Preparation method and application of bismuth telluride micro-nano powder material

By adding ethyl acetate to the dry ball mill, the problems of material agglomeration and uneven particle size in the preparation of micro-nanothermoelectric materials were solved, and the uniform preparation of bismuth telluride micro-nano powder and the improvement of thermoelectric properties were achieved. A high-efficiency and low-energy consumption preparation method is provided.

CN115385307BActive Publication Date: 2024-11-12ZHEJIANG ADVANCED THERMOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210837107.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-15
Publication Date
2024-11-12
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

In the existing preparation methods of micro-nanothermoelectric materials, dry ball milling can easily lead to material agglomeration and uneven particle size distribution, and the equipment is expensive or energy consumption is high, making it difficult to achieve high-efficiency and low-energy batch preparation.

Method used

The method of smelting combined with ball milling is adopted to prepare tellurium by adding ethyl acetate in the dry ball milling process, taking advantage of its strong surface tension and permeability to avoid the aggregation of powder into blocks and improve the uniformity of particle size. Bismuth micro-nano powder.

Benefits of technology

It effectively avoids the phenomenon of powder aggregation and blocking in dry ball mills, improves the uniformity of powder particle size and preparation efficiency, significantly reduces the powder particle size, and improves the thermoelectric performance of the obtained bismuth telluride block. The thermoelectric superiority zT is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115385307B_ABST
    Figure CN115385307B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation of thermoelectric semiconductor materials, and specifically relates to a method for preparing bismuth telluride micro-nano powder materials, comprising crushing an alloy ingot of bismuth telluride into particles, placing the ingot in a ball mill, adding ethyl acetate for dry ball milling, discharging the material, and drying, wherein the mass ratio of bismuth telluride to ethyl acetate is ≥5:1. In the method for preparing bismuth telluride micro-nano powder of the present invention, a method of combining smelting ingots and dry ball milling is adopted, and ethyl acetate is added to assist dispersion during the ball milling process, which effectively avoids the aggregation of powders into lumps during the dry ball milling process, improves the uniformity of the powder particle size, and the preparation process is highly efficient and has low energy consumption. At the same time, after the prepared bismuth telluride micro-nano powder is prepared into a bismuth telluride block, the thermoelectric performance of the obtained bismuth telluride block is significantly improved, and the thermoelectric figure of merit is . zT Be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoelectric semiconductor material preparation, and specifically relates to a preparation method and application of bismuth telluride micro-nano powder material. Background Art

[0002] Thermoelectric materials can directly realize the conversion of heat and electricity, and have great potential in power generation and refrigeration applications. They play an important role in solving energy and environmental problems. The commonly used thermoelectric materials are mainly bismuth telluride. The thermoelectric performance of thermoelectric materials is mutually restricted by the Seebeck coefficient, electrical conductivity and thermal conductivity, and it is difficult to regulate independently. Since micro-nano powders can increase the crystal interface, resulting in increased phonon scattering, effectively reducing the thermal conductivity of the material lattice, and the degree of reduction in thermal conductivity is greater than the degree of change in electrical properties, the thermoelectric performance of the material can be enhanced.

[0003] At present, the preparation methods of micro-nano thermoelectric materials include mechanical alloying method, melt spinning method, etc. However, the equipment of melt spinning method is expensive and the energy consumption is high. The long-term ball milling of mechanical alloying method easily leads to serious powder contamination and low grain orientation. Therefore, it is particularly important to develop a method with high efficiency, low energy consumption and batch preparation of micro-nano powders. The above problems can be effectively avoided by combining smelting with ball milling. Ball milling can be divided into wet ball milling and dry ball milling. Wet ball milling requires the use of high-purity alcohol, hexane, acetone, etc. as wet milling media. Because the amount of added media is large and has a pungent odor, it is easy to cause powder oxidation during the ball milling process, and there are problems such as complicated subsequent separation. Dry ball milling does not require the introduction of a large amount of wet milling media and is easy to operate. However, during the dry ball milling process, the time is extended, and the material is prone to agglomeration and uneven particle size distribution. Summary of the invention

[0004] In view of the problems that material agglomeration and uneven particle size distribution are prone to occur during dry ball milling, the purpose of the present invention is to provide a method for preparing bismuth telluride micro-nano powder, which combines smelting with ball milling to prepare powder, and adds ethyl acetate during ball milling to avoid agglomeration during dry ball milling. The obtained bismuth telluride micro-nano powder has a uniform particle size distribution.

