodiment. Furthermore, the total thickness of the sheet 841 constituting the main body 801 and the proportion of paper (pulp fiber) can be set within the same range as in the first embodiment. One or more layers other than the paper layer 132 and sealant layer 135 can be omitted from the sheet 841.

[0512] In this embodiment, the area weight of the paper used for paper layer 132 is 30 to 300 g / m². 2 The preferred value is 50-150 g / m³. 2 In addition, in this embodiment, the sealant layer 135 is provided for welding the strip 820 to the main body 801 in the overlapping portion 807 and for welding the injection port portion 802 to the main body 801.

[0513] The paper protective layer 137 is used to protect the paper layer 132 constituting the sheet 841 from the adhesion of contents and dirt. The material of the paper protective layer 137 is not particularly limited, but by being made of a material that can be fused to the sealant layer 135 of the main body 801, the sealant layer 135 and the paper protective layer 137 are completely fused at the overlap 807, which can suppress curling of the overlap 807 and improve the barrier properties and durability of the main body 801. The method of forming the paper protective layer 137 is not particularly limited; it can be laminated by extrusion coating of a thermoplastic resin, coating with a water-resistant agent or an oil-resistant agent, etc. The thickness of the paper protective layer 137 is preferably 0.2 to 50 μm, more preferably 0.5 to 20 μm. When the thickness of the paper protective layer 137 is less than 0.2 μm, pinholes may occur in the paper protective layer 137, and the protection of the paper layer 132 may become insufficient. Furthermore, when the thickness of the paper protective layer 137 exceeds 50 μm, it is not preferable from the perspective of resin usage and manufacturing cost. It should be noted that even without the paper protective layer 137, the sealant layer 135 is pseudo-bonded to the surface of the paper layer 132, and the overlap 807 is reinforced by the tape 820, therefore there are no problems with barrier properties and durability. However, as described above, from the viewpoint of suppressing curling of the overlap 807 and further improving barrier properties and durability, it is preferable to provide the paper protective layer 137.

[0514] The stacking order of ink layer 138 and paper protective layer 137 is similar to... Figure 46 Conversely, a clear varnish layer can be laminated over the ink layer 138 to impart abrasion resistance, etc.

[0515] (Strip)

[0516] The tape 820 is composed of a film that can bond to the sealant layer 135 and does not contain adhesive, and is sealed to the inside of the main body 801 in such a way that it covers the entire end edge of the sheet 841 located on the innermost side of the main body 801. The tape 820 is arranged such that the center of the tape 820 is substantially aligned with the end edge of the sheet 841 located on the innermost side. There are no particular limitations on the material of the tape 820, for example, the same material as the sealant layer 135 can be used. In addition, the tape 820 can be a single layer or a multi-layer laminated structure, as long as it does not contain adhesive, for example: a single-layer film made of a heat-sealable resin such as polyethylene or polypropylene, a co-extruded film of a heat-sealable resin, or a film formed by extruding and laminating a heat-sealable resin onto other films.

[0517] Since the main body 801 of the tubular container 8100 in this embodiment is formed by sealing and bonding, barrier properties can be ensured by the barrier layer 134 of the sheet 841. Therefore, it is not necessary to bond the barrier layer to the tape, nor is it necessary to use an adhesive for bonding the barrier layer to the tape. As a result, since the tape 820 does not contain adhesive, even if the tape is used for bonding the main body 801, the adhesive components of the tape cannot dissolve. Furthermore, by providing the tape 820 in a manner that covers the end face of the sheet 841 located inside the main body 801, the end face of the sheet 841 can be protected, preventing the adhesive contained in the sheet 841 from dissolving into the tubular container from the end face, and preventing the contents of the tubular container 8100 from permeating into the paper layer 132 from the end face.

[0518] As described above, in this embodiment, the main body 801 is formed by bonding a sleeve that overlaps the outermost layer of a portion within a predetermined range from one end edge of the sheet 841 with the innermost layer of a portion within a predetermined range from the other end edge. This provides a tubular container 8100 in which the overlapping portion 807 has high durability, does not protrude from the main body 801, has high aesthetic appeal, and provides high barrier properties even without a barrier layer on the strip.

[0519] Furthermore, even when the main body 801 is formed using a sealed adhesive, the strip 820 also protects the end face of the sheet 841 located inside the main body 801. This prevents the adhesive contained in the sheet 841 from dissolving into the tubular container from the end face, and also prevents the contents of the tubular container 8100 from permeating into the paper layer 132 from the end face.

[0520] In addition, since the adhesive tape 820, which is made of a film without adhesive, is used in the sealing adhesive, the adhesive components of the tape will not leach into the tubular container.

[0521] (Other variations)

[0522] The shape of the flange portion of the injection port, the molding material and molding method of the injection port, the annular protrusion and recess provided in the flange portion of the injection port, the dimensions of these protrusions and recesses, the screw cap, hinged cap, sealing membrane of the injection port, and one or more of the partition wall and pull ring provided in the injection port, which can be attached and detached in the injection cylinder portion, can also be applied to embodiments 2 through 8. Furthermore, the configurations of the various parts described in embodiments 1 through 8 can be appropriately combined, and the configuration of the tubular container obtained by combining the various embodiments is also included in this disclosure.

[0523] Example

[0524] The following describes specific embodiments of this disclosure.

[0525] <Examples and Comparative Examples of the First Embodiment>

[0526] (Example 1-1)

[0527] Using dry lamination and a two-component curing urethane adhesive at a weight of 100 g / m² 2 A sheet for forming the main body was made by sequentially pasting a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD) and a 50μm thick unstretched polypropylene film (manufactured by Futamura Chemical Co., Ltd., trade name: FHK2) onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). The sheet was then processed using a backing bag making machine to produce a cylindrical backing bag (main body) with a diameter of 35mm and a length of 200mm.

[0528] The nozzle is manufactured by extruding a molding material (MAPKA, Inc., trade name: Environmental Management Research Institute) that is a mixture of 49% by mass polypropylene and 51% by mass paper powder. The nozzle has a volume of 1.35 ml. Furthermore, on the outside of the nozzle flange, a 0.5 mm high protrusion and a 0.3 mm deep recess are formed concentrically with the nozzle barrel.

[0529] A tubular container with a diameter of 35 mm was produced by heat-fusion of the main body and the injection port using a specialized processing device.

[0530] (Examples 1-2)

[0531] Except that no protrusions or recesses are formed on the outside of the flange at the injection port, a tubular container with a diameter of 35 mm was manufactured in the same manner as in Example 1-1.

[0532] (Examples 1-3)

[0533] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 120 g / m². 2 A sheet for forming the main body was made by sequentially pasting a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitika Co., Ltd., trade name: ONBC), and a 50μm thick unstretched polypropylene film (manufactured by Futamura Chemical Co., Ltd., trade name: FHK2) onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). Otherwise, a tubular container with a diameter of 35mm was made in the same manner as in Example 1-1.

[0534] (Examples 1-4)

[0535] In addition to using a unit area weight of 120g / m² 2 Except for the original kraft paper (manufactured by Oji Paper Co., Ltd.), a tubular container with a diameter of 35 mm was made in the same manner as in Example 1-1.

[0536] (Examples 1-5)

[0537] By using a unit area weight of 120g / m² 2 The sheet material for forming the main body was made of natural kraft paper (manufactured by Oji Paper Co., Ltd.), and the injection port was made by extruding a molding material made of a mixture of 70% by mass of polypropylene and 30% by mass of calcium carbonate. Otherwise, a tubular container with a diameter of 35 mm was made in the same manner as in Example 1-1.

[0538] (Examples 1-6)

[0539] In addition to using a unit area weight of 180g / m² 2 Except for the sheet material for forming the main body made of natural kraft paper (manufactured by Oji Paper Co., Ltd.), a tubular container with a diameter of 35 mm was made in the same manner as in Example 1-1.

[0540] (Comparative Example 1-1)

[0541] A sheet for forming the main body was produced by sequentially bonding a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitika Co., Ltd., trade name: ONBC), and a 100μm thick unstretched polypropylene film (manufactured by Futamura Chemical Co., Ltd., trade name: FHK2) using dry lamination and a two-component curable urethane adhesive. The sheet was then processed using a backing bag making machine to produce a cylindrical backing bag (main body) with a diameter of 35mm and a length of 200mm.

[0542] The injection nozzle is manufactured by extruding polypropylene (100% by mass). The volume of the injection nozzle is 1.35 ml. In addition, outside the flange of the injection nozzle, a 0.5 mm high protrusion and a 0.3 mm deep recess are formed concentrically with the injection cylinder.

[0543] A tubular container with a diameter of 35 mm was produced by heat-fusion of the main body and the injection port using a specialized processing device.

[0544] (Comparative Examples 1-2)

[0545] In addition to using a unit area weight of 250g / m² 2Except for the sheet material for forming the main body made of natural kraft paper (manufactured by Oji Paper Co., Ltd.), a tubular container with a diameter of 35 mm was made in the same manner as in Example 1-1.

[0546] (Comparative Examples 1-3)

[0547] A sheet for forming the main body was fabricated by sequentially bonding a 60μm thick polyethylene film, a 12μm thick polyethylene terephthalate film, a 160μm thick polyethylene film, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), and a 100μm thick polyethylene film using dry lamination and a two-component curing urethane adhesive. The fabricated sheet was then processed using a tube-making machine for laminated tubes to produce a tubular container with a diameter of 35mm. By compression molding, the tube was simultaneously fused to the nozzle section (shoulder) formed from high-density polyethylene, thus creating a tubular container with a diameter of 35mm.

[0548] (Comparative Examples 1-4)

[0549] A film was produced by dry lamination using a two-component curing urethane adhesive, sequentially bonding a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitika Co., Ltd., trade name: ONBC), and a 60μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Co., Ltd., trade name: SE625A). The film and a nozzle made from high-density polyethylene extrusion were then processed using a bag-making machine equipped with a nozzle welding machine to produce a gusset-type bag with a nozzle.

[0550] Table 1 shows the configuration of the containers involved in each embodiment and comparative example. The values ​​listed in the "Configuration of Main Body" column of Table 1 represent the weight per unit area of ​​paper (g / m²). 2 () or the thickness of the resin layer (μm).

[0551]

[0552] In addition, Table 2 shows the material composition of the containers involved in each embodiment and comparative example, the amount of resin used in each container, the thickness of the main body, the amount of resin used, the moldability, the self-supporting ability of the main body, and the overall evaluation.

