Antifouling and semi-permeable membrane

By using a porous support layer, cross-linked PVA layer and aquaporin water channel structure on the reverse osmosis membrane, the problems of membrane fouling and water flux are solved, achieving efficient water treatment and long-life membrane performance.

CN115461136BActive Publication Date: 2024-10-15AQUAPORIN AS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080096426.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-16
Filing Date
2020-12-14
Publication Date
2024-10-15
Estimated Expiration
2040-12-14

AI Technical Summary

Technical Problem

Existing reverse osmosis membranes are prone to contamination during use, resulting in a decrease in membrane performance. Although the additional PVA layer reduces the tendency to contaminate, it also reduces water flux.

Method used

A porous support layer and a cross-linked polyvinyl alcohol (PVA) layer are used. The cross-linking agent is polybasic acid, which combines aquaporin water channels and vesicle structures to form a TFC layer through interfacial polymerization to improve the smoothness and water flux of the membrane.

Benefits of technology

Maintain or improve the smoothness of the membrane, reduce the tendency of fouling, while increasing the water flux, extending the service life of the membrane and increasing the water permeability rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003793831350000051
    Figure BDA0003793831350000051
  • Figure BDA0003793831350000052
    Figure BDA0003793831350000052
  • Figure BDA0003793831350000132
    Figure BDA0003793831350000132
Patent Text Reader

Abstract

The present invention relates to an antifouling semipermeable membrane, the antifouling semipermeable membrane comprising a porous support layer, a thin film composite (TFC) layer formed on the surface of the support layer, and a cross-linked polyvinyl alcohol (PVA) layer formed on the top of the TFC layer, wherein the cross-linked PVA layer is a reaction product of PVA and a cross-linking agent, the cross-linking agent is a polyacid including three or more acid groups or a precursor thereof. The obtained membrane shows high water flux and low roughness, and is suitable for being an effective membrane for feed solutions having a tendency to foul the membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an antifouling and semipermeable membrane and more particularly to an antifouling semipermeable membrane comprising a porous support layer, a thin film composite (TFC) layer formed on the surface of the support layer and a cross-linked polyvinyl alcohol (PVA) layer formed on top of the TFC layer. In addition, the present invention relates to modules comprising the antifouling and semipermeable membrane and the use of these modules for processing streams derived from liquid food such as whey, coffee extract, fruit juice, coconut milk, etc. Background Art

[0002] Reverse osmosis (RO) is commonly used to treat water containing dissolved salts. An example of the application of reverse osmosis technology is the production of desalinated drinking water using seawater or brackish water. In recent years, forward osmosis (FO) has become increasingly popular. In a forward osmosis device, the feed is typically dehydrated to concentrate the feed stream, while the draw solution is diluted by the water that migrates across the membrane.

[0003] For RO membranes as well as FO membranes, deposits on the membrane surface become apparent after a period of use. This phenomenon is generally referred to as fouling and usually results in a decrease in membrane performance.

[0004] Polyvinyl alcohol (PVA) has been used as a coating in US2005077243 (A1) to prevent or delay the deposition of contaminants on reverse osmosis membranes. PVA coatings are made from water-swellable but water-insoluble polymers. Since the polymers are insoluble in water, no cross-linking is required after the coating is deposited. The PVA layer is applied to smooth the surface and reduce the tendency of particulate matter to deposit.

[0005] US6413425 BA discloses an RO membrane comprising a support membrane and a polyamide thin film composite (TFC) layer. The surface of the separation layer is coated with a PVA (average degree of polymerization n=2,600) layer to reduce the specific surface area, thereby reducing the tendency to foul. PVA is insoluble in water at 25°C, but soluble in water at 80°C, and has a saponification degree in the range of 99% to 100%. The reverse osmosis composite membrane has high fouling tolerance and allows practical desalination at relatively low pressures.

