A brazing method for high volume fraction SiCp / Al-based composite material and AlN ceramics
Through the combined method of active solder metallization and pressure brazing, the difficult problem of brazing of high volume fraction silicon carbide particle reinforced aluminum matrix composites and aluminum nitride ceramics is solved, high-performance connection is achieved, the process is simplified and the cost is reduced. cost.
Patent Information
- Application Number
- CN202211075729.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-02
AI Technical Summary
It is difficult to braze high volume fraction silicon carbide particle reinforced aluminum matrix composites and aluminum nitride ceramics. The existing technology has poor wettability and complex surface metallization process, resulting in poor welding quality.
A combination method of active solder metallization + pressure brazing is used, by using AgCuTi solder on the surface of AlN ceramics for metallization, and using AlCuSi solder on the surface of SiCp/Al-based composite materials for vacuum pressure brazing to form a high-volume High-performance brazing connection of fractional SiCp/Al matrix composites to AlN ceramics.
It achieves high-performance connection between high volume fraction SiCp/Al-based composite materials and AlN ceramics, reduces the problems of poor welding quality and complexity of surface metallization process, and is suitable for the field of high-power electronic packaging.
Smart Images

Figure CN115446407B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic / aluminum-based composite material dissimilar material connection, and relates to a brazing method for a high volume fraction silicon carbide particle reinforced aluminum-based composite material (SiCp / Al-based composite material) and aluminum nitride (AlN) ceramic. Background Art
[0002] High volume fraction (in this field, it is generally considered that the volume fraction is above 55%, and further in the range of 55%-70% is a high volume fraction) silicon carbide particle reinforced aluminum-based composite materials (SiCp / Al-based composite materials) have important applications in the manufacture of precision parts for aerospace optoelectronic control systems and microelectronic packaging devices due to their excellent properties such as low expansion coefficient, high thermal conductivity and low density. Aluminum nitride (AlN) ceramics are often used as heat dissipation substrates for high-density, high-power electronic packaging due to their high thermal conductivity, low dielectric constant, and thermal expansion coefficient matching the chip. Therefore, in the field of electronic packaging, there are specific application requirements for the connection of high volume fraction silicon carbide particle reinforced aluminum-based composite materials and aluminum nitride ceramics.
[0003] At present, the brazing of ordinary low volume fraction (generally less than 20%) particle reinforced aluminum-based composite materials basically uses the brazing filler metal of aluminum alloy or metallizes the surface before brazing. However, conventional aluminum alloy brazing filler metals are not suitable for high volume fraction particle reinforced aluminum-based composite materials, and surface metallization cannot obtain good brazing performance. This is because: (1) High volume fraction SiC particle reinforced aluminum-based composite materials will expose a large number of SiC particles on the surface of the composite material, and SiC particles are difficult to be wetted by conventional metal brazing fillers; (2) The oxide film on the surface of the aluminum-based composite material also leads to poor wettability. Therefore, for high volume fraction SiC particle reinforced aluminum-based composite materials, especially when the SiC volume fraction is relatively large (generally greater than 50%), the brazing of this material is very difficult.
[0004] A large part of the research work on aluminum-based composites reinforced with high volume fraction SiC particles has been concentrated in the field of soft soldering. Lei Yuzhen et al. (Welding, 2016(3): 14-17) used Sn3.0Ag0.7Cu solder to solder SiCp / 2024Al composites with a volume fraction of 45% of the reinforcing phase after surface electroplating and SiC ceramics after surface chemical copper plating at 260°C. After copper plating on the surface of the welded materials, the wettability was good and the fracture occurred at the junction of the aluminum-based composite material and the electroplated copper.
[0005] Due to poor wettability, most research work includes surface treatment technology during brazing. The pre-metallization method of ceramics, that is, the surface metallization method, includes physical vapor deposition (PVD), chemical vapor deposition (CVD), thermal spraying, chemical deposition, ultrasonic method and plasma implantation, etc. However, the process is complicated, which limits its industrial application.
