Optical fiber drawing furnace and optical fiber manufacturing method

By designing the structure of the narrow part and gas inlet in the fiber drawing furnace, the concentration of silica powder is reduced, and the problem of reduced strength during the fiber drawing process is solved, production efficiency is improved and manufacturing cost is reduced.

CN115335337BActive Publication Date: 2024-11-22SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180023039.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-23
Filing Date
2021-03-22
Publication Date
2024-11-22
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

During the fiber drawing process, the SiO2 gas generated by the glass base material becomes cold into silica powder and floats in the wire drawing furnace, resulting in a decrease in the fiber intensity. The existing methods are difficult to effectively reduce dust concentration and increasing the gas flow will increase manufacturing costs.

Method used

An optical fiber wire drawing furnace is designed, including a furnace core tube, a lower chamber and a protective tube. By setting a narrow part and a gas inlet in the protective tube, an inert gas is introduced to reduce the concentration of silica powder and exhaust gas through the exhaust hole. , ensure that the optical fiber moves stably in the protection tube and reduce the probability of contact with the optical fiber.

Benefits of technology

The contact probability between the optical fiber and silica powder is effectively reduced, the reduction of the fiber intensity is suppressed, productivity is improved, and the manufacturing cost is reduced by using cheap gases such as argon or nitrogen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115335337B_ABST
    Figure CN115335337B_ABST
Patent Text Reader

Abstract

The wire drawing furnace includes: a furnace core tube into which a glass base material for optical fiber is to be inserted, a furnace body accommodating a heater for heating the glass base material for optical fiber from the outside, a lower chamber arranged below the furnace core tube, and a protection tube arranged below the lower chamber, wherein an inert gas flows from the upper side to the lower side in the furnace core tube. Furthermore, the wire drawing furnace has a gas introduction port for introducing a predetermined gas into the protection tube, and has a narrow portion on the upper side of the gas introduction port in which the radial cross-sectional area of ​​the internal space is smaller than that of the lower chamber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical fiber drawing furnace and an optical fiber manufacturing method.

[0002] This application claims the benefit of priority based on Japanese Patent Application No. 2020-051898 filed on March 23, 2020, and incorporates all the contents described in the patent application by reference. Background Art

[0003] Patent Document 1 discloses an optical fiber manufacturing apparatus that supplies helium gas into a drawing furnace to draw an optical fiber, and cools the drawn optical fiber in argon gas in a cooling tube connected to the drawing furnace.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2000-128566 Summary of the invention

[0007] Means for solving problems

[0008] One embodiment of the present disclosure relates to an optical fiber drawing furnace comprising: a furnace core tube into which a glass base material for an optical fiber is to be inserted, a heater for heating the glass base material for the optical fiber from the outside and a furnace body in which the furnace core tube is accommodated, a lower chamber arranged below the furnace core tube, a protective tube arranged below the lower chamber, and an in-furnace gas inlet portion for allowing an inert gas to flow from the top to the bottom in the furnace core tube, the optical fiber drawing furnace having a gas inlet port for introducing a predetermined gas into the protective tube, and having a narrow portion on the upper side of the gas inlet port whose radial cross-sectional area of ​​the internal space is smaller than that of the lower chamber.

[0009] Furthermore, an optical fiber production method according to one embodiment of the present disclosure is a method of producing an optical fiber using the above-mentioned optical fiber drawing furnace. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] [ Figure 1 ] Figure 1 Schematic diagram of an optical fiber drawing furnace according to an embodiment of the present disclosure.

[0011] [ Figure 2A ] Figure 2A It is a diagram showing another example of the gas inlet port of the protection tube.

[0012] [ Figure 2B ] Figure 2B It is a diagram showing another example of the gas inlet port of the protection tube.

[0013] [ Figure 3A ] Figure 3Ais a schematic diagram of an optical fiber drawing furnace according to another embodiment of the present disclosure.