[0006] US2010224555 (A1) discloses a nanocomposite film comprising a PVA film having a polymer matrix and nanoparticles disposed in the polymer matrix. The film can be contacted (e.g., from the PVA side) with a solution containing a crosslinking agent (e.g., a dialdehyde and a dibasic acid) and a catalyst (e.g., 2.4 wt% acetic acid) for about 1 second. The film can then be heated in an oven at a predetermined temperature for a predetermined period of time. Various crosslinking agents (glutaraldehyde, PVA-glutaraldehyde mixture, paraformaldehyde, formaldehyde, glyoxal) and additives (formaldehyde, ethanol, tetrahydrofuran, manganese chloride, and cyclohexane) in the PVA solution can be used to prepare a PVA film cast on an existing film, combined with heat treatment of the prepared PVA film to change film properties. US2010320143 (A1) and US2011027599 (A1) disclose a similar technique for enclosing nanoparticles in a PVA layer.

[0007] US2010178489 (A1) discloses a composite semipermeable membrane having a surface layer comprising a polyamide resin and a porous support supporting the surface layer. The surface layer may be coated with an antibacterial layer comprising a silver-based antibacterial agent and PVA. In order to attach the PVA layer to the polyamide-based resin of the surface layer, polyvinyl alcohol may be cross-linked. The cross-linking of the polyvinyl alcohol includes forming an antibacterial layer on the surface layer, and then immersing the antibacterial layer in a solution comprising glutaraldehyde acidified with hydrochloric acid.

[0008] The PVA layer suggested in the prior art can reduce the fouling tendency of the membrane due to the increased smoothness provided by the PVA layer. However, the additional layer on the membrane also has a tendency to reduce the water flux. The present invention is aimed at maintaining high surface smoothness to prevent or reduce the deposition of particulate matter in the feed, while achieving higher water flux. Summary of the invention

[0009] The present invention relates to an antifouling semipermeable membrane, which comprises a porous supporting layer, a thin film composite (TFC) layer formed on the surface of the supporting layer, and a cross-linked polyvinyl alcohol (PVA) layer formed on the top of the TFC layer, wherein the cross-linked PVA layer is a reaction product of PVA and a cross-linking agent, and the cross-linking agent is a polyacid including three or more acid groups or a precursor thereof.

[0010] Prior art crosslinkers focus on attaching the PVA layer to the TFC layer of the membrane to ensure long life of the membrane. The present invention proposes to use a polyacid comprising three or more acid groups or its precursors as a crosslinker to open the structure of the PVA layer while maintaining or even increasing the surface smoothness. The open structure of the PVA layer allows increased water penetration and therefore less rate restriction on water flux. Increased smoothness reduces the fouling tendency of the membrane.

[0011] The porous support layer used in the antifouling and semipermeable film of the present invention is a porous substrate, such as a nanoporous or microporous layer that does not substantially inhibit water penetration. In some cases, the porous support layer can be further enhanced by casting on a woven or nonwoven sheet such as formed by polyester fiber. The porous support layer is usually prepared by polyethersulfone (PES), polysulfone (PS), polyphenylsulfone, polyetherimide, polyvinylpyrrolidone and polyacrylonitrile (including its blends and mixtures). In an embodiment of the present invention, the porous support film is prepared by a coating comprising a polymer dissolved in a solvent. After the coating is cast into a layer of desired thickness, phase inversion is performed by quenching in a non-solvent such as water.

[0012] The porous support layer is modified by forming a thin film composite (TFC) layer on its face, for example, by interfacial polymerization. The TFC layer can be prepared using an amine reactant in aqueous solution, preferably an aromatic amine, such as a diamine or triamine, for example 1,3-diaminobenzene (meta-phenylenediamine-MPD) and an acyl halide reactant, such as a diacyl chloride or triacyl chloride, preferably an aromatic acyl halide, for example benzene-1,3,5-tricarbonyl chloride (TMC), dissolved in an organic solvent, wherein the reactants are combined in an interfacial polymerization reaction.

[0013] In a certain embodiment of the present invention, the TFC layer includes nanoporous water channels, such as aquaporin water channels. The nanoporous water channels ideally have a configuration that allows only water to penetrate. However, in practice, there are also relatively small amounts of refluxed solutes that penetrate the TFC layer from the feed solution and reach the draw solution or permeate. The nanoporous water channels reduce or eliminate the reabsorption of all or most other solutes from the feed solution. Preferably, the TFC layer includes aquaporin water channels that, due to their high selectivity, only allow water molecules to pass through. The aquaporin water channels can be stabilized before being introduced into the TFC layer.