[0006] The ultrasonic assisted brazing method uses ultrasonic vibration to remove the surface oxide film and achieves wetting of ceramics in an atmospheric environment without using a brazing flux (Zhang Yang, Ultrasonic brazing of high volume fraction SiC particle reinforced aluminum matrix composites, Welding, 2008, (8) 29-31).
[0007] Pressurized vacuum brazing. Niu Jitai et al. (Vacuum brazing of aluminium metal matrix composite (55 vol% SiCp / A356) using aluminium-based filler alloy, Materials Science and Engineering B, 2012, 177: 1707-1711) studied the vacuum brazing of aluminium-based composite materials containing 55 volume% SiC particles, and improved the brazing performance by applying pressure and adding elements such as Mg, Ti, and Ni to the brazing filler.
[0008] The active element brazing method adds active elements such as Ti, Zr, Hf, Nb, Cr, Mg, V, etc. to the brazing alloy, decomposes the ceramic surface through chemical reaction, forms a reaction layer, and can be wetted by metal. This brazing method is simple in process, low in cost, and has low welding stress. It is a method with broad application prospects. Wang Peng et al. (Preparation and brazing process of aluminum-based brazing material for high volume ratio SiCp / 6063Al composite material, Materials Guide B: Research, 2017, 31: 69-90) prepared (Al-10Si-20Cu-0.05Ce)-1Ti quenched foil brazing material by fast stripping technology, and carried out vacuum brazing experiments on SiCp / 6063Al composite material with a volume fraction of 60%, and obtained a shear strength of 112.6MPa under the brazing specification of 590℃ insulation for 30min.
[0009] Regarding AlN ceramic brazing, patents and literature are mostly focused on the interface bonding problems between aluminum nitride copper-clad boards and aluminum nitride and copper. Most of them improve the bonding strength with the copper substrate by metallizing the surface of AlN ceramics. For example, the patent "An aluminum nitride ceramic copper-clad substrate and its preparation method" (CN201010141328.7) provides a preparation method for an aluminum nitride ceramic copper-clad substrate. A metal mixture coating is first formed on an aluminum nitride ceramic substrate by magnetron sputtering, and then a metal modified layer is formed by high-temperature sintering to effectively improve the good bonding between aluminum nitride and copper foil.
[0010] There are currently no relevant reports or published patents on the brazing of dissimilar materials between aluminum-based composites reinforced with high volume fraction SiC particles and AlN ceramics. However, it is conceivable that the brazing wettability of aluminum-based composites reinforced with high volume fraction SiC particles is already very poor, and the wettability of AlN ceramic materials is also very poor. At the same time, the physical and chemical properties of aluminum-based composites are very different. It is very difficult to achieve interfacial metallurgical bonding of these two difficult-to-weld materials at the same time. Summary of the invention
[0011] In view of the above situation of the prior art, the purpose of the present invention is to provide a brazing method for a high volume fraction SiCp / Al-based composite material and an AlN ceramic, so as to solve the problems of poor welding quality and complex surface metallization process of the existing high volume fraction SiCp / Al-based composite material, and form a high-performance brazing connection between the high volume fraction SiCp / Al-based composite material and the AlN ceramic.
[0012] The purpose of the present invention is achieved through the following technical measures:
[0013] A brazing method for a high volume fraction SiCp / Al-based composite material and AlN ceramics is achieved by adopting a combined method of active brazing filler metallization + pressure brazing. First, the AlN ceramic surface is metallized using AgCuTi active brazing filler metal, and then the AlN ceramic metallized surface and the SiCp / Al-based composite material are vacuum pressure brazed using AlCuSi brazing filler metal, thereby achieving heterogeneous connection between the high volume fraction SiCp / Al-based composite material and the AlN ceramic.
