Water-based resin composition and coating agent
By using an aqueous resin composition of an acrylic polymer, a urethane resin and an aqueous medium, the problem of the hydrophilic treatment agent in the prior art failing under harsh conditions is solved, and the hydrophilic sustainability of the coating film is achieved.
Patent Information
- Application Number
- CN202180025619.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Existing hydrophilic treatment agents cannot fully maintain the hydrophilicity of the coating film under harsh thermal history conditions, especially after application of processing oil and cleaning.
An aqueous resin composition containing an acrylic polymer, a urethane resin and an aqueous medium is used. The acrylic polymer is composed of 2-hydroxyethyl (meth)acrylamide, unsaturated carboxylic acid or its anhydride and polyoxyalkylene. It is formed from monomer components of units and polymerizable unsaturated groups, and has a weight average molecular weight of 100,000 or more.
Even under severe thermal history conditions, good hydrophilicity can be maintained after coating with processing oil and cleaning.
Smart Images

Figure BDA0003870174490000181
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous resin composition and a coating agent. Background Art
[0002] Coating agents are used to prevent the deterioration of the surface of various substrates and to change the surface properties of substrates. Aluminum fins used in air conditioners and the like require hydrophilicity and corrosion resistance on the surface, and in particular, require that the hydrophilicity and corrosion resistance be maintained even under repeated conditions of wet and low temperature and dry and high temperature (persistent hydrophilicity).
[0003] As coating agents for achieving such surface hydrophilicity and sustained hydrophilicity, hydrophilic coating agents comprising copolymers obtained from acrylic acid, acrylic acid salts, maleic acid, maleic acid salts, itaconic acid, itaconic acid salts, acrylamide and acrylonitrile have been proposed (for example, see Patent Document 1). In addition, hydrophilic treatment agents comprising hydrophilic monomers having polymerizable double bonds and polyoxyalkylene chains, hydrophilic polymers obtained from acrylamide monomers, and crosslinking agents have been proposed (for example, see Patent Document 2).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-10764
[0007] Patent Document 2: Japanese Patent Application Publication No. 2017-20015 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, the above-mentioned hydrophilic treatment agents known in the past sometimes cannot fully satisfy the hydrophilic persistence. The present invention is made in view of the above situation, and its subject is to provide an aqueous resin composition that can exert hydrophilic persistence even under the conditions of a severe thermal history for drying the coating film and the conditions of use after coating with processing oil and washing.
[0010] Means for solving problems
[0011] The aqueous resin composition of the present invention comprises an acrylic polymer (A), a urethane resin (B) and an aqueous medium (C), wherein the acrylic polymer (A) is formed from monomer components containing at least 2-hydroxyethyl (meth)acrylamide, an unsaturated carboxylic acid or anhydride thereof, and a monomer having a polyoxyalkylene unit and a polymerizable unsaturated group, and has a weight average molecular weight of 100,000 or more.
[0012] Effects of the Invention
[0013] By using the aqueous resin composition of the present invention, it is possible to provide an aqueous resin composition that can exhibit sustained hydrophilicity even under conditions where a severe thermal history is applied for drying of a coating film or under conditions where a processing oil is applied and then used after washing. DETAILED DESCRIPTION
[0014] The aqueous resin composition of the present invention comprises an acrylic polymer (A), a urethane resin (B) and an aqueous medium (C).
[0015] The acrylic polymer (A) is formed from monomer components containing at least 2-hydroxyethyl (meth)acrylamide, an unsaturated carboxylic acid or anhydride thereof (a1), and a monomer (a2) having a polyoxyalkylene unit and a polymerizable unsaturated group, and is a copolymer of the monomer components.
[0016] 2-Hydroxyethyl(meth)acrylamide means 2-hydroxyethylacrylamide and / or 2-hydroxyethylmethacrylamide, and is preferably 2-hydroxyethylacrylamide.
[0017] The content of the 2-hydroxyethyl (meth)acrylamide in the monomer components is preferably 10% by mass or more, more preferably 20% by mass or more, further preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, further preferably 60% by mass or less.
[0018] As the above-mentioned unsaturated carboxylic acid or its anhydride (a1), one or more kinds can be used, and examples thereof include unsaturated monocarboxylic acids such as (meth) acrylic acid; (meth) acrylic acid esters of monocarboxylic acids such as (meth) acrylic acid β-carboxyethyl ester and 2-(meth) acryloyl propionic acid; unsaturated dicarboxylic acids such as crotonic acid, itaconic acid, maleic acid, fumaric acid, phthalic acid, succinic acid; half (meth) acrylic acid esters of the above-mentioned unsaturated dicarboxylic acids; anhydrides of the above-mentioned unsaturated dicarboxylic acids; compounds obtained by adding a (meth) acryloyloxyalkyl group (preferably a (meth) acryloyloxyethyl group) to at least one of the carboxyl groups of the above-mentioned unsaturated dicarboxylic acids, etc. Among them, unsaturated monocarboxylic acids are preferred, and acrylic acid is particularly preferred.
