A preparation method of siloxane-modified polyether and solid polycarboxylate water reducer

Through bulk polymerization of silicone-modified polyether macromonomers, a solid polycarboxylate water-reducing agent with good heat resistance is prepared, which solves the problem of denaturation and deactivation of existing solid water-reducing agents at high temperatures and achieves the same goal as Liquid water-reducing admixture has comparable water-reducing performance and low-cost production of solid water-reducing admixture.

CN115368517BActive Publication Date: 2024-10-15ANHUI CONCH MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211215594.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-10-15
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing solid water-reducing agent preparation process has the problems of high energy consumption, high cost and poor heat resistance, which leads to denaturation and deactivation at high temperatures, reduced water-reducing performance, and difficulty in transportation and storage.

Method used

Silicone-modified polyether is used as raw material, and through reasonable proportions and technological processes, a solid polycarboxylate water-reducing agent with good heat resistance is prepared, and the silicone-modified polyether macromonomer is used for bulk polymerization. Control the synthesis temperature between 40 and 70°C to reduce energy consumption and improve product stability.

Benefits of technology

The prepared solid polycarboxylate water-reducing agent has the same water-reducing and slump-preserving performance as the liquid water-reducing agent, and does not deactivate at high temperatures, reducing transportation and storage costs. The product has high purity, is safe and environmentally friendly, and produces no waste. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003875933250000081
    Figure BDA0003875933250000081
  • Figure BDA0003875933250000091
    Figure BDA0003875933250000091
  • Figure BDA0003875933250000101
    Figure BDA0003875933250000101
Patent Text Reader

Abstract

The invention discloses a preparation method of a siloxane-modified polyether and a solid polycarboxylate water-reducing agent. Firstly, cyclic siloxane, polyether and a catalyst are mixed and stirred and heated to 60-80 DEG C, then unsaturated alcohol is added dropwise, and after the addition is completed, the temperature is kept for 30-80 minutes to prepare the siloxane-modified polyether; then the temperature is stabilized at 40-70 DEG C, part of unsaturated carboxylic acid monomer and oxidant are added thereto, and then a mixture of the remaining part of unsaturated carboxylic acid monomer, chain transfer agent, functional monomer and auxiliary agent is added dropwise; after the addition is completed, a reducing agent is added or not, the temperature is kept for 1.0h-2.0h, and the solid polycarboxylate water-reducing agent is ground after cooling to obtain the solid polycarboxylate water-reducing agent; the water-reducing performance of the solid polycarboxylate water-reducing agent is slightly better than that of a traditional liquid polycarboxylate water-reducing agent, the collapse resistance is equivalent to that of a liquid water-reducing agent, and the solid polycarboxylate water-reducing agent has certain heat resistance and stability, and the solid polycarboxylate water-reducing agent can be used for the production of building materials such as dry-mixed mortar and grouting materials and shotcrete, and the solid polycarboxylate water-reducing agent has a wide market application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete admixtures, and particularly relates to a preparation method of a siloxane-modified polyether and a solid polycarboxylic acid water-reducing agent. Background Art

[0002] At present, most of the polycarboxylic acid water-reducing agents sold on the market are liquid, with a solid content of 10% to 50%. For long-distance construction, transportation is difficult and the cost is high. At the same time, it also limits its application areas. For example, in the production process of dry mortar, grouting materials and other construction products, when using water-reducing agents, solid water-reducing agents must be used. Although there are a small number of solid water-reducing agents produced by spray drying on the market, their curing process is complicated, energy consumption is high, cost is high, and there are certain safety hazards.

[0003] In addition to the drying method for preparing solid water reducers, there is also a bulk method for directly preparing solid water reducers. However, the temperature of the bulk polymerization method is relatively high. The common polyether macromonomers used to prepare solid water reducers have poor heat resistance and are easily denatured at high temperatures. This leads to a decrease in the water-reducing performance of the solid water reducer prepared by the bulk polymerization method. Therefore, the synthesis of polyethers with good heat resistance is a necessary condition for preparing solid water reducers by the bulk polymerization method. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a heat-resistant siloxane-modified polyether. The siloxane-modified polyether prepared by the preparation method has the characteristics of heat resistance and stability. When preparing a solid polycarboxylic acid water reducer, there is no obvious denaturation and deactivation at a higher reaction temperature and a longer reaction time, and a solid water reducer with good heat resistance and stability can be prepared.