[0014] Vesicle is the natural environment of aquaporin water channel, and vesicle can be formed by many different vesicle forming materials (including naturally occurring phospholipids). Suitably, stable aquaporin can be in the form of a vesicle formed by the self-assembly of an amphipathic matrix forming compound in the presence of aquaporin protein preparation, as disclosed in WO2018 / 141985 or WO18087289. Alternatively, aquaporin water channel can be stabilized by PEI (polyethyleneimine), as disclosed in WO2017137361 A1. The film prepared using these stable aquaporin water channels has been shown to be robust, with high water transport capacity and low reverse flux of ions. In a certain embodiment of the present invention, aquaporin water channel is present in vesicle.

[0015] Suitably, vesicle is a polymer vesicle prepared by one or more polymers. Polymer vesicle can withstand relatively high pressure, making it suitable for reverse osmosis process. The polymer of polymer vesicle can be appropriately selected as PMOXA-PDMS diblock copolymer (poly (2-methyloxazoline) -block-poly (dimethylsiloxane) diblock copolymer), to form a self-assembled vesicle with transmembrane protein (such as aquaporin water channel). Then these vesicles can be used to produce a TFC layer in which transmembrane protein is introduced or immobilized and is active for allowing water molecules to pass through the membrane. For example, in order to produce a film including aquaporin water channel, vesicles can be added to an aqueous liquid composition including aromatic amines, such as diamines or triamines, such as 1,3-diaminobenzene (MPD), applied to the surface of a porous support film, which, when contacted with a solution of acyl halide in an organic solvent, will participate in interfacial polymerization, forming a thin film composite layer on the support, thereby forming a separation membrane in which the vesicle has been immobilized or introduced.

[0016] In one aspect, PMOXA of the vesicle a-b -PDMS c-d Select from PMOXA 10-40 -PDMS 25-70 In order to increase the robustness of the vesicles, it is preferred to use at least one of the general formula PMOXA 10-28 -PDMS 25-70 The first amphiphilic diblock copolymer with the general formula PMOXA 28-40 -PDMS 25-70 The weight ratio between the first and second amphiphilic diblock copolymers is generally in the range of 0.1:1 to 1:0.1. The concentration of the amphiphilic diblock copolymer in the liquid composition is generally in the range of 0.1 to 50 mg / ml, such as 0.5 to 20 mg / ml, and preferably 1 to 10 mg / ml.

[0017] Functionalization of PDMS with reactive end groups of vesicles e-f (Reactive end-group functionalized poly(dimethylsiloxane)) is typically present in a concentration of about 0.05% to about 1% v / v of the liquid composition comprising the vesicles. Reactive end-group functionalized PDMS e-f It can be functionalized with one, two or more of amine, carboxylic acid and / or hydroxyl groups. Suitably, the integer e is selected from the range of 20 to 40, such as 30, and the integer f is selected from the range of 40 to 80, such as 50. In a certain aspect of the present invention, the reactive end-group functionalized PDMS e-f PDMS terminated with bis(aminoalkyl), bis(hydroxyalkyl) or bis(carboxylic acid alkyl) e-f, such as poly(dimethylsiloxane), bis(3-aminopropyl) or poly(dimethylsiloxane), bis(3-hydroxypropyl). In addition, PDMS with reactive end groups functionalized e-f Optional free H2N-PDMS 30-50 , HOOC-PDMS 30-50 and HO-PDMS 30-50 The terminal functionalized PDMS e-f An example of (where ef represents a range of 30 to 50) is a bis(aminopropyl) terminated poly(dimethylsiloxane) having the formula shown below, wherein (CAS No. 106214-84-0, Aldrich Product No. 481246, average Mn ~ 5,600 or CAS No. 106214-84-0, Product No. 481696 Aldrich, average Mn ~ 27,000:

[0018]

[0019] and bis(hydroxyalkyl)-terminated poly(dimethylsiloxane)s having the formula shown below, wherein n is about 30 to 50, and m and p are both integers between 2 and 5, such as 3 or 4, (CAS No. 156327-07-0, Aldrich Product No. 481246, average Mn -5,600):

[0020]

[0021] The vesicles may further comprise about 1% v / v to about 12% v / v PMOXA a-b -PDMS c-d -PMOXA a-b Typically, the vesicles include about 8% v / v to about 12% v / v PMOXA a-b -PDMS c-d -PMOXA a-b PMOXA is a triblock copolymer. a-b -PDMS c-d -PMOXA a-b The triblock copolymer of the type is usually selected from PMOXA 10-20 -PDMS 25-70 -PMOXA 10-20 .