[0005] The present invention provides the following technical solutions:

[0006] A method for preparing a bismuth telluride micro-nano powder material comprises the following steps: crushing a bismuth telluride alloy ingot into particles, placing the particles in a ball mill, adding ethyl acetate for dry ball milling, discharging the particles, and drying the particles, wherein the mass ratio of bismuth telluride to ethyl acetate is ≥5:1.

[0007] In the preparation method of the present invention, bismuth telluride micro-nano powder is prepared by combining smelting ingot and dry ball milling. Smelting ingot can improve the uniformity of alloy components. Ethyl acetate is added during dry ball milling. The high surface tension, strong permeability and easy separation of ethyl acetate can effectively improve the powder aggregation phenomenon in dry ball milling, improve the uniformity of powder particle size, and significantly reduce the powder particle size.

[0008] As a preferred embodiment of the method of the present invention, the particle size of the crushed bismuth telluride particles is 1 to 2 mm.

[0009] As a preferred embodiment of the method of the present invention, the bismuth telluride alloy ingot is prepared by the following process:

[0010] Take Bi powder, Sb powder and Te powder according to the molar ratio of the nominal composition, weigh and mix them evenly, seal them in a vacuum quartz tube with a vacuum degree less than 2Pa, seal the tube, and then heat to 780-800℃ at a rate of 12-18℃ / min, keep warm for 1-1.5h, then shake for 2-3h, the shaking frequency is 5-8rpm / min, the shaking angle is 60°-65°, and then cool. When preparing the alloy ingot, use Bi powder, Sb powder and Te powder with a purity of 99.99%.

[0011] As a preferred method of the present invention, the mass ratio of bismuth telluride to ethyl acetate is 5 to 10: 1. The amount of ethyl acetate introduced should not be too much or too little. Too little will not have a dispersing effect and agglomeration is still likely to occur. Too much will complicate separation and the material will be easily contaminated, affecting material performance.

[0012] As a preferred embodiment of the method of the present invention, the ball-to-material ratio of the grinding balls used in the ball milling to the bismuth telluride is 2 to 3:1.

[0013] As a preferred embodiment of the method of the present invention,

[0014] The size of the grinding balls is 0.6 to 1.2 mm;

[0015] and / or the ball milling speed is 350-500 rpm / min;

[0016] And / or the single cycle grinding time is 30 to 40 minutes, grinding for 1 to 2 hours. Preferably, the grinding is carried out for at least two weeks according to the single cycle grinding time, and more preferably, the interval is about 10 to 20 minutes.

[0017] As a preferred method of the present invention, the material is dried in the following manner: spread the material out and dry it under ventilation at room temperature, then heat it to 40-50°C and dry it. The ethyl acetate dispersant has a slightly fruity odor, a low boiling point, and is easy to separate: place the discharge on a sieve to separate the grinding balls and powder, then spread the powder out and place it at a vent to dry for 10-20 minutes, and then dry it in a blast oven for 20-30 minutes.

[0018] A bismuth telluride micro-nano powder material obtained by the above preparation method. The obtained bismuth telluride micro-nano powder has uniform particle size distribution, small particle size, no agglomeration, and no pollution.

[0019] A method for improving the thermoelectric performance of a bismuth telluride block, wherein the bismuth telluride block is obtained by vacuum hot pressing and sintering the above-mentioned bismuth telluride micro-nano powder material. The zT value of the prepared bismuth telluride block at room temperature is improved.

[0020] As a preferred embodiment of the present invention, the vacuum hot pressing sintering pressure is 70-100 MPa, the sintering temperature is 420-500° C., and the hot pressing sintering time is 60-120 min.

[0021] The beneficial effects of the present invention are as follows:

[0022] In the preparation method of bismuth telluride micro-nano powder of the present invention, a method of combining smelting ingot casting and dry ball milling is adopted, and ethyl acetate is added to assist dispersion during the ball milling process, which effectively avoids the powder from agglomerating into a mass during the dry ball milling process, improves the uniformity of the powder particle size, and has high efficiency and low energy consumption during the preparation process. At the same time, after the prepared bismuth telluride micro-nano powder is prepared into a bismuth telluride block, the thermoelectric performance of the obtained bismuth telluride block is significantly improved, and the thermoelectric figure of merit zT is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a SEM image of the bismuth telluride micro-nano powder prepared in Example 1.