[0005] Another object of the present invention is to provide a method for preparing a solid polycarboxylate water-reducing agent with good heat resistance. The solid polycarboxylate water-reducing agent prepared by using the siloxane-modified polyether as a raw material has a water-reducing performance slightly better than that of a traditional liquid polycarboxylate water-reducing agent, and has a collapse resistance equivalent to that of a liquid water-reducing agent, and has certain heat resistance and stability. The solid polycarboxylate water-reducing agent can be used for the production of building materials such as dry-mixed mortar and grouting materials, as well as shotcrete, and has broad market application prospects.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a siloxane-modified polyether comprises the following steps: mixing and stirring cyclic siloxane, polyether and a catalyst and heating to 60-80°C, then dropping unsaturated alcohol, and keeping the temperature for 30-80 minutes after the dropping is completed. The siloxane-modified unsaturated polyether prepared by this process has a reasonable molecular structure, the bond energy of the C-C bond in the structure is 347 kJ / mol, the bond energy of the Si-O bond is 462 kJ / mol, the heat resistance is good, and the conversion rate is high.

[0008] The mass ratio of the unsaturated alcohol, cyclic siloxane, polyether and catalyst is 1: (10-20): (30-50): (0.5-2.0). Within this ratio range, the prepared siloxane-modified polyether has a high conversion rate, good heat resistance and good molecular structure.

[0009] The unsaturated alcohol is any one or both of methyl allyl alcohol and isopentenyl alcohol; the dropwise addition time of the unsaturated alcohol is 20 to 40 minutes.

[0010] The cyclic siloxane is any one or two of hexamethylcyclotrisiloxane and octamethylcyclotetrasiloxane.

[0011] The polyether is an oligomer of ethylene oxide or an oligomer of propylene oxide; the molecular weight of the polyether is 600-1200.

[0012] The catalyst is an acid or a base, and the catalyst is preferably a sodium hydroxide solution with a mass fraction of 15 to 30%.

[0013] The present invention provides a method for preparing a solid polycarboxylate water-reducing agent, comprising the following steps:

[0014] (1) stabilizing the temperature of the siloxane-modified polyether at 40 to 70° C., and adding a portion of the unsaturated carboxylic acid monomer and an oxidant thereto;

[0015] (2) adding dropwise the remaining portion of the mixture of unsaturated carboxylic acid monomer, chain transfer agent, functional monomer and auxiliary agent into step (1);

[0016] (3) After the dropwise addition is completed, a reducing agent is added or not added, and the temperature is kept warm for 1.0 h to 2.0 h. After cooling, the solid polycarboxylate water-reducing agent is obtained by grinding.

[0017] The mass ratio of the siloxane-modified polyether, the unsaturated carboxylic acid monomer, the oxidant, the reducing agent, the chain transfer agent, the functional monomer and the auxiliary agent is 240: (25-30): (2-4): (0-1): (1.8-2.0): (1-12): (5-7). The water-reducing and slump-retaining performance of the solid polycarboxylate water-reducing agent prepared within this ratio range is equivalent to that of the traditional liquid polycarboxylate water-reducing agent, and is superior to that of the traditional solid polycarboxylate water-reducing agent.

[0018] The mass ratio of the unsaturated carboxylic acid monomer in step (1) to the unsaturated carboxylic acid monomer in step (2) is 1:20-40.

[0019] The unsaturated carboxylic acid monomer is any one or both of acrylic acid and methacrylic acid.

[0020] The functional monomer is any one or more of hydroxyethyl acrylate, hydroxypropyl acrylate and sodium methacrylate sulfonate.

[0021] The auxiliary agent is one or both of dimethyl maleate and sodium hydroxide solution; the mass fraction of the sodium hydroxide solution is 15-30%.

[0022] The oxidant is any one or more of hydrogen peroxide, ammonium persulfate, azobisisobutyronitrile, and dibenzoyl peroxide.

[0023] The reducing agent is any one or more of bleaching agent, ascorbic acid, sodium pyrosulfite and ferrous salt.