[0022] The vesicles in the liquid formulation of the present invention may further include a flux improver to increase water flux or reduce reverse salt flux or both. The flux improver can be selected from a large group of compounds, but is generally preferably alkylene glycol monoalkyl ether alkylate, beta cyclodextrin or polyethylene glycol (15)-hydroxystearate. The flux enhancer is generally present in an amount of 0.1% to 1% by weight of the liquid composition.

[0023] Without wishing to be bound by any particular theory, it is believed that vesicles containing free available reactive groups on the surface will not only be physically introduced or immobilized (adsorbed) in, but also chemically bound in the TFC layer, because reactive free end groups such as amino groups, hydroxyl groups and carboxyl groups will participate in interfacial polymerization reactions with acyl chlorides such as trimesoyl chloride (TMC). In this way, it is believed that the vesicles will be covalently bound in the TFC layer, resulting in a relatively high vesicle loading, and therefore a higher water flux through the membrane. In addition, it is believed that when introduced into a selective membrane layer, the covalent coupling of the vesicles in the TFC layer results in a higher stability and / or lifespan of the aquaporin water channels and the vesicles containing the aquaporin water channels.

[0024] Polyvinyl alcohol (PVA) is typically prepared from poly(vinyl acetate). The degree of polymerization of poly(vinyl acetate) is typically between 100 and 5000. The ester groups of poly(vinyl acetate) are susceptible to alkaline hydrolysis, which converts poly(vinyl acetate) into polyvinyl alcohol and acetic acid. This process is referred to herein as hydrolysis, but may also be referred to as saponification in the prior art.

[0025] In a certain embodiment of the present invention, PVA is derived from the hydrolysis of polyvinyl acetate, and the degree of hydrolysis of polyvinyl acetate is 90% to 99.9%. Preferably, the degree of hydrolysis is between 95% and 99.5%, such as 98.0 to 99.0%. Therefore, the PVA polymer is actually a copolymer of vinyl alcohol and a small proportion of vinyl acetate comonomer.

[0026] The degree of polymerization is usually measured as viscosity because viscosity increases with increasing degree of polymerization. In a certain aspect, the viscosity of PVA measured as a 4% aqueous solution at 20°C is between 20 and 80 mPa·s. In a preferred embodiment, the degree of polymerization is suitably between 50 and 70 mPa·s to obtain high water flux. Polyvinyl alcohol can be obtained from various suppliers, but is currently obtained from Kuraray Poval. Suitable grades include fully hydrolyzed grades, i.e., 98 to 99 mol-% hydrolyzates, with a viscosity of about 30 or about 60 mPa·s.

[0027] PVA polymer can utilize chemical agent such as aldehyde and acid and ultraviolet radiation crosslinking.According to the present invention, polyacid is used, i.e. compound with three or more acid groups or the precursor of such acid groups.The precursor group of acid group includes for example aldehyde (-CHO), acyl halide (-COOX, wherein X is Cl, Br or I) and alkali metal salt (-COOM, wherein M is Li, Na or K) of carboxylic acid.Usually, aliphatic crosslinking agent is preferred, even if aromatic crosslinking agent such as trimesic acid can also be used in some cases.Suitably, polyacid is selected from the group consisting of citric acid, 1,2,3,4-butane tetracarboxylic acid, 2,3,5-hexane tricarboxylic acid and 1,2,3-butane tricarboxylic acid.In preferred aspect, polyacid is citric acid. Citric acid has high biological tolerance, and therefore can be used for preparing food without reservation.Therefore, the film produced using citric acid as crosslinking agent is generally considered to have a wider range of application fields, which also includes food processing.

