A welding process for ductile iron traction motor for rail transit
Through special processes such as preheating nickel-iron electrodes, flame preheating, grinding and crater treatment, combined with tempering and aging vibration, the problem of weld cracks in the welding of dissimilar materials is solved, and good welding effects and welding stability are achieved.
Patent Information
- Application Number
- CN202211250832.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-13
AI Technical Summary
In rail transit, weld cracks often occur during the welding process of dissimilar materials between ductile iron traction motors and SUS304 stainless steel, which are difficult to effectively solve with existing welding processes.
Preheating nickel iron electrodes, flame preheating, grinding welds, arc crater filling and hemispherical percussion hammer treatment are used, combined with tempering and aging vibration, dehydrogenation treatment and heat preservation and slow cooling, and finally PT penetration testing and Rework to ensure welding quality.
It can effectively avoid weld cracks, improve welding effect, significantly improve welding toughness and fatigue resistance, and ensure welding stability and strength.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of welding technology, and in particular to a welding process for a ductile iron traction motor for rail transportation. Background Art
[0002] High-speed rail traction motor, the motor housing is TQ500-7 ductile iron, the motor junction box connection plate is SUS304 stainless steel. The welding of two different materials is called dissimilar material welding, which is a special welding process. The two materials have different material properties such as material quality, yield strength, elongation, and tensile strength. The general welding process cannot complete the welding and there will be a full-length weld crack. Therefore, a ductile iron traction motor welding process for rail transit is needed to solve this problem. Summary of the invention
[0003] The object of the present invention is to provide a welding process for a ductile iron traction motor for rail transit to solve the problems raised in the above-mentioned background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a welding process for a ductile iron traction motor for rail transit, comprising the following steps:
[0005] 1) Before welding, clean the stainless steel at the junction box position of the traction casing with alcohol;
[0006] 2) The welding room is temperature controlled by air conditioning and heating devices;
[0007] 3) Preheat the nickel-iron welding rod to 180°C in a heating furnace and measure with a contact temperature meter;
[0008] 4) Preheat the flame to 180℃ at the junction box position of the traction casing welding; measure with a contact temperature meter;
[0009] 5) Use screws to fix the junction box to the traction machine casing and then weld it. After repeated experiments, it is found that the welding needs to use the ESAB imported nickel-iron welding rod OK92.58, which has better matching with the two base materials; the length of the rivet welding point is 3 cm;
[0010] 6) After welding, grind the rivet weld seam at 2 / 3 of its height; this is beneficial to the formation of the appearance weld seam;
[0011] 7) After grinding, measure the temperature of the welding position and the base material, which should not be lower than 180°C; measure with a contact thermometer;
[0012] 8) For formal welding, for A4 welding angle and 2.5 diameter welding rod, only 1 / 3 of the length can be used. Overheating of the welding rod will cause burning, which will reduce the welding type; control the length of the welding seam;
[0013] 9) When the arc is stopped during welding, the arc pit must be filled to prevent cracks in the arc pit; after welding a section, the weld should be struck quickly with a pneumatic hammer. The end of the hammer should be hemispherical. Striking the semi-molten weld is equivalent to secondary forging, which can remove stress, improve the solidification crystal structure and solid phase change structure; improve the toughness and fatigue resistance of the weld, thereby eliminating the risk of weld cracking;
[0014] 10) After the tapping is completed, use flame to heat the welding and heat-affected zone, the temperature is greater than or equal to 300°C; quickly dehydrogenate to prevent the occurrence of hydrogen-induced cracks;
[0015] 11) Immediately after dehydrogenation treatment, heat preservation treatment is carried out, and industrial heat blanket is used for heat preservation and slow cooling until the welding is completed;
[0016] 12) Put the casing into the tempering furnace for tempering treatment. After the furnace body is tempered, the furnace temperature naturally drops below 100°C and the furnace is opened;
[0017] 13) After being fired, the casing is subjected to aging vibration to eliminate stress, refine grains and improve strength;
[0018] 14) Sandblasting after leaving the furnace to remove surface impurities;
[0019] 15) Perform PT penetration testing on the welding positions of the casing; if defects are found, perform welding repairs. Preheating must be performed before repair, and the positions where the PT penetrant has leaked must be polished off before welding.