[0024] The chain transfer agent is any one or more of thioglycolic acid, mercaptopropionic acid, and mercaptoethanol.

[0025] In step (2), the dropwise addition time of the mixture is 2.5-4.0 hours.

[0026] In the preparation method of the solid polycarboxylate water-reducing agent provided by the present invention, the synthesis temperature in the preparation process can be controlled at 40-70° C., and the waste heat during the polymerization synthesis can be fully utilized, and the energy consumption is small. Within the synthesis temperature range of the present invention, the water-reducing and slump-retaining performance of the prepared solid polycarboxylate water-reducing agent is not only equivalent to that of the traditional liquid polycarboxylate water-reducing agent, but also has better initial expansion of the net slurry than the solid polycarboxylate water-reducing agent prepared by the traditional method, and has better self-fluidity retention performance within the same time.

[0027] During the preparation of solid water-reducing agent, the viscosity of the molten reaction system is high, and the viscosity of the system is usually reduced by increasing the temperature. However, the unsaturated polyether macromonomer is not heat-resistant, and the double bond retention rate decreases at high temperature for a long time, resulting in a decrease in the conversion rate of the reaction and a decrease in the water-reducing performance of the prepared water-reducing agent. In the present invention, a heat-resistant siloxane-modified polyether macromonomer is firstly obtained by using a siloxane-modified polyether macromonomer, and then the heat-resistant siloxane-modified polyether macromonomer is used as a raw material to prepare a solid polycarboxylic acid water-reducing agent. In this way, even if the reaction is carried out for a long time at a temperature of 40 to 70°C, the material will not be inactivated.

[0028] In the preparation method of the solid polycarboxylate water-reducing agent provided by the present invention, a heat-resistant siloxane-modified polyether macromonomer is used as a raw material, and a bulk polymerization method is adopted to directly synthesize the solid polycarboxylate water-reducing agent, which not only improves the utilization rate of the reaction kettle during the synthesis, but also makes the product easy to package and transport while maintaining the high-efficiency water-reducing performance of the original product, reduces the packaging and transportation costs, and is also easy to store. Compared with the prior art, the preparation process of the present invention is simple, the preparation cost is low, the repetitive stability is good, and the solid water-reducing agent product has a high purity compared with the liquid water-reducing agent, and the purity can reach more than 97%, and the preparation process is safe and environmentally friendly, and no waste is generated. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to the embodiments.

[0030] Example 1

[0031] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0032] 1) 75.0 g of hexamethylcyclotrisiloxane, 165.0 g of polyethylene glycol with a molecular weight of 600 and 5.0 g of a 20% sodium hydroxide solution are added to a reactor placed in a constant temperature water bath and stirred. When the temperature of the reactor is constant at 60.0° C., 5.0 g of methyl allyl alcohol is added through a high-precision peristaltic pump for 30 minutes. After the addition is completed, the mixture is kept warm for 30 minutes to obtain a siloxane-modified polyether;

[0033] 2) 240.0 g of siloxane-modified polyether was taken and stirred mechanically until the temperature in the reactor was constant at 60.0° C. After the temperature was constant, 1.0 g of acrylic acid, 1.2 g of hydrogen peroxide and 1.8 g of ammonium persulfate were added in sequence, and a mixed solution consisting of 30.0 g of acrylic acid, 2.0 g of mercaptopropionic acid, 5.0 g of 20% mass fraction sodium hydroxide solution and 1.0 g of dimethyl maleate was added dropwise for 3.5 h. After the addition was completed, the mixture was kept warm for 1.5 h. The discharged material was cooled and ground to obtain a solid powdered polycarboxylate water reducer.

[0034] Example 2

[0035] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0036] 1) 75.0 g of hexamethylcyclotrisiloxane, 165.0 g of polyethylene glycol with a molecular weight of 800 and 5.0 g of a 20% sodium hydroxide solution are added to a reactor placed in a constant temperature water bath and stirred. When the temperature of the reactor is constant at 60.0° C., 5.0 g of methyl allyl alcohol is added through a high-precision peristaltic pump for 30 minutes. After the addition is completed, the mixture is kept warm for 30 minutes to obtain a siloxane-modified polyether;

[0037] 2) 240.0 g of siloxane-modified polyether was taken and stirred mechanically until the temperature in the reactor was constant at 60.0° C. After the temperature was constant, 1.0 g of acrylic acid, 1.2 g of hydrogen peroxide and 1.8 g of ammonium persulfate were added in sequence, and a mixed solution consisting of 30.0 g of acrylic acid, 2.0 g of mercaptopropionic acid, 5.0 g of 20% mass fraction of sodium hydroxide solution and 1.0 g of dimethyl maleate was added dropwise for 3.5 h. After the addition was completed, the mixture was kept warm for 1.5 h. The discharged material was cooled and ground to obtain a solid powdered polycarboxylate water reducer.