[0028] The amount of the polyacid is typically adjusted to the amount of hydroxyl groups available for reaction on the PVA polymer. Thus, in a certain embodiment, the amount of the polyacid is adjusted so that at least 40% of the hydroxyl groups on the PVA polymer can react. In a preferred aspect of the invention, the amount of the polyacid is at least 60%, such as at least 80%, of the hydroxyl groups on the PVA polymer. In a preferred embodiment, the amount of the polyacid is adjusted so that about 100% of the available hydroxyl groups can react with the acid groups of the polyacid.

[0029] The porous support membrane can be a hollow fiber membrane or a flat sheet membrane. Currently, flat sheet membranes are suitable and may be used to produce various modules, such as plate and frame modules or spiral wound modules.

[0030] The present invention also relates to a method for preparing an antifouling semipermeable membrane, the method comprising the following steps:

[0031] providing a semipermeable membrane comprising a porous supporting layer having a thin film composite (TFC) layer formed on a surface thereof,

[0032] applying a layer of an aqueous PVA mixture of polyvinyl alcohol and a cross-linking agent to the TFC layer surface of the membrane, and

[0033] reacting the mixture,

[0034] The crosslinking agent is a polyacid having three or more acid groups or a precursor thereof.

[0035] Although the aqueous mixture can be applied to the semipermeable membrane without pretreatment, it is appropriate to treat the semipermeable membrane comprising a support layer having a thin film composite layer formed on its surface with an aqueous glycerol solution prior to applying the aqueous PVA mixture. The aqueous glycerol solution can be applied to the porous side, the TFC layer side, or both prior to applying the aqueous PVA mixture, but typically the glycerol solution is applied only to the support layer surface of the TFC membrane prior to applying the aqueous PVA mixture. Applying the aqueous glycerol solution to the porous side of the membrane only allows the production of a membrane that is more tolerant to, for example, changes in glycerol concentration and less variation in water flux.

[0036] Suitably, the concentration of glycerol in the glycerol solution may be between 5% and 50%, such as 10 to 40. Generally, it is preferred that the concentration of glycerol in the glycerol solution is from 13% by weight to 80% by weight.

[0037] The aqueous PVA mixture can be applied to the TFC membrane using a variety of methods, including casting and spraying. In a preferred method, to achieve higher water flux, the aqueous PVA mixture is applied to the TFC membrane by spraying.

[0038] Typically, the polyacid is selected from the group consisting of citric acid, 1,2,3,4-butanetetracarboxylic acid, 2,3,5-hexanetricarboxylic acid and 1,2,3-butanetricarboxylic acid. In one aspect, the polyacid is citric acid. The polyacid is believed to open up the structure of the PVA layer, thereby increasing water flux.

[0039] In a certain embodiment, the concentration by weight of the polyacid is equal to or higher than the concentration by weight of PVA in the aqueous PVA mixture. Preferably, the concentration by weight of citric acid is at least twice the concentration of PVA in the aqueous mixture.

[0040] The addition of polyacids to aqueous PVA mixtures unexpectedly resulted in a reduction in average roughness when the membrane was coated with a PVA layer. Furthermore, when polyacids were added to PVA solutions, contact angles and zeta potentials were significantly reduced. Low surface roughness and low zeta potential are generally considered to improve the antifouling properties of membranes. The fact that the surface charge tends to be neutral when citric acid is added to PVA solutions is also considered to improve antifouling properties. Example

[0041] Example 1.1: Production of support membrane

[0042] The coating was prepared by dissolving 17% polysulfone (Solvay P3500 MB7 LCD) in 83% DMF (N,N-dimethylformamide) obtained from TACT Chemie. The coating was mixed in a closed container at 45°C at a mixing speed of 90 rpm for 8 hours to obtain a uniform viscosity.

[0043] The coating was cast in knife over roll casting mode on a nonwoven polyester sheet (model PMB-SKC) obtained from Mitsubishi using a casting gap of 230 μm. After an exposure time of 1.9 s, the phase inversion was performed by quenching in water at 13° C. for 16 s. Subsequently, the support film was washed in water at 60° C. for 120 s. A thickness of about 130 μm was obtained.