[0019] The content of the unsaturated carboxylic acid or its anhydride (a1) in the monomer component is preferably 0.5% by mass or more and preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less.
[0020] The above-mentioned monomer (a2) having a polyoxyalkylene unit and a polymerizable unsaturated group is a monomer in which the polyoxyalkylene unit and the polymerizable unsaturated group are bonded directly or via a linking group. Examples of the above-mentioned linking group include -CO-, -O-, -NH-, a divalent hydrocarbon group (an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or a group having 20 or less carbon atoms formed by a combination of these), or a group formed by a combination of these, preferably -CO-. -OR (R is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or a group having 20 or less carbon atoms formed by a combination of these) may be bonded to the other end of the polyoxyalkylene unit (the end not bonded to the polymerizable unsaturated group), and the above R is preferably an aliphatic hydrocarbon group (preferably an alkyl group), and the number of carbon atoms of the aliphatic hydrocarbon group is preferably 1 to 5, and more preferably 1 to 2.
[0021] The polyoxyalkylene units preferably contain oxyethylene units. The content of oxyethylene units in the polyoxyalkylene units is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and the upper limit is 100% by mass.
[0022] In the polyoxyalkylene unit, the number of repetitions of the oxyalkylene unit is preferably 3 or more, more preferably 5 or more, and even more preferably 7 or more, and is preferably 20 or less, more preferably 18 or less, and even more preferably 15 or less.
[0023] The number average molecular weight of the monomer (a2) having a polyoxyalkylene unit and a polymerizable unsaturated group is preferably 200 or more, more preferably 300 or more, further preferably 400 or more, preferably 1,500 or less, more preferably 1,000 or less, further preferably 800 or less, and further preferably 600 or less.
[0024] The monomer component may contain other monomers (a3) in addition to 2-hydroxyethyl (meth)acrylamide, the unsaturated carboxylic acid or its anhydride (a1), and the monomer (a2) having an oxyalkylene unit and a polymerizable unsaturated group.
[0025] Examples of the other monomer (a3) include (meth)acrylates, acrylic monomers having a hydrophilic group (hydroxyl group, imide group, cyano group, amino group, sulfonic acid group, quaternary ammonium group, etc.), (meth)acrylamide monomers other than 2-hydroxyethyl (meth)acrylamide, and other vinyl compounds.
[0026] As the (meth)acrylate, one or more kinds can be used, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate. , isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, n-octadecyl (meth)acrylate, isooctadecyl (meth)acrylate and the like aliphatic (meth)acrylates; cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate and the like alicyclic (meth)acrylates; benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyl (meth)acrylate and the like aromatic (meth)acrylates; and the like.
[0027] As the acrylic monomer having an imide group, one or more kinds can be used, for example, (meth)acrylimide, N-hydroxymethylmaleimide, N-hydroxyethylmaleimide, N-glycidylmaleimide, N-4-chloromethylphenylmaleimide, N-acetoxyethylmaleimide, etc.
[0028] As the above-mentioned acrylic monomer having a cyano group, one or more kinds can be used, for example, acrylonitrile, cyanomethyl acrylate, 2-cyanoethyl acrylate, cyanopropyl acrylate, 1-cyanomethylethyl acrylate, 2-cyanopropyl acrylate, 1-cyanocyclopropyl acrylate, 1-cyanocycloheptyl acrylate, 1,1-dicyanoethyl acrylate, 2-cyanophenyl acrylate, 3-cyanophenyl acrylate, 4-cyanophenyl acrylate, 3-cyanobenzyl acrylate, 4-cyanobenzyl acrylate, etc.
[0029] As the acrylic monomer having an amino group, one or more kinds may be used, and examples thereof include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, N-tert-butylaminoethyl (meth)acrylate, and (meth)acryloyloxyethyltrimethylammonium chloride.
[0030] As the acrylic monomer having a quaternary ammonium group, one or more kinds may be used, and examples thereof include tetrabutylammonium (meth)acrylate and trimethylbenzylammonium (meth)acrylate.
[0031] As the acrylic monomer having a sulfonic acid group, one or more kinds may be used, and examples thereof include sodium sulfopropyl (meth)acrylate, sodium 2-sulfoethyl (meth)acrylate, and sodium 2-acrylamide-2-methylpropanesulfonate.
[0032] Examples of the (meth)acrylamide monomers other than 2-hydroxyethyl (meth)acrylamide include (meth)acrylamide; (meth)acrylonitrile; N-monosubstituted (meth)acrylamide monomers such as (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, and dimethylaminopropyl (meth)acrylamide; and N,N-disubstituted (meth)acrylamide monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloyl-4-piperidone, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-methylenebis (meth)acrylamide, and N,N-dimethylaminopropyl (meth)acrylamide.