[0014] The specific steps are as follows: firstly, the surface of the AlN ceramic to be welded is polished on 800#-1000# sandpaper, and then ultrasonically cleaned in an acetone solution; the AgCuTi solder foil is attached to the surface of the AlN ceramic to be welded, so that the AgCuTi solder foil completely covers the surface of the AlN ceramic to be welded, and the thickness is uniform. The thickness of the AgCuTi solder foil is preferably 30μm-50μm. If the thickness is higher than this range, the pre-metallized ceramic substrate will be deformed. If the thickness is lower than this range, defects are likely to occur in the metallized layer, and the preparation of the solder foil is difficult. In addition, the composition of the AgCuTi solder can be Ag-(20-40%)Cu-(1-8%)Ti (wherein the percentage is mass percentage). Then put the assembled AlN ceramic into a vacuum brazing furnace with a holding temperature of 840°C to 900°C, which corresponds to the composition of the brazing material. After the brazing material is selected, the optimal temperature range for brazing is determined. The holding time is more than 10 minutes, preferably 10 minutes to 30 minutes. If the holding time is too long, the reaction time is too long, and the reaction between the brazing material and the ceramic surface is too strong, which will reduce the joint strength of the AlN and aluminum-based composite materials. Cool to below 400°C at a cooling rate not higher than 5°C / min, and cool to room temperature with the furnace. The AgCuTi solder alloy reacts with the AlN ceramic to form a metallurgical bond, thereby achieving surface metallization of the aluminum nitride ceramic with high bonding strength; the surface of the SiCp / Al-based composite material to be welded is polished on 800#~1000# sandpaper, and is ultrasonically cleaned in an acetone solution; an AlCuSi or AlSiMg solder foil with a thickness of 50μm~150μm is clamped between the AlN metallized surface and the SiCp / Al-based composite material, and the thickness of the AlCuSi or AlSiMg solder foil is preferably 50μm~150μm. If the solder foil is too thick, the residual stress of the joint after welding is too large, which is easy to cause cracking, while if it is too thin, it is easy to cause defects caused by the lack of solder. The assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 560°C to 600°C and pressurized for holding for more than 5 minutes, preferably 5 minutes to 20 minutes, and a pressure of 1MPa to 2MPa. After the holding is completed, it is cooled to below 300°C at a cooling rate not higher than 5°C / min, and then cooled to room temperature with the furnace to obtain a brazing joint of the SiCp / Al-based composite material and the AlN ceramic.
[0015] The present invention solves the problems of poor welding quality and complex surface metallization process of existing high volume fraction SiCp / Al-based composite materials, and can meet the brazing requirements of high volume fraction SiCp / Al-based composite materials and AlN ceramics in the field of high-power electronic packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1It is an electron microscope photograph of the brazed joint between the SiCp / Al-based composite material and the AlN ceramic obtained according to Example 1 of the present invention. DETAILED DESCRIPTION
[0017] In order to more clearly understand the purpose, technical solutions and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0018] The brazing method of a high volume fraction silicon carbide particle reinforced aluminum-based composite material and aluminum nitride ceramic of the present invention is realized by a combined method of active brazing filler metallization + pressure brazing, and the specific steps are firstly polishing the AlN surface to be welded on 800#~1000# sandpaper, and ultrasonically cleaning it in an acetone solution; attaching a commercial AgCuTi brazing filler foil with a thickness of 30μm~50μm to the surface of the AlN ceramic to be welded, so that the brazing filler foil completely covers the surface of the AlN ceramic to be welded, and the thickness is consistent. Then, the assembled AlN ceramic is placed in a vacuum brazing furnace, the holding temperature is 840℃~900℃, the holding time is 10min~30min, and it is cooled to below 400℃ at a cooling rate not higher than 5℃ / min, and then cooled to room temperature with the furnace. AgCuTi solder alloy reacts with AlN ceramics to form metallurgical bonding, thereby achieving surface metallization of AlN ceramics with high bonding strength; the surface of the SiCp / Al-based composite material to be welded is polished on 800#~1000# sandpaper and ultrasonically cleaned in acetone solution; AlCuSi or AlSiMg solder foil with a thickness of 50μm~150μm is clamped between the AlN metallized surface and the SiCp / Al-based composite material. The assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 560℃~600℃, a holding time of 5min~20min, and a pressure of 1MPa~2MPa. After the holding is completed, it is cooled to below 300℃ at a cooling rate not higher than 5℃ / min, and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0019] Embodiment 1:
[0020] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 60%.
