Preparation method, product and application of high-performance photothermal nanofluid derived from waste cutting fluid

By combining waste cutting liquid with photothermal conversion nanomaterials, high-performance photothermal nanofluids are prepared, which solves the problems of low photothermal conversion efficiency and difficulty in resource utilization of waste liquids by directly absorbing solar collectors, and achieves high-efficiency photoelectricity Low-cost solutions for heat conversion and environmental protection.

CN115449354BActive Publication Date: 2024-11-01SHAANXI HIGH TECH ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211033410.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-11-01
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

In the prior art, the photothermal conversion efficiency of the direct absorption solar heat collector is limited by the low-light absorption capacity of conventional fluid working fluids, and the liquid components in the waste cutting liquid are difficult to purify, which limits its resource utilization.

Method used

By combining the waste cutting liquid with a standstill settlement and high-speed centrifugation, and combining it with photothermal conversion nanomaterials (such as nanocarbon materials, metal nanoparticles, non-metallic nanoparticles, etc.), a stable high-performance photothermal nanofluid is prepared. Its excellent dispersion and heat transfer properties are used to improve the photothermal conversion efficiency.

Benefits of technology

It significantly improves the light absorption rate and photothermal conversion performance of photothermal nanofluids, realizes efficient utilization of waste cutting liquid, reduces production costs, and has good product stability. It is suitable for direct absorption solar collectors and photothermal seawater. Desalination and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115449354B_ABST
    Figure CN115449354B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method, product and application of a high-performance photothermal nanofluid derived from waste cutting fluid, comprising the following steps: (1) standing and settling: standing the waste cutting fluid slurry to allow large-sized solid particles to settle naturally, and taking the upper liquid portion; (2) centrifugation: further separating the upper liquid obtained in step (1) by high-speed centrifugation to remove unstable suspended particles and obtain an extremely stable base liquid; (3) adding photothermal conversion nanomaterials to the centrifuged base liquid, and obtaining a stable photothermal nanofluid after uniform dispersion. The product prepared by the above method exhibits strong light absorption characteristics and efficient photothermal conversion performance within the wavelength range of the solar spectrum, and has excellent dispersion stability. The present invention can not only effectively alleviate the emission pollution of cutting waste fluid, but can also be applied to fields such as direct absorption solar collectors, and is an energy-saving and emission-reduction technology with great application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photothermal conversion and waste liquid recycling, and in particular to a preparation method, product and application of a high-performance photothermal nanofluid derived from waste cutting fluid. Background Art

[0002] Effective use of clean renewable energy such as solar energy is an urgent need for low-carbon energy transformation. Studies have shown that in the energy distribution of solar radiation, wavelengths between 0.15 and 4 μm account for more than 99%, and are mainly distributed in the visible and infrared light bands. Making full use of sunlight in this band for photothermal conversion is one of the mainstream technologies for direct use of solar energy by humans. Solar thermal conversion technology can be divided into indirect absorption and direct absorption. Compared with indirect absorption technology, direct absorption solar collectors have lower heat loss, but the light absorption capacity of conventional fluid working fluids is weak, which limits the development of direct absorption solar collectors. The photothermal nanofluid obtained by mixing photothermal conversion nanomaterials and base fluids has excellent solar light absorption performance and can significantly improve the photothermal conversion efficiency of liquid working fluids. It can be seen that the preparation of low-cost, high-performance photothermal nanofluids is the key to improving direct absorption solar collectors and one of the difficulties in promoting solar thermal conversion technology.