[0014] [ Figure 3B ] Figure 3B yes Figure 3A 3B-3B arrow cross-sectional view. DETAILED DESCRIPTION

[0015] [Problems to be Solved by the Present Disclosure]

[0016] The drawing furnace is provided with a lower chamber (lower chimney) and a protective tube located below the lower chamber, and the optical fiber (glass fiber portion) is protected in the lower chamber and the protective tube in such a way that the glass diameter of the optical fiber is stabilized. On the other hand, since SiO2 gas etc. is generated from the high-temperature glass matrix, the SiO2 gas etc. cools down in the lower chamber and generates silicon dioxide.

[0017] (SiO2) powder. Silica powder floats in the inert gas blown into the drawing furnace, deposits in the drawing furnace, or is discharged from the lower chamber of the drawing furnace and the outlet of the protective tube to the outside of the furnace, or contacts or collides with the optical fiber. When the glass fiber part in the drawing contacts or collides with the silica powder floating in the gas in the drawing furnace, the strength of the optical fiber decreases. When the strength of the optical fiber decreases, the frequency of optical fiber breakage increases in the optical fiber screening test (verification test) performed after the drawing is completed, and productivity may decrease.

[0018] In order to reduce the amount of silica powder generated from the glass matrix, there is a method of lowering the temperature of the wire drawing furnace. However, in addition to affecting the desired glass tension in the wire drawing, the temperature of the wire drawing furnace also depends on the size of the matrix, etc., so it is difficult to simply lower the temperature of the wire drawing furnace. In addition, in order to reduce the concentration of silica powder floating in the gas in the wire drawing furnace per unit gas flow, it is also considered to increase the gas flow in the wire drawing furnace, but the manufacturing cost may increase.

[0019] [Description of Embodiments of the Present Disclosure]

[0020] First, embodiments of the present disclosure will be listed and described.

[0021] The optical fiber drawing furnace (1) disclosed in the present invention comprises: a furnace core tube into which a glass matrix for optical fiber is to be inserted, a heater for heating the glass matrix for optical fiber from the outside and a furnace body in which the furnace core tube is housed, a lower chamber arranged below the furnace core tube, a protective tube arranged below the lower chamber, and a furnace gas inlet portion for allowing an inert gas to flow from the top to the bottom in the furnace core tube, wherein the optical fiber drawing furnace has a gas inlet port for introducing a predetermined gas into the protective tube, and a narrow portion on the upper side of the gas inlet port having an internal space with a radial cross-sectional area smaller than that of the lower chamber.

[0022] This can reduce the concentration of silica powder per gas flow rate in the protection tube, so the probability of silica powder contacting or colliding with the optical fiber is reduced, and the occurrence of reduction in the strength of the optical fiber can be suppressed.

[0023] (2) The protection tube may be connected below the lower chamber.

[0024] As a result, the optical fiber is not exposed to the outside air between the lower chamber and the protective tube, and the glass diameter is stabilized.

[0025] (3) It is preferable that the gas introduction port is provided on the upper side of the center of the protection tube.

[0026] As a result, the concentration of silica powder per gas flow rate can be reduced in most of the protective tube, so the probability of silica powder contacting or colliding with the optical fiber is reduced, and the occurrence of reduction in the strength of the optical fiber can be suppressed.

[0027] (4) The lower chamber may have an exhaust hole at the lower portion thereof for exhausting the inert gas in the lower chamber to the outside.

[0028] This further reduces the probability that the silica powder contacts or collides with the optical fiber, and can suppress the occurrence of a decrease in the strength of the optical fiber.

[0029] (5) Gas can be forcibly exhausted from the exhaust hole.

[0030] This further reduces the probability that the silica powder contacts or collides with the optical fiber, and can suppress the occurrence of a decrease in the strength of the optical fiber.

[0031] (6) It is preferable that the gas introduction port is provided at the upper end portion of the protection tube.

[0032] As a result, the concentration of silica powder can be rapidly reduced in the protective tube over the substantially entire length of the protective tube, and the probability of the silica powder contacting or colliding with the optical fiber is further reduced.

[0033] (7) The predetermined gas may be argon, nitrogen or air.

[0034] Thus, by using an inexpensive gas, it is possible to reduce the manufacturing cost and suppress the occurrence of a decrease in the strength of the optical fiber.