[0033] The content of the (meth)acrylamide monomer other than 2-hydroxyethyl (meth)acrylamide is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 10 parts by mass or less, and further preferably 1 part by mass or less, with the lower limit being 0 parts by mass, based on 100 parts by mass of 2-hydroxyethyl (meth)acrylamide.
[0034] As the other vinyl compound, one or more kinds may be used, and examples thereof include styrene, α-methylstyrene, chlorostyrene, chloromethylstyrene, methyl vinyl ether, ethyl vinyl ether, and isobutyl vinyl ether.
[0035] The content of the other monomer (a3) in the monomer components is preferably 20% by mass or less, more preferably 10% by mass or less, further preferably 3% by mass or less, and the lower limit is 0% by mass.
[0036] The acrylic polymer (A) can be obtained by polymerizing the above-mentioned monomer components. As the polymerization method, free radical polymerization, anionic polymerization, cationic polymerization, etc. can be mentioned, and free radical polymerization is preferred. During the polymerization, one or more polymerization initiators can be used. As the above-mentioned polymerization initiator, specifically, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]disulfate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-amidinopropane) 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis(1-imino-1-pyrrolidinyl-2-methylpropane) dihydrochloride, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutylamidine ) (Japanese: 2,2'-Azobis (N,N'-dimethylbenzene) and other azo initiators; hydrogen peroxide, potassium persulfate, sodium persulfate, ammonium persulfate, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, cumene hydroperoxide and other peroxide initiators; persulfate initiators; carbonyl initiators; redox initiators, etc., preferably azo initiators.
[0037] The above-mentioned polymerization can be carried out in water, a hydrophilic organic solvent or a mixture of water and a hydrophilic organic solvent. Examples of the above-mentioned hydrophilic solvent include alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, etc.; ketone solvents such as acetone, methyl ethyl ketone, etc.; alkylene glycol solvents such as ethylene glycol, diethylene glycol, propylene glycol, etc.; alkyl ether solvents of polyalkylene glycols; lactam solvents such as N-methyl-2-pyrrolidone, etc.
[0038] The weight average molecular weight of the acrylic polymer (A) is 100,000 or more, preferably 150,000 or more, more preferably 220,000 or more, further preferably 250,000 or more, and further preferably 260,000 or more, and may be, for example, 1,000,000 or less, 700,000 or less, or 500,000 or less.
[0039] The weight average molecular weight of the acrylic polymer (A) can be measured by gel permeation chromatography as a converted value using polystyrene as a standard sample.
[0040] The urethane resin (B) is a polymer having a urethane bond in the molecule, and is preferably a reaction product of a polyol (b1), a polyisocyanate (b2), and a chain extender (b3) and / or a terminal blocker (b4) used as required. When a chain extender (b3) and / or a terminal blocker (b4) is used, it is preferred that the polyol (b1) and the polyisocyanate (b2) react to prepare a urethane prepolymer having an isocyanate group at the terminal, and then react with the chain extender (b3) and / or the terminal blocker (b4).
[0041] Examples of the polyol (b1) include polymer polyols (b1-1) of polyether polyols, polyester polyols, polycarbonate polyols, and polyolefin polyols; polyols having a hydrophilic group (b1-2); and low molecular weight polyols (b1-3).
[0042] The number average molecular weight of the polymer polyol (b1-1) is preferably 500 or more, more preferably 800 or more, and is preferably 5,000 or less, more preferably 4,000 or less, and further preferably 3,000 or less.
[0043] Examples of the polyether polyol include polyether polyols obtained by addition polymerization of alkylene oxides using, as necessary, one or more compounds having two or more active hydrogen atoms such as ethylene glycol and diethylene glycol as initiators.
[0044] Examples of the initiator include ethylene glycol, diethylene glycol, triethylene glycol, trimethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, glycerol, trimethylolethane, trimethylolpropane, sorbitol, sucrose, aconitose, trimellitic acid, trimellitic acid, phosphoric acid, ethylenediamine, diethylenetriamine, triisopropanolamine, pyrogallol, dihydroxybenzoic acid, hydroxyphthalic acid, and 1,2,3-propanetrithiol.
[0045] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, and tetrahydrofuran.
[0046] As the polyether polyol, polyoxytetramethylene glycol obtained by ring-opening polymerization of tetrahydrofuran is preferred.
[0047] The number average molecular weight of the polyether polyol is preferably 500 or more and 3,000 or less.
[0048] Examples of the polyester polyol include polyester polyols obtained by reacting a low molecular weight polyol with a polycarboxylic acid; polyester polyols obtained by ring-opening polymerization of a cyclic ester compound such as ε-caprolactone; and polyester polyols obtained by copolymerizing these.