[0553] The resin usage, moldability, self-supporting properties of the main body, and overall evaluation in Table 2 were evaluated according to the following criteria. It should be noted that since the containers involved in Comparative Examples 1-3 and 1-4 are different in form from those involved in Examples 1-1 to 1-6, moldability was not evaluated.

[0554] <Resin Usage>

[0555] ○: Paper accounts for the highest proportion of the container's mass.

[0556] ×: Paper does not constitute the highest proportion of the container's mass.

[0557] <Moldability>

[0558] ◎: The main body of the backing bag making machine can be processed without any problems, as well as the welding of the main body to the injection outlet. It has good formability.

[0559] ○: The main body of the backing bag making machine can be processed without problems, as well as the welding of the main body to the injection outlet. The formability is good. However, compared with the case of "◎", the productivity is slightly worse, such as the production cycle time is worse.

[0560] ×: Unable to process the main body of the backing bag making machine or weld the main body to the injection outlet, or the welded area is charred, resulting in problems with formability.

[0561] <Self-reliance>

[0562] ○: When the dispensing end of the unfilled container is facing down, the main body remains upright without bending.

[0563] ×: Unable to stand on its own

[0564] <Overall Evaluation>

[0565] ○: Resin usage, moldability, and self-standing properties are all good (◎ or ○)

[0566] ×: Any one of the following is a difference: resin usage, moldability, or self-standing properties (×)

[0567]

[0568] As shown in Table 2, in the tubular containers involved in Examples 1-1 to 1-6, the proportion of paper to the total mass of the container is the highest, the amount of resin used is reduced, but the sheet material constituting the main body has a unit area weight of 30-200 g / m². 2 The paper has rigidity, so the main body can stand upright even when the contents are reduced, and there is no problem with the formability of the processing device.

[0569] Furthermore, for the tubular containers described in Examples 1-1, 1-3 to 1-6, which have protrusions and recesses on the flange portion of the injection port, compared to Comparative Example 1-2, which does not have protrusions and recesses, the main body is firmly fused to the flange portion with the portion having protrusions and recesses as the center, and the sealing strength of both is superior.

[0570] In contrast, in the tubular container of Comparative Example 1-1, the sheet constituting the main body is made of a resin film, which results in insufficient rigidity, preventing the main body from standing upright when the contents are reduced. Furthermore, both the main body and the inlet are made of resin, making it unsuitable for reducing the amount of resin used.

[0571] For the tubular containers involved in Comparative Examples 1-2, the paper contained in the sheet constituting the main body is too thick, making it impossible to perform welding during the backing of the main body and welding of the main body towards the injection outlet. The tubular containers involved in Comparative Examples 1-2 cannot be formed, therefore their self-standing ability cannot be evaluated.

[0572] For the laminated tubes involved in Comparative Examples 1-3, the thickness of the resin laminated sheet constituting the main body is relatively large. Therefore, the main body can stand upright when the contents are reduced. However, the amount of resin used is large, making it unsuitable to reduce the amount of resin used.

[0573] For the bags with spouts involved in Comparative Examples 1-4, the sheet constituting the main body is made of resin film, which results in insufficient rigidity and an unsuitable container shape for standing upright. Therefore, it cannot stand upright when the contents are reduced. In addition, both the main body and the spout are made of resin, making it unsuitable for reducing the amount of resin used.

[0574] <Examples and Comparative Examples of the Second Embodiment>

[0575] (Example 2-1)

[0576] Using a two-component curing dry lamination adhesive (manufactured by Mitsui Chemicals, Ltd., trade names: Takelac (registered trademark) A626 and Takenate (registered trademark) A50) at a unit area weight of 70 g / m² 2 A sheet for the main body was made by sequentially bonding a 12μm thick transparent vapor-deposited PET film (manufactured by Toppan Printing Co., Ltd., trade name: GL-ARH-F), a 15μm thick biaxially stretched nylon (manufactured by Unitika Co., Ltd., ONBC), and a 60μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Co., Ltd., trade name: SE620L). The sheet was then processed using a clasp-bonding bag-making machine to produce a sleeve with a bag width of 55mm, a length of 180mm, and a sealing width of 8mm.

[0577] Next, a two-component dry lamination adhesive (manufactured by Mitsui Chemicals, Ltd., trade names: Takelac (registered trademark) A626 and Takenate (registered trademark) A50) was applied at a weight of 200 g / m². 2On one side of a cup base paper (manufactured by Oji Ftex Co., Ltd.), a 12μm thick transparent vapor-deposited PET film (manufactured by Toppan Printing Co., Ltd., trade name: GL-ARH-F) and a 60μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Co., Ltd., trade name: SE620L) are sequentially pasted. On the other side of the cup base paper, low-melting-point polyethylene (LDPE, manufactured by Asahi Kasei Corporation, trade name: L1850K) is extruded to a thickness of 20μm, thus producing a sheet material for the injection nozzle section (bottle section and flat section).

[0578] The sheet material for the injection nozzle is stamped into a donut shape with an outer diameter of φ39mm and an inner diameter of φ21mm. The outer periphery is rolled inwards using a curling tool, and then the rolled edge is flattened using an ultrasonic sealing machine, thus creating a component for the flat section with an outer diameter of φ35mm. On the other hand, the sheet material for the injection nozzle is cut into rectangles 88mm wide × 40mm long. By folding the short side back (bending) to the opposite side, it is rolled into a cylinder, and then heat-sealed with the bent portion, thus creating a cylindrical intermediate body with a diameter of φ21mm. The aforementioned component for the flat section is inserted into the cylindrical intermediate body, and then both ends of the cylindrical intermediate body are rolled outwards with a curling diameter of φ2mm. The other rolled part is flattened and integrated with the component for the flat section using ultrasonic sealing, thus creating a paper injection nozzle.

[0579] Insert the manufactured injection port into the sleeve, fold the sleeve sheet along the folding portion of the outer periphery of the flat portion, and perform ultrasonic sealing to install the main body (sleeve) onto the flat portion of the injection port.

[0580] A top sealing material was prepared by bonding a 12μm thick transparent vapor-deposited PET film (manufactured by Toppan Printing Co., Ltd., trade name: Takelac (registered trademark) A626 and Takenate (registered trademark) A50) together using a two-component dry lamination adhesive (manufactured by Mitsui Chemicals Co., Ltd., trade name: GL-ARH-F) and an easy-peel film (manufactured by Toray Film Processing Co., Ltd., trade name: CF9501EA). The top sealing material was then heat-sealed to the open end of the tube portion of the injection port, thereby producing the paper tubular container according to Example 2-1.

[0581] (Comparative Example 2-1)

[0582] As a comparative example 2-1, a paper-laminated tube was used to make the middle layer of the main body.

[0583] Using a two-component curing dry lamination adhesive (Mitsui Chemicals, Ltd., trade names: Takelac (registered trademark) A626 and Takenate (registered trademark) A50), 50 g / m² of adhesive per unit area was sequentially bonded to one side of a 130 μm thick low-melting-point polyethylene film (LDPE, Tamapoli Co., Ltd., trade name: V-1). 2 The raw materials for pipe manufacturing consist of unbleached kraft paper (manufactured by OjiMateria Co., Ltd.), a 12μm thick transparent vapor-deposited PET film (manufactured by Toppan Printing Co., Ltd., trade name: GL-ARH-F), and a 150μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Co., Ltd., trade name: SE620L). Next, a 30μm thick polyethylene (SPE, manufactured by Asahi Kasei Corporation, trade name: L1850K) is extruded using an extruder, and the other side of the LDPE film is laminated together with a 40μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Co., Ltd., trade name: SE620L) to produce the raw materials for pipe manufacturing.

[0584] Using a conventional laminated tube manufacturing apparatus, a sleeve (main body) was made from the raw material, and the shoulder was formed and integrated with the main body by in-line pressing, thereby producing the laminated tube described in Comparative Example 2-1. It should be noted that the shoulder was molded using high-density polyethylene.

[0585] (Comparative Example 2-2)

[0586] As a comparative example 2-2, a conventional resin laminated tube was fabricated.

[0587] Using a two-component dry lamination adhesive (Mitsui Chemicals, Inc., trade names: Takelac (registered trademark) A626 and Takenate (registered trademark) A50), a 12μm thick biaxially stretched polyethylene terephthalate film (Toray Industries, Inc., trade name: P60), a 12μm thick transparent vapor-deposited PET film (Toppan Printing Co., Ltd., trade name: GL-ARH-F), and a 150μm thick linear low-melting-point polyethylene film (LLDPE, Tamapoli Co., Ltd., trade name: SE620L) were sequentially bonded to one side of a 130μm thick low-melting-point polyethylene film (LDPE, Tamapoli Co., Ltd., trade name: V-1). Next, a 30μm thick polyethylene (SPE, manufactured by Asahi Kasei Corporation, trade name: L1850K) extruded using an extruder is sandwiched between the other side of the LDPE film and a 40μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Corporation, trade name: SE620L), thereby producing the raw material for pipe manufacturing.

[0588] Using a conventional laminated tube manufacturing apparatus, a sleeve (main body) was made from the raw material, and the shoulder was formed and integrated with the main body by in-line pressing, thereby producing the laminated tube described in Comparative Example 2-2. It should be noted that the shoulder was molded using high-density polyethylene.

[0589] Table 3 shows the paper ratio, presence or absence of barrier properties, opening permeability, wasteability, and overall evaluation of the tubular containers involved in Example 2-1 and Comparative Examples 2-1 and 2-2. The paper ratio in Table 3 is the proportion of the mass of paper to the total mass of the tubular container (mass %). For the evaluation of barrier properties, "◎" is marked for cases where both the main body and the shoulder (note: the outlet) have barrier properties, and "×" is marked for other cases. Regarding opening permeability, "◎" is marked for cases where the top sealing material is easily opened, and "×" is marked for other cases; "-" indicates no evaluation. Furthermore, regarding recyclability, "◎" is marked for cases where the paper is recyclable, and "×" is marked for other cases. For the overall evaluation, "○" is marked for cases where all evaluations of barrier properties, opening permeability, and recyclability are "◎", and "×" is marked for other cases.

[0590]

[0591] As shown in Table 3, in the paper tubular container of Example 2-1, the paper ratio exceeds 50% of the total container mass, allowing for paper recycling. Furthermore, by using barrier films in the sheets used for the main body and the inlet / outlet, both the main body and the inlet / outlet are made barrier-free. Additionally, by sealing the inlet / outlet with a top sealing material that combines the barrier film and an easy-peel film, the contents can be kept sealed before opening, and the top sealing material can be easily removed. Therefore, the paper tubular container of this embodiment is constructed from a sheet primarily of paper and exhibits excellent sealing properties.