[0035] (8) The gas introduction ports may be provided at equal intervals in the circumferential direction of the protection tube.

[0036] Thus, since the gas is evenly distributed around the optical fiber, the optical fiber can be prevented from shaking in the protective tube, and the influence of the optical fiber diameter variation and the bending of the optical fiber (fiber curling) caused by temperature non-uniformity can be suppressed.

[0037] (9) The gas introduction port may be provided downward so as to introduce the predetermined gas downward into the interior of the protection tube.

[0038] This can suppress turbulence of the airflow in the protection tube.

[0039] (10) The gas introduction port may be tilted downward and directed along the wall surface of the protection tube so as to introduce the predetermined gas into the protection tube in a spiral shape.

[0040] This makes it easier to separate the silica powder from around the fibers. In addition, it is possible to reduce turbulence of the airflow around the fibers.

[0041] An optical fiber manufacturing method (11) according to one embodiment of the present disclosure is a method for manufacturing an optical fiber using the above-mentioned optical fiber drawing furnace.

[0042] This can reduce the concentration of silica powder per gas flow rate in the protection tube, so the probability of silica powder contacting or colliding with the optical fiber is reduced, and the occurrence of reduction in the strength of the optical fiber can be suppressed.

[0043] [Details of the embodiments of the present disclosure]

[0044] Hereinafter, with reference to the accompanying drawings, preferred embodiments of the optical fiber drawing furnace and the optical fiber manufacturing method involved in the present disclosure are described. In the following description, the components marked with the same symbols in different drawings are also the same, and their descriptions are sometimes omitted. It should be noted that the present disclosure is not limited to the examples in these embodiments, and includes all changes within the scope and equivalent scope described in the claims. In addition, as long as multiple embodiments can be combined, the present disclosure includes a method of combining any embodiments.

[0045] (First embodiment)

[0046] Figure 1 It is a schematic diagram of an optical fiber drawing furnace involved in one embodiment of the present disclosure. The optical fiber drawing furnace (hereinafter referred to as the "drawing furnace") 10 has a furnace body 11, an upper chamber 12 arranged above the furnace body 11, and a lower chamber 13 arranged below. The upper chamber 12 and the lower chamber 13 are hollow tube shapes. A heater 15 for heating and melting the glass mother material 1 is arranged inside the furnace body 11, and a cylindrical furnace core tube 14 is arranged in a manner surrounded by the heater 15. Between the heater 15 and the furnace body 11, in order to prevent the heat from the heater 15 from being dissipated to the outside, an insulating material 16 is arranged in a manner surrounding the heater 15. It should be noted that the heater can also use induction heating.

[0047] A protective tube 20 described in detail below is disposed below the lower chamber 13. The protective tube 20 is preferably tightly connected to the lower chamber 13, but regardless of the number, a gap may exist between the protective tube 20 and the lower chamber 13. In addition, in the present embodiment, the configuration in which the lower chamber 13 and the protective tube 20 are provided separately is described, but each may be divided into a plurality of parts or may be integrated.

[0048] The drawing of the optical fiber 2 is a process in which the glass mother material 1 is suspended in the furnace core tube 14 by a mother material suspension mechanism (not shown), the lower part of the glass mother material 1 is heated by a heater 15, and the optical fiber (glass fiber part) 2 is melted and drooped from the lower end of the molten glass mother material 1, so that the optical fiber 2 taken out from the bottom of the drawing furnace 10 has a predetermined outer diameter. Nitrogen, helium, argon or other inert gas introduced from the furnace gas inlet 17 is supplied from the top to the bottom into the furnace core tube 14. Since the furnace core tube 14 is in an inert gas atmosphere, oxidation of the furnace core tube 14 and the like, which are carbon components, can be prevented, and the inside can be kept clean.

[0049] The inert gas introduced into the furnace core tube 14 is heated to about 2000° C. or more in the furnace core tube 14. A portion of the heated inert gas flows downward, passes through the space inside the furnace core tube 14, and is discharged to the outside together with the optical fiber 2 via the lower chamber 13 and the protection tube 20.

