Laminated glass
By arranging the functional components in the laminated glass so that the distance d is more than 15mm in the top view, and using the interlayer film to fill the gap, the problem that the functional components are prone to wrinkles and bubbles remaining in the curved glass is solved, and the laminated glass is realized Bubble reduction and thickness uniformity maintenance.
Patent Information
- Application Number
- CN202180026326.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-04-02
AI Technical Summary
In laminated glass, when the functional components have high rigidity and the glass substrate has a curved surface, it is difficult for the functional components to conform to the curved surface and wrinkles are likely to occur. Moreover, air bubbles are likely to remain in the gaps between the divided functional components, resulting in close contact between the functional components and the interlayer film. The resistance is reduced and the possibility of interface delamination is increased.
By arranging two functional components in the laminated glass to be separated from each other by a distance d in a top view, ensuring that the distance d is more than 15 mm, reducing the residual bubbles between the functional components, and using multiple functional components to interact with each other along the surface direction of the glass substrate. Separated configuration, using an intermediate membrane to fill the gap to reduce air bubble retention.
It significantly reduces the internal residual bubbles in the laminated glass, prevents wrinkles in functional components, maintains the uniformity of the thickness of the laminated glass, and avoids reflection image deformation.
Smart Images

Figure CN115362139B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to laminated glass. Background Art
[0002] Laminated glass including a pair of glass substrates laminated together via an interlayer film provided on the surfaces of the glass substrates is widely used, for example, as a glass member for a vehicle.
[0003] In recent years, people have begun to seal various functional components inside laminated glass to give laminated glass additional functions. For example, when a dimming film is sealed between a pair of interlayer films, the transmittance of the laminated glass can be appropriately adjusted according to the environment (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-36967 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] When a functional component is sealed inside a laminated glass, the functional component may wrinkle. In particular, when the glass substrate has a curved surface and the functional component has a higher rigidity than the interlayer film, the functional component cannot conform to the curved surface of the glass substrate and tends to wrinkle more.
[0009] Therefore, in order to suppress the occurrence of such wrinkles, it is conceivable to divide the functional components and arrange them inside the intermediate film.
[0010] However, in the configuration in which the divided multiple functional components are arranged in a mutually spaced manner along the surface direction of the glass substrate, the possibility of residual bubbles in the gaps between the functional components becomes high. If the residual bubbles become significant, the adhesion between the functional component and the intermediate film will decrease, and the possibility of peeling at the interface between the functional component and the intermediate film becomes high.
[0011] The present invention has been made based on the above background, and an object of the present invention is to provide a laminated glass capable of significantly reducing internal residual bubbles.
[0012] Technical solutions adopted to solve technical problems
[0013] The present invention provides a laminated glass, which is formed by laminating a first glass substrate and a second glass substrate.
[0014] a first intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the first glass substrate;
[0015] a second intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the second glass substrate,
[0016] first and second functional components disposed between the first intermediate film and the second intermediate film and in contact with the first intermediate film and the second intermediate film,
[0017] The first and second functional components have higher rigidity than the first and second intermediate films,
[0018] The first and second functional components are arranged so as to be spaced apart from each other by a distance d when the laminated glass is viewed from above.
[0019] The distance d is greater than 15 mm.
[0020] Effects of the Invention
[0021] The invention provides a laminated glass capable of significantly reducing internal residual bubbles. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 FIG. 1 is a schematic top view of a laminated glass according to an embodiment of the present invention.
[0023] Figure 2 Shown Figure 1 FIG. 1 is a schematic perspective view of a laminated glass according to an embodiment of the present invention.
[0024] Figure 3 Shown Figure 1 Schematic cross-sectional view of the I-I line section.
[0025] Figure 4 A schematic cross-sectional view showing a configuration example of a light-adjusting film enclosed in a laminated glass according to an embodiment of the present invention.
[0026] Figure 5 FIG. 1 is a schematic flow chart of a method for manufacturing laminated glass according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] Hereinafter, one embodiment of the present invention will be described.
[0028] As mentioned above, when a single functional component is enclosed between the interlayer films of laminated glass, wrinkles may occur in the functional component. In particular, when the glass substrate has a curved surface and the functional component has a higher rigidity than the interlayer film, it becomes difficult for the functional component to conform to the curved surface of the glass substrate, and wrinkles become more prominent.
[0029] In this regard, one embodiment of the present invention provides a laminated glass.
[0030] The laminated glass is formed by laminating a first glass substrate and a second glass substrate.
[0031] a first intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the first glass substrate;
[0032] a second intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the second glass substrate,
[0033] first and second functional components disposed between the first intermediate film and the second intermediate film and in contact with the first intermediate film and the second intermediate film,
[0034] The first and second functional components have higher rigidity than the first and second intermediate films,
[0035] The first and second functional components are arranged so as to be spaced apart from each other by a distance d when the laminated glass is viewed from above.
[0036] The distance d is greater than 15 mm.
[0037] In one embodiment of the present invention, a plurality of functional components are arranged between the first intermediate film and the second intermediate film in a mutually spaced manner along the surface direction of the first or second glass substrate. Compared with the case where a single "large" functional component is enclosed between the intermediate films, such an arrangement of the functional components can significantly suppress the generation of wrinkles that may be generated at the functional components.
[0038] In the present application, the “plane direction” refers to the extending direction of the surface of the first glass substrate on which the first intermediate film is provided or the surface of the second glass substrate on which the second intermediate film is provided.
[0039] In addition, the term "viewed from above" means observing the specified area from the normal direction of the specified area. Unless otherwise specified, "viewed from above" simply means observing the laminated glass from the normal direction of the laminated glass. The planar shape means the shape of the specified area when it is observed from the normal direction of the specified area.
[0040] When the divided functional members are simply arranged to be spaced apart from each other along the surface direction of the first or second glass substrate, bubbles are more likely to remain in the regions between the functional members (hereinafter referred to as “gaps”).
[0041] However, in one embodiment of the present invention, the two functional members are spaced apart from each other so that the distance d therebetween is 15 mm or more when the laminated glass is viewed from above.
[0042] In this case, during the manufacturing process of the first laminated glass 100 , bubbles are less likely to remain in the gap between the two functional members.
[0043] As a result, one embodiment of the present invention can provide a laminated glass with significantly reduced internal residual bubbles.
[0044] Here, the distance d mentioned above is defined as the minimum straight line length of the gap between the two functional members when the laminated glass is viewed from above when the laminated glass is in a flat shape.
[0045] In the case of a laminated glass having a curved surface, the distance d is not the minimum straight length of the gap between the two functional components, but is defined as the minimum length of the curved line between the two functional components. In this case, the size of the distance d slightly varies between the first glass substrate side and the second glass substrate side of the laminated glass. Therefore, in the present application, in the case of a laminated glass having a curved surface, the value obtained when measuring the outer convex surface is defined as the distance d.
[0046] In the laminated glass of one embodiment of the present invention, the distance d is preferably 20 mm or more. In this case, the bubbles remaining inside can be further reduced. The distance d is more preferably 30 mm or more, further preferably 40 mm or more, and particularly preferably 60 mm or more.
