Seals
By optimizing the composition and process of hydrogenated nitrile butadiene rubber seals and using materials such as fatty acid amides and carbon black for crosslinking, the problem of insufficient wear resistance and durability of hydrogenated nitrile butadiene rubber seals in sliding surface applications has been solved, and the manufacturing of high-performance seals has been achieved.
Patent Information
- Application Number
- CN202210439721.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-13
- Filing Date
- 2022-04-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-04-25
AI Technical Summary
Existing hydrogenated nitrile rubber seals lack sufficient wear resistance and durability in sliding surface applications, making it difficult to meet high-performance requirements.
A rubber composition with hydrogenated nitrile butadiene rubber as the main component is cross-linked with fatty acid amide, carbon black, organic peroxide, co-crosslinking agent and sulfur to form a seal. The component ratio and process parameters are optimized to improve the performance of the sliding surface.
It significantly improves the wear resistance and durability of seals, making them suitable for sliding surface applications and meeting high-performance requirements.
Smart Images

Figure CN115340639B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a sealing element. Background Technology
[0002] Hydrogenated nitrile butadiene rubber is known to be used as a forming material for seals. For example, JP2015-63634A1 discloses a rubber composition comprising a carboxyl-containing hydrogenated nitrile butadiene rubber, hydrogenated nitrile butadiene rubber, and a polyamide resin as a sealant. Summary of the Invention
[0003] This invention relates to an annular seal formed from a rubber composition, the rubber composition containing a rubber component mainly composed of hydrogenated nitrile butadiene rubber, a fatty acid amide, and carbon black with an average particle size of less than 60 nm, and the rubber component being crosslinked using an organic peroxide, a co-crosslinking agent, and sulfur. Attached Figure Description
[0004] Figure 1 This is a cross-sectional view showing the structure in which the seal according to the embodiment is installed;
[0005] Figure 2 This is an explanatory diagram of the abrasion resistance test method.
[0006] - Symbol Explanation -
[0007] 10 – Seal; 21 – Housing; 22 – Cylindrical hole; 23 – Seal receiving groove; 24 – Internal insertion component; 31 – Sample; 32 – Fixing component; 33 – Metal plate. Detailed Implementation
[0008] The implementation method will now be described in detail.
[0009] Figure 1 The diagram shows a structure in which the seal 10 according to the embodiment is installed. The seal 10 is a so-called O-ring, used as follows: the seal 10 is embedded in a seal receiving groove 23 formed on the inner circumferential surface of a cylindrical bore 22 within the housing 21, and an axially movable insert member 24 is inserted into the inner side of the seal 10 in a sliding manner along the inner circumferential surface. Specifically, for example, in a solenoid valve, the seal 10 is embedded in the inner circumferential groove (seal receiving groove 23) of a valve stem insertion hole (cylindrical bore 22) installed within the valve body (housing 21), and the valve stem (insertion member 24) is inserted into the seal 10, thereby clamping the seal 10 between the valve body and the valve stem, serving as a pneumatic gasket.
[0010] The sealing element 10 involved in the embodiment is formed of a rubber composition X, which comprises a rubber component mainly composed of hydrogenated nitrile butadiene rubber (hereinafter referred to as "HNBR"), fatty acid amide A, and carbon black B with an average particle size of less than 60 nm, and the rubber component is crosslinked using an organic peroxide P, a co-crosslinking agent Q, and sulfur R.
[0011] According to the embodiment of the seal 10, the rubber composition X forming the seal 10 includes a rubber component with HNBR as the main component, fatty acid amide A and carbon black B, and the rubber component is crosslinked using an organic peroxide P, a co-crosslinking agent Q and sulfur R, thereby enabling the seal 10 to be used for its inner circumferential surface as a sliding surface.
[0012] The HNBR content in the rubber component is greater than 50% by mass, which is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass, from the viewpoint of obtaining properties applicable when the inner circumferential surface of the seal 10 is used as a sliding surface. It should be noted that, in addition to HNBR, the rubber component may also contain, for example, nitrile rubber, silicone rubber, fluororubber, EPDM, etc.