[0050] In the present embodiment, the lower chamber 13 is connected to the protection tube 20, and a narrow portion 13a of the lower chamber 13 and a narrow portion 20a of the protection tube 20 are formed at the connection portion, respectively, in which the cross-sectional area of ​​the internal space is smaller than that of the lower chamber 13. In addition, a gas inlet 21 is provided just below the narrow portion 20a of the protection tube 20. The gas inlet 21 is provided at four locations at equal intervals in the circumferential direction of the protection tube 20, for example. The narrow portions 13a and 20a are used to maintain the pressure inside the core tube 14 and the lower chamber 13 above these narrow portions 13a and 20a at a pressure that is positive to the pressure inside the protection tube 20 below the narrow portions 13a and 20a.

[0051] The narrow portion only needs to be on the upper side of the gas inlet port 21, and is not limited to being set at the connection portion between the lower chamber 13 and the protection tube 20, and may also be set only at either the lower chamber 13 or the protection tube 20. In addition, the gas inlet port 21 is preferably set at the upper end portion of the protection tube 20 (including not only the upper end but also the vicinity of the upper end), but it only needs to be set at the upper side of the center in the longitudinal direction of the protection tube 20. It should be noted that when the lower chamber 13 and the protection tube 20 are integrated, it is preferred to set the gas inlet port 21 near the central portion thereof. Then, a gas cheaper than helium, such as argon, nitrogen or air in a clean state, is introduced into the gas inlet port 21 from the outside.

[0052] In this embodiment, the concentration of silica powder floating in the inert gas in the drawing furnace 10 per unit gas flow rate is reduced in the protection tube 20 having the gas inlet port 21, thereby reducing the probability of contact or collision between the optical fiber 2 being drawn and the silica powder.

[0053] For example, when an inert gas with a flow rate of Q1slm (converted to Q1 liter / minute in standard state) flows downward in the furnace core tube 14, assuming that each Q1 liter contains N silica powders, the concentration of silica powder per gas flow rate in the lower chamber 13 is N / Q1. Furthermore, when Q2slm of gas is introduced into the protection tube 20 from the gas inlet 21 of the protection tube 20, the gas flow rate flowing through the protection tube 20 from the top to the bottom is Q3 (=Q1+Q2)slm. Therefore, the concentration of silica powder per gas flow rate in the protection tube 20 is N / Q3, and the concentration of silica powder per unit gas flow rate floating in the inert gas in the wire drawing furnace 10 can be reduced in the protection tube 20 having the gas inlet 21. It should be noted that by providing the narrow portion 13a of the lower chamber 13 and the narrow portion 20a of the protection tube 20, the pressure in the lower chamber 13 can be maintained higher than the pressure inside the protection tube 20 below the narrow portions 13a and 20a. As a result, the gas introduced from the gas inlet 21 is suppressed from flowing to the lower chamber 13 side.

[0054] Thus, the probability of contact or collision between silica powder and the optical fiber 2 in the protective tube 20 can be reduced. In addition, the silica powder contained in the gas flowing in the furnace core tube 14 is rapidly discharged from the protective tube 20 to the outside by the gas introduced from the gas inlet 21 of the protective tube 20. The optical fiber 2 moves at a constant speed in the furnace core tube 14, the lower chamber 13, and the protective tube 20. However, since the concentration of silica powder per unit gas flow rate when passing through the protective tube 20 is lower than that in the case where no gas is introduced, the probability of contact or collision between silica powder can be reduced as a whole, and the occurrence of reduction in the strength of the optical fiber can be suppressed.

[0055] In addition, the gas introduced into the protection tube 20 can be introduced from the uppermost part of the protection tube 20 to quickly reduce the concentration of silica powder in the protection tube 20 below the gas introduction port 21. Therefore, it is preferred to reduce the concentration of silica powder over the entire length of the protection tube 20 by providing the gas introduction port 21 near the upper end of the protection tube 20. In addition, the gas introduced into the protection tube 20 preferably flows evenly from the circumference of the optical fiber 2 so that the optical fiber 2 does not shake.