[0592] In the laminated tube of Comparative Example 2-1, the middle layer of the sheet constituting the main body has a paper layer, so the main body looks like paper. However, the actual paper ratio is less than 10%, which cannot reduce the amount of plastic used, and it needs to be discarded as a plastic container. The laminated tube of Comparative Example 2-2 has a plastic ratio of 100%, so it also cannot reduce the amount of plastic used and needs to be discarded as a plastic container. In the laminated tubes of Comparative Examples 2-1 and 2-2, the shoulder is molded from HDPE, so it cannot provide barrier properties to the shoulder. In addition, no top sealing material is provided at the injection port of the shoulder, so the sealing performance before opening is worse compared with the paper-based easy-to-use tube of Example 2-1.

[0593] <Examples and Comparative Examples of the Third Embodiment>

[0594] (Example 3-1)

[0595] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD) and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Co., Ltd., trade name: SE620A) are sequentially pasted. On another surface of the paper, an ink layer and an outer varnish layer are formed by printing. A thermoplastic resin-containing hot-melt coating agent is patterned and applied to the overlapping areas where the backing seal and the main body overlap, and in the overlapping areas folded when sealing the main body to the flange of the injection port. Figure 16 (Shaded areas in the image). The application rate of the heat-fusion coating agent is set to 10 g / m². 2 A backing bag making machine was used to process the sheet material with a heat-weldable coating layer to produce a backing bag (main body) with a diameter of 35mm and a length of 200mm.

[0596] The injection nozzle is made by extruding polyethylene.

[0597] A tubular container with a diameter of 35 mm was produced by heat-fusion of the main body and the injection port using a specialized processing device.

[0598] (Example 3-2)

[0599] In addition to setting the coating amount of the hot-melt coating agent to 1g / m 2 In addition, a tubular container with a diameter of 35 mm was made in the same manner as in Example 3-1.

[0600] (Example 3-3)

[0601] In addition to setting the coating amount of the hot-melt coating agent to 20g / m 2 In addition, a tubular container with a diameter of 35 mm was made in the same manner as in Example 3-1.

[0602] (Examples 3-4)

[0603] In addition to applying the heat-fusion coating agent to the entire surface of the sheet, a tubular container with a diameter of 35 mm was made in the same manner as in Example 3-1.

[0604] (Comparative Example 3-1)

[0605] Except for not applying a heat-melting coating agent, a tubular container with a diameter of 35 mm was made in the same manner as in Example 3-1.

[0606] (Comparative Example 3-2)

[0607] In addition to setting the coating amount of the heat-fusion coating agent to 0.1 g / m 2 In addition, a tubular container with a diameter of 35 mm was made in the same manner as in Example 3-1.

[0608] Table 4 shows the unit area weight of paper, coating amount and coating method of the heat-melting coating agent, bag-making adaptability (mechanical adaptability), stiffness of the main body and evaluation results of paper springback in each embodiment and comparative example.

[0609] It should be noted that the bag-making adaptability (mechanical adaptability), body stiffness, and paper springback in Table 4 were evaluated according to the following criteria. Additionally, "-" in Table 4 indicates that no evaluation was conducted.

[0610] <Bag-making adaptability (mechanical adaptability)>

[0611] ○: Good mechanical adaptability when processing the main body using a bag-making machine.

[0612] △: Mechanical adaptability decreases slightly due to the increased coefficient of friction, but remains at a problem-free level.

[0613] ×: The coefficient of friction is too high and the sliding performance is poor, making it difficult to process using a bag-making machine.

[0614] <Stiffness of the main body>

[0615] ○: The increased rigidity is felt due to the sealing of the backing.

[0616] ×: I did not feel any increase in rigidity due to the backing seal.

[0617] <Paper bounces>

[0618] ◎: Paperless pop-up, seamless overlapping of sheets

[0619] ○: No paper pops up, but the overlapping parts of the sheet appear to float slightly.

[0620] ×: Paper bounces up

[0621]

[0622] As shown in Table 4, in the tubular containers described in Examples 3-1 to 3-4, no paper bounce occurred at the backing seal and shoulder (the welded portion from the main body to the flange) of the main body, resulting in high aesthetic appeal. Furthermore, by welding the backing seal to the main body, the rigidity of the main body is increased, and the increased rigidity of the main body can be felt. Additionally, in Examples 3-1 to 3-4, the bag-making adaptability during the formation of the main body is also good.

[0623] In the tubular container of Comparative Example 3-1, paper bounce occurred at both the backing seal and the shoulder (the welded portion from the main body to the flange) of the main body because a heat-welding coating was not provided. In the tubular container of Comparative Example 3-2, paper bounce also occurred at both the backing seal and the shoulder (the welded portion from the main body to the flange) of the main body because the amount of heat-welding coating was too small. Therefore, the tubular containers of Comparative Examples 3-1 and 3-2 are less aesthetically pleasing than those of Examples 3-1 to 3-4. Furthermore, since the backing seal is not welded to the main body, the rigidity of the main body is lower than that of Examples 3-1 to 3-4.

[0624] <Examples and Comparative Examples of the Fourth Embodiment>

[0625] The inventors of this application conducted tests using the tubular containers of Examples 4-1 to 4-4 and Comparative Examples 4-1 and 4-2 to confirm the following: the spring-up condition of the sealing portion of the main body forming the cylindrical shape, whether the contents permeated into the paper layer, and the leakage condition of the welded portion of the injection port. Examples 4-1 to 4-4 and Comparative Examples 4-1 and 4-2 all consist of a main body and an injection port, and the structure and material of the injection port are the same as those of the injection port of the tubular container of the first embodiment described above. Furthermore, the method of mounting the injection port to the main body in Examples 4-1 to 4-4 and Comparative Examples 4-1 and 4-2, as well as the method of bonding the bottom laminated sheets to each other, are the same as those of the tubular container of the first embodiment described above.

[0626] Next, the structure of the main body of Examples 4-1 to 4-4, and Comparative Examples 4-1 and 4-2 will be described respectively.

[0627] (Example 4-1)

[0628] Starting from the innermost layer, a linear low-density polyethylene resin (LLDPE) film (manufactured by Tamapoli Co., Ltd., trade name: SE620A) (50μm) and an inorganic vapor-deposited polyethylene terephthalate film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD) (12μm) are sequentially laminated, and dry lamination is performed using a dry lamination adhesive to create the inner laminated film. The adhesive used is a two-component curing urethane adhesive (manufactured by Mitsui Chemicals Co., Ltd., main component A626 / curing agent A5).

[0629] In addition, low-density polyethylene resin (LDPE) (manufactured by Nippon Polyethylene Co., Ltd., trade name: LC600A) (15μm) and polyethylene terephthalate (PET) (manufactured by Toray Industries, Ltd., trade name: P60) (12μm) are sequentially laminated from the outermost side, and formed by extrusion lamination to create the outer laminated film.

[0630] Using SPE (manufactured by Nippon Polyethylene Co., Ltd., trade name: Novatec LC600A) (15μm), extrusion lamination was applied to unbleached kraft paper (manufactured by Oji Materia Co., Ltd., unbleached lightweight packaging paper) (70g / m²). 2 The inner laminated film is bonded to one side of the sheet, and the outer laminated film is bonded to the opposite side, thereby completing the laminated sheet that constitutes the main body.

[0631] When laminating the unbleached kraft paper, the inner laminated film, and the outer laminated film, multiple strips of unbleached kraft paper, each 110 mm wide, are supplied in a strip and adhered between the entire surface of the inner and outer laminated films in the width direction. Then, the unbleached kraft paper is cut in such a way that film portions of only 8 mm are formed on both sides, with the unbleached kraft paper portion as the center. The method for forming the cylindrical shape is the same as the method for forming the cylindrical body of the tubular container described in the first embodiment.

[0632] (Example 4-2)

[0633] Starting from the innermost layer, a linear low-density polyethylene resin (LLDPE) film (manufactured by Tamapoli Co., Ltd., trade name: SE620A) (50μm) and an inorganic vapor-deposited polyethylene terephthalate film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD) (12μm) are sequentially laminated, and dry lamination is performed using a dry lamination adhesive to create the inner laminated film. The adhesive used is a two-component curing urethane adhesive (manufactured by Mitsui Chemicals Co., Ltd., main component A626 / curing agent A5).

[0634] Using SPE (manufactured by Nippon Polyethylene Co., Ltd., trade name: Novatec LC600A) (15μm), it is extruded and laminated onto unbleached kraft paper (manufactured by Oji Materia Co., Ltd., unbleached lightweight packaging paper) (70g / m²). 2 The inner laminated film is bonded to one side of the body, and a single layer of low-density polyethylene resin (LDPE) (manufactured by Nippon Polyethylene Co., Ltd., trade name: LC600A) (15μm) is similarly bonded to the opposite side by extrusion lamination, thereby completing the laminated sheet constituting the main body.

[0635] When laminating the unbleached kraft paper, the inner laminate film, and the single layer of low-density polyethylene resin (LDPE), multiple strips of unbleached kraft paper, each 110 mm wide, are supplied in strips and adhered to the entire surface of the inner laminate film and the single layer of low-density polyethylene resin (LDPE). Then, the unbleached kraft paper is cut in such a way that film portions of only 8 mm are formed on both sides, with the unbleached kraft paper portion as the center. The method for forming the tube is the same as the method for forming the tube in Example 4-1.

[0636] (Example 4-3)

[0637] Starting from the innermost layer, a linear low-density polyethylene resin (LLDPE) film (manufactured by Tamapoli Co., Ltd., trade name: SE620A) (50μm), an aluminum foil (7μm), and a polyethylene terephthalate (PET) film (manufactured by Toray Industries, Ltd., trade name: P60) (12μm) are sequentially laminated, and dry lamination is performed using a dry lamination adhesive to create the inner laminated film. The adhesive used is a two-component curing urethane adhesive (manufactured by Mitsui Chemicals Co., Ltd., main component A626 / curing agent A5).

[0638] Using SPE (manufactured by Nippon Polyethylene Co., Ltd., trade name: Novatec LC600A) (15μm), it is extruded and laminated onto unbleached kraft paper (manufactured by Oji Materia Co., Ltd., unbleached lightweight packaging paper) (70g / m²). 2 The inner laminated film is bonded to one side of the body, and a single layer of low-density polyethylene resin (LDPE) (manufactured by Nippon Polyethylene Co., Ltd., trade name: LC600A) (15μm) is similarly bonded to the opposite side by extrusion lamination, thereby completing the laminated sheet constituting the main body.