[0013] From the viewpoint of obtaining properties suitable when the inner circumferential surface of the seal 10 is used as a sliding surface, the amount of acrylonitrile bound in the HNBR is preferably 18% by mass or more and 52% by mass or less, more preferably 30% by mass or more and 40% by mass or less, and even more preferably 35% by mass or more and 37% by mass or less. From the same viewpoint, the iodine value of the HNBR is preferably 8 mg / 100 mg or more and 28 mg / 100 mg or less, more preferably 10 mg / 100 mg or more and 15 mg / 100 mg or less.
[0014] Examples of fatty acid amide A include erucamide, oleamide, stearamide, behenamide, N-oleopalmitamide, N-stearylerucamide ethylene bis-stearamide, and methylene bis-stearamide. Fatty acid amide A preferably contains one or more of the above substances. From the viewpoint of obtaining properties suitable for use when the inner circumferential surface of the seal 10 is used as a sliding surface, it is preferable to contain unsaturated fatty acid amides, more preferably ω-9 fatty acid amides, and even more preferably erucamide. From the same viewpoint, the melting point of fatty acid amide A is preferably 70°C to 90°C, more preferably 75°C to 85°C.
[0015] From the viewpoint of obtaining the properties applicable when the inner circumferential surface of the seal 10 is used as a sliding surface, the content a of fatty acid amide A in the rubber composition X is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 2 parts by mass or more and 6 parts by mass or less, relative to 100 parts by mass of rubber component.
[0016] Examples of carbon black B include FEF, SAF, N234, ISAF, N339, N351, HAF, and MAF. Carbon black B preferably contains one or more of the above substances, and from the viewpoint of obtaining properties suitable for use when the inner circumferential surface of the seal 10 is used as a sliding surface, it is more preferably to contain FEF.
[0017] The average particle size of carbon black B is 60 nm or less. From the viewpoint of obtaining properties suitable for use when the inner circumferential surface of the seal 10 is used as a sliding surface, it is preferably 20 nm or more and 60 nm or less, more preferably 20 nm or more and 55 nm or less, even more preferably 25 nm or more and 50 nm or less, and even more preferably 40 nm or more and 45 nm or less. The average particle size of this carbon black B is the arithmetic mean particle size.
[0018] From the viewpoint of obtaining properties suitable for use when the inner circumferential surface of the seal 10 is used as a sliding surface, the content b of carbon black B in the rubber composition X is preferably 10 parts by mass or more and 80 parts by mass or less, more preferably 35 parts by mass or more and 60 parts by mass or less, and even more preferably 50 parts by mass or more and 58 parts by mass or less, relative to 100 parts by mass of the rubber component. From the same viewpoint, the ratio (b / a) of the content b of carbon black B to the content a of fatty acid amide A in the rubber composition X is preferably 5 or more and 20 or less, more preferably 7 or more and 15 or less, and even more preferably 12 or more and 14 or less.
[0019] Examples of organic peroxides P include, for example: dialkyl peroxides such as di(tert-butylperoxy)diisopropylbenzene, 1,3-di(tert-butylperoxy)diisopropylbenzene, 1,4-di(tert-butylperoxy)diisopropylbenzene, tert-butylisopropylbenzene peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane-3; peroxide ketals such as 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, and n-butyl-4,4-di(tert-butylperoxy)valerate; and peroxide esters such as 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-hexyl peroxybenzoate, and tert-butyl peroxybenzoate.
[0020] The organic peroxide P preferably contains one or more of the above-mentioned substances. From the viewpoint of obtaining properties applicable when the inner circumferential surface of the seal 10 is used as a sliding surface, it preferably contains a dialkyl peroxide, more preferably a dialkyl peroxide having an aromatic ring in the molecule, even more preferably a dialkyl peroxide having one aromatic ring in the molecule, and even more preferably 1,3-bis(tert-butylperoxy)diisopropylbenzene.
[0021] From the viewpoint of obtaining the properties applicable when the inner circumferential surface of the seal 10 is used as a sliding surface, the amount of organic peroxide P added p in the uncrosslinked rubber composition before crosslinking of the rubber composition X is preferably 0.5 parts by mass or more and 5 parts by mass or less, more preferably 1 part by mass or more and 4 parts by mass or less, and even more preferably 2 parts by mass or more and 3 parts by mass or less, relative to 100 parts by mass of rubber component X.