[0038] Example 3

[0039] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0040] 1) 100.0 g of octamethylcyclotetrasiloxane, 165.0 g of polyethylene glycol with a molecular weight of 800 and 5.0 g of a 20% sodium hydroxide solution are added to a reactor placed in a constant temperature water bath and stirred. When the temperature of the reactor is constant at 60.0° C., 5.0 g of isopentenol is added by a high-precision peristaltic pump for 30 minutes. After the addition is completed, the mixture is kept warm for 30 minutes to obtain a siloxane-modified polyether;

[0041] 2) 240.0 g of siloxane-modified polyether was taken and stirred mechanically until the temperature in the reactor was constant at 60.0° C. After the temperature was constant, 1.0 g of acrylic acid, 1.2 g of hydrogen peroxide and 1.8 g of ammonium persulfate were added in sequence, and a mixed solution consisting of 30.0 g of acrylic acid, 2.0 g of mercaptopropionic acid, 5.0 g of 20% mass fraction of sodium hydroxide solution and 1.0 g of dimethyl maleate was added dropwise for 3.5 h. After the addition was completed, the mixture was kept warm for 1.5 h. The discharged material was cooled and ground to obtain a solid powdered polycarboxylate water reducer.

[0042] Example 4

[0043] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0044] 1) 100.0 g of octamethylcyclotetrasiloxane, 165.0 g of poly(1,2-propylene glycol) ether with a molecular weight of 800 and 5.0 g of a sodium hydroxide solution with a mass fraction of 20% are added to a reactor placed in a constant temperature water bath and stirred. When the temperature of the reactor is constant at 60.0° C., 5.0 g of isopentenol is added by a high-precision peristaltic pump for 30 minutes. After the addition is completed, the mixture is kept warm for 30 minutes to obtain a siloxane-modified polyether;

[0045] 2) 240.0 g of siloxane-modified polyether was taken and stirred mechanically until the temperature in the reactor was constant at 60.0° C. After the temperature was constant, 1.0 g of acrylic acid, 1.2 g of hydrogen peroxide and 1.8 g of ammonium persulfate were added in sequence, and a mixed solution consisting of 30.0 g of acrylic acid, 2.0 g of mercaptopropionic acid, 5.0 g of 20% mass fraction of sodium hydroxide solution and 1.0 g of dimethyl maleate was added dropwise for 3.5 h. After the addition was completed, the mixture was kept warm for 1.5 h. The discharged material was cooled and ground to obtain a solid powdered polycarboxylate water reducer.

[0046] Example 5

[0047] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0048] 1) 100.0 g of octamethylcyclotetrasiloxane, 165.0 g of polyethylene oxide with a molecular weight of 800 and 5.0 g of a 20% sodium hydroxide solution are added to a reactor placed in a constant temperature water bath and stirred. When the temperature of the reactor is constant at 60.0° C., 5.0 g of isopentenol is added through a high-precision peristaltic pump for 30 minutes. After the addition is completed, the mixture is kept warm for 30 minutes to obtain a siloxane-modified polyether;

[0049] 2) 240.0 g of siloxane-modified polyether was taken and stirred mechanically until the temperature in the reactor was constant at 60.0° C. After the temperature was constant, 1.0 g of acrylic acid, 1.2 g of hydrogen peroxide and 1.8 g of ammonium persulfate were added in sequence, and a mixed solution consisting of 30.0 g of acrylic acid, 2.0 g of mercaptopropionic acid, 5.0 g of hydroxyethyl acrylate, 1.0 g of dimethyl maleate and 5.0 g of 20% by mass sodium hydroxide solution was added dropwise for 3.5 h. After the addition was completed, the mixture was kept warm for 1.5 h. The discharged material was cooled and ground to obtain a solid powdered polycarboxylate water reducer.