[0639] When laminating the unbleached kraft paper, the inner laminate film, and the single layer of low-density polyethylene resin (LDPE), multiple strips of unbleached kraft paper, each 110 mm wide, are supplied in strips and adhered to the entire surface of the inner laminate film and the single layer of low-density polyethylene resin (LDPE). Then, the unbleached kraft paper is cut in such a way that film portions of only 8 mm are formed on both sides, with the unbleached kraft paper portion as the center. The method for forming the tube is the same as the method for forming the tube in Example 4-1.

[0640] (Example 4-4)

[0641] Starting from the innermost layer, EMAA resin (manufactured by Mitsui Dow Polychemical Co., Ltd., trade name: AN4228C) (50μm) and inorganic vapor-deposited polyethylene terephthalate film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD) (12μm) are sequentially laminated and bonded together using extrusion lamination to create the inner laminated film.

[0642] EMAA resin (manufactured by Mitsui Dow Polychemical Co., Ltd., trade name: AN4228C) (15μm) was used, and it was extruded and laminated onto unbleached kraft paper (manufactured by Oji Materia Co., Ltd., unbleached lightweight packaging paper) (70g / m²). 2The inner laminated film is pasted onto one side of the main body, and a single layer of EMAA resin (manufactured by Mitsui Dow Polychemical Co., Ltd., trade name: AN4228C) (15μm) is formed on the opposite side, thereby completing the laminated sheet constituting the main body.

[0643] When laminating the unbleached kraft paper, the inner laminated film, and the monolayer of EMAA resin, multiple strips of unbleached kraft paper, each 110 mm wide, are supplied in strips along the entire width of the inner laminated film and the monolayer of EMAA resin and then adhered. Then, the unbleached kraft paper is cut in such a way that film portions of only 8 mm are formed on both sides, with the unbleached kraft paper portion as the center. The method for forming the tube is the same as the method for forming the tube in Example 4-1.

[0644] (Comparative Example 4-1)

[0645] By pasting the same lamination structure as in Example 4-1, the laminated sheet constituting the main body was completed. However, when laminating the kraft paper, the inner laminated film, and the outer laminated film, the following structure was created: the kraft paper was pasted to the inner laminated film and the outer laminated film on its entire surface in the width direction, and the main body was formed by cutting strips in the height direction of the main body, with the two end edges of the blank protruding from the end faces of the kraft paper.

[0646] The method for forming the tube is the same as that for forming the tube in Example 4-1.

[0647] (Comparative Example 4-2)

[0648] The laminated structure of the sheet material constituting the main body and the structure of the blank material for forming the main body with the end faces of the original kraft paper exposed at both ends are the same as those in Comparative Example 4-1.

[0649] The method of forming the tubular shape is different from that of Comparative Example 4-1. The tubular shape is formed by bonding the innermost linear low-density polyethylene resin (LLDPE) film together with each other using a clap-together bonding method.

[0650] (Experimental Methods)

[0651] For the tubular containers of Examples 4-1 to 4-4, and Comparative Examples 4-1 and 4-2, the sealing part of the main body used to form the cylindrical shape was visually judged to see if it popped up and whether the appearance deteriorated.

[0652] In addition, the tubular containers of Examples 4-1 to 4-4, Comparative Examples 4-1 and 4-2 were filled with butter as the contents and stored at 40°C for 2 weeks to confirm whether oil stains were generated on the original kraft paper.

[0653] Furthermore, the tubular containers of Examples 4-1 to 4-4, Comparative Examples 4-1 and 4-2 were ultrasonically welded under the same conditions described below, and leakage at the injection outlet was confirmed using an inspection solution.

[0654] Conditions: Transmission time 0.3 seconds, hold time 0.3 seconds, vibration frequency 30kHz.

[0655] For each of the 100 tubular containers in Examples 4-1 to 4-4, and Comparative Examples 4-1 and 4-2, leakage at the injection port was confirmed, and the number of tubular containers that leaked was confirmed (number of leaks / number of evaluations).

[0656] (Experimental Results & Investigation)

[0657] The test results of the above test methods are shown in Table 5.

[0658] In Table 5, the evaluation item "Body Part Sealing Part Spring-Up" refers to the spring-up of the sealing part used to form the cylindrical body part. "○" indicates no spring-up and a good appearance, while "×" indicates the presence of spring-up and a poorer appearance. In the evaluation item "Content Penetration into Paper Layer," the paper layer is unbleached kraft paper. "○" indicates the contents have not penetrated the paper layer of the body part, while "×" indicates the contents have penetrated the paper layer of the body part. Furthermore, in the evaluation item "Leakage at the Welded Part of the Injection Port," "○" indicates zero leaks, while "×" indicates one or more leaks. Finally, in the "Comprehensive Evaluation," "○" indicates a good overall assessment of the above evaluations, while "×" indicates a poor overall assessment.

[0659] In addition, the values ​​listed in the composition column of the laminated sheets in Table 5 represent the weight per unit area of ​​the paper (g / m²). 2 ), the thickness of the resin (μm) or the thickness of the aluminum foil (μm).

[0660] In Examples 4-1 to 4-4, the sealing part of the main body used to form the cylindrical shape did not bounce, the appearance was good, and the contents did not penetrate into the paper layer of the main body (oil stains). Furthermore, the number of leaks at the welded part of the injection port in 100 tubular containers was 0.

[0661] On the other hand, in Comparative Example 4-1, the sealing portion of the main body used to form the cylindrical shape did not spring back, but the contents permeated into the paper layer of the main body (oil stains). Furthermore, in 10 out of 100 tubular containers, leakage occurred at the welded portion of the injection port. In Comparative Example 4-2, the contents did not permeate into the paper layer of the main body (oil stains), but the sealing portion of the main body used to form the cylindrical shape spring back. Furthermore, in 30 out of 100 tubular containers, leakage occurred at the welded portion of the injection port.

[0662] Based on the above test results, it can be seen that the end faces of the paper layer are not exposed at both ends after the laminated sheet constituting the main body is cut, and a part consisting only of the film portion is formed. Furthermore, the outermost and innermost surfaces of the two end edges are overlapped to form a cylindrical shape. The tubular container of the main body obtained in this way has a good appearance, prevents the contents from penetrating into the paper layer, and has good sealing performance.

[0663]

[0664] As described above, in the main body of the tubular container according to the fourth embodiment, the end faces of the paper layer are not exposed on the two opposing end edges of the main body forming blank, which is composed of a laminated sheet with an innermost and outermost thermoplastic resin layer and a middle paper layer. Since the two end edges of the main body forming blank, where the end faces of the paper layer are not exposed, are overlapped to form a cylindrical shape, the end faces of the paper layer are not exposed inside the main body of the tubular container and do not come into contact with the contents. Furthermore, in the main body of the tubular container according to the fourth embodiment, the opposing end edges of the main body forming blank are thermally fused together by overlapping the surfaces of the outermost and innermost layers. Therefore, the sealing portion of the main body does not become thickened as in (for example) a clasp-on adhesive, resulting in a good appearance.

[0665] <Examples and Comparative Examples of the Fifth Embodiment>

[0666] (Example 5-1)

[0667] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 A sheet for forming the main body is made by sequentially pasting a 30μm thick EP material (manufactured by DIC Corporation, trade name: E3701T) with a peel strength of 0.50N / 15mm, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low melting point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.).

[0668] An ink layer and an outer varnish layer are layered on the prepared sheet, and then processed using a backing bag making machine to produce a backing bag (main body) with a diameter of 35mm and a length of 180mm.

[0669] The injection nozzle plug is made of polyethylene resin by extrusion molding.

[0670] A tubular container with a diameter of 35 mm was produced by heat-fusion of the main body and the injection port using a specialized processing device.

[0671] (Example 5-2)

[0672] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), an EP material (manufactured by DIC Co., Ltd., trade name: E3701T) with a peel strength of 1 N / 15 mm and a thickness of 30 μm, a PET film (manufactured by Toray Industries, Ltd., trade name: E5100) with a thickness of 12 μm, an aluminum foil (manufactured by Toyo Aluminium Co., Ltd.) with a thickness of 9 μm, and linear low melting point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) with a thickness of 50 μm were sequentially pasted, so that the peel strength between the unbleached kraft paper and the PET film was 1 N / 15 mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35 mm was produced in the same manner as in Example 5-1.

[0673] (Example 5-3)

[0674] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), EP material (manufactured by DIC Co., Ltd., trade name: E3701T) with a peel strength of 3.1 N / 15 mm and a thickness of 30 μm, stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC) with a thickness of 15 μm, aluminum foil (manufactured by Toyo Aluminium Co., Ltd.) with a thickness of 9 μm, and linear low melting point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) with a thickness of 50 μm were sequentially pasted, so that the peel strength between the unbleached kraft paper and the stretched nylon film was 3.1 N / 15 mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35 mm was produced in the same manner as in Example 5-1.

[0675] (Example 5-4)

[0676] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2A transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD) with a thickness of 12 μm, a stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC) with a thickness of 15 μm, and a linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) with a thickness of 50 μm were sequentially pasted onto the unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). At this time, a silicone-based release varnish was patterned and coated between the unbleached kraft paper and the transparent barrier film, so that the peel strength between the unbleached kraft paper and the transparent barrier film was 0.70 N / 15 mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35 mm was produced in the same manner as in Example 5-1.

[0677] (Example 5-5)

[0678] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 A sheet for forming the main body was sequentially pasted onto a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.) consisting of an aluminum foil (manufactured by Toyo Aluminium Co., Ltd.) with a thickness of 9 μm, a stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC) with a thickness of 15 μm, and a linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) with a thickness of 50 μm. At this time, a silicone-based release varnish was patterned and coated between the unbleached kraft paper and the aluminum foil, so that the peel strength between the unbleached kraft paper and the aluminum foil was 1.2 N / 15 mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35 mm was produced in the same manner as in Example 5-1.

[0679] (Examples 5-6)

[0680] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 A 9μm thick aluminum foil (manufactured by Toyo Aluminium Co., Ltd.), a 12μm thick PET film (manufactured by Toray Industries, Ltd., trade name: E5100), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). At this time, a silicone-based release varnish was patterned and coated between the unbleached kraft paper and the aluminum foil, so that the peel strength between the unbleached kraft paper and Al was 2.5N / 15mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35mm was produced in the same manner as in Example 5-1.