[0049] As the low molecular weight polyol used in the production of the polyester polyol, one or more kinds of polyols can be used, for example, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, neopentyl glycol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,1 Aliphatic polyols having a molecular weight of 50 or more and 300 or less, such as 1-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, glycerol, trimethylolpropane, ditrimethylolpropane, trimethylolpropane, and pentaerythritol; polyols having an alicyclic structure, such as cyclohexanedimethanol and hydrogenated bisphenol A; polyols having an aromatic structure, such as bisphenol A and bisphenol F, etc.
[0050] As the above-mentioned polycarboxylic acid, one or more kinds can be used, for example, aliphatic polycarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedicarboxylic acid; alicyclic polycarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and cyclohexanetricarboxylic acid; aromatic polycarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and naphthalene dicarboxylic acid; their anhydrides or esters, etc.
[0051] Examples of the polycarbonate polyol include esterification reaction products of carbonate and polyol, and reaction products of polyol and phosgene.
[0052] As the above-mentioned carbonate, one or more than two kinds can be used, for example, aliphatic carbonate, alicyclic carbonate (hereinafter, containing alicyclic structure is sometimes referred to as "alicyclic".), aromatic carbonate (hereinafter, containing aromatic structure is sometimes referred to as "aromatic".). As aliphatic carbonate, saturated aliphatic carbonates such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, di-n-butyl carbonate, diisobutyl carbonate, ethyl n-butyl carbonate, ethyl isobutyl carbonate, etc. can be mentioned; unsaturated aliphatic carbonates such as ethylene carbonate, trimethylene carbonate, tetramethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 1,3-pentylene carbonate, 1,4-pentylene carbonate, 1,5-pentylene carbonate, 2,3-pentylene carbonate and 2,4-pentylene carbonate can be mentioned. Examples of the aromatic carbonate include diphenyl carbonate and dibenzyl carbonate.
[0053] As the above-mentioned polyol, one or more kinds can be used, for example, linear or branched diols such as ethylene glycol, propylene glycol, butanediol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; trifunctional or higher polyols such as trimethylolmethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, etc., etc.
[0054] Examples of the polyolefin polyol include polyethylene polyol, polypropylene polyol, polyisobutylene polyol, hydrogenated polybutadiene polyol, and hydrogenated polyisoprene polyol.
[0055] As the polymer polyol (b1-1), polyether polyol, polyester polyol and polycarbonate polyol are preferred.
[0056] The content of the polymer polyol (b1-1) in the polyol (b1) is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 93% by mass or more, and the upper limit is 100% by mass.
[0057] Examples of the above-mentioned polyol having a hydrophilic group (b1-2) include polyols having anionic groups, polyols having cationic groups, polyols having nonionic groups, etc., preferably polyols having anionic groups or cationic groups, and more preferably polyols having anionic groups.
[0058] Examples of the polyol having an anionic group include a polyol having a carboxyl group and a polyol having a sulfonic acid group.
[0059] Examples of the polyol having a carboxyl group include 2,2-dimethylol propionic acid, 2,2-dimethylol butyric acid, 2,2-dimethylol butyric acid, and 2,2-dimethylol valeric acid. Among them, 2,2-dimethylol propionic acid is preferred. In addition, polyester polyols having a carboxyl group obtained by reacting the polyol having a carboxyl group with various polycarboxylic acids may also be used.
[0060] Examples of the polyol having a sulfonic acid group include polyester polyols obtained by reacting dicarboxylic acids such as 5-sulfoisophthalic acid, sulfoterephthalic acid, 4-sulfophthalic acid, and 5[4-sulfophenoxy]isophthalic acid, or salts thereof with the low molecular weight polyols exemplified as those that can be used in the production of the polyester polyol having an aromatic structure.
[0061] The anionic groups are preferably partially or entirely neutralized by basic groups. Examples of the basic compounds include organic amines having a boiling point of 200°C or higher, such as ammonia, triethylamine, morpholine, monoethanolamine, and diethylethanolamine, and metal hydroxides such as sodium hydroxide, potassium hydroxide, and lithium hydroxide. From the viewpoint of improving the water dispersion stability of the urethane resin composition, the basic compound is preferably used in a range of basic group / anionic group of the basic compound = 0.5 to 3.0 (molar ratio), and more preferably in a range of 0.8 to 2.0 (molar ratio).
[0062] Examples of the polyol having a cationic group include polyols having a tertiary amino group, and more specifically, polyols obtained by reacting a compound having two epoxy groups in one molecule with a secondary amine, and the like.
[0063] It is preferred that a part or all of the cationic groups be neutralized with an acidic compound such as formic acid, acetic acid, propionic acid, succinic acid, glutaric acid, tartaric acid, or adipic acid.
[0064] In addition, the tertiary amino group as the above-mentioned cationic group is preferably partially or completely quaternized. As the above-mentioned quaternizing agent, for example, dimethyl sulfate, diethyl sulfate, methyl chloride, ethyl chloride, etc. can be mentioned. Among them, dimethyl sulfate is preferably used.