[0050] Comparative Example 1

[0051] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0052] Take 240.0g of isopentanol polyoxyethylene ether and stir mechanically until the temperature in the reactor is constant at 60.0°C. After the temperature is constant, add 1.0g of acrylic acid, 1.2g of hydrogen peroxide and 1.8g of ammonium persulfate in sequence, and start to drop a mixed solution consisting of 30.0g of acrylic acid, 2.0g of mercaptopropionic acid, 5.0g of 20% mass fraction of sodium hydroxide solution and 1.0g of dimethyl maleate. The dropping time is 3.5h. After the dropping is completed, keep warm for 1.5h. After the discharge is cooled, grind to obtain a solid powdered polycarboxylate water reducer.

[0053] Comparative Example 2

[0054] A method for preparing a solid polycarboxylate water-reducing agent comprises the following steps:

[0055] 1) 165.0 g of polyethylene glycol with a molecular weight of 800 and 5.0 g of a 20% sodium hydroxide solution were added to a reactor placed in a constant temperature water bath and stirred. When the temperature of the reactor was constant at 60.0° C., 5.0 g of isopentenol was added by a high-precision peristaltic pump for 30 minutes. After the addition was completed, the mixture was kept warm for 30 minutes to obtain an unmodified polyether;

[0056] 2) 240.0 g of unmodified polyether was taken and stirred mechanically until the temperature in the reactor was constant at 60.0° C. After the temperature was constant, 1.0 g of acrylic acid, 1.2 g of hydrogen peroxide and 1.8 g of ammonium persulfate were added in sequence, and a mixed solution consisting of 30.0 g of acrylic acid, 2.0 g of mercaptopropionic acid, 5.0 g of 20% mass fraction of sodium hydroxide solution and 1.0 g of dimethyl maleate was added dropwise for 3.5 h. After the addition was completed, the mixture was kept warm for 1.5 h. The discharged material was cooled and ground to obtain a solid powdered polycarboxylate water reducer.

[0057] Experimental Example 1

[0058] Cement paste fluidity test

[0059] (1) Experimental materials: solid polycarboxylate water reducers provided in Examples 1-5 and Comparative Examples 1-2, commercially available KYD-A powder polycarboxylate water reducer from Kaiyuda as comparative example 1, and commercially available RHEOPLUS 416 liquid polycarboxylate water reducer from BASF as comparative example 2.

[0060] (2) Experimental grouping: Take the same amount of the powdered polycarboxylate water reducer provided in Examples 1-5 and Comparative Examples 1-2, the commercially available KYD-A powdered polycarboxylate produced by Kaiyuda, and the commercially available RHEOPLUS 416 liquid polycarboxylate water reducer produced by BASF.

[0061] (3) Experimental treatment method: The test was carried out in accordance with GB / T8077-2000 "Test method for homogeneity of concrete admixtures", W / C = 0.29, the dosage was solid dosage, and the neat paste fluidity of each embodiment in the benchmark cement was measured at the same dosage.

[0062] (4) Observation indicators: The test results are shown in Table 1.

[0063] Table 1 Time-dependent changes in cement paste fluidity

[0064]

[0065]

[0066] It can be seen from the cement paste fluidity data that the solid polycarboxylate water reducer prepared by the present invention has a close initial paste fluidity value to that of solid and liquid water reducers on the market. After adding a monomer with a collapse-preserving function, the problem of poor collapse-preserving performance of solid water reducers is solved. The prepared solid water reducer has a water-reducing performance equivalent to that of liquid water reducers and is superior to that of solid water reducers on the market. However, the water reducer prepared in the comparative example has a large gap in initial paste fluidity and paste fluidity after 1 hour compared with solid and liquid water reducers on the market.

[0067] Experimental Example 2

[0068] Concrete properties:

[0069] (1) Experimental materials: solid polycarboxylate water reducers provided in Examples 1-5 and Comparative Examples 1-2, commercially available BASF RHEOPLUS 416 powder polycarboxylate water reducer as Comparative Example 1, and commercially available KYD-A liquid polycarboxylate water reducer as Comparative Example 2.