[0024] Figure 2 3 is a particle size distribution diagram of the bismuth telluride micro-nano powder prepared in Example 1.

[0025] Figure 3 This is a particle size distribution diagram of the bismuth telluride micro-nano powder prepared in Comparative Example 1.

[0026] Figure 4 This is a particle size distribution diagram of the bismuth telluride micro-nano powder prepared in Comparative Example 2. DETAILED DESCRIPTION

[0027] The specific implementation modes of the present invention are further described below.

[0028] Unless otherwise specified, the raw materials used in the present invention can be purchased from the market or are commonly used in the art. Unless otherwise specified, the methods in the following embodiments are all conventional methods in the art.

[0029] The present invention provides an implementation scheme of a method for preparing a bismuth telluride micro-nano powder material. Specifically, an alloy ingot of bismuth telluride is crushed into particles, placed in a ball milling device such as a ball milling jar, dry-milled with ethyl acetate, discharged, and dried, wherein the mass ratio of bismuth telluride to ethyl acetate is ≥5:1.

[0030] In some embodiments provided by the present invention, the preparation process of the bismuth telluride alloy ingot is as follows: take Bi powder, Sb powder and Te powder according to the molar stoichiometric ratio of the nominal composition, weigh and mix them evenly, seal them in a vacuum quartz tube with a vacuum degree less than 2 Pa, seal the tube, and then heat to 780-800°C at a rate of 12-18°C / min, keep warm for 1-1.5h, then shake for 2-3h, the shaking frequency is 5-8rpm / min, the shaking angle is 60°-65°, and then cool.

[0031] Preferably, the chemical formula of the alloy ingot is Bi 0.5 Sb 1.5 Te3 is prepared using Bi powder, Sb powder and Te powder with a purity of 99.99%.

[0032] In some embodiments provided by the present invention, the particle size of the crushed bismuth telluride particles is 1 to 2 mm.

[0033] In some embodiments provided by the present invention, the mass ratio of bismuth telluride to ethyl acetate is 5 to 10:1, preferably 5:1, 6:1, 7:1, 8:1, 9:1, and 10:1.

[0034] In some embodiments provided by the present invention, the ratio of grinding balls to bismuth telluride used in ball milling is 2 to 3: 1. During ball milling, the order of feeding is: weighing the crushed bismuth telluride particles into a ball mill according to a certain ratio of grinding balls to materials, and the order of feeding is first putting the grinding balls, then the crushed bismuth telluride particles, and then adding ethyl acetate, and setting the ball milling parameters.

[0035] In some embodiments provided by the present invention, the size of the grinding ball is 0.6-1.2 mm; the ball mill speed is 350-500 rpm / min; the single-cycle grinding time is 30-40 min, and the grinding is 1-2 h. Preferably, there is a time interval between two single-cycle grinding operations, the interval time is 10-20 min, preferably 10 min.

[0036] In some embodiments provided by the present invention, the material is dried by spreading the material and drying it under ventilation at room temperature, and then heating it to 40-50° C. for drying. Preferably, the wind speed of the room temperature ventilation drying is 2-3 m / s, the drying time is 10-20 min, and the heating drying time is 10-20 min.

[0037] Some embodiments provided by the present invention are bismuth telluride micro-nano powder materials obtained by the above-mentioned preparation method.

[0038] The present invention provides an implementation scheme of a method for improving the thermoelectric performance of a bismuth telluride block. Specifically, the bismuth telluride block is obtained by vacuum hot pressing and sintering the bismuth telluride micro-nano powder material obtained above.

[0039] In some embodiments provided by the present invention, the pressure of vacuum hot pressing sintering is 70-100 MPa, the sintering temperature is 420-500° C., and the hot pressing sintering time is 60-120 min.