[0056] (Second embodiment)

[0057] Next, another example of the gas introduction port 21 provided in the protection tube 20 will be described. Figure 2A2 is a diagram showing other examples of the gas inlet of the protective tube, which is a cross-sectional view in the longitudinal direction. In the present embodiment, the plurality of gas inlet ports 21' provided in the protective tube 20 are provided in a manner inclined downward toward the protective tube 20. Therefore, the gas introduced into the protective tube 20 from the gas inlet port 21' is introduced into the interior of the protective tube 20 at a downward angle. Thus, the gas introduced into the protective tube 20 flows smoothly in the traveling direction of the optical fiber 2, thereby suppressing the turbulence of the airflow, suppressing the influence on the diameter variation of the optical fiber 2 and the influence on the curling of the optical fiber. It should be noted that, in the present embodiment, the gas introduced into the protective tube 20 preferably flows evenly from the circumference of the optical fiber 2.

[0058] (Third embodiment)

[0059] Next, another example of the gas introduction port 21 provided in the protection tube 20 will be described. Figure 2B 2 is a diagram showing other examples of the gas inlet port of the protective tube, which is a radial cross-sectional view. In the present embodiment, the multiple gas inlet ports 21" provided in the protective tube 20 are not provided in a direction toward the center of the protective tube 20, but are provided in a manner of introducing the gas obliquely downward and along the wall surface. Thus, the gas introduced into the protective tube 20 rotates along the inner wall of the protective tube 20, that is, flows in a spiral shape along the circumferential direction, and the silica powder is easily separated from the periphery of the optical fiber 2. It should be noted that the gas introduced into the protective tube 20 may flow from one gas inlet port, or may flow evenly from multiple gas inlet ports 21".

[0060] (Fourth embodiment)

[0061] Figure 3A Schematic diagram of an optical fiber drawing furnace according to another embodiment of the present invention. Figure 3B yes Figure 3A In this embodiment, an exhaust hole 13b opened to the outside is provided below the lower chamber 13, which is different from the first to third embodiments, but the other structures are the same, so the description of the repeated structures is omitted.

[0062] In this embodiment, if Figure 3B As shown, a plurality of exhaust holes 13b are provided at equal intervals around a narrow portion 13a provided below the lower chamber 13. A portion of the inert gas flowing through the furnace core tube 14 and the lower chamber 13 is discharged to the outside from the exhaust holes 13b together with the silica powder.

[0063] The exhaust hole 13 b is configured to exhaust the inert gas to the bottom of the lower chamber 13 , but may be provided on the side surface of the lower portion of the lower chamber so as to exhaust the inert gas to the side of the lower chamber.

[0064] For example, similarly to the first embodiment, when the inert gas at a flow rate of Q1slm flows downward in the furnace core tube 14, assuming that N silica powders are contained per Q1 liter, the concentration of silica powder per gas flow rate in the lower chamber 13 is N / Q1. Furthermore, in the case of the present embodiment, when the inert gas of Q4slm is discharged to the outside from the exhaust hole 13b, (Q1-Q4)slm of gas is introduced from the lower chamber 13 into the protection tube 20. It should be noted that the concentration of silica powder per gas flow rate contained in the inert gas introduced into the protection tube 20 is the same as N / Q1, but the amount of silica powder entering the protection tube 20 per minute is N×(1-Q4 / Q1).

[0065] Furthermore, similarly to the first embodiment, when Q2 slm of gas is introduced into the protection tube 20 from the gas inlet port 21 of the protection tube 20, the gas flow rate flowing from the top to the bottom in the protection tube 20 is made Q5 (= Q1-Q4+Q2) slm. Therefore, the concentration of silica powder per gas flow rate in the protection tube 20 is {N×(1-Q4 / Q1)} / Q5. Therefore, compared with the first embodiment, the concentration of silica powder per unit gas flow rate floating in the inert gas in the protection tube 20 can be reduced.