[0047] On the other hand, the distance d is preferably 110 mm or less.
[0048] If the distance d is too large, the region without the functional component along the surface direction of the first glass substrate or the second glass substrate becomes wider, and the thickness uniformity of the first or second intermediate film and the thickness uniformity of the laminated glass are likely to decrease. Moreover, as a result, the image reflected by the laminated glass may be deformed.
[0049] By setting the distance d to be 110 mm or less, it is possible to suppress a decrease in thickness uniformity of the laminated glass, thereby suppressing the problem of deformation of the reflected image.
[0050] The distance d is more preferably 100 mm or less, further preferably 80 mm or less, and particularly preferably 60 mm or less.
[0051] (Laminated glass according to one embodiment of the present invention)
[0052] Next, refer to Figure 1 to Figure 3 The laminated glass according to one embodiment of the present invention will be described in more detail.
[0053] Figure 1 FIG. 1 is a schematic top view of a laminated glass according to an embodiment of the present invention. Figure 2 Shown Figure 1 FIG. 1 is a schematic perspective view of a laminated glass according to an embodiment of the present invention. Figure 3 Shown Figure 1Schematic diagram of the I-line-I line cross section.
[0054] like Figure 1 to Figure 3 As shown, a laminated glass (hereinafter referred to as "first laminated glass") 100 according to one embodiment of the present invention includes a first glass substrate 110, a first intermediate film 130, a second intermediate film 136, and a second glass substrate 120. Figure 3 As shown, the first laminated glass 100 has a first side 102 and a second side 104 .
[0055] like Figure 2 and Figure 3 As shown, the first laminated glass 100 has a curved surface shape. The curved surface shape includes a so-called "single curved" shape in which the laminated glass has a curvature in one direction and a so-called "multi-curved" shape in which the laminated glass has curvature in two orthogonal directions. However, this is only an example, and the first laminated glass 100 may also be a flat shape.
[0056] The first glass substrate 110 has a first surface 112 and a second surface 114 facing each other, and the first intermediate film 130 is arranged on the first surface 112 side of the first glass substrate 110. Similarly, the second glass substrate 120 has a first surface 122 and a second surface 124 facing each other, and the second intermediate film 136 is arranged on the first surface 122 side of the second glass substrate 120. In addition, in the first glass substrate 110, the surface in contact with the first intermediate film 130 is referred to as the first surface B, and the surface not in contact with the first intermediate film 130 is referred to as the second surface B. In addition, in the second glass substrate 120, the surface in contact with the second intermediate film 136 is referred to as the first surface A, and the surface not in contact with the second intermediate film 136 is referred to as the second surface A.
[0057] The first glass substrate 110 and the second glass substrate 120, and the first intermediate film 130 and the second intermediate film 136 are stacked to face each other. The second surface 114 of the first glass substrate 110 corresponds to the first side 102 of the first laminated glass 100, and the second surface 124 of the second glass substrate 120 corresponds to the second side 104 of the first laminated glass 100.
[0058] In one embodiment of the present invention, the laminated glass has Figure 2 and Figure 3 In the case of the convex shape shown in FIG. 1 , the first side 102 located inside the convex surface is referred to as the “inside (of the laminated glass)”, and the second side 104 located outside the convex surface is referred to as the “outside (of the laminated glass)”. Therefore, the first glass substrate 110 is arranged inside the first laminated glass 100, and the second glass substrate 120 is arranged outside the first laminated glass 100.
[0059] On the other hand, when the laminated glass according to one embodiment of the present invention is flat, either the first side 102 or the second side 104 may be referred to as the “inside (of the laminated glass)” and the other may be referred to as the “outside (of the laminated glass)”.
[0060] Furthermore, the first laminated glass 100 includes a shielding layer 180 disposed in a frame shape along the peripheral edge of the second surface 114 on the first glass substrate 110 .
[0061] The first laminated glass 100 further includes a first functional component 150A and a second functional component 150B sealed between the first intermediate film 130 and the second intermediate film 136. The first functional component 150A and the second functional component 150B are arranged along the surface direction of the first laminated glass 100. Moreover, the first functional component 150A and the second functional component 150B are arranged in a manner spaced apart from each other in the surface direction. In other words, there is a region (hereinafter referred to as a "gap") 140 without a functional component between the first functional component 150A and the second functional component 150B.
[0062] Furthermore, when three or more functional components are arranged in the plane direction of the first laminated glass 100 , it is preferred that a gap 140 exists between any two closest functional components among the three or more functional components.
[0063] As described above, the “plane direction” refers to the direction in which the first surface 112 of the first glass substrate 110 or the first surface 122 of the second glass substrate 120 in the first laminated glass 100 extends.
[0064] The first functional component 150A and the second functional component 150B are arranged to be spaced apart from each other so that a distance d therebetween becomes 15 mm or more.
[0065] In the case of the first laminated glass 100 having a curved surface, as described above, the distance d is not the minimum straight-line distance of the gap 140 between the first functional component 150A and the second functional component 150B, but is defined as the minimum length of the curved line therebetween (see Figure 2 and Figure 3 ).
[0066] In the first laminated glass 100 , the two functional components 150A and 150B are arranged to be spaced apart from each other. Therefore, the generation of wrinkles that may be generated in the two functional components 150A and 150B can be significantly suppressed.
[0067] In addition, in the first laminated glass 100 , the two functional components 150A and 150B are spaced apart from each other so that the distance d therebetween becomes 15 mm or more. Therefore, in the first laminated glass 100 , the bubbles remaining inside can be significantly reduced.
[0068] (Each component)
[0069] Next, each component included in the laminated glass according to one embodiment of the present invention will be described in more detail. Here, the first laminated glass 100 described above will be used as an example to describe its components. Therefore, when representing each component, the term "" is used. Figure 1 to Figure 3 Reference symbols used.
[0070] (First Glass Substrate 110 and Second Glass Substrate 120)
[0071] The composition of the first glass substrate 110 is not particularly limited. The first glass substrate 110 may be, for example, inorganic glass such as soda-lime glass or aluminosilicate glass, or organic glass, but inorganic glass is preferred.
[0072] The thickness of the first glass substrate 110 is not particularly limited, and is generally within the range of 0.1 mm to 10 mm, and can be appropriately selected according to the type or location of the vehicle to which the first laminated glass 100 is applied. From the viewpoint of stone impact resistance, the thickness of the first glass substrate 110 is preferably 0.3 mm or more, more preferably 0.5 mm or more, further preferably 0.7 mm or more, particularly preferably 1.1 mm or more, and most preferably 1.6 mm or more.
[0073] Furthermore, in order to reduce the mass of the first laminated glass 100 , the thickness of the first glass substrate 110 is preferably 3 mm or less, more preferably 2.6 mm or less, and even more preferably 2.1 mm or less.
[0074] The second glass substrate 120 can be said to be the same as the first glass substrate 110. In addition, the second glass substrate 120 can have a different composition and / or a different thickness than the first glass substrate 110. For example, the first glass substrate 110 can be thinner than the second glass substrate 120.