[0044] Example 1.2: Production of aquaporin water channels

[0045] Expression of His-tagged Aquaporins from Oryza sativa Japonica (Japanese Rice) in Escherichia coli and their purification using immobilized metal affinity chromatography (IMAC)

[0046] The gene encoding water channel protein from japonica rice (UNIPROT: A3C132) was codon optimized using the service of Geneart (a subsidiary of Thermo Fischer Scientific) to improve expression in Escherichia coli. The resulting gene (gene ID: aquaporin_Oryza_sativa_Japonica) was synthesized by adding ten histidine encoding codons at the C-terminus and adding flanking NdeI / XhoI restriction sites at the N-terminus and C-terminus, respectively. The synthetic gene fragment was digested with NdeI / XhoI restriction enzymes and connected to the vector pUP1909 fragment digested and purified by NdeI / XhoI. The resulting connection mixture was transformed into Escherichia coli DH10B, and kanamycin resistant transformants were selected on LB agar plates with kanamycin. The transformants were confirmed by sequencing of the genetic construct. The separated vector DNA was subsequently transferred to the production host Escherichia coli BL21.

[0047] For heterologous expression of aquaporins in E. coli, the production host was grown in minimal medium consisting of 30 g / L glycerol, 6 g / L (NH4)2HPO4, 3 g / L KH2PO4, 5 g / L NaCl, 0.25 g / L MgSO4·7H2O, 0.4 g / L Fe(III) citrate, and 1 mL / L sterile filtered trace metal solution. The trace metal solution consisted of 1 g / LEDTA, 0.8 g / L CoCl2·6H2O, 1.5 MnCl2·4H2O, 0.4 g / L CuCl2·2H2O, 0.4 g / L H3BO3, 0.8 g / L Na2MoO4·2H2O, 1.3 g / L Zn(CH3COO)2·2H2O. After inoculation and overnight growth, an additional 0.25 g / L MgSO4·7H2O was added.

[0048] E. coli was cultured in a batch fermentation process in a 3 L Applikon bioreactor with ez-Control. Protein production was induced by adding IPTG to a final concentration of 0.5 mM at an optical density (OD 600 nm) of about 30. The culture was induced for about 24 hours and the bacterial cells were harvested by centrifugation at 5300 g for 20 min.

[0049] The pellet including the E. coli cells was resuspended in a buffer (an aqueous solution of the protease inhibitors PMSF and EDTA) and homogenized in a Stansted nm-GEN 7575 homogenizer at 1000 bar. The temperature was maintained at about 10-15°C. The mixture was centrifuged at a maximum speed of 5300g for 30 minutes. The pellet contained membrane proteins and the supernatant was discarded.

[0050] The pellet was resuspended in 0.9% sodium chloride solution to obtain a total protein concentration of about 50 mg / ml. Membrane proteins were dissolved by adding 28 L of TRIS binding buffer and 4.5 liters of 5% n-lauryl dimethylamine N-oxide (LDAO) to 5 L of resuspended pellet material. The mixture was incubated for 2 to 24 hours at room temperature and gentle stirring.

[0051] After the solubilization process, the mixture was centrifuged at 5300 g for 90 min in a 2 L container. The supernatant was recovered and the LDAO concentration was adjusted to 0.2% by adding dilution buffer.

[0052] After dissolution and clarification, the protein was captured using IMAC and eluted in an elution buffer containing 1000mM imidazole and 0.2% w / v LDAO. The eluted portion was analyzed by SDS Page and only showed a single major band migrating at 27kDa, which corresponds to the size of aquaporin from Japanese rice. In addition, the result was confirmed by comparison with a negative control purification from Escherichia coli transformed with an empty vector. The negative control resulted in no purified protein. Western blot analysis using an antibody specific for the histidine tag (TaKaRa Bio) resulted in clear signals from the purified protein as expected and no signals from the negative control, confirming that the source of the purified protein was a histidine-tagged membrane protein.

[0053] The stock solution was prepared by adjusting the protein concentration to 5 mg / ml by adding ice-cold imidazole-free buffer containing 2% LDAO. Finally, the aquaporin stock solution was sterilized by filtration through a 0.45 μM sterilizing cup and stored in a 4°C refrigerator for use within one month or in a -80°C freezer.

