A SLA heat-resistant photosensitive resin for 3D printing and its preparation and use method
Through the specific formula of SLA temperature-resistant photosensitive resin and heat treatment technology, the problem of unstable performance of light-cured 3D printing materials under different seasons and humidity conditions is solved, and the material's high toughness and temperature resistance are achieved, which is suitable for large-size SLA machines. Produced in Taiwan.
Patent Information
- Application Number
- CN202211031625.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-26
AI Technical Summary
Existing light-curing 3D printing materials have unstable performance under different seasons and humidity conditions. They become soft in summer and brittle in winter, and the impact properties of high-temperature-resistant resin are poor, making it difficult to meet the production needs of large-format machines.
Using SLA temperature-resistant photosensitive resin composed of bismaleimide, epoxy monomer, acrylate monomer, epoxy resin, acrylate resin, free radical initiator, cationic initiator and defoaming agent, through specific The formula ratio and preparation method are used to prepare a low shrinkage and high toughness resin, and heat treatment is performed on the SLA machine to improve performance.
It achieves the stability of mechanical properties under four-season temperature and humidity conditions, improves the temperature resistance and toughness of the resin, is suitable for large-size SLA machine production, and ensures material stability and printing efficiency.
Smart Images

Figure CN115386049B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a photocurable resin material and a preparation method and a use method thereof, and in particular to a SLA temperature-resistant photosensitive resin for 3D printing and a preparation method and a use method thereof, and belongs to the field of new 3D printing material development. Background Art
[0002] Due to their high precision, high efficiency and simple operation methods, photocuring 3D printers and materials have a high market share in the 3D printing market. In particular, SLA printers are widely used in the prototype industry, and more and more design works are presented through 3D printing technology. With the popularization of photocuring 3D printing market applications, the performance shortcomings of adapted materials are becoming increasingly prominent. For example, in different seasons, the material properties change too much. In summer, the material becomes soft, causing the sample to deform. In winter, the material has poor toughness, causing the sample to be fragile. The high-temperature resistant resin materials on the market have poor notch impact performance and are difficult to use in actual applications. Therefore, it is urgent to develop materials with good mechanical property stability under the temperature and humidity of the four seasons, and with certain temperature resistance and toughness, while meeting the actual needs of large-format machine production - good material storage stability, high molding rate and printing efficiency, and easy operation.
[0003] A Chinese patent application with publication number CN107513247A discloses a high-temperature resistant toughened photocurable resin for 3D printing. By introducing photocuring and thermosetting free radical initiators, a dual curing method of curing and thermal curing is achieved for 3D printing, resulting in a photosensitive resin with high curing efficiency, good temperature resistance and toughness. Thermosetting initiators are sensitive to heat. During the printing process, the local temperature rise of the resin polymerization exothermic heat can easily cause the resin in the non-molding area to solidify, thereby shortening the service life of the resin in the resin tank and even affecting the accuracy of the printed parts, which brings great inconvenience to the actual operation. Therefore, this method is not suitable for large-format SLA production machines; the Chinese patent application with publication number CN109517340A discloses a heat-resistant transparent photosensitive resin for 3D printing. The optimized formula has a maximum notched impact strength of 32J / m, and the hardness is 85D and 69D at room temperature and 80°C respectively; the formula with a small hardness difference has a notched impact strength of 18-27J / m, and the resin toughness is poor. During the shoveling and washing process, the sample is easily damaged by human beings, resulting in material waste and affecting production efficiency. Although the above two patents have the effect of improving heat resistance and toughening, it is difficult to meet market requirements in terms of service life and actual use and operation. Therefore, a photosensitive resin with excellent heat resistance and suitable for large-scale machine production is urgently needed. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a SLA heat-resistant photosensitive resin for 3D printing and its preparation and use method. The heat-resistant photosensitive resin material of the present invention has low shrinkage and excellent toughness, and is suitable for most mainstream SLA machines on the market.