[0070] (2) Experimental grouping: Take the same amount of the powdered polycarboxylate water reducer provided in Examples 1-5 and Comparative Examples 1-2, the commercially available KYD-A powdered polycarboxylate produced by Kaiyuda, and the commercially available RHEOPLUS 416 liquid polycarboxylate water reducer produced by BASF.

[0071] (3) Experimental treatment method: The concrete performance test was carried out on the samples obtained in the embodiment and the control example according to GB / T8077-2000 "Concrete admixture homogeneity test method". The dosage is the solid dosage, and the raw material mix ratio is shown in Table 2.

[0072] (4) Observation indicators: The test results are shown in Table 3.

[0073] Table 2 Raw material ratio

[0074]

[0075] Table 3 Performance of water reducing agent concrete

[0076]

[0077] From the concrete slump and expansion data, it can be seen that the initial concrete slump and expansion values ​​of the water reducers prepared in each implementation are close to those of the solid and liquid water reducers on the market. After adding the monomer with slump-retaining function, the problem of poor slump-retaining performance of the solid water reducer is solved. The water-reducing performance of the prepared solid water reducer is equivalent to that of the liquid water reducer, and is better than that of the solid water reducer on the market. However, the initial concrete slump and expansion values ​​of the water reducer prepared in the comparative example are much different from those of the solid and liquid water reducers on the market.

[0078] The detailed description of the preparation method of a siloxane-modified polyether and a solid polycarboxylic acid water-reducing agent with reference to the above-mentioned examples is illustrative rather than restrictive, and several examples can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.

Claims

1. A method for preparing a solid polycarboxylate water-reducing agent, characterized in that: The preparation method comprises the following steps: (1) stabilizing the temperature of the siloxane-modified polyether at 40 to 70° C., and adding a portion of the unsaturated carboxylic acid monomer and the oxidant thereto; (2) adding dropwise a portion of the mixture of unsaturated carboxylic acid monomer, chain transfer agent, functional monomer and auxiliary agent prepared in step (1); (3) After the dropwise addition is completed, a reducing agent is added or not added, and the temperature is kept warm for 1.0 h to 2.0 h. After cooling, the solid polycarboxylate water reducer is obtained by grinding. The preparation method of the siloxane-modified polyether comprises the following steps: mixing cyclic siloxane, polyether and a catalyst and heating to 60-80° C., then dropping unsaturated alcohol, and keeping the temperature for 30-80 minutes after the dropping is completed; The unsaturated alcohol is any one or both of methyl allyl alcohol and isopentenyl alcohol; The cyclic siloxane is any one or two of hexamethylcyclotrisiloxane and octamethylcyclotetrasiloxane; The polyether is an oligomer of ethylene oxide or an oligomer of propylene oxide.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the unsaturated alcohol, cyclic siloxane, polyether and catalyst is 1: (10-20): (30-50): (0.5-2.0).

3. The preparation method according to claim 1, characterized in that: The molecular weight of the polyether is 600-1200; and the catalyst is an acid or a base.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the silicone modified polyether, unsaturated carboxylic acid monomer, oxidant, reducing agent, chain transfer agent, functional monomer and auxiliary agent is 240: (25-30): (2-4): (0-1): (1.8-2.0): (1-12): (5-7).

5. The preparation method according to claim 1, characterized in that: The unsaturated carboxylic acid monomer is any one or both of acrylic acid and methacrylic acid; the functional monomer is any one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, and sodium methacrylate sulfonate; and the auxiliary agent is one or both of dimethyl maleic anhydride and sodium hydroxide solution.

6. The preparation method according to claim 1, characterized in that: The oxidant is any one or more of hydrogen peroxide, ammonium persulfate, azobisisobutyronitrile, and dibenzoyl peroxide; the reducing agent is any one or more of bleaching powder, ascorbic acid, sodium pyrosulfite, and ferrous salt; and the chain transfer agent is any one or more of thioglycolic acid, mercaptopropionic acid, and mercaptoethanol.

7. The preparation method according to claim 1, characterized in that: In step (2), the mixture is added dropwise for 2.5-4.0 hours.

8. The solid polycarboxylate water-reducing agent prepared by the preparation method according to any one of claims 1 to 7.