[0075] (First Intermediate Film 130 and Second Intermediate Film 136)
[0076] The first intermediate film 130 is usually made of resin. The first intermediate film 130 can be made of, for example, a thermoplastic resin, a thermosetting resin, or a photocurable composition. As the thermoplastic resin, for example, plasticized polyvinyl acetal resins, plasticized polyvinyl chloride resins, saturated polyester resins, plasticized saturated polyester resins, polyurethane resins, plasticized polyurethane resins, ethylene-vinyl acetate copolymer resins (EVA), cycloolefin polymer resins (COP), ethylene-ethyl acrylate copolymer resins, etc. can be used. In addition, a resin composition containing a modified block copolymer hydrogenate described in Japanese Patent No. 6065221 can also be used.
[0077] Among them, plasticized polyvinyl acetal resins and EVA are preferred because they are excellent in balance of various properties such as transparency, weather resistance, strength, adhesion, impact energy absorption, moisture resistance, heat insulation and sound insulation.
[0078] The “plasticity” in the plasticized polyvinyl acetal resin means that it can be plasticized by adding a plasticizer, and the same applies to other plasticized resins.
[0079] The aforementioned thermoplastic resins may be used alone or in combination of two or more.
[0080] As polyvinyl acetal resins, polyvinyl formal resins obtained by reacting polyvinyl alcohol (PVA) with formaldehyde, polyvinyl acetal resins in a narrow sense obtained by reacting PVA with acetaldehyde, polyvinyl butyral resins (PVB) obtained by reacting PVA with n-butyraldehyde, etc. can be cited. In particular, PVB is preferred from the viewpoint of excellent balance of various properties such as transparency, weather resistance, strength, adhesion, penetration resistance, impact energy absorption, moisture resistance, heat insulation and sound insulation. Such polyvinyl acetal resins can be used alone or in combination of two or more.
[0081] The first intermediate film 130 may further contain functional particles such as an infrared absorber, an ultraviolet absorber, a colorant, and a luminescent agent.
[0082] In addition, the first intermediate film 130 may be composed of two or more layers. For example, by making the first intermediate film 130 composed of three layers and making the hardness of the central layer lower than the hardness of each layer on both sides, the sound insulation can be improved. In this case, the hardness of the layers on both sides may be the same or different.
[0083] The first interlayer film 130 has a thickness of, for example, 0.3 mm or more at the thinnest portion and 3 mm or less at the thickest portion. By setting the thickness to 0.3 mm or more, impact resistance can be improved. In addition, by setting the thickness to 3 mm or less, the mass of the first laminated glass 100 can be suppressed.
[0084] The second intermediate film 136 can also be said to be the same as the first intermediate film 130 . In addition, the second intermediate film 136 may be made of a material different from that of the first intermediate film 130 and / or may have a thickness different from that of the first intermediate film 130 .
[0085] In addition, in the gap 140, the first intermediate film 130 may be directly in contact with the second intermediate film 136. In this case, the height level of the contact between the two is not particularly limited. Figure 3As shown, in the gap 140, the second intermediate film 136 may be in contact with the first intermediate film 130 at the surface of the first side 102 in the surface of the first functional component 150A and the second functional component 150B. Alternatively, the second intermediate film 136 may be in contact with the first intermediate film 130 at the surface of the second side 104 in the surface of the first functional component 150A and the second functional component 150B. Alternatively, the second intermediate film 136 may be in contact with the first intermediate film 130 at any position between the surface of the first side 102 and the surface of the second side 104 in the surface of the first functional component 150A and the second functional component 150B.
[0086] The first laminated glass 100 may further include a third interlayer film (not shown) at the peripheral portion between the first interlayer film 130 and the second interlayer film 136. The material and thickness of the third interlayer film are the same as those described for the first interlayer film 130.
[0087] (First Functional Component 150A and Second Functional Component 150B)
[0088] The first functional component 150A and the second functional component 150B (hereinafter collectively referred to as "functional component 150") enclosed between the first intermediate film 130 and the second intermediate film 136 have a thickness in the range of 50 μm to 500 μm, for example. The functional component 150 may have a thickness of 100 μm to 250 μm. In addition, when the first laminated glass 100 has three or more functional components, all of the three or more functional components are collectively referred to as "functional component 150".
[0089] The functional member 150 may be composed of a single layer or a plurality of layers.
[0090] The functional component 150 has higher rigidity than the first intermediate film 130 and the second intermediate film 136. Rigidity can be represented by tensile elastic modulus, for example. The tensile elastic modulus of the functional component 150 measured at 25° C. and 1 Hz using DVA220 manufactured by IT Keisei Seiyu Co., Ltd. is preferably 1 GPa or more, for example.
[0091] In addition, when the functional member 150 is composed of a plurality of layers, the tensile elastic modulus of the functional member 150 indicates the highest tensile elastic modulus among the layers constituting the functional member 150 .
[0092] Furthermore, the functional component 150 has a maximum dimension within a range of 300 mm to 3000 mm.
[0093] Herein, " maximum dimension " refers to the longest dimension after considering the gap 140 in the functional component 150. The maximum dimension of the functional component 150 can also be said to be the maximum dimension of " functional component area " described later. For example, when the functional component 150 is a rectangular film, " maximum dimension " represents the length between 2 vertices that are most apart in the rectangle. In addition, when the functional component 150 is a circular film, " maximum dimension " represents the length after the diameter length adds the distance d. Under the situation of other forms, maximum dimension is also defined in the same way.
[0094] The type of functional component 150 is not particularly limited. For example, the functional component 150 may be a display or a dimming film. The display may be a display using a light emitting diode (LED), an organic light emitting diode (OLED), an inorganic EL, a laser, etc. The following describes an example in which the functional component 150 is a dimming film, but the present invention is not limited thereto.
[0095] Figure 4 This is a schematic cross-sectional view showing a configuration example of a light-adjusting film that can be used in a laminated glass according to an embodiment of the present invention.
[0096] like Figure 4 As shown, the dimming film 250 includes a first resin layer 252 , a first conductive layer 254 , a dimming element 256 , a second conductive layer 258 , and a second resin layer 260 in this order.
[0097] In addition, despite Figure 4 Although not shown, the light-adjusting film 250 has electrodes electrically connected to the first conductive layer 254 and the second conductive layer 258. A voltage is applied between the first conductive layer 254 and the second conductive layer 258 via the electrodes, thereby driving the light-adjusting element 256.
[0098] The first resin layer 252 is made of, for example, a transparent resin.
[0099] The first resin layer 252 may, for example, have at least one selected from polyethylene terephthalate (PET), polyethylene naphthalate, polyamide, polyether, polysulfone, polyethersulfone, polycarbonate, polyarylate, polyetherimide, polyetherether copper, polyimide, aromatic polyamide, polybutylene terephthalate, triacetyl cellulose, polyurethane and cycloolefin polymer.
[0100] In particular, the first resin layer 252 preferably includes at least one selected from polyethylene terephthalate, polycarbonate, and cycloolefin polymer, and is preferably composed of any one of them.