[0005] To achieve the above-mentioned purpose, the present invention provides a SLA temperature-resistant photosensitive resin for 3D printing, wherein the raw material composition comprises, by weight percentage: 5%-15% bismaleimide, 30%-60% epoxy monomer, 20%-40% acrylate monomer, 10%-40% epoxy resin, 10%-30% acrylate resin, 1%-3% free radical initiator, 3%-6% cationic initiator, 0.02%-0.08% defoaming agent, and the sum of the weight percentages of the raw materials is 100%.
[0006] In the above-mentioned light-curable heat-resistant resin material, preferably, the bismaleimide is BMI-80 powder produced by Japan KI Company.
[0007] In the above-mentioned light-curable heat-resistant resin material, preferably, the epoxy monomer is one or a combination of 3-ethyl-3-oxetanol and 3,3-[oxybismethylene]-bis[3-ethyl]oxetane.
[0008] In the above-mentioned photocurable heat-resistant resin material, preferably, the acrylate monomer is one or a combination of trimethylolpropane triacrylate (TMPTA), N-acryloylmorpholine (ACMO), tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA).
[0009] In the above-mentioned light-curable heat-resistant resin material, preferably, the defoaming agent is one or a combination of BYK 055 and BYK 067A.
[0010] In the above-mentioned light-curable heat-resistant resin material, preferably, the cationic initiator is one or a combination of triarylsulfonium hexafluoroantimonate and triarylsulfonium hexafluorophosphate.
[0011] In the above-mentioned light-curable heat-resistant resin material, preferably, the free radical initiator is one or a combination of acetophenone, α-hydroxyketone, α-aminoketone, bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide.
[0012] In the above-mentioned light-curing heat-resistant resin material, preferably, the epoxy resin is one or a combination of aliphatic epoxy resins UVACURE1534, UVR6110, and UVR6128.
[0013] In the above-mentioned light-curing heat-resistant resin material, preferably, the acrylate resin is one or a combination of phenolic epoxy acrylate and aromatic polyurethane acrylate.
[0014] The present invention also provides a method for preparing the above-mentioned light-curable heat-resistant resin material, which comprises the following steps:
[0015] (1) Weigh epoxy monomer, acrylate monomer, and bismaleimide in sequence and add them into a beaker, insert a temperature probe, turn on the heating plate, and stir at a low speed to obtain a mixed liquid;
[0016] (2) weighing a defoamer, a free radical initiator, a cationic initiator, an epoxy resin, and an acrylate resin in sequence and adding them to the mixed liquid of step (1), and stirring to obtain a temperature-resistant resin mixed liquid;
[0017] (3) The stirred mixed resin liquid is screened, vacuumed and defoamed to obtain the finished heat-resistant resin liquid product.
[0018] In the above preparation method, preferably, the speed of the low-speed stirring in step (1) is 300-800 r / min.
[0019] In the above preparation method, preferably, the stirring speed in step (2) is 400-1000 r / min.
[0020] In the above preparation method, preferably, the mesh size of the sieving filter in step (3) is 40-100 meshes.
[0021] In the above preparation method, preferably, the vacuum temperature in step (3) is 50-90° C. and the time is 1-3 hours.
[0022] The present invention also provides a method for using the above-mentioned light-curable heat-resistant resin material, which comprises the following steps:
[0023] (1) Scrape off the printed data model sample from the SLA machine printing platform and remove the support;
[0024] (2) After cleaning the sample in a special cleaning solution, use an air gun to blow away the surface cleaning solution;
[0025] (3) After setting the oven heating program, place the sample in the oven for heat treatment.
[0026] In the above preparation method, preferably, the temperature in step (3) is 60-300°C.
[0027] In the above preparation method, preferably, the time in step (3) is 4-12 hours.
[0028] In the above preparation method, the amounts of monomer, resin, initiator and defoamer can be adjusted routinely by those skilled in the art, as long as all raw materials can be completely mixed and in the right proportion.
[0029] The model printed by the light-curing heat-resistant resin material of the present invention has a heat deformation temperature of 80-150°C, a notched impact strength of 40-70 J / m, a high molding rate, and a smooth and delicate surface. The sample made of the resin of the present invention has stable mechanical properties and can be used as a terminal part. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 These are SEM photos of the sample printed out of the heat-resistant resin material of Example 1 before and after heat treatment.