[0681] (Examples 5-7)

[0682] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached greaseproof paper (manufactured by Taiko Paper Co., Ltd.), a 9μm thick aluminum foil (manufactured by Toyo Aluminium Co., Ltd.), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially pasted. At this time, a silicone-based release varnish is patterned between the unbleached kraft paper and the aluminum foil, so that the peel strength between the unbleached kraft paper and the aluminum foil is 6N / 15mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35mm is produced in the same manner as in Example 5-1.

[0683] (Examples 5-8)

[0684] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), a 12μm thick PET film (manufactured by Toray Industries, Ltd., trade name: E5100), a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) is sequentially pasted. At this point, a re-peel adhesive (manufactured by Toyochem Co., Ltd., trade name: Siavine SP-205) at a thickness of 10g / m² is applied between the PET film and the transparent barrier film. 2 A dry coating was applied and laminated to achieve a peel strength of 0.70 N / 15 mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35 mm was produced in the same manner as in Example 5-1.

[0685] (Examples 5-9)

[0686] Using dry lamination, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially bonded using a 5-100μm thick polyolefin resin. The resulting film has a smoothness of 20-300 seconds and a unit area weight of 100g / m². 2 A sheet for forming the main body was made by bonding the glossy side of a single-sided glossy kraft paper (manufactured by Oji Paper Co., Ltd.) to a transparent barrier film, so that the peel strength between the kraft paper and the transparent barrier film is 1.4N / 15mm. Otherwise, a tubular container with a diameter of 35mm was made in the same manner as in Example 5-1.

[0687] (Examples 5-10)

[0688] Using dry lamination, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially bonded using a 5-100μm thick polyolefin resin. The resulting film has a smoothness of 20-300 seconds and a unit area weight of 100g / m². 2 A sheet for forming the main body was made by bonding the glossy side of a single-sided glossy varnished paper (manufactured by Taiko Paper Co., Ltd.) to a transparent barrier film, thereby making the peel strength between the varnished paper and the transparent barrier film 2.8 N / 15 mm. In addition, a tubular container with a diameter of 35 mm was made in the same manner as in Example 5-1.

[0689] (Comparative Example 5-1)

[0690] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially pasted. At this point, the coating amount between the unbleached kraft paper and the transparent barrier film is set to 2 g / m².2 (Dry coating), and set the coating amount for other parts to 5 g / m². 2 (Dry method). Except for omitting the process of making the sheet for forming the main body by giving it easy peelability, a tubular container with a diameter of 35 mm was made in the same manner as in Example 5-1.

[0691] (Comparative Example 5-2)

[0692] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially pasted. At this point, the coating amount between the unbleached kraft paper and the transparent barrier film is set to 7 g / m². 2 (Dry coating), and set the coating amount for other parts to 5 g / m². 2 (Dry method). Except for omitting the process of making the sheet for forming the main body by giving it easy peelability, a tubular container with a diameter of 35 mm was made in the same manner as in Example 5-1.

[0693] (Comparative Example 5-3)

[0694] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), a 30μm thick EP material (manufactured by DIC Co., Ltd., trade name: E3701T), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), a 9μm thick aluminum foil (manufactured by Toyo Aluminium Co., Ltd.), and a 50μm thick linear low melting point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted, resulting in a peel strength of 0.35N / 15mm between the unbleached kraft paper and the transparent barrier film, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35mm was produced in the same manner as in Example 5-1.

[0695] (Comparative Example 5-4)

[0696] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2A 9μm thick aluminum foil (Toyo Aluminium Co., Ltd.), a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). At this time, a silicone-based release varnish was patterned and coated between the unbleached kraft paper and the aluminum foil, so that the peel strength between the unbleached kraft paper and the aluminum foil was 13N / 15mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35mm was produced in the same manner as in Example 5-1.

[0697] (Comparative Example 5-5)

[0698] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 On a sheet of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.), a 12μm thick PET film (manufactured by Toray Industries, Ltd., trade name: E5100), a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) is sequentially pasted. At this point, a re-peel adhesive (manufactured by Toyochem Co., Ltd., trade name: Siavine SP-205) at a thickness of 30g / m² is applied between the PET film and the transparent barrier film. 2 The dry coating was laminated to achieve a peel strength of 12 N / 15 mm, thereby producing a sheet for forming the main body. In addition, a tubular container with a diameter of 35 mm was produced in the same manner as in Example 5-1.

[0699] (Comparative Examples 5-6)

[0700] Using dry lamination and a two-component curable urethane adhesive, a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC) and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially bonded onto a 12μm thick transparent barrier film (Toppan Printing Co., Ltd., trade name: GL-RD). A polyolefin resin with a thickness of 5–100μm is then used to bond the film. The resulting film has a smoothness of 5–less than 20 seconds and a unit area weight of 100g / m². 2A sheet for forming the main body was made by bonding unbleached kraft paper (manufactured by Oji Paper Co., Ltd.) with a transparent barrier film, such that the peel strength between the unbleached kraft paper and the transparent barrier film is 0.35N / 15mm. Otherwise, a tubular container with a diameter of 35mm was made in the same manner as in Example 5-1.

[0701] The tubular containers prepared in Examples 5-1 to 5-10 and Comparative Examples 5-1 to 5-6 were subjected to kneading tests, drop tests, vibration tests, and separation tests. In the kneading test, the tubular container was kneaded 100 times with 100 mL of water filled to confirm the paper layer's peeling condition. In the drop test, the tubular container was dropped 10 times from a height of 1.5 m with 100 mL of water filled to confirm the paper layer's peeling condition. In the vibration test, the tubular container was vibrated in the z-axis direction (vertical direction, the container's axial direction) for 15 minutes with random amplitude and frequency of vibration applied to it to confirm the paper layer's peeling condition. In the separation test, the paper layer was separated from the main body, and it was determined whether the mass of the paper layer remaining on the substrate film side was 5% or less of the mass of the paper layer before separation (paper residue 5% or less), or whether the mass of the substrate film layer remaining on the paper layer side was 5% or less of the mass of the substrate film layer before separation (resin residue 5% or less).

[0702] Table 6 shows the structure of the tubular container involved in each embodiment and comparative example, the method of imparting easy peelability, the peel strength, the evaluation of each test, and the overall evaluation. It should be noted that the values ​​recorded in the "Structure of the Main Body" column of Table 6 represent the weight per unit area of ​​the paper (g / m²). 2 ) or the thickness of the layer (μm).

[0703] The test results and overall evaluations in Table 6 are evaluated according to the following criteria.

[0704] <Kneading test / Drop test / Vibration test>

[0705] +: No peeling

[0706] -: There is peeling

[0707] <Separation Test>

[0708] +: Paper or resin residue is less than 5%.

[0709] -: Paper or resin residue exceeding 5%

[0710] <Overall Evaluation>

[0711] ++: Peel strength of 1N / 15mm or higher and 3N / 15mm or lower is preferred. All tests (kneading, drop, vibration, and peel) are good (all +).

[0712] +: Peel strength is above 0.5N / 15mm and below 1N / 15mm, or above 3N / 15mm and below 10N / 15mm, and all kneading test / drop test / vibration test / peel test are good (all +).

[0713] -: Peel strength less than 0.5N / 15mm or greater than 10N / 15mm, and all results in poor performance in the kneading test / drop test / vibration test / peel test (all are -).

[0714]

[0715] As shown in Table 6, the tubular containers involved in Examples 5-1 to 5-10 did not experience paper peeling in the kneading test, drop test, and vibration test, demonstrating excellent durability. Furthermore, in the separation test, both paper and resin residues were below 5%, indicating excellent separation performance. In particular, in Examples 5-2, 5-5, 5-6, 5-9, and 5-10, the peel strength was preferably 1 N / 15 mm or more and 3 N / 15 mm or less, showing a superior balance between durability and separation performance compared to Examples 5-1, 5-3, 5-4, 5-7, and 5-8, which had peel strengths of 0.5 N / 15 mm or more and less than 1 N / 15 mm, or more than 3 N / 15 mm and less than 10 N / 15 mm.

[0716] In contrast, the tubular containers involved in Comparative Examples 5-1, 5-3, and 5-6 exhibited excellent separation performance, with both paper and resin residues below 5% in the separation test, and no peeling occurred in the drop and vibration tests. However, due to a peel strength of less than 0.5 N / 15 mm, paper peeling occurred in the kneading test.

[0717] The tubular containers involved in Comparative Examples 5-2, 5-4, and 5-5 showed excellent durability as the paper layer did not peel off during the kneading test, drop test, and vibration test. However, due to the peel strength exceeding 10 N / 15 mm, both paper and resin residues exceeded 5% in the separation test, indicating poor separation performance.

[0718] <Examples and Comparative Examples of the Sixth Embodiment>

[0719] (Sheet production)

[0720] Sheets A through E were produced. The specific production methods are explained.

[0721] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 70 g / m². 2A 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd.), and a 50μm thick polyethylene film are sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). A 15μm thick polyethylene film is then laminated onto the unbleached kraft paper to create sheet A for forming the main body.

[0722] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 70 g / m². 2 Sheet B for forming the main body is made by sequentially pasting a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd.), and a 50μm thick polyethylene film onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.).

[0723] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 120 g / m². 2 A sheet C for forming the main body is made by sequentially pasting a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd.), and a 50μm thick polyethylene film onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.).

[0724] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 70 g / m². 2 A sheet D for forming the main body is made by sequentially pasting a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), a 9μm thick aluminum foil (manufactured by Toyo Aluminium Co., Ltd.), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd.), and a 50μm thick polyethylene film onto a piece of unbleached kraft paper (manufactured by Oji Paper Co., Ltd.).

[0725] By using dry lamination, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd.), and a 100μm thick polyethylene film are sequentially bonded together using a two-component curing urethane adhesive, thereby producing sheet E for forming the main body.

[0726] Table 7 shows the composition of the sheets A through E produced. It should be noted that the values ​​listed in the "Composition of the Main Body" column of Table 7 represent the weight per unit area of ​​the paper (g / m²). 2 ) or the thickness of the layer (μm).

[0727]

[0728] (Example 6-1)

[0729] A strip with a width of 8 mm was produced by sequentially layering a 30 μm thick polyethylene, a 12 μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 30 μm thick polyethylene (PE) to expose the substrate from the end face.

[0730] For each of sheets A to E, a sealing strip wider than the strip (12mm in width) is used to weld the fabricated strip from the inside of the sheet to the butt joint formed by the two ends of the sheet, thereby creating 5 main body parts with a diameter of 35mm and a length of 180mm.

[0731] The nozzle is made of polyethylene resin by extrusion molding. The cap is made of polypropylene resin by extrusion molding.

[0732] Five tubular containers with an inner diameter of 35 mm were produced by heat-fusion welding the five main body parts to the injection port using a specialized processing device.