[0101] The thickness of the first resin layer 252 is, for example, in the range of 5 μm to 500 μm. The thickness of the first resin layer 252 is preferably in the range of 10 μm to 200 μm, and more preferably in the range of 50 μm to 150 μm.
[0102] The second resin layer 260 can be said to be the same as the first resin layer 252. In addition, the second resin layer 260 can be made of a material different from that of the first resin layer 252 and / or have a thickness different from that of the first resin layer 252.
[0103] The first conductive layer 254 may be made of, for example, a transparent conductive oxide (TCO: Transparent Conductive Oxide).
[0104] Examples of TCO include tin-doped indium oxide (ITO: Tin-doped Indium Oxide), aluminum-doped zinc oxide (AZO: Aluminum-doped Zinc Oxide), and indium-doped cadmium oxide.
[0105] Alternatively, as the first conductive layer 254 , a transparent conductive polymer such as poly(3,4-ethylenedioxythiophene: PEDOT) or poly(4,4-dioctylcyclopentadithiophene) can be used.
[0106] Alternatively, as the first conductive layer 254, a stacked film of a metal layer and a dielectric layer, silver nanowires, a silver or copper metal mesh, or the like can be used.
[0107] The first conductive layer 254 can be formed by, for example, physical vapor deposition (PVD) such as sputtering, vacuum deposition, or ion plating, or by chemical vapor deposition (CVD) or wet coating.
[0108] The thickness of the first conductive layer 254 is not particularly limited, and may be, for example, in the range of 200 nm to 2 μm.
[0109] The second conductive layer 258 can be said to be the same as the first conductive layer 254. However, the second conductive layer 258 may be made of a different material from the first conductive layer 254 and / or have a different thickness from the first conductive layer 254.
[0110] The dimming element 256 can be selected from, for example, a suspended particle device (SPD), a polymer dispersed liquid crystal (PDLC), a polymer network liquid crystal (PNLC), a guest-host effect liquid crystal, a photochromic substance, an electrochromic substance, and an electrodynamic substance.
[0111] In addition, a commercially available film can be used as the light-adjusting film 250. For example, as the light-adjusting element 256, a film using SPD (LCF-1103DHA: Hitachi Chemical Co., Ltd.) can be used.
[0112] When the light regulating film 250 is used as the functional member 150 , the light transmittance of the first laminated glass 100 can be appropriately switched according to the environment.
[0113] In addition, the above description assumes that the functional component 150 has a substantially rectangular planar shape when viewed from above. However, the planar shape of the functional component 150 is not limited to a rectangle. The functional component 150 may also have a circular, elliptical, triangular or n-gonal planar shape (n is an integer greater than 5).
[0114] In addition, the above description assumes that the first functional member 150A and the second functional member 150B each have two opposing surfaces and four side surfaces in a rectangular planar shape.
[0115] The above description also assumes that the first functional component 150A and the second functional component 150B are arranged in a manner that one side surface (referred to as "first side surface") 171A of the first functional component 150A and one side surface (hereinafter referred to as "first side surface") 171B of the second functional component 150B are opposed to each other in a substantially parallel manner (refer to Figure 3 ).
[0116] In this case, the width W between the first side surface 171A of the first functional component 150A and the first side surface 171B of the second functional component 150B is equivalent to the aforementioned distance d. Therefore, in this case, when looking down at the first laminated glass 100, the distance d can be specified in the region where the first side surface 171A of the first functional component 150A and the first side surface 171B of the second functional component 150B face each other.
[0117] However, it should be noted that this form is only an example.
[0118] For example, when both the first functional component 150A and the second functional component 150B have a circular planar shape, there is only one section that can define the distance d in the gap 140 between the two functional components 150A and 150B. The same is true when the two functional components 150 have a polygonal planar shape and are arranged in a manner that the vertices face each other.
[0119] Alternatively, when the functional component 150 includes more than three functional components, for example, when the functional component 150 is arranged in the form of four rectangular functional components, two in the vertical direction and two in the horizontal direction, there is only one section that can define the distance d. In addition, the distance d can be defined for each of the two closest functional components.
[0120] However, in such a case, as long as the distance d≥15mm is satisfied, the residual bubbles described above can obviously be brought into play. In addition, when the functional component 150 includes more than 3 functional components and the distance d can be respectively specified for the two closest functional components, as long as at least one distance d satisfies the distance d≥15mm, the residual bubbles described above can be brought into play. However, it is preferred that any distance d satisfies the distance d≥15mm.
[0121] (Shielding layer 180)
[0122] The shielding layer 180 may be an opaque layer, as long as it can shield visible light to a degree that can conceal at least the portion to be shielded. For example, the shielding layer 180 may be made of organic ink or colored ceramics. The shielding layer 180 may be any color, but preferably a dark color such as black, brown, gray, navy blue, and more preferably black.
[0123] The thickness of the shielding layer 180 is not particularly limited, and may be, for example, in the range of 1 μm to 30 μm, preferably 5 μm to 20 μm.
[0124] In addition, Figure 1 to Figure 3 In the example shown, the shielding layer 180 is provided on the first side 102 of the first laminated glass 100. Specifically, it is provided on the second surface 114 of the first glass substrate 110. However, this is only an example, and the shielding layer 180 may also be provided on the first surface 122 of the second glass substrate 120. Alternatively, the shielding layer 180 may be provided on both the second surface 114 of the first glass substrate 110 and the first surface 122 of the second glass substrate 120.
[0125] When the first side 102 of the first laminated glass 100 is used indoors (inside the vehicle) and the second side 104 is used outdoors (outside the vehicle), by providing a shielding layer 180 on the first surface 122 and / or the second surface 114, degradation of the urethane resin used when bonding the first laminated glass 100 to the vehicle due to ultraviolet rays, etc. can be suppressed.
[0126] Furthermore, by providing the shielding layer 180 on the second surface 114 and / or the first surface 122 , various wirings and the like provided on the peripheral portion of the first laminated glass 100 can be less easily recognized from the outside.
[0127] In addition, when the functional component 150 has a rectangular planar shape, at least one of the functional components 150 may be configured so that at least one side is covered by the shielding layer 180 when viewed from above. This makes it difficult to identify the boundary of the functional component 150. For example, in the aforementioned Figure 1 In the illustrated example, in a plan view, all sides of the first functional component 150A except for one long side (the side corresponding to the first side surface 171A) are covered by the shielding layer 180. The same is true for the second functional component 150B.
[0128] (First laminated glass 100)
[0129] The first laminated glass 100 having the above-mentioned characteristics may be suitably used as a glass member for a vehicle, for example, a front window glass, a rear window glass, other built-in window glass, a side window glass, or a sunroof glass.
[0130] When the first laminated glass 100 is applied to a glass member for a vehicle, the first laminated glass 100 may be applied so that the first side 102 is on the vehicle interior side and the second side 104 is on the vehicle exterior side.
[0131] In addition, as described above, the first laminated glass 100 may be flat or curved.