[0021] (1) Polish the AlN ceramic surface to be welded on 1000# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0022] (2) A 30 μm thick Cusil-ABA (Ag-35.25Cu-1.75Ti (mass fraction, %) brazing foil is attached to the AlN surface to be welded, so that the brazing foil completely covers the AlN ceramic surface to be welded and has a uniform thickness. Then the assembled AlN ceramic is placed in a vacuum brazing furnace at a holding temperature of 880°C for 10 min, cooled to below 400°C at a cooling rate of no more than 5°C / min, and then cooled to room temperature along with the furnace;
[0023] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0024] (4) A brazing foil with a thickness of 100 μm and a brazing grade of B-Al67CuSi is clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material, and the assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 570°C for 10 min and a pressure of 1.5 MPa. After the holding is completed, it is cooled to below 300°C at a cooling rate of 5°C / min, and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0025] The electron microscope photograph of the brazed joint of the SiCp / Al-based composite material and the AlN ceramic obtained in this example is shown in FIG. Figure 1 As shown, the electron microscope photographs of the brazed joints of SiCp / Al-based composite materials and AlN ceramics obtained in the subsequent embodiments are similar to those of this embodiment and are not shown in the figure again.
[0026] Embodiment 2:
[0027] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 60%.
[0028] (1) Polish the AlN surface to be welded on 1000# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0029] (2) A 30 μm thick Ticusil (Ag-26.7Cu-4.5Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil completely covers the surface of the AlN ceramic to be welded and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace with a holding temperature of 880°C for 10 min, cooled to below 400°C at a cooling rate of no more than 5°C / min, and then cooled to room temperature along with the furnace;
[0030] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0031] (4) A brazing material foil with a thickness of 100 μm and a grade of B-Al86CuSi is clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 570°C for 10 min and a pressure of 1.5 MPa. After the holding is completed, it is cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0032] Embodiment 3:
[0033] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 65%.
[0034] (1) Polish the AlN surface to be welded on 1000# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0035] (2) A 50 μm thick Cusil-ABA (Ag-35.25Cu-1.75Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil completely covers the surface of the AlN ceramic to be welded and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace with a holding temperature of 890°C for 10 min, cooled to 400°C at a cooling rate of no more than 5°C / min, and then cooled to room temperature with the furnace;
[0036] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0037] (4) A brazing material foil with a thickness of 100 μm and a grade of B-Al86SiMg was clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample was placed in a vacuum diffusion furnace with a holding temperature of 570°C for 10 min and a pressure of 2.0 MPa. After the holding temperature was completed, it was cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0038] Embodiment 4:
[0039] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 65%.
[0040] (1) Polish the AlN surface to be welded on 1000# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0041] (2) A 50 μm thick Ticusil (Ag-26.7Cu-4.5Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil completely covers the surface of the AlN ceramic to be welded and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace with a holding temperature of 890°C for 10 min, cooled to 400°C at a cooling rate of no more than 5°C / min, and then cooled to room temperature with the furnace;
[0042] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0043] (4) A brazing material foil with a thickness of 100 μm and a grade of B-Al88SiMg was clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample was placed in a vacuum diffusion furnace with a holding temperature of 570°C for 10 min and a pressure of 2.0 MPa. After the holding temperature was completed, it was cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0044] Embodiment 5:
[0045] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 70%.