[0022] Examples of co-crosslinking agents Q include: maleimide co-crosslinking agents such as N,N'-m-phenylenebismaleimide, maleimide, and phenylmaleimide; methacrylate co-crosslinking agents such as trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate; allyl co-crosslinking agents such as triallyl cyanurate, diallyl fumarate, diallyl phthalate, tetraallylpropoxyethane, triallyl isocyanurate, and trimethylallyl isocyanurate; and 1,2-polybutadiene. The co-crosslinking agent Q preferably comprises one or more of the above substances. From the viewpoint of obtaining properties suitable when the inner circumferential surface of the seal 10 is used as a sliding surface, it is preferable to include a maleimide co-crosslinking agent, and more preferably, N,N'-m-phenylenebismaleimide.
[0023] From the viewpoint of obtaining properties applicable when the inner circumferential surface of the seal 10 is used as a sliding surface, the amount of co-crosslinking agent Q added to the uncrosslinked rubber composition X before crosslinking is preferably 0.5 parts by mass or more and 10 parts by mass or less, more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of rubber component X.
[0024] From the viewpoint of obtaining properties suitable for use when the inner circumferential surface of the seal 10 is used as a sliding surface, the ratio (q / p) of the amount of co-crosslinking agent Q added to the amount of organic peroxide P added in the uncrosslinked rubber composition before crosslinking of rubber composition X is preferably 0.8 to 3, more preferably 1 to 1.5. From the same viewpoint, the amount of co-crosslinking agent Q added to the uncrosslinked rubber composition before crosslinking of rubber composition X is preferably more than the amount of organic peroxide P added, p.
[0025] From the viewpoint of obtaining properties applicable when the inner circumferential surface of the seal 10 is used as a sliding surface, the amount of sulfur R added r in the uncrosslinked rubber composition before crosslinking of the rubber composition X is preferably 0.1 parts by mass or more and 1 part by mass or less, more preferably 0.2 parts by mass or more and 0.6 parts by mass or less, relative to 100 parts by mass of rubber component X.
[0026] From the viewpoint of obtaining properties suitable for use as a sliding surface when the inner peripheral surface of the seal 10 is used, the ratio (r / p) of the amount of sulfur R added r in the uncrosslinked rubber composition before crosslinking of rubber composition X to the amount of organic peroxide P added p is preferably 0.03 or more and 0.3 or less, more preferably 0.1 or more and 0.5 or less, and even more preferably 0.15 or more and 0.2 or less. From the viewpoint of obtaining properties suitable for use as a sliding surface when the inner peripheral surface of the seal 10 is used, the ratio (r / q) of the amount of sulfur R added r in the uncrosslinked rubber composition before crosslinking of rubber composition X to the amount of cocrosslinking agent Q added q is preferably 0.04 or more and 0.2 or less, more preferably 0.1 or more and 0.15 or less.
[0027] In addition, rubber composition X may also contain processing aids, anti-aging agents, plasticizers, vulcanization accelerators, vulcanization accelerators, etc.
[0028] The hardness Hs of the rubber composition X is preferably A60 or higher and A95 or lower. This hardness Hs is measured using a type A hardness tester based on JIS K6253-3:2012.
[0029] The tensile strength Tb of rubber composition X is preferably 10 MPa or more. The elongation Eb of rubber composition X is preferably 200% or more. The tensile stress S100 of rubber composition X at 100% elongation is preferably 1 MPa or more and 10 MPa or less. The above-mentioned tensile strength Tb, elongation Eb, and tensile stress S100 at 100% elongation are measured based on JIS K6251:2017.
[0030] The compression set CS of the rubber composition X is preferably 20% to 40%, more preferably 25% to 35%. This compression set CS is measured based on JIS K6262:2013 at a test temperature of 120°C and a test duration of 72 hours.
[0031] The tear strength TS of rubber composition X is preferably 50 N / mm or higher. This tear strength TS is measured based on JIS K6252-1:2015.
[0032] Next, the manufacturing method of the seal 10 according to the embodiment will be described.
[0033] First, rubber components containing HNBR are added to a rubber mixing mill such as an internal mixer and then plasticized. Various rubber additives, including fatty acid amide A, carbon black B, organic peroxide P, co-crosslinking agent Q, and sulfur R, are added and mixed to prepare an uncrosslinked rubber composition.