[0065] Moreover, as said polyol which has a nonionic group, a polyol which has a polyoxyethylene structure etc. are mentioned, for example.
[0066] The content of the polyol (b1-2) having a hydrophilic group is preferably 0.3% by mass or more and 10% by mass or less in the polyol (b1).
[0067] The low molecular weight polyol (b1-3) is a polyol having a molecular weight of less than 500 (preferably 450 or less, more preferably 400 or less, with a lower limit of about 50), and examples thereof include ethylene glycol, diethylene glycol, 1,2-propylene glycol, dipropylene glycol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,4-cyclohexanediol, 1,6-hexanediol, aliphatic polyols such as cyclobutanediol, cyclopentanediol, 1,4-cyclohexanediol, cycloheptanediol, cyclooctanediol, butylcyclohexanediol, cyclohexanedimethanol, hydroxypropyl cyclohexanol, dicyclohexanediol, hydrogenated bisphenol A, 1,3-adamantanediol, 1,1'-biscyclohexylene glycol, cyclohexanetriol, etc.; aromatic polyols such as bisphenol A, bisphenol F, bisphenol AD and their ethylene oxide, propylene oxide adducts, etc.
[0068] When the low molecular weight polyol (b1-3) is contained, the content thereof is preferably 0.1% by mass or more and 15% by mass or less in the polyol (b1).
[0069] As the polyisocyanate (b2), one or more kinds may be used, and examples thereof include aliphatic polyisocyanate, alicyclic polyisocyanate, and aromatic polyisocyanate.
[0070] Examples of the aliphatic polyisocyanate include hexamethylene diisocyanate, lysine diisocyanate methyl ester, xylylene diisocyanate, tetramethylxylylene diisocyanate, etc. These aliphatic polyisocyanates may be used alone or in combination of two or more.
[0071] Examples of the alicyclic polyisocyanate include isophorone diisocyanate, bis(isocyanatomethyl)cyclohexane, dicyclohexylmethane diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, dicyclohexyldimethylmethane diisocyanate, 2,2'-dimethyldicyclohexylmethane diisocyanate, bis(4-isocyanato-n-butylene)pentaerythritol, dimer acid diisocyanate, 2-isocyanato- Methyl-3-(3-isocyanatopropyl)-5-isocyanatomethyl-bicyclo〔2,2,1〕-heptane, 2-isocyanatomethyl-3-(3-isocyanatopropyl)-6-isocyanatomethyl-bicyclo〔2,2,1〕-heptane, 2-isocyanatomethyl-2-(3-isocyanatopropyl)-5-isocyanatomethyl-bicyclo〔2,2,1〕-heptane, 2-isocyanatomethyl- 2-(3-isocyanatopropyl)-6-isocyanatomethyl-bicyclo〔2,2,1〕-heptane, 2-isocyanatomethyl-3-(3-isocyanatopropyl)-6-(2-isocyanatoethyl)-bicyclo〔2,2,1〕-heptane, 2-isocyanatomethyl-3-(3-isocyanatopropyl)-6-(2-isocyanatoethyl)-bicyclo〔2,2,1〕-heptane, 2-isocyanatomethyl-3-(3-isocyanatopropyl)-6-(2-isocyanatoethyl)-bicyclo〔2,1,1〕-heptane, Preferably, the polyisocyanate is a saturated alicyclic polyisocyanate, preferably a monocyclic (non-condensed) alicyclic polyisocyanate, preferably a saturated alicyclic polyisocyanate, preferably a saturated alicyclic polyisocyanate. These alicyclic polyisocyanates may be used alone or in combination of two or more.
[0072] Examples of the aromatic polyisocyanate include phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, etc. These aromatic polyisocyanates may be used alone or in combination of two or more.
[0073] Among them, from the viewpoint of the hydrophilicity of the obtained coating film, it is preferred to contain an alicyclic polyisocyanate or an aromatic polyisocyanate, and it is more preferred to contain an alicyclic polyisocyanate.
[0074] The molar ratio (NCO / OH) of the isocyanate group contained in the polyisocyanate (b2) to the hydroxyl group contained in the polyol (b1) is preferably 1.05 or more, preferably 3 or less, and more preferably 2 or less.
[0075] The chain extender (b3) is a compound having two or more groups having active hydrogen atoms (preferably substituted or unsubstituted amino groups) in the molecule, and one or more kinds thereof can be used. Examples thereof include ethylenediamine, 1,3-propylenediamine, 1,3-butylenediamine, 1,4-butylenediamine, 1,6-hexamethylenediamine, 1,4-cyclohexyldiamine, 3-aminomethyl-3,5,5-trimethylcyclohexylamine (isophoronediamine), 4,4'-dicyclohexylmethanediamine, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 1,3-bis(aminomethyl)cyclohexane, hydrazine, o-toluenediamine, m-toluenediamine, p-toluenediamine, and the like; triamine compounds such as diethylenetriamine, and polyamine compounds having four or more amino groups such as triethylenetetramine and tetraethylenepentamine.