[0040] Example 1

[0041] (1) Ingredient smelting / material preparation:

[0042] Bi powder, Sb powder and Te powder with a purity of 99.99% are prepared according to the nominal composition of Bi 0.5 Sb 1.5 The stoichiometric ratio of Te3 is weighed and evenly mixed, sealed in a vacuum quartz tube with a vacuum degree of less than 2Pa, and the quartz tube is sealed with an oxyacetylene flame, and then the temperature is raised to 780°C at a rate of 15°C / min, and then kept warm for 1h, followed by shaking for 2h, with a shaking frequency of 5rpm / min and a shaking angle of 60°, and condensed by furnace cooling to obtain a bismuth telluride alloy ingot;

[0043] (2) Crushed particles:

[0044] The alloy ingot is crushed in a jaw crusher, the jaw plate material is manganese steel, and coarse particles with a particle size of 1 to 2 mm are obtained;

[0045] (3) Dry ball milling:

[0046] The coarse material particles were put into a ball mill, which was filled with stainless steel grinding balls with a diameter of 1 mm, and the mass ratio of balls to materials was 1:1. Ethyl acetate was added to the coarse material particles, and the mass ratio of ethyl acetate to coarse material particles was 1:5. The particles were ground continuously for 2 cycles for 1 h at a speed of 400 rpm / min, a duty cycle of 1:1, and a single cycle of 30 min.

[0047] (4) Ethyl acetate separation:

[0048] After the ball milling is completed, the material is discharged and placed on a 850um sieve to separate the grinding balls and the powder. The separated powder is then placed at a vent for preliminary drying for 10 minutes at a ventilation rate of 2m / s. The powder is then placed in an oven at 50°C for drying for 10 minutes to completely remove the ethyl acetate, thereby obtaining bismuth telluride micro-nano powder with uniform particle size distribution.

[0049] The SEM image of the prepared bismuth telluride micro-nano powder is shown in Figure 1 The particle size distribution diagram is shown in Figure 2 As shown in the figure, it can be seen that the obtained bismuth telluride micro-nano powder has no aggregation and agglomeration, and the particle size distribution is uniform and within the micro-nano range, wherein D(50) is about 1.2 μm and D(100) is about 13.6 μm.

[0050] Example 2

[0051] (1) Ingredient smelting / material preparation: the same as in Example 1;

[0052] (2) Crushing and grinding: the same as in Example 1;

[0053] The alloy ingot is crushed in a jaw crusher, the jaw plate material is manganese steel, and a coarse material with a particle size of 1 to 2 mm is obtained;

[0054] (3) Dry ball milling:

[0055] The coarse material particles were put into a ball mill, which was filled with stainless steel grinding balls with a diameter of 1 mm, and the mass ratio of balls to materials was 1:1. Ethyl acetate was added to the coarse material particles, and the mass ratio of ethyl acetate to coarse material particles was 1:10. The rotation speed was 400 rpm / min, the duty cycle was 1:1, and the single cycle grinding was 40 minutes. The grinding was continued for 2 cycles of 80 minutes;

[0056] (4) Dispersant separation: Same as Example 1.

[0057] The obtained bismuth telluride micro-nano powder has no aggregation and agglomeration, and has a uniform particle size distribution within the micro-nano range, wherein D(50) is about 1.02 μm and D(100) is about 12.8 μm.

[0058] Example 3

[0059] The difference from Example 1 is that in the dry ball milling process of step (3), the interval between two single-cycle grindings is 10 minutes.

[0060] The obtained bismuth telluride micro-nano powder has no aggregation and agglomeration, and has a uniform particle size distribution within the micro-nano range, wherein D(50) is about 1.1 μm and D(100) is about 13.2 μm.

[0061] Comparative Example 1

[0062] The difference from Example 1 is that no ethyl acetate was added during the preparation process. The particle size distribution of the obtained powder is as follows: Figure 3 shown.

[0063] from Figure 2 It can be seen that the particle size distribution uniformity of the prepared bismuth telluride micro-nano powder is reduced, and aggregation occurs, wherein D(50) is about 7 μm and D(100) is about 63 μm.

[0064] Comparative Example 2

[0065] The difference from Example 1 is that alcohol is used instead of ethyl acetate in the preparation process. The particle size distribution of the powder is as follows: Figure 4 shown.

[0066] It can be seen from the figure that the obtained bismuth telluride micro-nano powder is aggregated and agglomerated, wherein D(50) is about 5.1 μm and D(100) is about 20 μm.