[0003] On the other hand, whether it is the semiconductor chip or solar cell industry, cutting single crystal silicon into silicon wafers is an indispensable process. In the process of cutting crystalline silicon, wire cutting technology is generally used, and the silicon carbide abrasive is driven by a metal wire in the cutting fluid for cutting. Along with the cutting process, silicon powder and metal shavings will gradually accumulate in the cutting fluid, causing the properties of the cutting fluid to change, and eventually become waste slurry and lose its use value. There is no doubt that waste cutting fluid is an inevitable product in the process of producing silicon wafers. It is a mixture of various substances, mainly including polyols (such as polyethylene glycol, propylene glycol, etc.), silicon carbide abrasives, silicon powder, metal shavings, water and other impurities. With the vigorous development of the semiconductor and photovoltaic new energy industries, the amount of waste cutting fluid generated is increasing accordingly. The recycling of waste cutting fluid can create economic benefits for enterprises on the one hand, and on the other hand, it can also alleviate the pollution of waste liquid discharge, which has important environmental significance. The technology for recycling and resource utilization of solid components in waste cutting fluid is relatively mature; however, it is difficult to purify the liquid component. If we can turn waste into treasure and cleverly utilize its many advantages such as dispersing and lubricating properties to synthesize high value-added products, it will effectively promote the comprehensive recycling and utilization of waste cutting fluid, and its application prospects are very broad. Summary of the invention

[0004] In order to overcome the above technical problems, the purpose of the present invention is to provide a preparation method, product and application of high-performance photothermal nanofluid derived from waste cutting fluid. The waste cutting fluid generated in the silicon wafer processing process is treated as a base liquid and combined with photothermal conversion nanomaterials to prepare a low-cost, high-performance nanofluid.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a high-performance photothermal nanofluid derived from waste cutting fluid comprises the following steps;

[0007] (1) Standing sedimentation: The waste cutting fluid slurry is allowed to stand to allow large-sized solid particles to settle naturally, and the liquid portion of the upper layer is taken;

[0008] (2) Centrifugation: The upper layer of liquid obtained in step (1) still contains solid particles. High-speed centrifugation is used to further separate the solid and liquid to remove unstable suspended particles, thereby obtaining an extremely stable base liquid (no solid sedimentation after 12 months of storage);

[0009] (3) Add a certain proportion of photothermal conversion nanomaterials to the centrifuged base liquid, and use a homogenizer or ultrasonic oscillation to evenly disperse the photothermal conversion nanomaterials to obtain a stable photothermal nanofluid.

[0010] The waste cutting fluid in step (1) is waste liquid generated by cutting crystalline silicon and the like in industries such as semiconductor chips or solar panels, and mainly comprises polyols (alcohols such as polyethylene glycol and propylene glycol), water, silicon powder, iron filings, dispersants, silicon carbide and other ingredients.

[0011] In step (2), the centrifugal process uses a rotation speed of 100 rpm to 10000 rpm. The base liquid after centrifugation is a stable and easy-flowing liquid, and there is no precipitation and stratification phenomenon within 12 months of standing. According to the use requirements, water and other additives can be added to the base liquid to adjust the viscosity and other parameters of the liquid.

[0012] The photothermal conversion nanomaterial in step (3) is one or more combinations of nanocarbon materials (carbon nanotubes, graphene, etc.), metal nanoparticles (gold, silver, etc.), non-metallic nanoparticles (antimony tin oxide, molybdenum oxide, cesium tungsten bronze, copper oxide, etc.) and organic light absorbing materials.

[0013] Different types of photothermal nanofluids can be obtained according to the types of photothermal conversion nanomaterials added.

[0014] The addition ratio of the photothermal conversion nanomaterial in the base liquid is adjustable, and the mass ratio is in the range of 0.05wt%-5wt%, which can make the photothermal nanofluid have excellent light absorption characteristics in different bands and improve its photothermal conversion efficiency.

[0015] In the step (3), a dispersion method is selected according to the selected photothermal conversion nanomaterial, including shearing homogenization, ultrasonic oscillation, mechanical stirring, etc., so that the photothermal conversion nanomaterial is finally stably dispersed in the base liquid to obtain the product.

[0016] A photothermal nanofluid product prepared based on the above method has excellent light absorption rate and efficient photothermal conversion performance within the wavelength range of the solar spectrum. The product has good fluidity and is stable without precipitation.

[0017] The stable photothermal nanofluid prepared according to the above method is used in direct absorption solar thermal collectors, photothermal seawater desalination and other solar thermal utilization fields.