[0031] Figure 2 These are SEM photos of the sample printed out of the heat-resistant resin material of Example 2 before and after heat treatment.
[0032] Figure 3 These are SEM photos of the sample printed out of the heat-resistant resin material of Example 3 before and after heat treatment.
[0033] Figure 4 These are SEM photos of the sample printed out of the heat-resistant resin material of Example 4 before and after heat treatment.
[0034] Figure 5 This is a photo of the tapping operation of the heat-resistant resin material printed sample of Example 3 after heat treatment. DETAILED DESCRIPTION
[0035] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0036] It should be noted that in the following examples, all raw materials used are commercially available; and all percentages mentioned are by weight. Specific embodiment 1
[0038] The present invention provides a SLA heat-resistant photosensitive resin for 3D printing, and the raw material composition thereof includes, by weight percentage: 10% of BMI-80, 33% of 3-ethyl-3-oxetanol, 15% of N-acryloylmorpholine (ACMO), 10% of tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA), 0.05% of BYK 055, 4% of triarylsulfonium hexafluoroantimonate, 2.95% of bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide, 12% of UVR6110, and 13% of novolac epoxy acrylate. The BMI-80 powder is produced by KI Company of Japan.
[0039] The above-mentioned SLA heat-resistant resin for 3D printing is prepared by the following method:
[0040] (1) 3-ethyl-3-oxetanol, ACMO, THEICTA, and BMI-80 were weighed and added to a beaker in sequence, and a temperature probe was inserted and the heating temperature was set to 70°C. The mixture was stirred at 450 r / min for 60 minutes to obtain a mixed liquid;
[0041] (2) BYK 055, triarylsulfonium hexafluoroantimonate, bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide, UVR6110, and phenolic epoxy acrylate were weighed in sequence and added to the mixed liquid of step (1), and stirred at 600 r / min for 70 minutes to obtain a heat-resistant resin mixed liquid;
[0042] (3) The stirred mixed resin liquid is sieved through a 60-mesh screen and vacuumed at 70° C. for 120 minutes to defoam, thereby obtaining the finished heat-resistant resin liquid.
[0043] The method for using the SLA heat-resistant resin for 3D printing comprises the following steps:
[0044] (1) Scrape off the printed data model sample from the SLA machine printing platform and remove the support;
[0045] (2) After cleaning the sample in a special cleaning solution, use an air gun to blow away the surface cleaning solution;
[0046] (3) Set the oven temperature program to 180°C for 5 hours, then place the sample in the oven for heat treatment.
[0047] The heat-resistant photosensitive resin was printed using the Liantai SLA printer. The SEM photos of the surface of the cured resin model before and after heat treatment are shown in the attached figure. Figure 1 As shown, after heat treatment, the resin has a flexural strength of 96 MPa, a flexural modulus of 2809 MPa, a heat deformation temperature of 97°C, and a notched impact strength of 61 J / m. Specific embodiment 2
[0049] The present invention provides a SLA heat-resistant photosensitive resin for 3D printing, and its raw material composition includes, by weight percentage:
[0050] BMI-80 12%, 3-[oxybismethylene]-bis[3-ethyl]oxetane 30%, TMPTA 15%, THEICTA 8%, BYK 055 0.05%, triarylsulfonium hexafluoroantimonate 5%, α-hydroxy ketone 1.95%, UVR6110 11%, aromatic polyurethane acrylate 18%.
[0051] The above-mentioned SLA heat-resistant resin for 3D printing is prepared by the following method:
[0052] (1) 3-[oxybismethylene]-bis[3-ethyl]oxetane, TMPTA, THEICTA, and BMI-80 were weighed in sequence and added into a beaker, a temperature probe was inserted, the heating temperature was set to 75°C, and the mixture was stirred at 500 r / min for 50 minutes to obtain a mixed liquid;
[0053] (2) BYK 055, triarylsulfonium hexafluoroantimonate, α-hydroxyketone, UVR6110, and aromatic polyurethane acrylate were weighed in sequence and added to the mixed liquid of step (1), and stirred at 700 r / min for 60 minutes to obtain a heat-resistant resin mixed liquid;
[0054] (3) The stirred mixed resin liquid is sieved through a 70-mesh screen and vacuumed at 80° C. for 110 minutes to defoam, thereby obtaining the finished heat-resistant resin liquid.