[0067] The bismuth telluride micro-nano powders (three parallel samples) prepared in the above embodiments and comparative examples were fed into a mold and maintained at a pressure of 100 MPa and a sintering temperature of 500°C for 100 min to obtain a bismuth telluride block. The zT value of the bismuth telluride block at room temperature of 298K was tested and calculated. The results are shown in Table 1 below.

[0068] Table 1 Thermoelectric figure of merit results of bismuth telluride bulk

[0069]

[0070] As can be seen from the above table, when no dispersing agent such as ethyl acetate is added during dry ball milling, as shown in Comparative Example 1, due to the occurrence of agglomeration, and the particle size is large and unevenly distributed, the thermoelectric merit of the resulting bismuth telluride block is 0.917 (mean), and the volatility of the zT value of the block is relatively large. After introducing ethyl acetate, as shown in Examples 1 and 2, the zT value is improved, and the volatility of the zT value is reduced. When a single cycle is ground for a period of time, as shown in Example 3, the volatility of the zT value is further reduced. When ethyl acetate is replaced by ethanol, as shown in Comparative Example 2, the zT value is slightly improved relative to Comparative Example 1, but the volatility is still relatively large, and the effect is lower than ethyl acetate. This may be because ethanol is more volatile, and permeability, etc. are not as good as ethyl acetate, which shows that the ball milling medium used for wet ball milling is more inclined to provide a kind of effect of dispersing occasions, and it cannot reach the desired effect when used in dry ball milling.

Claims

1. A method for preparing bismuth telluride micro-nano powder material, characterized in that: The bismuth telluride alloy ingot is crushed into particles, placed in a ball mill, dry-milled with ethyl acetate, discharged, and dried, wherein the mass ratio of bismuth telluride to ethyl acetate is ≥5:1; the bismuth telluride alloy ingot is Bi 0.5 Sb 1.5 Te3 is obtained by mixing Bi powder, Sb powder and Te powder and then melting and casting an ingot.

2. The method for preparing bismuth telluride micro-nano powder material according to claim 1, characterized in that: The particle size of the crushed bismuth telluride particles is 1 to 2 mm.

3. The method for preparing bismuth telluride micro-nano powder material according to claim 1 or 2, characterized in that: The alloy ingot of bismuth telluride is prepared by the following process: Take Bi powder, Sb powder and Te powder according to the molar ratio of the nominal composition, weigh and mix them evenly, seal them in a vacuum quartz tube with a vacuum degree less than 2 Pa, seal the tube, and then heat to 780-800°C at a rate of 12-18°C / min, keep warm for 1-1.5h, then shake for 2-3h, with a shaking frequency of 5-8 rpm / min and a shaking angle of 60°-65°, and then cool.

4. The method for preparing bismuth telluride micro-nano powder material according to claim 1, characterized in that: The mass ratio of bismuth telluride to ethyl acetate is 5 to 10:

1.

5. The method for preparing bismuth telluride micro-nano powder material according to claim 1, characterized in that: The ball-to-material ratio of the grinding balls used in the ball mill to the bismuth telluride is 2 to 3:

1.

6. The method for preparing bismuth telluride micro-nano powder material according to claim 5, characterized in that: The size of the grinding balls is 0.6 to 1.2 mm; and / or the ball milling speed is 350-500 rpm / min; And / or the single cycle grinding time is 30 to 40 minutes, grinding for 1 to 2 hours.

7. The method for preparing bismuth telluride micro-nano powder material according to claim 1, characterized in that: The method of drying the material is: spread the material out and dry it under ventilation at room temperature, then heat it to 40-50°C and dry it.

8. A bismuth telluride micro-nano powder material obtained by the preparation method according to any one of claims 1 to 7.

9. A method for improving the thermoelectric performance of bismuth telluride bulk, characterized in that: The bismuth telluride block is obtained by vacuum hot pressing and sintering the bismuth telluride micro-nano powder material as claimed in claim 8.

10. The method for improving the thermoelectric performance of bismuth telluride bulk according to claim 9, characterized in that: The pressure of vacuum hot pressing sintering is 70-100 MPa, the sintering temperature is 420-500°C, and the hot pressing sintering time is 60-120 min.