[0132] When the first laminated glass 100 is a curved surface, the section including the normal line at the center of gravity of the second surface 124 of the second glass substrate 120, in which the curvature radius of the second surface 124 is the smallest, is referred to as a longitudinal section. In addition, when the longitudinal section is viewed from the normal line direction, the direction in which the longitudinal section extends is referred to as a first direction, and the direction orthogonal to the first direction is referred to as a second direction.
[0133] For example, Figure 1 In the embodiment, the first direction may be the X direction, and the second direction may be the Y direction. In addition, the first direction and the second direction may be defined even when the first laminated glass 100 is single-bend.
[0134] In addition, the first functional component 150A, the second functional component 150B, and the gap 140 therebetween when looking down at the first laminated glass 100 are collectively referred to as a functional component region. When the first laminated glass 100 includes three or more functional components, the three or more functional components and the respective gaps 140 when looking down at the first laminated glass 100 are collectively referred to as a functional component region.
[0135] Furthermore, when the first laminated glass 100 is viewed in plan, a portion including the first functional member 150A is also referred to as a first functional member region, and a portion including the second functional member 150B is also referred to as a second functional member region.
[0136] For example, Figure 1 In FIG. 1 , the functional component region is a region surrounded by the sides (dashed lines) constituting the peripheries of the first functional component 150A and the second functional component 150B when they extend in their respective directions.
[0137] The present inventors have found that in the first laminated glass 100 , when the radius of curvature of the second glass substrate 120 and the size of the functional component region satisfy a specific relationship, that is, when the following equation (1) is satisfied, wrinkles in the functional component 150 can be significantly prevented.
[0138]
Mathematical formula 1
[0139]
[0140] Here, in formula (1), Rx is the average value (unit: mm) of the radius of curvature of the second surface 124 measured every 50 mm along the first direction in the functional component region of the second glass substrate 120. Ry is the average value (unit: mm) of the radius of curvature of the second surface 124 measured every 50 mm along the second direction in the functional component region of the second glass substrate 120.
[0141] The radius of curvature can be measured, for example, by evaluating the shape of three points using a micrometer or the like. The interval between the three points can be arbitrarily selected to be a predetermined value between 10 mm and 150 mm. That is, for example, the radius of curvature can be measured in such a way that the central points of the three points spaced 100 mm apart are spaced 50 mm apart from each other.
[0142] In formula (1), Lx is the maximum length of the functional component region along the plane direction in the first direction (unit: mm), and Ly is the maximum length of the functional component region along the plane direction in the second direction (unit: mm).
[0143] When the above formula (1) is satisfied, wrinkles of the functional component 150 can be more effectively suppressed. The value of formula (1) is preferably less than 2100, and more preferably less than 1750. In these cases, wrinkles of the functional component 150 can be more effectively suppressed. Formula (1) can approximately reflect the mutual influence between the curvature in the first direction and the curvature in the second direction of the first laminated glass 100 having a three-dimensional curved surface shape.
[0144] In addition, the inventors have found that, in the first laminated glass 100, when the shape of the first glass substrate 110 and the size of the first functional component 150A in the sealing area of the first functional component 150A form a specific relationship, that is, when the first functional component area of the first glass substrate 110 satisfies the following formula (2), wrinkles of the first functional component 150A can be significantly prevented.
[0145]
Mathematical formula 2
[0146]
[0147] Here, in formula (2), Dx is the maximum bending depth of the first glass substrate 110 in the first direction in the first functional component region (unit: mm), and Dy is the maximum bending depth of the first glass substrate 110 in the second direction in the first functional component region (unit: mm). Dx can be obtained, for example, as follows.
[0148] In the first functional component region of the second surface 114 of the first glass substrate 110, draw an imaginary straight line S that is orthogonal to a pair of sides extending in the second direction of the first functional component region and extending in the first direction. Then draw a vertical line from the imaginary straight line S to the first glass substrate 110 (second surface 114). The maximum length of the vertical line is recorded as Dx. In addition, the length of the vertical line varies depending on the drawing method of the imaginary straight line S, and the maximum length Dx refers to the longest of these vertical lines of different lengths. As for Dy, in the first functional component region of the second surface 114 of the first glass substrate 110, draw an imaginary straight line S that is orthogonal to a pair of sides extending in the first direction of the first functional component region and extending in the second direction, and then obtain it in the same way as Dx.
[0149] In addition, in formula (2), Lx0 is the maximum length (unit: mm) of the first functional component region in the first direction along the second surface 114, and Ly0 is the maximum length (unit: mm) of the first functional component region in the second direction along the second surface 114. Lx0 and Ly0 can be obtained by measuring the second surface 124 in the first direction and the second direction in the first functional component region of the second glass substrate 120, respectively.
[0150] When the first functional component 150A satisfies the above formula (2), wrinkles of the first functional component 150A can be more effectively suppressed. The value on the left side of formula (2) is more preferably 4.5 or less, more preferably 4.0 or less, and further preferably 3.5 or less. Formula (2) can approximately reflect the mutual influence between the curvature in the first direction and the curvature in the second direction of the first laminated glass 100 having a three-dimensional curved surface shape.
[0151] Similarly, the above-mentioned (2) formula can also be applied to the second functional component 150B. That is, when the maximum bending depth of the first glass substrate 110 and the size of the second functional component 150B are established with the (2) formula, the wrinkles of the second functional component 150B can be significantly prevented. In addition, when the above-mentioned (2) formula is applicable to the second functional component 150B, the first functional component 150A is replaced with the second functional component 150B. The above-mentioned (2) formula is preferably established to at least one of the first functional component 150A and the second functional component 150B, and more preferably established to both sides.
[0152] When the first laminated glass 100 includes three or more functional components, any two functional components can be used as the first functional component 150A and the second functional component 150B to apply the above formula (2). However, it is most preferred that any one functional component be used as the first functional component 150A or the second functional component 150B to satisfy the above formula (2).
[0153] (Method for Manufacturing Laminated Glass According to One Embodiment of the Present Invention)
[0154] Next, refer to Figure 5 An example of a method for producing laminated glass according to an embodiment of the present invention will be described.
[0155] Figure 5 FIG. 1 is a schematic flow chart of a method for manufacturing laminated glass according to an embodiment of the present invention.
[0156] like Figure 5 As shown, a method for manufacturing laminated glass according to one embodiment of the present invention comprises:
[0157] (1) a step of preparing a first glass substrate and a second glass substrate (step S110),
[0158] (2) a step of sequentially stacking the first glass substrate, the first intermediate film, the functional member, the second intermediate film, and the second glass substrate to form an assembly (step S120), and (3) a step of heat-treating the assembly to bond it (step S130).
[0159] Each step is described below. For the sake of clarity, the first laminated glass 100 is used as an example to describe its manufacturing method. Figure 1 to Figure 3 Reference symbols are recorded.
[0160] (Process S110)
[0161] First, the first glass substrate 110 and the second glass substrate 120 are prepared.
[0162] If necessary, the shielding layer 180 may be provided in a frame-like manner along the peripheral portion of one surface (e.g., the second surface 114) of the first glass substrate 110. The shielding layer 180 may be formed, for example, by providing a paste for the shielding layer 180 on the peripheral portion of the second surface 114 of the first glass substrate 110 and then firing the paste. As a method for providing the paste, any conventional method such as a screen printing method may be used.