[0733] (Example 6-2)

[0734] A strip was made by sequentially layering a 50μm thick polyethylene, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and another 50μm thick polyethylene, exposing the substrate from the end face. In addition, five tubular containers with an inner diameter of pseudo 35mm were made in the same manner as in Example 6-1.

[0735] (Example 6-3)

[0736] A strip with a width of 8 mm was produced by sequentially layering a 30 μm thick polyethylene, a 12 μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 70 μm thick polyethylene, exposing the substrate from the end face. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0737] (Example 6-4)

[0738] A 70μm thick polyethylene, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 30μm thick polyethylene were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8mm. In addition, five tubular containers with an inner diameter of pseudo 35mm were produced in the same manner as in Example 6-1.

[0739] (Examples 6-5)

[0740] A 10μm thick polyethylene, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 10μm thick polyethylene were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8mm. In addition, five tubular containers with an inner diameter of pseudo 35mm were produced in the same manner as in Example 6-1.

[0741] (Example 6-6)

[0742] An ionomer with a thickness of 30 μm, an aluminum foil with a thickness of 9 μm (manufactured by Toyo Aluminium Co., Ltd.), and an ionomer with a thickness of 40 μm were sequentially stacked to expose the substrate from the end face, thereby producing a strip with a width of 8 mm. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0743] (Examples 6-7)

[0744] An ionomer with a thickness of 70 μm, an aluminum foil with a thickness of 9 μm (manufactured by Toyo Aluminium Co., Ltd.), and another ionomer with a thickness of 70 μm were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8 mm. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0745] (Examples 6-8)

[0746] A 30μm thick polyethylene, a 25μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 30μm thick polyethylene were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8mm. In addition, five tubular containers with an inner diameter of pseudo 35mm were produced in the same manner as in Example 6-1.

[0747] (Examples 6-9)

[0748] A strip with a width of 8 mm was fabricated by sequentially layering a 30 μm thick polyethylene film, a 25 μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and another 30 μm thick polyethylene film, and then using ultrasonic slit coating on the substrate end face. Using a sealing strip narrower than the strip, the fabricated strip was welded to sheets A through E respectively, thus creating five main body sections with a diameter of 35 mm and a length of 180 mm. In addition, five tubular containers with an inner diameter of pseudo-35 mm were fabricated in the same manner as in Example 6-1.

[0749] (Examples 6-10)

[0750] A strip with a width of 8 mm was produced by sequentially stacking polyethylene with a thickness of 40 μm, stretched polypropylene with a thickness of 40 μm, and polyethylene with a thickness of 40 μm, so that the substrate is exposed from the end face. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0751] (Comparative Example 6-1)

[0752] A strip with a width of 8 mm was produced by sequentially layering a 9 μm thick polyethylene, a 12 μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and another 9 μm thick polyethylene, exposing the substrate from the end face. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0753] (Comparative Example 6-2)

[0754] A 7μm thick polyethylene, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 7μm thick polyethylene were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8mm. In addition, five tubular containers with an inner diameter of pseudo 35mm were produced in the same manner as in Example 6-1.

[0755] (Comparative Example 6-3)

[0756] A 4μm thick polyethylene, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and a 70μm thick polyethylene were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8mm. In addition, five tubular containers with an inner diameter of pseudo 35mm were produced in the same manner as in Example 6-1.

[0757] (Comparative Example 6-4)

[0758] In addition to using polyethylene with a thickness of 100 μm to make a strip with a width of 8 mm, five tubular containers with an inner diameter of pseudo 35 mm were made in the same manner as in Example 6-1.

[0759] (Comparative Example 6-5)

[0760] A strip with a width of 8 mm was produced by sequentially layering a 30 μm thick polyethylene, a 12 μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and another 30 μm thick polyethylene, exposing the substrate from the end face. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0761] (Comparative Example 6-6)

[0762] The main body was made by joining and fusing the inner surfaces of the strip-shaped portions containing a pair of end edges of the sheets A to E together in a clasping shape. In addition, five tubular containers with an inner diameter of pseudo 35 mm were made in the same manner as in Example 6-1.

[0763] (Comparative Examples 6-7)

[0764] A 70μm thick polyethylene, a 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd.), and an 80μm thick polyethylene were sequentially stacked, exposing the substrate from the end face, thereby producing a strip with a width of 8mm. In addition, five tubular containers with an inner diameter of pseudo 35mm were produced in the same manner as in Example 6-1.

[0765] (Comparative Examples 6-8)

[0766] A strip with a width of 8 mm was produced by sequentially layering a polyethylene with a thickness of 80 μm, a transparent barrier film with a thickness of 12 μm (manufactured by Toppan Printing Co., Ltd.), and another polyethylene with a thickness of 80 μm, so that the substrate is exposed from the end face. In addition, five tubular containers with an inner diameter of pseudo 35 mm were produced in the same manner as in Example 6-1.

[0767] The tubular containers prepared in Examples 6-1 to 6-10 and Comparative Examples 6-1 to 6-8 were evaluated for end-face protection, formability, operability, and chemical resistance, respectively.

[0768] End face protection is evaluated by observing the end face of the strip using a microscope. If the substrate is not exposed at the end face of the strip, it is evaluated as having end face protection (○ in Table 8); if the substrate is exposed, it is evaluated as not having end face protection (× in Table 8).

[0769] In the formability evaluation, cases where tubular containers can be made without problems are evaluated as having good formability (○ in Table 8), cases where tubular containers are made slightly more difficult to form but can be made with basically no problems are evaluated as having fair formability (Δ in Table 8), and cases where tubular containers are difficult to make or cannot be made are evaluated as having poor formability (× in Table 8).

[0770] In the operational evaluation, 20 observers were asked to share their experiences using the product. If more than 15 people reported a positive experience, the product was rated as good (○ in Table 8); if fewer than 14 people reported a positive experience, the product was rated as poor (× in Table 8).

[0771] In the chemical resistance evaluation, each prepared tubular container was filled with 50% ethanol and stored for one month at room temperature (40°C) and humidity (75%). The presence or absence of interlayer delamination of the tape was then checked. If no delamination occurred, the material was rated as having good chemical resistance (○ in Table 8); if delamination occurred, the material was rated as having poor chemical resistance (× in Table 8).

[0772] For evaluations of surface protection, formability, operability, and chemical resistance, the case where there is no "×" in the evaluation results is evaluated as "○", and the case where there is an "×" in any of the evaluation results is evaluated as "×".

[0773] Table 8 shows the composition of the strip involved in each embodiment and comparative example, the width of the sealing strip relative to the strip width, the presence or absence of end-face resin in the end face of the strip before welding, the evaluation results, and the comprehensive evaluation results. It should be noted that the values ​​recorded in the strip composition column of Table 8 represent the layer thickness (μm).

[0774]

[0775] In the tubular containers described in Examples 6-1 to 6-8 and 6-10, the substrate is exposed from the end face of the strip 620 in the state before welding. However, in the state before welding, since the thickness of the first resin layer 621 and the second resin layer 622 of the strip 620 is both 10 μm or more and 70 μm or less, and a sealing strip wider than the strip 620 is used to weld the strip 620, the end face of the substrate 623 can be protected by the resin of the first resin layer 621 or the second resin layer 622 that has melted during welding.

[0776] In the tubular containers described in Examples 6-5, the thickness of the first resin layer 621 and the second resin layer 622 of the strip is 10 μm, which is slightly thin. Therefore, the amount of resin on the end face of the substrate is less, but the tubular container can be manufactured almost without problems.

[0777] In the tubular container strips described in Examples 6-6 and 6-7, since the first resin layer 621 and the second resin layer 622 are ionomers and the substrate 623 is aluminum foil, the strips can be given light-shielding properties in addition to barrier properties.

[0778] Furthermore, in the tubular containers described in Examples 6-9, in the state before welding, the thickness of the first resin layer 621 and the second resin layer 622 of the strip 620 is both 10 μm or more and 70 μm or less, and the end face of the substrate 623 is covered by end face resin 624. Therefore, even if a sealing strip narrower than the strip 620 is used to weld the strip 620, the end face of the substrate 623 can be protected.

[0779] In the tubular container strip involved in Comparative Example 6-1, the thickness of both the first and second resin layers is as thin as 9 μm, making it difficult to cover the end face of the substrate and resulting in low chemical resistance. In addition, poor welding with the main body is prone to occur.

[0780] In the tubular container strip involved in Comparative Example 6-2, the thickness of both the first and second resin layers is as thin as 7 μm. Therefore, the end faces of the substrate are not covered, resulting in low chemical resistance. In addition, poor welding with the main body is prone to occur.

[0781] In the tubular container strip involved in Comparative Example 6-3, since the thickness of the first resin layer is as thin as 4 μm, it may be impossible to form a film of the first resin layer, and it is also difficult to weld it to the main body. However, since the thickness of the second resin layer is 70 μm, it is thicker and thus protects the end face of the substrate.

[0782] Comparative Example 6-4 involves a tubular container whose tape is a single layer of polyethylene. Therefore, the tape does not have the stretch allowance from the stretchable substrate, making it difficult to produce stable tubular containers.

[0783] In the tubular container strip involved in Comparative Examples 6-5, in the state before welding, although a strip with the substrate exposed from the end face of the strip was used, the end face of the substrate was not covered because a sealing strip narrower than the strip was used to weld the strip, resulting in low chemical resistance.

[0784] In the tubular container involved in Comparative Examples 6-6, the main body is made by clasping and gluing, so the clasped sealing part protruding from the main body touches the hand during use, resulting in poor operability. In addition, due to the high rigidity of the clasped sealing part, it is difficult to make bags for the tubular container.

[0785] In the tubular container tapes involved in Comparative Examples 6-7, the thickness of the tape itself increases due to the thickness of the first resin layer reaching 80 μm, making it difficult to perform end sealing on the main body during bag making.

[0786] In the tubular container tapes involved in Comparative Examples 6-8, the thickness of both the first and second resin layers is up to 80 μm. The increased thickness of the tape itself makes it difficult to perform end sealing on the main body during bag making.

[0787] <Examples and Comparative Examples of the 7th Embodiment>

[0788] (Example 7-1)

[0789] The tubular container in the seventh embodiment is... Figure 37 The tubular container 7100 of the above-described embodiments shown in the figure has the same structure as the tubular container.

[0790] The injection port section is made by extrusion molding of polyethylene (PE) resin. The layer composition of the laminated sheet that constitutes the main body is polyethylene (PE) (15μm) / paper (70g) / transparent vapor-deposited polyethylene terephthalate (PET) (12µm) / nylon (NY) (15µm) / polyethylene (PE) (50µm) from the outermost layer side of the outer peripheral surface of the main body.