[0034] Next, a predetermined amount of the prepared uncrosslinked rubber composition is filled into a cavity with the shape of a seal 10 formed in a mold. The mold is then closed, and the rubber component of the uncrosslinked rubber composition is initially crosslinked by stamping to obtain a primary crosslinked product. In the above-mentioned stamping, the product is subjected to heating at a predetermined temperature (e.g., 165°C to 175°C) for a predetermined time (e.g., 5 to 15 minutes) and pressurization at a predetermined pressure (e.g., 10 MPa to 20 MPa).
[0035] Then, after the primary crosslinked material is demolded from the mold, it is placed in an oven for annealing to allow the rubber components to crosslink again, thereby obtaining the seal 10 according to the embodiment. In the annealing process, the material is heated at a temperature lower than that of the primary crosslinking (e.g., 140°C to 160°C) and the heating time is longer than that of the primary crosslinking (e.g., 3 to 5 hours).
[0036] [Example]
[0037] (Uncrosslinked rubber composition)
[0038] Uncrosslinked rubber compositions of Example 1 and Comparative Examples 1 to 4 were prepared. Their respective compositions are also shown in Table 1.
[0039] <Example 1>
[0040] HNBR (acrylonitrile content: 36.2% by mass, iodine value: 11 mg / 100 mg) rubber component was formed. 100 parts by mass of this rubber component were mixed with 4 parts by mass of erucamide as a fatty acid amide, 55 parts by mass of FEF (average particle size: 43 nm) as carbon black, 5.5 parts by mass of processing aid, 3 parts by mass of anti-aging agent, 5 parts by mass of plasticizer, 5 parts by mass of vulcanization accelerator, 2.4 parts by mass of 1,3-di(tert-butylperoxy)diisopropylbenzene as an organic peroxide, 3 parts by mass of N,N'-m-phenylenebismaleimide as a co-crosslinking agent, and 0.4 parts by mass of sulfur to obtain an uncrosslinked rubber composition. This uncrosslinked rubber composition is designated as Example 1.
[0041] <Comparative Example 1>
[0042] Except that no erucamide, which is a fatty acid amide, was added, and the amount of processing aid added relative to 100 parts by weight of rubber component was 1.5 parts by weight, an uncrosslinked rubber composition was prepared in the same manner as in Example 1. The above-mentioned uncrosslinked rubber composition is designated as Comparative Example 1.
[0043] <Comparative Example 2>
[0044] Except for adding SRF (average particle size: 66 nm) as carbon black to replace FEF as carbon black, an uncrosslinked rubber composition was prepared in the same manner as in Example 1, and the above uncrosslinked rubber composition was designated as Comparative Example 2.
[0045] <Comparative Example 3>
[0046] Except for the absence of N,N'-m-phenylenebismaleimide as a co-crosslinking agent, an uncrosslinked rubber composition was prepared in the same manner as in Example 1, and the above uncrosslinked rubber composition was designated as Comparative Example 3.
[0047] <Comparative Example 4>
[0048] Except for the absence of added sulfur, an uncrosslinked rubber composition was prepared in the same manner as in Example 1, and the above uncrosslinked rubber composition was designated as Comparative Example 4.
[0049] [Table 1]
[0050]
[0051]
[0052] (Experimental methods and results)
[0053] A sample of a rubber composition was prepared using the above-described uncrosslinked rubber composition, and the following tests were conducted using this sample. The results are shown in Table 1.
[0054] <Hardness>
[0055] Prescribed specimens were prepared using the uncrosslinked rubber compositions of Example 1 and Comparative Examples 1 to 4, respectively, and the hardness Hs was measured using a type A durometer based on JIS K6253-3:2012. It should be noted that the initial crosslinking temperature was set to 170°C and the time to 10 minutes, and the secondary crosslinking temperature was set to 150°C and the time to 4 hours (hereinafter the same).
[0056] <Tension Properties>
[0057] Prescribed specimens were prepared using the uncrosslinked rubber compositions of Example 1 and Comparative Examples 1 to 4, respectively. Based on JIS K6251:2017, the tensile strength Tb, elongation Eb, and tensile stress S100 at 100% elongation were measured.
[0058] <Tear Strength>
[0059] Prescribed slit specimens were prepared using the uncrosslinked rubber compositions of Example 1 and Comparative Examples 1 to 2, respectively, and the tear strength TS was measured using Test Method B based on JIS K6252-1:2015.