[0046] (1) Polish the AlN surface to be welded on 1000# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0047] (2) A 30 μm thick Cusil-ABA (Ag-35.25Cu-1.75Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil completely covers the surface of the AlN ceramic to be welded and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace with a holding temperature of 880°C for 10 min, cooled to 400°C at a cooling rate of no more than 5°C / min, and then cooled to room temperature with the furnace;
[0048] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0049] (4) A brazing material foil with a thickness of 120 μm and a grade of B-Al67CuSi is clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 580°C for 10 min and a pressure of 2.0 MPa. After the holding is completed, it is cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0050] Embodiment 6:
[0051] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 70%.
[0052] (1) Polish the AlN surface to be welded on 800# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0053] (2) A 30 μm thick Ticusil (Ag-26.7Cu-4.5Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil is completely covered with the AlN ceramic and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace at a holding temperature of 880°C for 10 min, cooled to 400°C at a cooling rate of no more than 5°C / min, and then cooled to room temperature along with the furnace;
[0054] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0055] (4) A brazing material foil with a thickness of 120 μm and a grade of B-Al86CuSi is clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 580°C for 10 min and a pressure of 2.0 MPa. After the holding is completed, it is cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0056] Embodiment 7:
[0057] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 55%.
[0058] (1) Polish the AlN surface to be welded on 1000# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0059] (2) A 50 μm thick Cusil-ABA (Ag-35.25Cu-1.75Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil is completely covered with the AlN ceramic and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace at a holding temperature of 900 °C for 10 min, cooled to 400 °C at a cooling rate of no more than 5 °C / min, and then cooled to room temperature with the furnace;
[0060] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0061] (4) A brazing material foil with a thickness of 80 μm and a grade of B-Al67CuSi is clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample is placed in a vacuum diffusion furnace with a holding temperature of 570°C for 10 min and a pressure of 1.5 MPa. After the holding is completed, it is cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0062] Embodiment 8:
[0063] The volume fraction of SiC ceramic particles in the high volume fraction SiCp / Al-based composite material described in this embodiment is 55%.
[0064] (1) Polish the AlN surface to be welded on 800# sandpaper and clean it by ultrasonic cleaning in acetone solution;
[0065] (2) A 50 μm thick Ticusil (Ag-26.7Cu-4.5Ti (mass fraction, %) brazing foil is attached to the surface of the AlN ceramic to be welded, so that the brazing foil is completely covered with the AlN ceramic and the thickness is consistent. Then the assembled AlN ceramic is placed in a vacuum brazing furnace at a holding temperature of 900 °C for 10 min, cooled to 400 °C at a cooling rate of no more than 5 °C / min, and then cooled to room temperature along with the furnace;
[0066] (3) The surface of the SiCp / Al-based composite material to be welded was polished on 1000# sandpaper and then ultrasonically cleaned in acetone solution;
[0067] (4) A brazing material foil with a thickness of 80 μm and a grade of B-Al86SiMg was clamped between the metallized surface of the AlN ceramic and the SiCp / Al-based composite material. The assembled sample was placed in a vacuum diffusion furnace with a holding temperature of 570°C for 10 min and a pressure of 1.5 MPa. After the holding temperature was completed, it was cooled to 300°C at a cooling rate of 5°C / min and then cooled to room temperature with the furnace to obtain a brazed joint between the SiCp / Al-based composite material and the AlN ceramic.
[0068] Compared with the prior art, the method of the present invention has the following advantages:
[0069] 1. Ceramic surface metallization does not require complex surface metallization processes such as chemical plating, magnetron sputtering, ion implantation, and expensive metallization equipment. It only requires a vacuum brazing furnace, which is easy to implement and low in cost.