[0054] Example 1.3: Production of aquaporin preparations

[0055] 1. Prepare 0.5% by weight KHS by dissolving 5 g KHS in 1 l PBS (prepared by dissolving 8 g NaCl, 0.2 g KCl, 1.44 g Na2HPO4 and 0.24 g KH2PO4 in 800 mL MiliQ purified H2O, adjusting pH to 7.2 with HCl and completing volume to 1 L). HS 15 (polyethylene glycol (15)-hydroxystearate) (KHS) solution.

[0056] 2. Prepare a 0.05% by weight LDAO solution in PBS by dissolving 0.05 g LDAO in 100 mL PBS.

[0057] 3. In the preparation container, weigh 0.5 g of poly(2-methyloxazoline)-block-poly(dimethylsiloxane) diblock copolymer (PDMS 65 PMOXA 24 ) / L of the preparation.

[0058] 4. In the same preparation container, weigh poly(2-methyloxazoline)-block-poly(dimethylsiloxane) diblock copolymer (PDMS 65 PMOXA 32 ), to achieve 0.5 g / L of the prepared formulation (PDMS 65 PMOXA 24 and PDMS 65 PMOXA 32 The weight ratio is 1:1).

[0059] 5. In the same preparation container, add poly(2-methyloxazoline)-block-poly(dimethylsiloxane)-block-poly-(2-methyloxazoline) triblock copolymer PMOXA 12 PDMS 65 PMOXA 12 , to achieve a concentration of 0.12 g / L of the prepared formulation.

[0060] 6. Add 0.05% of LDAO prepared in step 2 at a ratio of 100 mL / L of prepared formulation.

[0061] 7. Add bis(3-aminopropyl) terminated poly(dimethylsiloxane) having a molecular weight of 2500 Da to a final concentration of 0.1%.

[0062] 8. Add aquaporin stock solution to achieve a concentration of 5 mg / L of prepared formulation, and a protein:polymer ratio of 1 / 400.

[0063] 9. Add 3% by weight of the KHS solution prepared in step 1 to reach the desired volume of the prepared formulation minus the volume of LDAO, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), and aquaporin added in steps 6 and 8.

[0064] 10. Stir the mixture from step 9 at 170 rpm at room temperature overnight (not more than 20 hours) to obtain the formulation.

[0065] 11. Take the prepared formulation obtained in the order of steps 1 to 10 the next morning and sterilize it by filtering it through a 200 nm pore size filter, put it in a closed sealed bottle and store it at room temperature for no more than 12 months.

[0066] Example 1.4: Production of TFC layer on support membrane

[0067] a. Prepare an aqueous solution by mixing the following in DI water:

[0068] i.3.0% MPD

[0069] ii.0.75% ε-caprolactam (CAP)

[0070] iii.3% Aquaporin Preparation

[0071] b. Prepare an organic solution in Isopar E with 0.13% TMC.

[0072] c. TFC formation

[0073] i. Immerse the support membrane in the aqueous solution for 50 seconds,

[0074] ii. The film was dried with an air gun at 1 bar,

[0075] iii. Add organic solution for 20-22 seconds

[0076] iv. Dry the membrane with an air gun at about 0.1 bar

[0077] d. The membrane with the TFC layer was placed in 10% citric acid at 70°C for 4 min, and then in DI water at 60°C for 2 min.

[0078] e. Immerse the membrane in 2000ppm sodium hypochlorite solution for 2min, then in room temperature DI water for 1min, and finally in 1% sodium bisulfite (SBS)

[0079] Example 2: Glycerol treatment before PVA layer

[0080] 10% and 20% aqueous glycerol solutions were prepared. In the first run, the membrane obtained in Example 1.4 was immersed in the glycerol solution for 1 min, treated with an air knife to remove excess glycerol solution, and then treated by pouring 0.35% PVA aqueous solution (Kuraray Poval, 60-98 type) for 30 s, treated with an air knife at 1 bar to remove excess PVA solution, and dried in an oven at 60° C. for 4 min.