[0076] The amount of the chain extender is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 5 parts by mass or less, based on 100 parts by mass of the urethane prepolymer.
[0077] Examples of the terminal blocking agent (b4) include compounds having one group having an active hydrogen atom (preferably a substituted or unsubstituted amino group or hydroxy group) in the molecule, and compounds having a hydroxy group and a group having an active hydrogen atom (preferably a substituted or unsubstituted amino group or hydroxy group) in the molecule.
[0078] Examples of the compound having one group having an active hydrogen atom (preferably a substituted or unsubstituted amino group or hydroxyl group) in the above-mentioned molecule include monohydric alcohol compounds such as methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, and undecanol; and monoamine compounds such as ammonia, dibutylamine, and aminosilane.
[0079] Examples of the compound having a hydroxyl group and a group having an active hydrogen atom (preferably a substituted or unsubstituted amino group or hydroxyl group) in the molecule include diol compounds such as propylene glycol, butanediol, pentanediol, and hexanediol; and amino alcohol compounds such as ethanolamine and diethanolamine.
[0080] The amount of the terminal blocking agent (b4) is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the urethane prepolymer.
[0081] The urethane resin (B) can be produced by reacting the polyol (b1), the polyisocyanate (b2), and the chain extender (b3) and / or the end-capping agent (b4) used as required. The reaction temperature is preferably 50 to 150° C. In addition, during the reaction, a urethane-forming catalyst such as an organic tin compound may coexist.
[0082] When a polyol having an anionic group is used as the polyol having a hydrophilic group, the acid value of the urethane resin is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, and preferably 70 mgKOH / g or less, more preferably 50 mgKOH / g or less.
[0083] The mass ratio ((A) / (B)) of the acrylic polymer (A) to the urethane resin (B) is preferably 5 / 95 or more, more preferably 10 / 90 or more, and is preferably 50 / 50 or less, more preferably 40 / 60 or less.
[0084] The urethane resin (B) may be dispersed in part or all of the aqueous medium (C) in advance and then mixed with the acrylic polymer (A) and the aqueous medium (C) described below.
[0085] As the aqueous medium (C), water, organic solvents miscible with water, and mixtures thereof can be cited. As organic solvents miscible with water, for example, alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, 1,2-propylene glycol, 1,3-butylene glycol, etc.; ketone solvents such as acetone and methyl ethyl ketone; glycol ether solvents such as ethylene glycol n-butyl ether, diethylene glycol n-butyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol dimethyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, dipropylene glycol dimethyl ether, dipropylene glycol n-butyl ether, tripropylene glycol methyl ether, etc.; lactam solvents such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone; amide solvents such as N,N-dimethylformamide, etc. These organic solvents miscible with water can be used alone or in combination of two or more.
[0086] In addition, the aqueous medium (C) is preferably water alone or a mixture of water and an organic solvent miscible with water, and more preferably water alone, in consideration of safety and reduction of environmental load.
[0087] The content of the aqueous medium (C) is preferably 30 to 80% by mass, more preferably 50 to 70% by mass, based on the total amount of the aqueous resin composition.
[0088] The aqueous resin composition may contain, in addition to the acrylic polymer (A) and the aqueous medium (C), other additives such as a crosslinking agent, a plasticizer, an antistatic agent, a wax, a surfactant, a light stabilizer, a flow regulator, a dye, a leveling agent, a rheology control agent, an ultraviolet absorber, an antioxidant, a photocatalytic compound, an inorganic pigment, an organic pigment, and a body pigment, as needed.
[0089] Examples of the cross-linking agent include amino resins, aziridine compounds, melamine compounds, epoxy compounds, oxazoline compounds, carbodiimide compounds, and isocyanate compounds.
[0090] In addition, by using the above-mentioned surfactant, the blending stability of the urethane resin composition of the present invention can be further improved. When using a surfactant, from the aspect of being able to maintain the substrate adhesion of the obtained coating film, it is preferably used in an amount of 20 parts by mass or less relative to 100 parts by mass of the above-mentioned urethane resin (A), and preferably not used as much as possible.
[0091] The content of the other additives in the nonvolatile component of the aqueous resin composition is, for example, 30 mass % or less, for example, 20 mass % or less, with a lower limit of 0 mass %, and may be 0.1 mass % or more.
[0092] A coating agent containing the above-mentioned aqueous resin composition is also included in the technical scope of the present invention. Examples of the substrate of the above-mentioned coating agent include metals, various plastics, films thereof, glass, paper, wood, and the like.
[0093] Examples of the metal substrate include galvanized steel sheets, aluminum-galvanized steel sheets, aluminum sheets, aluminum alloy sheets, electromagnetic steel sheets, copper sheets, and stainless steel sheets used in applications such as automobiles, home appliances, and building materials.