[0018] Beneficial effects of the present invention:

[0019] The present invention obtains a base liquid from waste silicon wafer cutting fluid by a simple treatment method, giving full play to the intrinsic characteristics of the liquid component (such as excellent dispersion performance, heat transfer performance, lubrication performance, etc.), and as a dispersion medium for photothermal nanomaterials, significantly improving the utilization rate and added value of waste cutting fluid. In addition, the photothermal nanofluid product prepared by the present invention has outstanding light absorption capacity and photothermal conversion performance, and has excellent dispersion stability. In addition, the product prepared by the present invention is environmentally friendly, low-cost, and easy to mass produce, and is an ideal material in the field of solar thermal utilization.

[0020] The present invention converts waste cutting fluid into valuables in a low-cost, simple and gentle manner, which can not only effectively alleviate the emission pollution of waste cutting fluid, but can also be applied to fields such as direct absorption solar collectors. It is an energy-saving and emission-reduction technology with great application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a process flow chart for preparing photothermal nanofluid from waste cutting fluid.

[0022] Figure 2 It is the base liquid obtained after centrifugation of waste cutting fluid. After being placed for 12 months, the liquid is stable without stratification and precipitation.

[0023] Figure 3 The spectral transmittance diagram of the base liquid obtained after the waste cutting liquid is centrifuged. By comparing the thickness of different liquids, it can be seen that the pure base liquid has poor absorption of infrared light with a wavelength greater than 800 nanometers.

[0024] Figure 4 The spectral transmittance diagram of the photothermal nanofluid prepared by adding antimony tin oxide (ATO) nanoparticles to the base liquid shows that it has a broad spectrum of light absorption capability within the wavelength range of 250-2500 nanometers.

[0025] Figure 5 The photothermal conversion performance of the photothermal nanofluid prepared by adding antimony tin oxide (ATO) nanoparticles to the base liquid is excellent. After being irradiated by sunlight, the nanofluid has a significant heating ability.

[0026] Figure 6 The XRD spectrum of the ATO nanoparticles used in Example 1, the nanoparticles have a typical ATO material crystal structure and are high in purity. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with embodiments.

[0028] Embodiment 1:

[0029] (1) The waste cutting fluid generated by a company producing silicon wafers was left to stand for 3 days to allow the solid part to settle naturally, and the liquid part on the top was taken;

[0030] (2) The upper layer liquid in step (1) is placed in a centrifuge tube and centrifuged at 5000 rpm to obtain a stable base liquid after solid-liquid separation.

[0031] (3) adding 2% by mass of ATO nanoparticles to the centrifuged base liquid, and mixing the above liquids evenly using a homogenizer to obtain a photothermal nanofluid; Figure 1 shown.

[0032] Figure 2 The base liquid obtained by centrifuging the waste cutting liquid shown is stable after being placed for 12 months, without stratification and precipitation.

[0033] contrast Figure 3 and Figure 4 It can be seen that the base liquid obtained by centrifugation has good absorption performance in the visible light band, but weak light absorption performance in the infrared band. After adding ATO nanoparticles to prepare nanofluid, the light absorption performance is significantly improved. The photothermal nanofluid with a thickness of only 2mm almost completely absorbs light in the wavelength range of 250-2500nm. Figure 5 As shown, the temperature of the nanofluid prepared with ATO nanoparticles rose to 52°C after 10 minutes of sunlight exposure, showing excellent photothermal conversion ability. Figure 6 This is the XRD spectrum of the ATO nanoparticles used in this example. The nanomaterial is a crystalline powder with high purity.

[0034] Embodiment 2:

[0035] (1) The waste cutting fluid generated by a company producing silicon wafers was left to stand for 7 days to allow the solid part to settle naturally, and the liquid part on the top was taken;

[0036] (2) The upper layer liquid in step (1) is placed in a centrifuge tube and centrifuged at 1000 rpm to obtain a stable base liquid after solid-liquid separation.

[0037] (3) Add 1% by mass of molybdenum oxide nanoparticles to the centrifuged base liquid, and use a homogenizer to mix the above liquids evenly to obtain a photothermal nanofluid.

