A polymer insulating coating and preparation method thereof

By coating the lithium-ion battery electrode sheets with an insulating coating of polymers such as aramid fiber and polyimide, the problem of insufficient adhesion of the ceramic coating is solved, significantly improving the safety and electrolyte resistance of the lithium-ion battery. performance, avoiding short circuits caused by diaphragm shrinkage and pole piece extension.

CN115377609BActive Publication Date: 2024-10-25ZHEJIANG DAXIANG NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210960967.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-11
Publication Date
2024-10-25
Estimated Expiration
2042-08-11

AI Technical Summary

Technical Problem

The existing lithium-ion battery separator shrinks under high temperature conditions, causing short circuits between the positive and negative electrodes. The existing ceramic coating has high hardness but weak adhesion, and is prone to powder loss and loss of function, affecting battery safety.

Method used

A polymer insulating coating is used, including aramid fiber and its derivatives, polymers such as polyimide, and a cross-linking agent. The modified polymer is soaked in the cross-linking agent solution and dissolved in N with the second polymer. N-dimethylacetamide is coated on the current collector empty foil area of ​​the electrode sheet to form a polymer insulating coating with a thickness of 5 to 20 μm to enhance adhesion and mechanical strength.

Benefits of technology

It improves the heat resistance and electrolyte resistance of the coating, enhances the bonding ability and mechanical strength through hydrogen bonding and conjugated bonding, avoids cell short circuit caused by separator shrinkage and pole piece extension, and significantly improves the performance of lithium-ion batteries. security.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a polymer insulating coating and a preparation method thereof, belonging to the technical field of lithium ion batteries. The method comprises the following steps: step 1, dispersing an equivalent cross-linking agent in a solvent to prepare a cross-linking agent solution with a concentration of 1g / L-5g / L; step 2, soaking a first polymer in a cross-linking agent solution, adjusting the solution pH to 8.5, stirring for 5 to 24 hours at room temperature, filtering, and drying to prepare a modified first polymer; step 3, dissolving the modified first polymer and the second polymer in an N,N-dimethylacetamide solvent, stirring for 2 to 12 hours at room temperature, and then coating the empty foil area of ​​the current collector of the electrode sheet, drying, and obtaining a polymer insulating coating. The present invention can improve the adhesion and mechanical strength of the coating, solve the problems of powder loss and ear tearing of the existing commercial ceramic coating, significantly improve the ear wrinkles when the electrode sheet is rolled, effectively avoid the phenomenon of internal short circuit of the battery cell due to membrane shrinkage, pole piece extension, etc., and improve the safety of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a polymer insulating coating and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have been widely used in mobile phones, power tools, energy storage and electric vehicles due to their high specific energy, long cycle life, low self-discharge, no memory effect and environmental protection. However, with the demand for high specific energy and super fast charging, battery safety has received more and more attention.

[0003] Lithium-ion batteries are mainly composed of materials such as positive electrodes, negative electrodes, electrolytes and diaphragms. The diaphragm is located between the positive and negative electrodes. Its main function is to separate the active materials of the positive and negative electrodes to prevent the positive and negative electrodes from directly contacting and short-circuiting. However, the diaphragms currently used are mainly polyolefin diaphragms and ceramic diaphragms with polyolefin diaphragms as base films. The melting temperature of polyethylene diaphragms is about 135°C, and the melting temperature of polypropylene diaphragms is about 165°C. Even if the heat resistance of ceramic diaphragms is improved to a certain extent, under high temperature conditions, the diaphragm will also shrink, resulting in short circuits between the positive and negative electrodes, creating safety risks. Therefore, at this stage, when preparing the positive electrode, battery manufacturers apply a layer of ceramic coating on the empty foil of the pole ear to effectively avoid the risk of short circuits due to the shrinkage of the diaphragm, but the prepared ceramic coating has high hardness, weak adhesion, and is easy to fall off. After being soaked in the electrolyte, it is easy to fall off and lose its function. Therefore, it is urgent to develop a coating with strong adhesion and toughness to improve the safety of lithium batteries. Summary of the invention

[0004] The purpose of the present invention is to provide a polymer insulating coating and a preparation method thereof, aiming to improve the adhesion and mechanical strength of the insulating coating, improve the wrinkles of the rolled electrode tabs, avoid the phenomenon of internal short circuit of the battery cell due to diaphragm shrinkage, electrode extension, etc., improve the safety of lithium-ion batteries, thereby solving the problems raised in the above-mentioned background technology.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A polymer insulating coating comprises a first polymer, a second polymer and a cross-linking agent. The polymer insulating coating is coated on a current collector empty foil area of ​​an electrode sheet.