[0066] (Example)

[0067] When no narrowing portion was provided at the connection part and no gas was introduced, the disconnection frequency (= disconnection times per 1 Mm (= 1000 km)) of the optical fiber in the screening test was 2 times / Mm. On the other hand, when a narrowing portion was provided and gas was introduced, the disconnection frequency was reduced to 1.5 times / Mm. Furthermore, when an exhaust hole was provided at the lower part of the lower chamber and gas was introduced, the disconnection frequency was reduced to 1 time / Mm.

[0068] It should be noted that, in the fourth embodiment, similarly to the second and third embodiments, the gas introduced into the protective tube 20 is preferably introduced into the protective tube 20 at a downward angle, or introduced in a manner that flows in a spiral shape in the circumferential direction along the inner wall of the protective tube 20. In addition, in order to make the flow rate of the inert gas discharged to the outside from the exhaust hole 13b greater than the flow rate of the inert gas toward the protective tube 20, the inert gas in the lower chamber 13 may be sucked from the exhaust hole 13b and forcibly exhausted. In this way, by exhausting the inert gas to the outside from the exhaust hole 13b, the ratio of the gas flow rate for optical fiber pulling and the gas flow rate discharged from the exhaust hole can be controlled.

[0069] Description of the label

[0070] 1…Glass base material, 2…Optical fiber, 10…Wire drawing furnace, 11…Furnace body, 12…Upper chamber, 13…Lower chamber, 13a…Narrow portion, 13b…Exhaust hole, 14…Furnace core tube, 15…Heater, 16…Insulating material, 17…Furnace gas inlet, 20…Protective tube, 20a…Narrow portion, 21, 21', 21"…Gas inlet

Claims

1. An optical fiber drawing furnace, comprising: The furnace core tube into which the glass matrix for optical fiber is to be inserted, a furnace body in which a heater for heating the optical fiber glass base material from the outside and the furnace core tube are housed, a lower chamber disposed below the furnace core tube, a protective tube disposed below the lower chamber, and a furnace gas inlet portion for allowing the inert gas to flow from the upper side to the lower side in the furnace core tube; The optical fiber drawing furnace has a gas inlet for introducing a predetermined gas into the protection tube, and the gas inlet is provided on the upper side of the center of the protection tube or on the upper end of the protection tube. The protective tube is connected to the bottom of the lower chamber, and a narrow portion of the lower chamber and / or a narrow portion of the protective tube whose internal space has a smaller cross-sectional area than the lower chamber are formed at the connecting portion. The gas inlet is provided below the narrow portion. The narrow portion of the lower chamber and / or the narrow portion of the protective tube are used to maintain the pressure inside the lower chamber above these narrow portions at a pressure that is positive than the pressure inside the protective tube below these narrow portions.

2. The optical fiber drawing furnace according to claim 1, wherein: The lower chamber has an exhaust hole at a lower portion thereof for exhausting the inert gas in the lower chamber to the outside.

3. The optical fiber drawing furnace according to claim 2, wherein: The gas is forcibly exhausted from the exhaust hole.

4. The optical fiber drawing furnace according to any one of claims 1 to 3, wherein: The predetermined gas is argon, nitrogen or air.

5. The optical fiber drawing furnace according to any one of claims 1 to 3, wherein: The gas introduction ports are provided at equal intervals in a circumferential direction of the protection tube.

6. The optical fiber drawing furnace according to any one of claims 1 to 3, wherein: The gas introduction port is disposed downward to introduce the predetermined gas downward into the protection tube.

7. The optical fiber drawing furnace according to any one of claims 1 to 3, wherein: The gas introduction port is inclined downward and faces a direction along the wall surface of the protection tube so as to introduce the predetermined gas into the interior of the protection tube in a spiral shape.

8. An optical fiber manufacturing method for manufacturing an optical fiber, using the optical fiber drawing furnace according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method and device for production of optical fiber

    JP2000128566A

  • Measurement system and measurement result presentation program

    JP2020051898A

  • Optical fiber production heating furnace capable of reducing usage amount of helium

    CN105948478A

  • Production device and method for optical fiber

    CN1353674A

  • Manufacture of optical fiber