[0163] Furthermore, if necessary, another shielding layer may be provided in a frame shape along the peripheral edge of one surface (eg, the first surface 122 ) of the second glass substrate 120 .
[0164] If necessary, the first glass substrate 110 and / or the second glass substrate 120 may be bent. For example, only the second glass substrate 120 may be bent. In this case, the first glass substrate 110 and the second glass substrate 120 in a flat state may be made into a laminated glass.
[0165] The bending process may be a gravity forming process or a press forming process. In addition, the bending process may be performed while the first glass substrate 110 and the second glass substrate 120 are heated. The two glass substrates 110 and 120 may be bent separately or simultaneously. The heating temperature varies depending on the type of glass substrate, for example, within a range of 550° C. to 700° C.
[0166] In addition, when a paste for the shielding layer 180 is provided on the first glass substrate 110, the paste may be fired during the bending process to form the shielding layer 180. Alternatively, pre-firing may be performed before the bending process.
[0167] (Process S120)
[0168] Next, a first resin sheet for the first intermediate film 130 is provided on the first surface 112 of the first glass substrate 110 .
[0169] Next, two or more functional components 150 are provided on the first resin sheet.
[0170] The functional components 150A and 150B may be, for example, a dimming film 250 .
[0171] The functional members 150 are arranged to be spaced apart from each other along the plane direction of the first surface 112 of the first glass substrate 110. The two functional members 150 are arranged so that the distance d between the two functional members 150 is 15 mm or more.
[0172] Next, the second resin sheet for the second intermediate film 136 is provided on the functional member 150. The second resin sheet can be made of the same resin as the first resin sheet.
[0173] Furthermore, if necessary, a third resin sheet for a third intermediate film may be provided at the periphery of the first surface 112 of the first glass substrate 110. Furthermore, the third resin sheet may be provided before providing each functional component 150. The installation position of each functional component 150 becomes easy to align.
[0174] Next, the second glass substrate 120 is placed on the second resin sheet to form an assembly.
[0175] (Process S130)
[0176] Next, the assembly is placed in a container. The pressure in the container is reduced to, for example, 730 mmHg or less. Thereafter, the container is heated to a temperature in the range of 70 to 110° C. in a sealed state.
[0177] Instead of placing the assembly in a container for decompression, the assembly may be pressurized by clamping the assembly with a pair of clamping rollers, or the periphery of the assembly may be covered with a rubber chamber for decompression. The assembly may be heated within a range of 70 to 110°C.
[0178] The first resin sheet is heated to soften and form the first intermediate film 130. The second resin sheet is softened and form the second intermediate film 136. Therefore, the first glass substrate 110 and the functional component 150 are bonded via the first intermediate film 130, and the second glass substrate 120 and the functional component 150 are bonded via the second intermediate film 136.
[0179] In addition, the gap 140 between the first functional member 150A and the second functional member 150B is filled with the components of the first resin sheet and / or the components of the second resin sheet which have intruded into the gap 140 due to softening.
[0180] Therefore, after the heat treatment, the gap 140 is filled with the first intermediate film 130 and / or the second intermediate film 136. In addition, in the gap 140, the first intermediate film 130 and the second intermediate film 136 are directly bonded.
[0181] The aforementioned Figure 1 to Figure 3 The first laminated glass 100 is shown.
[0182] The above description is merely an example, and the laminated glass according to one embodiment of the present invention may be produced by other methods.
[0183] Example
[0184] In the following description, Examples 1 to 10 are Examples, and Examples 11 to 14 are Comparative Examples.
[0185] (Example 1)
[0186] Laminated glass was produced by the following method. The laminated glass is composed of a first glass substrate, a first intermediate film, a functional component, a second intermediate film, and a second glass substrate in this order. The laminated glass is flat in shape. No shielding layer is provided.
[0187] First, the first and second glass substrates were prepared. The dimensions of the first and second glass substrates were 300 mm in length, 300 mm in width, and 2 mm in thickness.
[0188] Next, a first resin sheet for a first intermediate film is provided on the first glass substrate. The first resin sheet is arranged so as to almost overlap with the first surface of the first glass substrate when viewed from above. The first resin sheet is an ethylene-vinyl acetate copolymer (EVA) sheet (MERSON G7055: manufactured by Tosoh Nichem Co., Ltd.) having a thickness of 0.4 mm.
[0189] Next, two functional components are arranged on the first resin sheet in parallel with each other along the surface direction of the first surface of the first glass substrate. The functional components are square PET films with a length of 80 mm and a width of 80 mm. The thickness of the PET film is 100 μm. The PET film is arranged at the approximate center of the first resin sheet in a manner that is approximately parallel to the lower side of the first glass substrate.
[0190] The width W of the gap between the two PET films when viewed from above was 20 mm.
[0191] Next, a second resin sheet for a second intermediate film is placed on these PET films. The second resin sheet is made of the same material as the first resin sheet. The second resin sheet has the same size as the first resin sheet and is placed so as to overlap the first resin sheet in a plan view.
[0192] Next, the second glass substrate is placed on the second resin sheet. The second glass substrate is placed so that each side overlaps each side of the first glass substrate in a plan view. Thus, an assembly is formed.
[0193] The obtained assembly was placed in a plastic container, and the pressure in the container was reduced to 730 mmHg over 5 minutes. Thereafter, the container was sealed, and the container was heated to 100° C. and maintained for 1 hour.
[0194] In this way, a laminated glass (hereinafter referred to as "Sample 1") was produced.
[0195] (Example 2)
[0196] Laminated glass was produced by the same method as in Example 1. However, in Example 2, the width W of the gap between the two functional components was 30 mm. The other conditions were the same as in Example 1. Laminated glass (hereinafter referred to as "Sample 2") was thus produced.
[0197] (Example 3)
[0198] Laminated glass was produced by the same method as in Example 1. However, in Example 3, the width W of the gap between the two functional components was 60 mm. The other conditions were the same as in Example 1. Laminated glass (hereinafter referred to as "Sample 3") was thus produced.
[0199] (Example 4)
[0200] Laminated glass was produced by the same method as in Example 1. However, in Example 4, the width W of the gap between the two functional components was 100 mm. The other conditions were the same as in Example 1. Laminated glass (hereinafter referred to as "Sample 4") was thus produced.
[0201] (Example 5)
[0202] Laminated glass was produced by the same method as in Example 1. However, in Example 5, the width W of the gap between the two functional components was 120 mm. The other conditions were the same as in Example 1. Laminated glass (hereinafter referred to as "Sample 5") was thus produced.
[0203] (Example 6)
[0204] Laminated glass was produced by the same method as in Example 1. However, in Example 6, two PET films with a thickness of 125 μm were overlapped and used as each functional component. Therefore, the thickness of each functional component was 250 μm. Other conditions were the same as in Example 1. Laminated glass (hereinafter referred to as "Sample 6") was thus produced.