[0055] The method for using the SLA heat-resistant resin for 3D printing comprises the following steps:
[0056] (1) Scrape off the printed data model sample from the SLA machine printing platform and remove the support.
[0057] (2) After cleaning the sample in a special cleaning solution, use an air gun to blow away the surface cleaning solution.
[0058] (3) After setting the oven temperature program to 220°C for 4.5 hours, the sample is placed in the oven for heat treatment.
[0059] The heat-resistant photosensitive resin was printed using the Liantai SLA printer. The SEM photos of the surface of the cured resin model before and after heat treatment are shown in the attached figure. Figure 2 As shown, after heat treatment, the resin has a flexural strength of 116 MPa, a flexural modulus of 3142 MPa, a heat deformation temperature of 105°C, and a notched impact strength of 59 J / m. Specific embodiment 3
[0061] The invention provides an SLA heat-resistant photosensitive resin for 3D printing. The raw material composition thereof comprises, by weight percentage, 15% of BMI-80%, 25% of 3-[oxybismethylene]-bis[3-ethyl]oxetane, 22% of THEICTA, 0.05% of BYK 055, 4% of triarylsulfonium hexafluoroantimonate, 3.95% of bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide, 15% of UVR6110, and 15% of phenolic epoxy acrylate.
[0062] The above-mentioned SLA heat-resistant resin for 3D printing is prepared by the following method:
[0063] (1) Weigh 3-[oxybismethylene]-bis[3-ethyl]oxetane, THEICTA, and BMI-80 in sequence and add them into a beaker. Insert a temperature probe and set the heating temperature to 85°C. Stir at a speed of 400 r / min for 50 minutes to obtain a mixed liquid.
[0064] (2) BYK 055, triarylsulfonium hexafluoroantimonate, bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide, UVR6110, and phenolic epoxy acrylate were weighed in sequence and added to the mixed liquid of step (1), and stirred at 550 r / min for 80 minutes to obtain a heat-resistant resin mixed liquid;
[0065] (3) The stirred mixed resin liquid is sieved through a 50-mesh screen and vacuumed at 80° C. for 120 minutes to defoam, thereby obtaining the finished heat-resistant resin liquid.
[0066] The method for using the SLA heat-resistant resin for 3D printing comprises the following steps:
[0067] (1) Scrape off the printed data model sample from the SLA machine printing platform and remove the support.
[0068] (2) After cleaning the sample in a special cleaning solution, use an air gun to blow away the surface cleaning solution.
[0069] (3) After setting the oven temperature program to 260°C for 6 hours, the sample is placed in the oven for heat treatment.
[0070] The heat-resistant photosensitive resin was printed using the Liantai SLA printer. The SEM photos of the surface of the cured resin model before and after heat treatment are shown in the attached figure. Figure 3 As shown, after heat treatment, the resin has a flexural strength of 143 MPa, a flexural modulus of 3789 MPa, a heat deformation temperature of 147°C, and a notched impact strength of 43 J / m. Specific embodiment 4
[0072] The present invention provides an SLA temperature-resistant photosensitive resin for 3D printing. The raw material composition thereof includes, by weight percentage: 7% BMI-80, 30% 3-ethyl-3-oxetanol, 10% THEICTA, 12% TMPTA, 0.05% BYK 055, 3% triarylsulfonium hexafluoroantimonate, 2.95% bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide, 15% UVR6128, and 20% aromatic polyurethane acrylate.