[0007] The first polymer is one or more of aramid fiber and its derivatives.

[0008] The second polymer is one or more of polyimide, polyacrylonitrile, polyacrylate, polyvinylidene fluoride and polytetrafluoroethylene.

[0009] The cross-linking agent is one or more of polydopamine and its derivatives.

[0010] The thickness of the polymer insulating coating is 5-20 μm.

[0011] The method for preparing the polymer insulating coating comprises the following steps:

[0012] Step 1: dispersing an equivalent amount of a cross-linking agent in a solvent to prepare a cross-linking agent solution with a concentration of 1 g / L-5 g / L;

[0013] Step 2: soaking the first polymer in the crosslinking agent solution prepared in step 1, then adjusting the solution pH to 8.5, stirring at room temperature for 5 to 24 hours, filtering, and drying to prepare a modified first polymer;

[0014] Step 3: dissolve the modified first polymer and the second polymer prepared in step 2 in N,N-dimethylacetamide solvent, stir at room temperature for 2 to 12 hours, then apply them on the empty foil area of ​​the current collector of the electrode sheet, and dry them to obtain a polymer insulating coating.

[0015] In step 2, the mass ratio of the first polymer to the cross-linking agent is 45-49:1-5.

[0016] In step three, the mass ratio of the modified first polymer to the second polymer is 2-5:5-8.

[0017] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0018] The insulating coatings prepared by the present invention all use polymers with excellent heat resistance and electrolyte resistance. At the same time, through the super strong bonding ability of polydopamine, the polymers in the insulating coating are bonded through hydrogen bonds and conjugated bonds, thereby improving the bonding ability and mechanical strength of the coating, solving the problems of powder shedding and tab tearing of existing commercial ceramic coatings, and significantly improving the tab wrinkles when the electrode sheet is rolled, effectively avoiding the phenomenon of internal short circuit of the battery cell due to membrane shrinkage, pole sheet extension and the like, improving the safety of lithium-ion batteries, and facilitating popularization and use. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0020] Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] This embodiment provides a polymer insulating coating, which is prepared by the following steps:

[0023] Step 1: dispersing polydopamine in a solvent to prepare a polydopamine solution with a concentration of 5 g / L;

[0024] Step 2: 95 g of aramid fiber was soaked in 1000 mL of polydopamine solution, and then the pH of the solution was adjusted to 8.5, stirred at room temperature for 24 h, filtered, and dried to prepare modified aramid fiber;

[0025] Step 3: Dissolve 30 g of modified aramid fiber and 70 g of polyacrylate in 1000 mL of N,N-dimethylacetamide solvent, stir at room temperature for 5 hours, then apply it on the current collector empty foil of the electrode sheet of the lithium ion battery, dry it, and prepare a polymer insulating coating with a thickness of 12 μm.

[0026] Embodiment 2:

[0027] This embodiment provides a polymer insulating coating, which is prepared by the following steps:

[0028] Step 1: dispersing polydopamine in a solvent to prepare a polydopamine solution with a concentration of 5 g / L;

[0029] Step 2: 95 g of aramid fiber was soaked in 1000 mL of polydopamine solution, and then the pH of the solution was adjusted to 8.5, stirred at room temperature for 24 h, filtered, and dried to prepare modified aramid fiber;

[0030] Step 3: Dissolve 40 g of modified aramid fiber and 60 g of polyacrylate in 1000 mL of N,N-dimethylacetamide solvent, stir at room temperature for 5 h, then apply it on the current collector empty foil of the electrode sheet of the lithium ion battery, dry it, and prepare a polymer insulating coating with a thickness of 12 μm.

[0031] Embodiment 3:

[0032] This embodiment provides a polymer insulating coating, which is prepared by the following steps:

[0033] Step 1: dispersing polydopamine in a solvent to prepare a polydopamine solution with a concentration of 5 g / L;

[0034] Step 2: 95 g of aramid fiber was soaked in 1000 mL of polydopamine solution, and then the pH of the solution was adjusted to 8.5, stirred at room temperature for 24 h, filtered, and dried to prepare modified aramid fiber;

[0035] Step 3: Dissolve 50 g of modified aramid fiber and 50 g of polyacrylate in 1000 mL of N,N-dimethylacetamide solvent, stir at room temperature for 5 hours, then apply it on the empty foil of the current collector of the electrode sheet of the lithium-ion battery, dry it, and prepare a polymer insulating coating with a thickness of 12 μm.