[0205] (Example 7)
[0206] Laminated glass was produced by the same method as in Example 6. However, in Example 7, the width W of the gap between the two functional components was 100 mm. The other conditions were the same as in Example 6. Laminated glass (hereinafter referred to as "Sample 7") was thus produced.
[0207] (Example 8)
[0208] Laminated glass was produced by the same method as in Example 6. However, in Example 8, the width W of the gap between the two functional members was 120 mm. Other conditions were the same as in Example 6. Laminated glass (hereinafter referred to as "Sample 8") was thus produced.
[0209] (Example 9)
[0210] Laminated glass was produced by the following method. The laminated glass is composed of a first glass substrate, a first interlayer film, a functional component, a second interlayer film, and a second glass substrate in this order. In Example 9, the laminated glass has a multi-bend shape. In addition, no shielding layer is provided.
[0211] First, prepare the first and second curved glass substrates. The dimensions of the first and second glass substrates are 300 mm in length, 300 mm in width, and 2 mm in thickness. The lengths in length and width are measured along the main surfaces of the curved first and second glass substrates. In addition, the three-dimensional shapes of the first and second glass substrates are substantially the same.
[0212] Next, the first resin sheet for the first interlayer film was placed on the first glass substrate. The first resin sheet was arranged so as to substantially overlap the first surface of the first glass substrate in a plan view. The first resin sheet was an ethylene-vinyl acetate copolymer (EVA) sheet (MERSON G7055: manufactured by Tosoh Chemicals Co., Ltd.) having a thickness of 0.4 mm.
[0213] Next, two functional components are arranged on the first resin sheet in parallel with each other along the surface direction of the first surface of the first glass substrate. The functional components are rectangular PET films with a length of 125 mm in the longitudinal direction and 280 mm in the transverse direction. The thickness of the PET film is 250 μm. Each PET film is linearly symmetrical to the first resin sheet in a manner that the lower side of the PET film is roughly parallel to the lower side of the first glass substrate. At this time, they are spaced apart so that the distance from the periphery of the first glass substrate and the second glass substrate to the two functional components (PET films) is 10 mm respectively.
[0214] The width W of the gap between the two PET films when viewed from above was 30 mm.
[0215] Next, a second resin sheet for a second intermediate film is placed on these PET films. The second resin sheet is made of the same material as the first resin sheet. The second resin sheet has the same size as the first resin sheet and is placed so as to overlap with the first resin sheet in a plan view.
[0216] Next, the second glass substrate is placed on the second resin sheet. The second glass substrate is placed so that each side overlaps each side of the first glass substrate in a plan view. Thus, an assembly is formed.
[0217] The obtained assembly was placed in a plastic container, and the pressure in the container was reduced to 730 mmHg over 5 minutes. Thereafter, the container was sealed, and the container was heated to 100° C. and maintained for 1 hour.
[0218] In this way, a laminated glass (hereinafter referred to as "Sample 9") was produced.
[0219] (Example 10)
[0220] Laminated glass was produced by the same method as in Example 9. However, in Example 10, the first and second glass substrates were prepared with curved shapes different from those in Example 9. The dimensions of the first and second glass substrates (300 mm in length, 300 mm in width, and 2 mm in thickness) and other conditions were the same as those in Example 9. Laminated glass (hereinafter referred to as "Sample 10") was thus produced.
[0221] (Example 11)
[0222] Laminated glass was produced by the same method as in Example 1. However, in Example 11, the width W of the gap between the two functional components was 10 mm. The other conditions were the same as in Example 1. Laminated glass (hereinafter referred to as "Sample 11") was thus produced.
[0223] (Example 12)
[0224] Laminated glass was produced by the same method as in Example 6. However, in Example 12, the width W of the gap between the two functional components was 10 mm. Other conditions were the same as in Example 6. Laminated glass (hereinafter referred to as "Sample 12") was thus produced.
[0225] (Example 13)
[0226] Laminated glass was produced by the same method as in Example 9. However, in Example 13, the first and second glass substrates were prepared with curved shapes different from those in Example 9. In addition, the two functional components were rectangular PET films with a length of 135 mm in the longitudinal direction, a width of 280 mm in the lateral direction, and a thickness of 250 μm, and the width W of the gap between the two PET films was 10 mm when viewed from above. The dimensions of the first and second glass substrates (300 mm in the longitudinal direction, 300 mm in the lateral direction, and a thickness of 2 mm) and other conditions were the same as those in Example 9. Thus, laminated glass (hereinafter referred to as "Sample 13") was produced.
[0227] (Example 14)
[0228] Laminated glass was produced by the same method as in Example 13. However, in Example 14, first and second glass substrates having curved shapes different from those in Example 13 were prepared. The dimensions of the first and second glass substrates (300 mm in length, 300 mm in width, and 2 mm in thickness) and other conditions were the same as those in Example 13. Laminated glass (hereinafter referred to as "Sample 14") was thus produced.
[0229] (evaluate)
[0230] The following evaluations were performed using each sample. In addition, for samples 9, 10, 13, and 14, predetermined dimensions were also measured.
[0231] (Amount of residual bubbles)
[0232] In each sample, the amount of bubbles present in the gap between the two functional members was visually evaluated by planar viewing from the second glass substrate side.
[0233] The total area of residual bubbles is less than 5mm 2 In the case of residual bubbles, the amount of residual bubbles is judged as "○". When the total area of the residual bubbles is 5mm 2 ~15mm 2 The residual bubble volume is judged as "△" in the case of residual bubbles.2 In the case of , the amount of residual bubbles is judged as "×".
[0234] (Deformation of reflected image)
[0235] A zebra stripe was placed on the second glass substrate side of each sample to evaluate the deformation of the image reflected from the sample. If no obvious deformation of the reflected image was observed, it was judged as "○". If obvious deformation of the reflected image was observed, it was judged as "×". In addition, the case between "○" and "×" was judged as "△".
[0236] Tables 1 and 2 summarize the results obtained for each sample.
[0237] [Table 1]
[0238]
[0239] [Table 2]
[0240]
[0241] As shown in Tables 1 and 2, many bubbles remain in the gap between the two functional members in Samples 11 to 14. In contrast, in Samples 1 to 10, bubbles remaining in the gap are significantly suppressed regardless of the thickness of the functional member.
[0242] In addition, in Samples 5 and 8, where the width of the gap between the two functional components is 120 mm, the deformation of the reflected image becomes larger than that of Samples 1 to 4 and Samples 6 to 7. This is considered to be because the width W of the gap is relatively wide in Samples 5 and 8, and thus the thickness uniformity of the laminated glass decreases.
[0243] Therefore, from the viewpoint of suppressing the deformation of the reflected image, it can be said that the width W of the gap is preferably less than 120 mm, for example, 110 mm or less.
[0244] In addition, the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2020-067824 filed on April 3, 2020 are cited herein as a disclosure of the present specification.