[0073] The above-mentioned SLA heat-resistant resin for 3D printing is prepared by the following method:
[0074] (1) 3-ethyl-3-oxetanol, THEICTA, and BMI-80 were weighed and added to a beaker in sequence, and a temperature probe was inserted and the heating temperature was set to 65°C. The mixture was stirred at a speed of 400 r / min for 50 minutes to obtain a mixed liquid;
[0075] (2) BYK 055, triarylsulfonium hexafluoroantimonate, bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide, UVR6110, and aromatic polyurethane acrylate were weighed in sequence and added to the mixed liquid of step (1), and stirred at 600 r / min for 70 minutes to obtain a heat-resistant resin mixed liquid;
[0076] (3) The stirred mixed resin liquid is sieved through a 60-mesh screen and vacuumed at 65° C. for 120 minutes to defoam, thereby obtaining the finished heat-resistant resin liquid.
[0077] The method for using the SLA heat-resistant resin for 3D printing comprises the following steps:
[0078] (1) Scrape off the printed data model sample from the SLA machine printing platform and remove the support.
[0079] (2) After cleaning the sample in a special cleaning solution, use an air gun to blow away the surface cleaning solution.
[0080] (3) After setting the oven temperature program to 170°C for 8 hours, the sample is placed in the oven for heat treatment.
[0081] The heat-resistant photosensitive resin was printed using the Liantai SLA printer. The SEM photos of the surface of the cured resin model before and after heat treatment are shown in the attached figure. Figure 4 As shown, after heat treatment, the resin has a flexural strength of 87 MPa, a flexural modulus of 2247 MPa, a heat deformation temperature of 82°C, and a notched impact strength of 70 J / m.
[0082] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.
Claims
1. A SLA heat-resistant photosensitive resin for 3D printing, characterized in that: The raw material composition comprises, by weight percentage, 5%-15% of bismaleimide, 30%-60% of epoxy monomer, 20%-40% of acrylate monomer, 10%-40% of epoxy resin, 10%-30% of acrylate resin, 1%-3% of free radical initiator, 3%-6% of cationic initiator, and 0.02%-0.08% of defoamer, and the sum of the weight percentages of the raw materials is 100%. The bismaleimide is BMI-80 powder produced by Japan KI Company.
2. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The epoxy monomer is one or a combination of 3-ethyl-3-oxetane methanol and 3,3-[oxybismethylene]-bis[3-ethyl]oxetane.
3. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The acrylate monomer is one or a combination of trimethylolpropane triacrylate (TMPTA) and tris(2-hydroxyethyl)isocyanuric acid triacrylate (THEICTA).
4. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The defoaming agent is one or a combination of BYK 055 and BYK 067A.
5. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The cationic initiator is one or a combination of triarylsulfonium hexafluoroantimonate and triarylsulfonium hexafluorophosphate.
6. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The free radical initiator is one or a combination of acetophenone, α-hydroxy ketone, α-amino ketone, and bis-(2,4,6)-trimethylbenzoylphenylphosphine oxide.
7. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The epoxy resin is one or a combination of aliphatic epoxy resins UVACURE1534, UVR6110, and UVR6128.
8. The SLA heat-resistant photosensitive resin for 3D printing according to claim 1, wherein: The acrylic resin is one or a combination of phenolic epoxy acrylate and aromatic polyurethane acrylate.
9. A method for preparing the heat-resistant photosensitive resin according to any one of claims 1 to 8, comprising the following steps: (1) Weigh epoxy monomer, acrylate monomer, and bismaleimide in sequence and add them into a beaker, insert a temperature probe, turn on the heating plate, and stir at a low speed to obtain a mixed liquid; (2) weighing a defoamer, a free radical initiator, a cationic initiator, an epoxy resin, and an acrylate resin in sequence and adding them to the mixed liquid of step (1), and stirring to obtain a temperature-resistant resin mixed liquid; (3) The stirred resin mixed liquid is sieved, vacuumed and defoamed to obtain a heat-resistant resin liquid product.
10. A method for using the heat-resistant photosensitive resin according to any one of claims 1 to 8, comprising the following steps: (1) Scrape off the printed data model sample from the SLA machine printing platform and remove the support; (2) After cleaning the sample in the cleaning solution, use an air gun to blow away the cleaning solution on the surface; (3) After setting the oven heating program, place the sample in the oven for heat treatment.