[0036] Embodiment 4:

[0037] This embodiment provides a polymer insulating coating, which is prepared by the following steps:

[0038] Step 1: dispersing polydopamine in a solvent to prepare a polydopamine solution with a concentration of 5 g / L;

[0039] Step 2: 98 g of aramid fiber was soaked in 400 mL of polydopamine solution, and then the pH of the solution was adjusted to 8.5, stirred at room temperature for 24 h, filtered, and dried to prepare modified aramid fiber;

[0040] Step 3: Dissolve 30 g of modified aramid fiber and 70 g of polyacrylate in 1000 mL of N,N-dimethylacetamide solvent, stir at room temperature for 5 h, then coat on the empty foil of the current collector, and dry to prepare a polymer insulating coating with a thickness of 12 μm.

[0041] Embodiment 5:

[0042] This embodiment provides a polymer insulating coating, which is prepared by the following steps:

[0043] Step 1: dispersing polydopamine in a solvent to prepare a polydopamine solution with a concentration of 5 g / L;

[0044] Step 2: 95 g of aramid fiber was soaked in 1000 mL of polydopamine solution, and then the pH of the solution was adjusted to 8.5, stirred at room temperature for 24 h, filtered, and dried to prepare modified aramid fiber;

[0045] Step 3: Dissolve 30 g of modified aramid fiber and 70 g of polyimide in 1000 mL of N,N-dimethylacetamide solvent, stir at room temperature for 5 hours, then apply it on the empty foil of the current collector, and dry it to prepare a polymer insulating coating with a thickness of 12 μm.

[0046] Comparative Example 1:

[0047] Comparative Example 1 is an electrode sheet coated with a commercial ceramic coating.

[0048] Comparative Example 2:

[0049] Comparative Example 2 is an electrode sheet without coating.

[0050] The electrode sheets with insulating coatings prepared in Examples 1 to 5 and Comparative Example 1 were immersed in an electrolyte solution containing lithium hexafluorophosphate as lithium salt and ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate as solvents.

[0051] Phenomenon after electrode rolling Bond strength after immersion After 48h of electrolyte immersion Example 1 No wrinkles on the ear 41N / m The coating does not fall off or peel off Example 2 No wrinkles on the ear 44N / m The coating does not fall off or peel off Example 3 No wrinkles on the ear 51N / m The coating does not fall off or peel off Example 4 No wrinkles on the ear 33N / m The coating does not fall off or peel off Example 5 No wrinkles on the ear 43N / m The coating does not fall off or peel off Comparative Example 1 Powder falling off, slight wrinkles on the ear 4.5N / m Coating peeling Comparative Example 2 The ear is severely wrinkled / /

[0052] From the results of Examples 1 to 5 and Comparative Example 1 in the above table after immersion in the electrolyte for 48 hours, it can be seen that the polymer insulating coating of the present invention can effectively improve the wrinkles of the tabs during rolling, avoid powder loss, improve the adhesion of the coating, and has excellent electrolyte resistance.

Claims

1. A polymer insulating coating, characterized in that The invention comprises a first polymer, a second polymer and a crosslinking agent, wherein the polymer insulating coating is coated on the empty foil area of ​​the current collector of the electrode sheet; the first polymer is one or more of aramid fiber and its derivatives; the second polymer is one or more of polyimide, polyacrylonitrile, polyacrylate, polyvinylidene fluoride and polytetrafluoroethylene; the crosslinking agent is one or more of polydopamine and its derivatives; the thickness of the polymer insulating coating is 5 to 20 μm; The method for preparing the polymer insulating coating comprises the following steps: Step 1: dispersing an equivalent amount of a cross-linking agent in a solvent to prepare a cross-linking agent solution with a concentration of 1 g / L-5 g / L; Step 2: soaking the first polymer in the cross-linking agent solution prepared in step 1, then adjusting the pH of the solution to 8.5, stirring at room temperature for 5 to 24 hours, filtering, and drying to prepare a modified first polymer; Step 3, dissolving the modified first polymer and the second polymer prepared in step 2 in N,N-dimethylacetamide solvent, stirring at room temperature for 2 to 12 hours, and then coating the empty foil area of ​​the current collector of the electrode sheet, and drying to obtain a polymer insulating coating; In step 2, the mass ratio of the first polymer to the cross-linking agent is 45-49:1-5; In step three, the mass ratio of the modified first polymer to the second polymer is 2-5:5-8.