[0020] Preferably, in step 2), the temperature is controlled above 15 degrees Celsius and the humidity is ≤30%.
[0021] Preferably, in step 8), the weld length can be 2.5-3 cm.
[0022] Preferably, in step 15), rework welding is performed, and the welding process repeats steps 1-15.
[0023] Preferably, the parent material is a traction machine casing and a junction box.
[0024] Beneficial effect: The beneficial effect of the present invention is that the welding process of ductile iron traction motor for rail transit of the present invention can effectively avoid cracks in the weld through early treatment, mid-term special process, and late special inspection and treatment, and achieve good welding effect, which is a significant improvement. DETAILED DESCRIPTION
[0025] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.
[0026] A welding process for a ductile iron traction motor for rail transit, comprising the following steps:
[0027] 1) Before welding, clean the stainless steel at the junction box position of the traction casing with alcohol;
[0028] 2) The welding room is temperature controlled by air conditioning and heating devices;
[0029] 3) Preheat the nickel-iron welding rod to 180°C in a heating furnace and measure with a contact temperature meter;
[0030] 4) Preheat the flame to 180℃ at the junction box position of the traction casing welding; measure with a contact temperature meter;
[0031] 5) Use screws to fix the junction box to the traction machine casing and then weld it. After repeated experiments, it is found that the welding needs to use the ESAB imported nickel-iron welding rod OK92.58, which has better matching with the two base materials; the length of the rivet welding point is 3 cm;
[0032] 6) After welding, grind the rivet weld seam at 2 / 3 of its height; this is beneficial to the formation of the appearance weld seam;
[0033] 7) After grinding, measure the temperature of the welding position and the base material, which should not be lower than 180°C; measure with a contact thermometer;
[0034] 8) For formal welding, for A4 welding angle and 2.5 diameter welding rod, only 1 / 3 of the length can be used. Overheating of the welding rod will cause burning, which will reduce the welding type; control the length of the welding seam;
[0035] 9) When the arc is stopped during welding, the arc pit must be filled to prevent cracks in the arc pit; after welding a section, the weld should be struck quickly with a pneumatic hammer. The end of the hammer should be hemispherical. Striking the semi-molten weld is equivalent to secondary forging, which can remove stress, improve the solidification crystal structure and solid phase change structure; improve the toughness and fatigue resistance of the weld, thereby eliminating the risk of weld cracking;
[0036] 10) After the tapping is completed, use flame to heat the welding and heat-affected zone, the temperature is greater than or equal to 300°C; quickly dehydrogenate to prevent the occurrence of hydrogen-induced cracks;
[0037] 11) Immediately after dehydrogenation treatment, heat preservation treatment is carried out, and industrial heat blanket is used for heat preservation and slow cooling until the welding is completed;
[0038] 12) Put the casing into the tempering furnace for tempering treatment. After the furnace body is tempered, the furnace temperature naturally drops below 100°C and the furnace is opened;
[0039] 13) After being fired, the casing is subjected to aging vibration to eliminate stress, refine grains and improve strength;
[0040] 14) Sandblasting after leaving the furnace to remove surface impurities;
[0041] 15) Perform PT penetration testing on the welding positions of the casing; if defects are found, perform welding repairs. Preheating must be performed before repair, and the positions where the PT penetrant has leaked must be polished off before welding.
[0042] In the present invention, in the step 2), the temperature is controlled to be above 15 degrees Celsius and the humidity is ≤30%.
[0043] In the present invention, in step 8), the weld length can be 2.5-3 cm.
[0044] In the present invention, in step 15), the rework welding is performed, and the welding process repeats steps 1-15.
[0045] In the present invention, the parent materials are traction machine casing and junction box.