[0791] The above-mentioned paper has a unit area weight greater than 30g / m². 2 And less than 300g / m 2 .

[0792] The length (A) of the outer perimeter of the main body near the periphery of the flange is approximately 110 mm, the diameter (B) of the outer perimeter of the main body near the periphery of the flange is 35 mm, and the length (C) of the line extending approximately perpendicularly to the first grid line from the edge of the other end of the main body is 5 mm. Therefore, the length of (BC×2) is 25 mm, and the circumference (F) of the circle with a diameter of 25 mm is approximately 78.5 mm. The length of (AF) is approximately 31.5 mm. With the number of groups (E) of a mountain fold line and the first and second valley fold lines to its left and right set to 10, the length (D) of the base of the isosceles triangle at the edge of the other end of the main body is (AF) / E, that is, approximately 31.5 / 10, or approximately 3.2 mm.

[0793] The fold on the outer side of the other end of the main body portion on the periphery of the flange portion is folded in one direction and sealed to the outer side of the other end of the main body portion. Additionally, a backing seal portion formed by butt-welding in a clasping manner forms the main body portion, as shown below. Figure 40 As shown in (a) and 40(b), no pleats are formed in the backing seal, but pleats are intentionally formed in the left and right parts of the backing seal.

[0794] The method for installing the main body onto the injection port is as follows.

[0795] The injection port is installed onto the upper part of the mandrel. Then, the main body, whose length in the height direction is longer than that in the height direction of the mandrel, is inserted into the mandrel, fixing the main body 720 at a position where its length C protrudes beyond that of the mandrel. Then, a female mold is used to heat and pressurize the main body at a temperature below its melting point, forming the first and second grid lines on the main body.

[0796] In addition, during the heating and pressurization process described above, the main body comes into contact with the female mold, and the contact portion in the main body undergoes thermal shrinkage, thereby forming the first grid line and the second grid line.

[0797] The other end of the main body is shaped like a male mold, and a mold corresponding to this male mold is used, such as... Figure 43The female mold 770 shown has a star-shaped frustum-shaped cross-section, with the first grid line and the second grid line formed at the other end of the main body.

[0798] (Example 7-2)

[0799] The tubular container of Example 7-2 is the same as that of Example 7-1 except that the layered structure of the laminated sheet constituting the main body is different.

[0800] The laminated sheet material constituting the main body of the tubular container in Example 7-2 is composed of paper (70g) / transparent vapor-deposited polyethylene terephthalate (PET) (12µm) / nylon (NY) (15µm) / polyethylene (PE) (50µm) from the outermost layer side having the outer peripheral surface of the main body.

[0801] (Example 7-3)

[0802] The tubular container of Example 7-3 is the same as that of Example 7-1 except that the layered structure of the laminated sheet constituting the main body is different.

[0803] The laminated sheet material constituting the main body of the tubular container in Examples 7-3 is composed of paper (120g) / transparent vapor-deposited polyethylene terephthalate (PET) (12µm) / nylon (NY) (15µm) / polyethylene (PE) (50µm) from the outermost layer side having the outer peripheral surface of the main body.

[0804] (Comparative Example 7-1)

[0805] The only difference between the tubular container in Comparative Example 7-1 and the tubular container in Example 7-1 is the weight per unit area of ​​the paper contained in the main body. The tubular container in Comparative Example 7-1 uses paper with a weight per unit area of ​​30 g / m². 2 The following paper.

[0806] (Comparative Example 7-2)

[0807] The only difference between the tubular container in Comparative Example 7-2 and the tubular container in Example 7-1 is the weight per unit area of ​​the paper contained in the main body. The tubular container in Comparative Example 7-2 uses paper with a weight per unit area of ​​300 g / m². 2 The above paper.

[0808] (Experimental Methods)

[0809] For the tubular containers of Examples 7-1 to 7-3 and Comparative Examples 7-1 and 7-2, the appearance of the tubular containers and the stability and ease of sealing between the other end of the main body and the periphery of the flange were confirmed.

[0810] (Experimental Results / Investigation)

[0811] In Examples 7-1 to 7-3, pleats are uniformly formed along the circumferential direction of the periphery, resulting in an aesthetically pleasing main body and a good appearance for the tubular container. Furthermore, the seal between the other end of the main body and the periphery of the flange is easily stabilized. In Example 7-1, the outermost layer of the laminated sheet constituting the main body uses a resin that softens upon heating, namely polyethylene. Compared to Examples 7-1 and 7-2, the main body is formed more aesthetically, the tubular container has a good appearance, and the seal between the other end of the main body and the periphery of the flange is easily stabilized.

[0812] On the other hand, in Comparative Example 7-1, the first and second grid lines were not aesthetically pleasingly formed. In Comparative Example 7-2, the height difference between the other end of the sealing body and the periphery of the flange was difficult to fill, resulting in leakage. Therefore, in Comparative Examples 7-1 and 7-2, the appearance of the folded portion deteriorated, and the sealing performance between the other end of the body and the periphery of the flange was difficult to maintain stably.

[0813] The above test results show that: When the main body has a first grid line and a second grid line, and the other end of the main body is bent along the first and second grid lines, a fold is formed on the outside of the other end of the main body on the periphery of the flange, and the tubular container is installed on the periphery of the flange, the unit area weight of the paper contained in the main body is greater than 30 g / m². 2 And less than 300g / m 2 In this case, the tubular container has a good appearance, and the seal between the other end of the main body and the periphery of the flange is easy to stabilize.

[0814] As described above, in the tubular container according to the seventh embodiment, the outlet has a flat flange that is orthogonal to the height direction of the main body, so it does not have a space that allows the contents to remain on the inner side, thus suppressing the residue of the contents inside the container, and further exerting the following effects.

[0815] In the tubular container according to the seventh embodiment, the main body has a weight per unit area greater than 30 g / m². 2 And less than 300g / m 2The main body of the flange has a first grid line and a second grid line. When viewed from the height of the main body, the periphery of the flange is approximately circular. The first grid line is a zigzag line that curves towards the center of the main body and forms along the circumference of the main body to be installed on the periphery of the flange. The second grid line is configured such that a zigzag line formed at a predetermined position and two valley zigzag lines symmetrically positioned relative to that zigzag line are grouped together, and two or more groups are evenly formed along the circumference of the flange. Furthermore, the other end of the main body curves along the first and second grid lines, forming a fold on the outside of the other end of the main body on the periphery of the flange, and is installed on the periphery of the flange. Therefore, the folds are evenly formed along the circumference of the main body, resulting in an aesthetically pleasing main body with a good appearance, and easy and stable sealing with the flange mounting portion.

[0816] <Examples and Comparative Examples of the 8th Embodiment>

[0817] (Example 8-1)

[0818] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 120 g / m². 2 A 12μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) are sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). Ink is applied to the unbleached kraft paper, and polyethylene (PE) is extruded onto it to produce a sheet for forming the main body.

[0819] A 4mm wide strip was inserted into the prepared sheet to create an overlap of 1.0mm. This was then processed using a backing bag-making machine to produce a sealed bag (main body) with a diameter of 35mm and a length of 180 (175.1±1.50)mm. At this point, the center of the strip was approximately aligned with the edge of the sheet located inside the main body. The strip used was obtained by micro-cutting a 50μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) monolayer.

[0820] The injection plug is made of polyethylene resin by injection molding.

[0821] Using a specialized processing device, the main body and the injection port were heat-fused together to create a tubular container with an inner diameter of 35 mm.

[0822] (Example 8-2)

[0823] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 A 9μm thick aluminum foil (Toyo Aluminium Co., Ltd.), a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). The width of the overlap was set to 3.0 mm, and the width of the strip was set to 8.0 mm. Otherwise, a tubular container with an inner diameter of 35 mm was fabricated in the same manner as in Example 8-1.

[0824] (Example 8-3)

[0825] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 150 g / m². 2 A 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), a 9μm thick aluminum foil (Toyo Aluminium Co., Ltd.), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). Ink was applied to the unbleached kraft paper, and ethylene-methacrylic acid copolymer (EMAA) was extruded onto it to produce a sheet for forming the main body. The width of the overlap was set to 5.0 mm, and the width of the strip was set to 12.0 mm. Otherwise, a tubular container with an inner diameter of 35 mm was produced in the same manner as in Example 8-1.

[0826] (Example 8-4)

[0827] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 70 g / m². 2A 12μm thick transparent barrier film (Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). Ink was applied to the unbleached kraft paper, and an ethylene-methacrylic acid copolymer was extruded onto it to produce a sheet for forming the main body. The width of the overlap was set to 8.0 mm, and the width of the strip was set to 15.0 mm. Otherwise, a tubular container with an inner diameter of 35 mm was produced in the same manner as in Example 8-1.

[0828] (Comparative Example 8-1)

[0829] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 120 g / m². 2 A 12μm thick transparent barrier film (Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). The width of the overlap was set to 0.0mm, and the width of the strip was set to 3.0mm. Otherwise, a tubular container with an inner diameter of 35mm was fabricated in the same manner as in Example 8-1.

[0830] (Comparative Example 8-2)

[0831] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 150 g / m². 2 A 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), a 9μm thick aluminum foil (Toyo Aluminium Co., Ltd.), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). Ink was applied to the unbleached kraft paper, and an ethylene-methacrylic acid copolymer was extruded onto it to produce a sheet for forming the main body. The width of the overlap was set to 3.0 mm, and the width of the strip was set to 2.0 mm. Otherwise, a tubular container with an inner diameter of 35 mm was produced in the same manner as in Example 8-1.

[0832] (Comparative Example 8-3)

[0833] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 100 g / m². 2 A 9μm thick aluminum foil (Toyo Aluminium Co., Ltd.), a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). The width of the overlap was set to 0.5mm, and the width of the strip was set to 15.0mm. Otherwise, a tubular container with an inner diameter of 35mm was fabricated in the same manner as in Example 8-1.

[0834] (Comparative Example 8-4)

[0835] Using dry lamination, a two-component curing urethane adhesive was applied at a weight of 70 g / m². 2 A 12μm thick transparent barrier film (Toppan Printing Co., Ltd., trade name: GL-RD), a 15μm thick stretched nylon film (Unitica Co., Ltd., trade name: ONBC), and a 50μm thick linear low-melting-point polyethylene (LLDPE, Tamapoli Chemical Co., Ltd., trade name: SE625N) were sequentially pasted onto unbleached kraft paper (manufactured by Oji Paper Co., Ltd.). Ink was applied to the unbleached kraft paper, and an ethylene-methacrylic acid copolymer was extruded onto it to produce a sheet for forming the main body. The width of the overlap was set to 9.0 mm, and the width of the strip was set to 16.0 mm. Otherwise, a tubular container with an inner diameter of 35 mm was produced in the same manner as in Example 8-1.