[0060] <Compression permanent deformation rate>
[0061] Prescribed specimens were prepared using the uncrosslinked rubber compositions of Examples 1 and Comparative Examples 1 to 4, respectively, and the compression set CS was measured based on JIS K6262:2013 at a test temperature of 120°C and a test time of 72 hours.
[0062] <Abrasion Resistance>
[0063] Cylindrical samples with a diameter of 6.3 mm and a height of 8.0 mm were prepared using the uncrosslinked rubber compositions of Example 1 and Comparative Examples 1 to 2, respectively. Figure 2 As shown, the sample 31 is fixed with the fastener 32 and pressed onto the metal plate 33. In this state, the metal plate 33 is moved back and forth by sliding contact between the bottom surface of the sample 31 and the metal plate 33. The material of the metal plate 33 is set to SS400, the surface roughness Ry is set to 3.2, and the finishing direction is set to be orthogonal to the sliding direction. In addition, the pressing pressure of the sample 31 against the metal plate 33 is set to 0.1 MPa, the number of reciprocating motions of the metal plate 33 is set to 60 times / min, the reciprocating stroke of the metal plate 33 is set to 10 mm, and the number of reciprocating motions of the metal plate 33 is set to 100,000 times. Then, the wear amount (mm) is calculated by dividing the decrease in mass of the sample 31 before and after the test by the specific gravity of the sample 31 and then by the bottom surface area.
Claims
1. A seal formed of a rubber composition and in a ring shape, characterized in that: The rubber composition contains a rubber component mainly composed of hydrogenated nitrile butadiene rubber, unsaturated fatty acid amides, and carbon black with an average particle size of 40 nm to 45 nm. The rubber component is crosslinked using organic peroxides, maleimide co-crosslinking agents, and sulfur. Relative to 100 parts by weight of the rubber component, the content of the unsaturated fatty acid amide in the rubber composition is more than 2 parts by weight and less than 6 parts by weight. Relative to 100 parts by weight of the rubber component, the carbon black content in the rubber composition is 50 parts by weight or more and 58 parts by weight or less. The amount of the organic peroxide added to the uncrosslinked rubber composition before crosslinking is more than 2 parts by mass and less than 3 parts by mass relative to 100 parts by mass of the rubber component. The amount of the maleimide co-crosslinking agent added to the uncrosslinked rubber composition before crosslinking is more than 1 part by weight and less than 5 parts by weight, relative to 100 parts by weight of the rubber component. The amount of sulfur added to the uncrosslinked rubber composition before crosslinking is more than 0.2 parts by mass and less than 0.6 parts by mass relative to 100 parts by mass of the rubber component.
2. The seal according to claim 1, characterized in that: The amount of acrylonitrile bound to the hydrogenated nitrile rubber is more than 18% by mass and less than 52% by mass.
3. The seal according to claim 1, characterized in that: The hydrogenated nitrile rubber has an iodine value of 8 mg / 100 mg or more and 28 mg / 100 mg or less.
4. The seal according to claim 1, characterized in that: The carbon black contains FEF.
5. The seal according to claim 1, characterized in that: In the rubber composition, the ratio of the carbon black content to the unsaturated fatty acid amide content is 5 to 20.
6. The seal according to claim 1, characterized in that: In the uncrosslinked rubber composition before crosslinking of the rubber composition, the ratio of the amount of maleimide cocrosslinking agent added to the amount of organic peroxide added is 0.8 to 3.
7. The seal according to claim 1, characterized in that: In the uncrosslinked rubber composition before crosslinking of the rubber composition, the amount of maleimide cocrosslinking agent added is greater than the amount of organic peroxide added.
8. The seal according to claim 1, characterized in that: In the uncrosslinked rubber composition before crosslinking of the rubber composition, the ratio of the amount of sulfur added to the amount of organic peroxide added is more than 0.03 and less than 0.
3.
9. The seal according to claim 1, characterized in that: In the uncrosslinked rubber composition before crosslinking of the rubber composition, the ratio of the amount of sulfur added to the amount of maleimide cocrosslinking agent added is 0.04 to 0.2.
Citation Information
Patent Citations
Highly saturated nitrile rubber composition for sheet and rubber crosslinked product