[0094] As the above-mentioned plastic substrate, usually, as a raw material used in plastic molded products such as mobile phones, home appliances, automobile interior and exterior materials, OA equipment, etc., acrylonitrile-butadiene-styrene resin (ABS resin), polycarbonate resin (PC resin), ABS / PC resin, polystyrene resin (PS resin), polymethyl methacrylate resin (PMMA resin), acrylic resin, polypropylene resin, polyethylene resin, etc. can be mentioned, and as the plastic film substrate, polyethylene terephthalate film, polyester film, polyethylene film, polypropylene film, TAC (triacetyl cellulose) film, polycarbonate film, polyvinyl chloride film, etc. can be used.
[0095] The coating agent can be used for aluminum fins, building parts such as outer walls and roofs, civil engineering components such as guardrails, soundproof walls, and drainage channels, home appliances, industrial machinery, automobile exterior materials, goggles, anti-fog films, anti-fog glass and other anti-fog materials, mirrors, medical instruments and other articles. Articles having a coating film of the coating agent are also included in the technical scope of the present invention.
[0096] The coating film can be formed by applying the aqueous resin composition to a substrate and drying and curing it. Examples of the coating method include spraying, curtain coating, flow coating, roller coating, brush coating, and dipping. The drying can be performed naturally at room temperature or by heating. The heating drying is usually preferably performed at 40 to 250° C. for about 1 to 600 seconds.
[0097] The aqueous resin composition can exhibit initial hydrophilicity, corrosion resistance, and sustained hydrophilicity even when the thickness of the crosslinked coating is, for example, 10 μm or less (further 5 μm or less, 2.5 μm or less). The lower limit of the thickness of the crosslinked coating is, for example, 0.1 μm.
[0098] Example
[0099] The present invention will be described in more detail below with reference to Examples. In the present Examples, the weight average molecular weight of the acrylic polymer was measured by the following method.
[0100] [Method for measuring weight average molecular weight of acrylic polymer]
[0101] The weight average molecular weight of the acrylic polymer (A) is measured under the following conditions.
[0102] HPLC: Shimadzu / L20 system
[0103] Column: Shodex OHpak SB-806MHQ
[0104] (8.0mmI.D.×300mmL.×2 pieces)
[0105] Guard column: Shodex OHpak SB-G
[0106] (4.6mm I.D.×10mm L.)
[0107] Column temperature: 40°C
[0108] Eluent: 0.2 mol / L sodium nitrate aqueous solution
[0109] Flow rate: 0.70mL / min
[0110] Detector: RI, UV254nm
[0111] Injection volume: 50μL
[0112] Usage: 0.2M_NaNO3.lcm
[0113] (Standard sample)
[0114] "Shodex Pullulan P-800" manufactured by Showa Denko K.K.
[0115] "Shodex Pullulan P-400" manufactured by Showa Denko K.K.
[0116] "Shodex Pullulan P-200" manufactured by Showa Denko K.K.
[0117] "Shodex Pullulan P-100" manufactured by Showa Denko K.K.
[0118] "Shodex Pullulan P-50" manufactured by Showa Denko K.K.
[0119] "Shodex Pullulan P-20" manufactured by Showa Denko K.K.
[0120] "Shodex Pullulan P-10" manufactured by Showa Denko K.K.
[0121] "Shodex Pullulan P-5" manufactured by Showa Denko K.K.
[0122] (Synthesis Example (A-1))
[0123] In a four-necked flask equipped with a thermometer, a stirrer, a reflux condenser and a dropping device, ion exchange water and isopropyl alcohol as polymerization solvents were added in a nitrogen atmosphere to a total of 350 parts by mass, 2-hydroxyethyl acrylamide (hereinafter referred to as "HEAA") 50 parts by mass, methoxy polyethylene glycol acrylate ("AM-90G" manufactured by Shin-Nakamura Chemical Co., Ltd., the average number of moles of oxyethylene added was 9 mol) 48 parts by mass, and acrylic acid (hereinafter referred to as "AA") 1 part by mass were added. Next, 0.05 parts by mass of an azo polymerization initiator ("VA-044" manufactured by Wako Pure Chemical Industries, Ltd.) was added dropwise, and free radical polymerization was performed while maintaining at 50° C. to obtain a composition of an acrylic polymer (A-1). The weight average molecular weight of the obtained composition of an acrylic polymer (A-1) was 340,000, and the non-volatile content was 20% by mass.
[0124] (Comparative Synthesis Example (1))
[0125] In Synthesis Example (A-1), a comparative acrylic polymer (1) composition was obtained in the same manner as in Synthesis Example 1 except that 50 parts by mass of 2,2-dimethylacrylamide (hereinafter referred to as "DMAA") was used instead of 50 parts by mass of HEAA.