[0046] The invention discloses a welding process for a ductile iron traction motor for rail transit, which can well avoid cracks in the weld and achieve good welding effect through early stage processing, mid-term special process and late stage special inspection and processing, and has significant progress.
[0047] The above specific embodiments further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0048] In the description of the present invention, it should be understood that the terms indicating orientation or positional relationship are based on orientation or positional relationship and are only used to facilitate the description of the present invention and simplify the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0049] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0050] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate positions or positional relationships based on the present invention, or the positions or positional relationships in which the product of the invention is usually placed when in use, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0051] In addition, the terms "horizontal", "vertical", "overhanging" and the like do not mean that the components are required to be absolutely horizontal or overhanging, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", and does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0052] In the present invention, unless otherwise clearly specified and limited, a first feature being above or below a second feature may include the first and second features being in direct contact, or may include the first and second features not being in direct contact but being in contact through another feature between them. Moreover, a first feature being above, above, and above a second feature includes the first feature being directly above and obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being below, below, and below a second feature includes the first feature being directly below and obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
Claims
1. A welding process for ductile iron traction motor for rail transit, characterized in that: The following steps are involved: 1) Before welding, clean the stainless steel at the junction box position of the traction casing with alcohol; 2) The welding room is temperature controlled by air conditioning and heating devices; 3) Preheat the nickel-iron welding rod to 180°C in a heating furnace and measure with a contact temperature meter; 4) Preheat the flame to 180℃ at the junction box position of the traction casing welding; measure with a contact temperature meter; 5) Use screws to fix the junction box to the traction machine casing and then weld it. After repeated experiments, it is found that the welding needs to use the ESAB imported nickel-iron welding rod OK92.58, which has better matching with the two base materials; the length of the rivet welding point is 3 cm; 6) After welding, grind the rivet weld seam at 2 / 3 of its height; this is beneficial to the formation of the appearance weld seam; 7) After grinding, measure the temperature of the welding position and the base material, which should not be lower than 180°C; measure with a contact thermometer; 8) For formal welding, welding angle A4, diameter 2.5 welding rod can only be used 1 / 3 length, controls the welding seam length; 9) When the arc is stopped during welding, the arc pit must be filled to prevent cracks in the arc pit; after welding a section, the weld should be struck quickly with a pneumatic hammer. The end of the hammer should be hemispherical. Striking the semi-molten weld is equivalent to secondary forging, which can remove stress, improve the solidification crystal structure and solid phase change structure; improve the toughness and fatigue resistance of the weld, thereby eliminating the risk of weld cracking; 10) After the tapping is completed, use flame to heat the welding and heat-affected zone, the temperature is greater than or equal to 300°C; quickly dehydrogenate to prevent the occurrence of hydrogen-induced cracks; 11) Immediately after dehydrogenation treatment, heat preservation treatment is carried out, and industrial heat blanket is used for heat preservation and slow cooling until the welding is completed; 12) Put the casing into the tempering furnace for tempering treatment. After the furnace body is tempered, the furnace temperature naturally drops below 100°C and the furnace is opened; 13) After being fired, the casing is subjected to aging vibration to eliminate stress, refine grains and improve strength; 14) Sandblasting after leaving the furnace to remove surface impurities; 15) Perform PT penetration testing on the welding positions of the casing; if defects are found, perform welding repairs. Preheating must be performed before repair, and the positions where the PT penetrant has leaked must be polished off before welding.
2. A welding process for ductile iron traction motor for rail transit according to claim 1, characterized in that: In the step 2), the temperature is controlled above 15 degrees Celsius and the humidity is ≤30%.
3. The welding process of a ductile iron traction motor for rail transit according to claim 1 is characterized in that: In step 8), the weld length can be 2.5-3 cm.
4. A welding process for a ductile iron traction motor for rail transit according to claim 1, characterized in that: In the step 15), the welding is repaired and the welding process repeats steps 1-15.
5. The welding process of ductile iron traction motor for rail transit according to claim 1 is characterized in that: The parent materials are the traction machine casing and the junction box.