[0070] 2. The metallization layer of AgCuTi on the surface of AlN ceramics is closely metallurgically bonded to the ceramic matrix, the bonding strength of the connection surface is high, and the thermal conductivity of the AgCu matrix is good, which can effectively solve the problem of poor wettability or non-wetting of low-temperature solder on the ceramic surface;
[0071] 3. AlCuSi or AlSiMg brazing filler metallized AlN was brazed with high volume fraction silicon carbide particle reinforced aluminum-based composites. The brazing temperature can be as low as 560°C. This brazing filler metal has a low melting point in the Al-based brazing filler system and a wider range of applications. At the same time, the relatively low welding temperature has less effect on the performance of the aluminum-based composite matrix.
[0072] 4. When brazing AlN metallized with AlCuSi brazing filler metal and aluminum-based composite materials reinforced with high volume fraction silicon carbide particles, it is preferred to apply a small pressure (1MPa to 2MPa as mentioned above). Under the action of this pressure, the contact area between the brazing filler metal and the material to be welded can be increased, and the flatness requirements for the connection surface are reduced, which effectively saves the ceramic metallization surface grinding process, making it more economical and operable in engineering applications.
[0073] 5. The AlCuSi solder contains a certain amount of Cu element, which is more conducive to the formation of good metallurgical bonding between the Ag and Cu in the AlN metallization layer and the Al matrix in the aluminum-based composite material, avoiding excessive reaction.
Claims
1. A brazing method for high volume fraction SiCp / Al-based composite materials and AlN ceramics, include: Firstly, the AlN ceramic surface is metallized by using AgCuTi active brazing filler metal: the AgCuTi brazing filler metal foil is attached to the AlN ceramic surface to be welded, so that the AgCuTi brazing filler metal foil completely covers the AlN ceramic surface to be welded and has a uniform thickness, and then the assembled AlN ceramic is placed in a vacuum brazing furnace, the holding temperature is 840°C to 900°C, the holding time is 10min to 30min, and after cooling to below 400°C at a cooling rate not higher than 5°C / min, the AlN ceramic is cooled to room temperature along with the furnace, wherein the composition of the AgCuTi brazing filler metal is Ag-20-40%Cu-1-8%Ti, and the percentages are by mass percentage; Then, the AlN ceramic metallized surface is connected to the SiCp / Al-based composite material by vacuum pressure brazing using AlCuSi or AlSiMg brazing filler metal, thereby realizing heterogeneous connection between the high volume fraction SiCp / Al-based composite material and the AlN ceramic.
2. The soldering method according to claim 1, wherein the thickness of the AgCuTi solder foil is 30 μm to 50 μm.
3. The brazing method according to claim 1 further comprises a pretreatment step of polishing the surface of the AlN ceramic to be welded on 800# to 1000# sandpaper and ultrasonically cleaning it in an acetone solution.
4. The brazing method according to claim 1, wherein the vacuum pressure brazing connection of the AlN ceramic metallized surface and the SiCp / Al-based composite material by using AlCuSi or AlSiMg brazing filler metal comprises clamping the AlCuSi or AlSiMg brazing filler metal foil between the AlN metallized surface and the SiCp / Al-based composite material, and then placing them together in a vacuum diffusion furnace for pressurization and insulation, the insulation temperature is 560°C to 600°C, the insulation time is 5min to 20min, and after the insulation is completed, cooling to below 300°C at a cooling rate not higher than 5°C / min, and then cooling to room temperature with the furnace.
5. The brazing method according to claim 4, wherein the thickness of the AlCuSi or AlSiMg brazing material foil is 50 μm to 150 μm.
6. The brazing method according to claim 4, wherein the pressure during pressurization and heat preservation is 1 MPa to 2 MPa.
7. The brazing method according to claim 4 further comprises a pretreatment step of polishing the surface of the SiCp / Al-based composite material to be welded on 800#-1000# sandpaper and ultrasonically cleaning it in an acetone solution.
Citation Information
Patent Citations
Aluminium nitride ceramic copper-clad substrate and preparation method thereof
CN102208371A
Method for connecting AlN (aluminum nitride) ceramics and SiC / Al composite material respectively plated with thin-film metal layer on surface
CN102009240A
Production of aln / cu clad base plate
JP1992170373A