[0836] (Comparative Example 8-5)

[0837] A sheet for forming the main body was fabricated by sequentially bonding a 12 μm thick transparent barrier film (manufactured by Toppan Printing Co., Ltd., trade name: GL-RD), a 15 μm thick stretched nylon film (manufactured by Unitica Co., Ltd., trade name: ONBC), and a 100 μm thick linear low-melting-point polyethylene (LLDPE, manufactured by Tamapoli Chemical Co., Ltd., trade name: SE625N) using a dry lamination process and a two-component curable urethane adhesive. The overlap width was set to 1.0 mm, and the strip width was set to 8.0 mm. Otherwise, a tubular container with an inner diameter of 35 mm was fabricated in the same manner as in Example 8-1.

[0838] The tubular containers made in Examples 8-1 to 8-4 and Comparative Examples 8-1 to 8-5 were evaluated for barrier properties, vibration, drop, suitability for plug welding, and usability.

[0839] In the barrier properties evaluation, methylene blue, which changes color from yellow to blue upon reaction with oxygen, was used. Specifically, agarose gel containing methylene blue was filled into a tubular container, and after standing at room temperature for 3 days, the main body was cut perpendicular to the direction of the overlapping portion to obtain a circular section, and the discoloration of the agarose gel in the cross-section was confirmed.

[0840] In the drop test, with 100 mL of water filled into a tubular container, the container was dropped 10 times from a height of 1.5 m in a random manner to check for any breakage.

[0841] In the vibration test, the tubular container is subjected to random amplitude and frequency vibrations along the z-axis (vertical direction, the axial direction of the container) for 15 minutes to check for any bag breakage.

[0842] In the evaluation of the adaptability of the plug welding, the heat welding process of the main body and the injection port in Examples 8-1 to 8-4 and Comparative Examples 8-1 to 8-5 was performed 200 times continuously to confirm whether the inspection machine would make a false inspection because the main body of the tubular container could not be formed into a true circle, and to confirm whether there was poor adhesion between the main body and the injection port.

[0843] In the evaluation of user experience, 10 observers were asked to describe their discomfort and difficulties in actual use.

[0844] Table 9 shows the structure of the tubular containers involved in each embodiment and comparative example, the width of the overlapping portion (overlap width), the strip width, the results of each test and evaluation, and the results of the comprehensive evaluation. It should be noted that the values ​​recorded in the "Structure of the Main Body" column of Table 9 represent the weight per unit area of ​​the paper (g / m²). 2 ) or the thickness of the layer (μm).

[0845] The tests, evaluations, and comprehensive evaluations in Table 9 are evaluated according to the following standards.

[0846] <Barrier Assessment>

[0847] 〇: No color change on agar gel

[0848] ×: Agar gel discoloration

[0849] Drop test / vibration test

[0850] 〇: No broken bags

[0851] ×: There is a torn bag.

[0852] <Evaluation of the Suitability of Filtration with Mouth Plugs>

[0853] 〇: The number of tubular containers that experienced false detection or poor adhesion is less than 50%.

[0854] ×: More than 50% of the tubular containers experienced false detection or poor adhesion.

[0855] <User Experience Review>

[0856] 〇: Regarding user experience, the number of people who felt uncomfortable or had difficulty using the product was 0.

[0857] ×: More than one person experienced discomfort or difficulty using the product.

[0858] <Overall Evaluation>

[0859] 〇: The results of the barrier performance evaluation, vibration test, drop test, plug welding suitability evaluation, and user experience evaluation were all good (〇).

[0860] ×: Any one of the following evaluation results is unsatisfactory: barrier performance evaluation, vibration test, drop test, plug welding suitability evaluation, or user experience evaluation (×).

[0861]

[0862] As shown in Table 9, the overlap width of the tubular containers involved in Examples 8-1 to 8-4 is in the range of 1.0 to 8.0 mm, and the strip width is in the range of 4.0 to 15.0 mm. Therefore, the results in all tests and evaluations were good, with excellent barrier properties and user experience. No bag breakage or poor formation occurred, and...

Claims

1. A tubular container, comprising: A tubular main body closed at one end, and The injection port is installed at the other end of the main body. The main body is formed of a paper-based material. The injection outlet has: The first cylindrical section is cylindrical and has a flange at one end in the axial direction; and The flat plate portion has an annular flat plate shape with an opening having a cross-sectional shape substantially the same as that of the first cylindrical portion, and with the first cylindrical portion passing through the opening, one side of the flange is sealed to the first cylindrical portion. A portion of the plate portion is sealed to the other side of the main body portion within a predetermined range from the other end. The first cylindrical section, the flat section, and the main body section are composed of sheets mainly made of paper.

2. The tubular container according to claim 1, wherein, The first cylindrical section has: The first adhesive section is formed by rolling a rectangular first blank, which is mainly composed of a sheet of paper, into a cylindrical shape, and overlapping and sealing a portion of a pair of oppositely facing end edges within a predetermined range. The flange is formed by rolling and flattening a portion of one end edge of the first blank, which is rolled into a cylindrical shape, outward from a predetermined distance in the axial direction. The pair of end edges are folded back into the interior of the first adhesive portion and sealed, and the axially oriented one end edge is rolled back into the interior of the flange and sealed.

3. The tubular container according to claim 2, wherein, The first cylindrical portion further has an outer peripheral portion, which is formed by rolling a portion of the first blank rolled into a cylindrical shape outward from another end edge in the axial direction within a predetermined range and flattening it along the outer peripheral surface of the first cylindrical portion. The other end edge in the axial direction is rolled back into the interior of the outer periphery and sealed.

4. The tubular container according to any one of claims 1 to 3, wherein, The flat section has a folded-back section, which is formed by folding back the annular portion of the outer periphery of the second blank, which is composed of a sheet mainly made of paper, to the other side. A portion of the portion at a predetermined range from the other end of the main body is sealed to the entirety of the folded portion, and a portion along the entire inner circumference of the folded portion on the other side of the flat plate.

5. The tubular container according to any one of claims 1 to 3, It further includes a cover made of a sheet material mainly composed of paper, which can be installed on the first cylindrical part. The cover comprises: It has a cylindrical second section and A flat, plate-shaped cover that is embedded inside the second cylindrical portion and closes one axial end of the second cylindrical portion. The second cylindrical section has: The second adhesive part is formed by rolling a rectangular third blank, which is mainly composed of a sheet of paper, into a cylindrical shape, and overlapping and sealing a portion of a pair of oppositely facing end edges within a predetermined range. A connecting portion, formed by inwardly curling and flattening a portion of the third blank rolled into a cylindrical shape within a predetermined range along one end edge in the axial direction, is sealed to the outer periphery of the cover portion embedded in the second cylindrical portion; and The inner circumference is formed by curling a portion of the third blank, which is rolled into a cylindrical shape, inwardly within a predetermined range from the other end edge in the axial direction and flattening it along the inner circumferential surface of the second cylindrical portion. The pair of end edges are folded back into the interior of the second adhesive portion and sealed, the axial one end edge is rolled back into the interior of the connecting portion and sealed, and the axial other end edge is rolled back into the interior of the inner circumference portion and sealed.

6. The tubular container according to claim 1, wherein, The main body portion is formed using a main body portion forming blank, which is composed of a laminated sheet material having at least an outermost and an innermost thermoplastic resin layer and an intermediate paper layer. The end faces of the paper layer are not exposed at least at the two opposite ends of the blank formed in the main body. The main body is formed by thermally fusing the opposite ends of the blank by overlapping the outermost and innermost surfaces.

7. The tubular container according to claim 6, wherein, The thickness of the laminated sheet is between 30 μm and 300 μm.

8. The tubular container according to claim 6 or 7, wherein, A barrier layer is stacked between the innermost thermoplastic resin layer and the paper layer.

9. The tubular container according to claim 6 or 7, wherein, The paper layer has a weight per unit area of 3 g / m 2 The above 300 g / m 2 The following.

10. The tubular container according to claim 6 or 7, wherein, The outermost thermoplastic resin layer is a sealant layer, and the thickness of the outermost sealant layer is more than 3 μm and less than 200 μm.

11. The tubular container according to claim 6 or 7, The paper has a first adhesive layer and a second adhesive layer sandwiching the paper layer, each of the first adhesive layer and the second adhesive layer having a thickness of 5 μm or more and 100 μm or less.

12. The tubular container according to claim 6 or 7, The inlet / outlet portion has a flat, closed portion that is orthogonal to the height direction of the main body of the tubular container. In the periphery of the closure, the other end of the main body of the tubular container is bonded to the side of the closure opposite to the end of the main body of the tubular container.

13. The tubular container according to claim 1, wherein, The main body is formed by making a sheet with a pair of opposing end edges into a cylindrical shape, and by attaching strips along portions of the pair of end edges on the inner surface of the sheet. The strip has a strip-shaped substrate. The two sides and end faces of the substrate are coated with resin.

14. The tubular container according to claim 13, wherein, The substrate of the strip is a barrier layer.

15. The tubular container according to claim 1, wherein, The main body is formed by rolling a sheet into a cylindrical shape, the sheet comprising a paper layer and an innermost sealant layer, and having a pair of opposing end edges. The main body portion has an overlapping portion formed by sealing the innermost layer of a portion within a predetermined range from one of the other end edges to the outermost layer of a portion within a predetermined range from one of the end edges. A strip is provided, which is composed of a film that can be bonded to the sealant layer but does not contain adhesive, and is sealed to the innermost layer of the sheet constituting the body portion in such a way as to cover one end edge.

16. The tubular container according to claim 15, wherein, The width of the overlapping portion is greater than 1.0 mm and less than 8.0 mm.

17. The tubular container according to claim 15 or 16, wherein, The width of the strip is between 4.0 mm and 15.0 mm.

18. The tubular container according to claim 15 or 16, wherein, A paper protective layer is provided on the outermost layer of the sheet, which is composed of a resin that is weldable to the sealant layer.

Citation Information

Patent Citations

  • Terminal structure of shielded wire

    JP1995045311A

  • Tube container

    JP2016199280A

  • Extrusion tube

    JP1996151056A

  • Paper container with pouring outlet cap

    JP2001213430A

  • Paper container for liquid

    JP2012025471A