[0038] Embodiment 3:

[0039] (1) The waste cutting fluid generated by a company producing silicon wafers was left to stand for 2 days to allow the solid part to settle naturally, and the liquid part on the top was taken;

[0040] (2) The upper layer liquid in step (1) is placed in a centrifuge tube and centrifuged at 9000 rpm using a centrifuge to obtain a stable base liquid after solid-liquid separation.

[0041] (3) Adding 0.5% by mass of cesium tungsten bronze nanoparticles to the centrifuged base liquid, and using ultrasonic oscillation to mix the above liquids evenly to obtain a photothermal nanofluid.

[0042] Embodiment 4:

[0043] (1) The waste cutting fluid generated by a company producing silicon wafers was left to stand for 3 days to allow the solid part to settle naturally, and the liquid part on the top was taken;

[0044] (2) The upper layer liquid in step (1) is placed in a centrifuge tube and centrifuged at 5000 rpm to obtain a stable base liquid after solid-liquid separation.

[0045] (3) Adding 1% by mass of carbon nanotube dispersion to the centrifuged base liquid, and mixing the above liquids evenly using ultrasonic oscillation to obtain a photothermal nanofluid.

[0046] Embodiment 5:

[0047] (1) The waste cutting fluid generated by a company producing silicon wafers was left to stand for 3 days to allow the solid part to settle naturally, and the liquid part on the top was taken;

[0048] (2) The upper layer liquid in step (1) is placed in a centrifuge tube and centrifuged at 5000 rpm to obtain a stable base liquid after solid-liquid separation.

[0049] (3) Add 0.5% by mass of copper oxide nanopowder to the centrifuged base liquid, and use ultrasonic oscillation to mix the above liquid evenly to obtain a photothermal nanofluid.

[0050] Application Examples

[0051] Due to its excellent light absorption ability, photothermal nanofluids can be used as liquid working fluids in direct absorption solar thermal collectors for photothermal conversion, thereby improving the utilization efficiency of solar energy. Application example: photothermal conversion fluid working fluids in direct absorption solar thermal collectors.

Claims

1. A method for preparing a high-performance photothermal nanofluid derived from waste cutting fluid, characterized in that: The steps include: (1) Standing sedimentation: Let the waste cutting fluid slurry stand to allow large-sized solid particles to settle naturally, and take the liquid portion of the upper layer; (2) Centrifugation: The upper layer liquid obtained in step (1) is further separated from the solid by high-speed centrifugation to remove unstable suspended particles and obtain an extremely stable base liquid; (3) adding a certain proportion of photothermal conversion nanomaterials to the centrifuged base liquid to uniformly disperse the photothermal conversion nanomaterials to obtain a stable photothermal nanofluid; In step (3), the photothermal conversion nanomaterial is one or more combinations of nanocarbon materials, metal nanoparticles, non-metallic nanoparticles and organic light absorbing materials; The waste cutting fluid in step (1) is waste fluid generated by cutting crystalline silicon and the like in the semiconductor chip or solar panel industry; The addition ratio of the photothermal conversion nanomaterial in the base liquid is adjustable, and the mass ratio is in the range of 0.05wt%-5wt%.

2. The method for preparing a high-performance photothermal nanofluid derived from waste cutting fluid according to claim 1, characterized in that: In the step (2), the centrifugal process uses a rotation speed of 100 rpm to 10,000 rpm. The base liquid after centrifugation is a stable, easy-flowing liquid, and there is no precipitation or stratification within 12 months of standing.

3. The method for preparing a high-performance photothermal nanofluid derived from waste cutting fluid according to claim 1, characterized in that: In the step (3), a dispersion method is selected according to the selected photothermal conversion nanomaterial, including shearing homogenization, ultrasonic oscillation, and mechanical stirring, so that the photothermal conversion nanomaterial is stably dispersed in the base liquid to obtain a product.

4. A photothermal nanofluid product, characterized in that: Prepared based on the preparation method according to any one of claims 1 to 3.

5. A stable photothermal nanofluid prepared by the method according to any one of claims 1 to 3 is applied to direct absorption solar thermal collectors, photothermal seawater desalination and solar thermal utilization.