[0126] (Synthesis Example (B-1))
[0127] In a nitrogen-substituted container equipped with a thermometer, a nitrogen inlet pipe, and a stirrer, 69.8 parts by mass of a polyester polyol having a number average molecular weight of 1,200 obtained by reacting ethylene glycol, neopentyl glycol, terephthalic acid, isophthalic acid, and adipic acid, 2.7 parts by mass of 2,2-dimethylolpropionic acid (DMPA), 25 parts by mass of dicyclohexylmethane diisocyanate (H12MDI), and 65 parts by mass of methyl ethyl ketone were charged and reacted at 70° C. to obtain an organic solvent solution of a urethane prepolymer having an isocyanate group at a molecular terminal.
[0128] The mixture was then cooled to 40°C, 2 parts by mass of triethylamine was added to neutralize part or all of the carboxyl groups of the urethane prepolymer, 335 parts by mass of water was added and stirred thoroughly, and 0.5 parts by mass of ethylenediamine (EDA) was added to obtain an aqueous dispersion of the urethane resin, which was then aged and desolvated to obtain a composition of the urethane resin (B-1) having a non-volatile component of 30% by mass.
[0129] (Example 1, Comparative Example 1)
[0130] In a four-necked flask equipped with a thermometer, a stirring device, a reflux condenser and a dropping device, solutions of acrylic polymer (A) and urethane resin (B) shown in the following table were added so that the mass ratio of the non-volatile components of acrylic polymer (A) and urethane resin (B) was 15 / 85 and ion exchange water as an aqueous medium (C) was 30 parts by mass relative to 10 parts by mass of the total non-volatile components of acrylic polymer (A) and urethane resin (B) to obtain an aqueous dispersion. The aqueous dispersion was subjected to reduced pressure distillation to obtain an aqueous resin composition (1) having a non-volatile component of 25% by mass and a comparative composition (1).
[0131] [Preparation of test pieces]
[0132] The aqueous resin composition (1) and comparative composition (1) obtained in Example 1 and Comparative Example 1 were applied to an aluminum plate at a thickness of 1 μm and dried under the conditions shown in Table 1 to prepare test pieces.
[0133] [Evaluation of initial hydrophilicity]
[0134] 8 μL of pure water was dropped onto the surface of the test piece, and the contact angle was measured after 8 seconds.
[0135] [Evaluation of hydrophilicity retention (cycle test)]
[0136] After repeating the wet-dry cycle of the test piece 20 times, 8 μL of pure water was dropped on the surface of the test piece, and the contact angle was measured 8 seconds later. The wet condition was immersed in 25°C water for 2 minutes, and the dry condition was kept at 40°C for 6 minutes.
[0137] [Evaluation of hydrophilicity retention (processing oil test)]
[0138] After the test piece was immersed in the processing oil, the test piece was stood up for 10 minutes to remove the oil, and then dried at 150° C. for 5 minutes, and the contact angle of the coating surface of the obtained test piece was measured.
[0139] The evaluation results are shown in Table 1. When the water contact angle was less than 40°, the hydrophilicity was considered to be good.
[0140] [Table 1]
[0141]
[0142] Example 1 is an example of the present invention, and the hydrophilicity is good. Comparative Example 1 is an example in which 2,2-dimethylacrylamide is used instead of 2-hydroxyethyl (meth)acrylamide, and the hydrophilicity after the process oil test is poor.
Claims
1. An aqueous resin composition comprising an acrylic polymer (A), a urethane resin (B) and an aqueous medium (C), wherein the acrylic polymer (A) is formed from monomer components containing at least 2-hydroxyethylacrylamide, an unsaturated carboxylic acid or anhydride thereof, and a monomer having a polyoxyalkylene unit and a polymerizable unsaturated group, and has a weight average molecular weight of 100,000 or more.
2. The aqueous resin composition according to claim 1, wherein The unsaturated carboxylic acid or its anhydride is methacrylic acid.
3. The aqueous resin composition according to claim 1 or 2, wherein The number average molecular weight of the monomer having a polyoxyalkylene unit and a polymerizable unsaturated group is 200 or more and 1,500 or less.
4. The aqueous resin composition according to claim 1 or 2, wherein The urethane resin (B) is a reaction product of a polyol (b1) and a polyisocyanate (b2), and the polyisocyanate (b2) includes an alicyclic polyisocyanate.
5. The aqueous resin composition according to claim 3, wherein The urethane resin (B) is a reaction product of a polyol (b1) and a polyisocyanate (b2), and the polyisocyanate (b2) includes an alicyclic polyisocyanate. 6 . A coating agent comprising the aqueous resin composition according to claim 1 .
7. An article having a coating film of the coating agent according to claim 6.
Citation Information
Patent Citations
Hydrophilic coating agent
JP2004010764A
Hydrophilic treatment agent for heat exchanger aluminum fin
JP2017020015A
Method for producing semi-IPN composite
CN109790371A
Modifier
JP2004027208A
Aqueous resin composition and coating agent
JP2020132708A