[0245] Explanation of symbols
[0246] 100 No.1 Laminated Glass
[0247] 102 Side 1
[0248] 104 Side 2
[0249] 110 1st glass substrate
[0250] 112 1st surface B
[0251] 114 2nd surface B
[0252] 120 Second glass substrate
[0253] 122 1st surface A
[0254] 124 2nd surface A
[0255] 130 1st interlayer film
[0256] 136 Second interlayer film
[0257] 140 Gap
[0258] 150 functional components
[0259] 150A 1st functional component
[0260] 150B Second functional component
[0261] 171A First side of the first functional component
[0262] 171B First side of the second functional component
[0263] 180 Shielding Layer
[0264] 250 dimming film
[0265] 252 1st resin layer
[0266] 254 1st conductive layer
[0267] 256 dimming elements
[0268] 258 Second conductive layer
[0269] 260 Second resin layer
Claims
1. A laminated glass, The laminated glass is formed by laminating a first glass substrate and a second glass substrate. a first intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the first glass substrate; a second intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the second glass substrate, first and second functional components disposed between the first intermediate film and the second intermediate film and in contact with the first intermediate film and the second intermediate film, The first and second functional components have higher rigidity than the first and second intermediate films, The first and second functional components are arranged so as to be spaced apart from each other by a distance d when the laminated glass is viewed from above. The distance d is above 15 mm, in, The first and second functional components are dimming films respectively, The light-adjusting film includes, in order from near to far from the first glass substrate, a first resin layer, a first conductive layer, a light-adjusting element, a second conductive layer, and a second resin layer.
2. The laminated glass according to claim 1, wherein: The distance d is greater than 20 mm.
3. The laminated glass according to claim 1 or 2, wherein: The distance d is less than 110 mm.
4. The laminated glass according to claim 3, wherein: The distance d is less than 100 mm.
5. The laminated glass according to claim 1, wherein: In a region where the first and second functional components are spaced apart from each other, the first intermediate film and the second intermediate film are in direct contact with each other.
6. The laminated glass according to claim 1, wherein: The thickness of the first and second functional members is respectively not less than 50 μm and not more than 250 μm.
7. The laminated glass according to claim 1, wherein: The first and second functional components each have a rectangular film shape, The first and second functional components are arranged such that a first side surface of the first functional component and a first side surface of the second functional component are substantially parallel to and face each other.
8. The laminated glass according to claim 1, wherein: The first and / or second functional component has a resin layer, which has at least one selected from polyethylene terephthalate, polyethylene naphthalate, polyamide, polyether, polysulfone, polyethersulfone, polycarbonate, polystyrene, cyclic polyolefin, polyarylate, polyetherimide, polyetherether copper, polyimide, aromatic polyamide, polybutylene terephthalate, triacetyl cellulose, polyurethane and cycloolefin polymer.
9. The laminated glass according to claim 1, wherein: The first and second functional members are composed of one or more layers, and the maximum value of the tensile elastic modulus of each layer is 1 GPa or more.
10. A laminated glass, The laminated glass is formed by laminating a first glass substrate and a second glass substrate. a first intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the first glass substrate; a second intermediate film disposed between the first glass substrate and the second glass substrate and in contact with the second glass substrate, first and second functional components disposed between the first intermediate film and the second intermediate film and in contact with the first intermediate film and the second intermediate film, The first and second functional components have higher rigidity than the first and second intermediate films, The first and second functional components are arranged so as to be spaced apart from each other by a distance d when the laminated glass is viewed from above. The distance d is above 15 mm, in, In the second glass substrate, the surface in contact with the second intermediate film is referred to as a first surface A, and the surface not in contact with the second intermediate film is referred to as a second surface A. In the first glass substrate, the surface in contact with the first intermediate film is referred to as a first surface B, and the surface not in contact with the first intermediate film is referred to as a second surface B. In the second glass substrate, when the laminated glass is viewed from above, a region including the first and second functional components and a gap between the first and second functional components is referred to as a functional component region, a region overlapping with the first functional component is referred to as a first functional component region, and a region overlapping with the second functional component is referred to as a second functional component region. In the second glass substrate, among the cross sections including the normal line at the center of gravity, the cross section having the smallest radius of curvature of the second surface A is referred to as a longitudinal cross section. The direction in which the longitudinal section extends when viewed from the normal direction is referred to as a first direction, and the direction perpendicular to the first direction is referred to as a second direction. The following formula (1) holds true, and the formula (2) holds true in the first functional component region and the second functional component region, respectively: in, Rx is an average value (mm) of the radius of curvature of the second surface A measured every 50 mm along the first direction in the functional component region of the second glass substrate, Ry is an average value (mm) of the radius of curvature of the second surface A measured every 50 mm along the second direction in the functional component region of the second glass substrate, Lx is the maximum length of the functional component area in the first direction in mm, Ly is the maximum length of the functional component region in the second direction in mm, Dx is the maximum bending depth (mm) of the first glass substrate in the first functional component region or the second functional component region in the first direction, Dy is the maximum bending depth (mm) of the first glass substrate in the first functional component region or the second functional component region in the second direction, Lx0 is the maximum length of the first functional component region or the second functional component region in the first direction along the second surface B in mm, Ly0 is the maximum length of the first functional component region or the second functional component region in the second direction along the second surface B in mm, Wherein, the maximum size of the functional component area is greater than 300 mm and less than 3000 mm.
11. The laminated glass according to claim 10, wherein: The distance d is greater than 20 mm.
12. The laminated glass according to claim 10 or 11, wherein: The distance d is less than 110 mm.
13. The laminated glass according to claim 12, wherein: The distance d is less than 100 mm.
14. The laminated glass according to claim 10, wherein: In a region where the first and second functional components are spaced apart from each other, the first intermediate film and the second intermediate film are in direct contact with each other.
15. The laminated glass according to claim 10, wherein: The thickness of the first and second functional members is respectively not less than 50 μm and not more than 250 μm.
16. The laminated glass according to claim 10, wherein: The first and second functional components each have a rectangular film shape, The first and second functional components are arranged such that a first side surface of the first functional component and a first side surface of the second functional component are substantially parallel to and face each other.
17. The laminated glass according to claim 10, wherein: The first and / or second functional component has a resin layer, which has at least one selected from polyethylene terephthalate, polyethylene naphthalate, polyamide, polyether, polysulfone, polyethersulfone, polycarbonate, polystyrene, cyclic polyolefin, polyarylate, polyetherimide, polyetherether copper, polyimide, aromatic polyamide, polybutylene terephthalate, triacetyl cellulose, polyurethane and cycloolefin polymer.
18. The laminated glass according to claim 10, wherein: The first and second functional members are composed of one or more layers, and the maximum value of the tensile elastic modulus of each layer is 1 GPa or more.
19. The laminated glass according to claim 10, wherein: When viewed from the second glass substrate side, the total area of bubbles present in the gap between the first and second functional members is less than 5 mm 2 .
Citation Information
Patent Citations
Cooling device of engine
JP1985065221A
Light control window material
JP2009036967A
Network system and electric device
JP2020067824A
Interlayer for laminated glass and laminated glass
JP2011088784A
Intermediate film for laminated glasses, laminated glass, and automobile
WO2019221218A1
Cited By
Component gap edge filling structure of laminated glass, laminated glass and preparation method of laminated glass
CN120840182A
Laminated glass and vehicle
CN224276539U