[0081] The results are shown in Table 1 below:

[0082] Table 1:

[0083] Glycerol impregnation A[LMH / Bar] Retention rate [%] 10%, 1min 5.0±0.5 99.0±0.0 20%, 1min 5.3±0.4 98.8±0.2

[0084] Another test run was performed by changing the application method from immersing the entire membrane in the glycerol solution to applying the glycerol solution only to the back side of the membrane obtained in Example 1.4. The results are shown in Table 2 below:

[0085] Table 2:

[0086] Glycerin on the back A[LMH / Bar] Retention rate [%] 10%, 1min 4.7±0.5 98.9±0.0 20%, 1min 5.1±0.4 98.9±0.1

[0087] The results shown in Tables 1 and 2 indicate an improvement in flux when using 20% ​​glycerol compared to 10% glycerol. A slight decrease in rejection was observed for glycerol impregnation. However, for backside glycerol, changes in glycerol concentration did not appear to affect rejection. The deviations in flux were also smaller compared to glycerol impregnation.

[0088] The test run was repeated and a longer reaction time of 3 min for the glycerol solution was included. The results are shown in Table 3.

[0089] Table 3

[0090] Glycerin on the back A[LMH / Bar] Retention rate [%] 10%, 1min 4.7±0.0 98.9±0.0 10%, 3min 4.9±0.1 98.9±0.1 20%, 1min 5.1±0.3 98.9±0.1 20%, 3min 5.6±0.1 98.9±0.0

[0091] The results in Table 3 show that treatment with 20% glycerol solution and a reaction time of 3 min with PVA solution provided the highest flux and the same retention rate.

[0092] Example 3: Reaction time and type of PVA solution

[0093] The films treated with 20% glycerol on the back side for 3 minutes were cast with 0.35% PVA 60-98 solution for 10 s or 30 s, treated with an air knife at 1 bar, and then dried in an oven at 60° C. for 4 minutes.

[0094] The results are shown in Table 4:

[0095] Table 4:

[0096] Glycerin on the back A[LMH / Bar] Retention rate [%] Control (without PVA) 5.7±0.0 98.9±0.1 PVA coating, 10s 4.5±0.1 99.3±0.2 PVA coating, 30s 4.5±0.1 99.2±0.3

[0097] The results show that the flux and retention rate remain essentially unchanged. Therefore, for further studies, a 10 s PVA reaction time was used.

[0098] Will be available from Kuraray The various types of PVA obtained were screened using the experience of the above test runs, i.e., 20% glycerol backside treatment for 3 min, 0.35% PVA solution using a casting method and allowed to react for 10 s, treated with a 1 bar air knife to remove excess PVA solution, and then dried in a 60° C. oven for 4 min. The results for various PVA types and qualities are shown in Table 5 below.

[0099] Table 5:

[0100]

[0101] The first number in the nomenclature indicates the viscosity of a 4% aqueous solution at 20° C. as a relative measure of the molar mass of the PVA. The second number indicates the degree of hydrolysis of the polyvinyl acetate from which the PVA is derived.

[0102] The results shown in Table 5 show that PVA 30-98 and PVA 60-98 are good candidates because they show high flux and rejection, and low bias at the same time. These candidates were compared with the commercially available Hypershell DOW membrane (benchmark). The results are shown in Table 6 below.

[0103] Table 6:

[0104] N=4 A[LMH / Bar] Retention rate [%] Control (without PVA) 5.8±0.1 99.0±0.1 PVA 30-98 4.2±0.1 99.2±0.1 PVA 60-98 4.4±0.2 99.4±0.0 DOW Hypershell 3.5±0.1 99.5±0.1

[0105] Based on the results shown in Table 6, PVA 60-98 was selected for further development due to higher flux and retention compared to PVA 30- 98. The retention was essentially at the same level as the benchmark, however the flux was approximately 25% higher.

[0106] Example 4: PVA application method

[0107] The PVA layer of the film was observed to be quite thick by the PVA dye test. Compared with the control film, the relatively thick layer may be the reason for the relatively high flux decline. Therefore, a spraying method applying the PVA solution was used and compared with the casting method. The results of the flux are shown in the following table 7.

[0108] Table 7:

[0109]

[0110] Test conditions:

[0111] *)10 bar, 25C, RO water

[0112] **) 15.5 bar, 25C, 2000 ppm NaCl feed, 1.8 LPM flow rate.

[0113] The results in Table 7 show that the membrane with the PVA solution applied by spraying improved the PWP flux by about 20% relative to the casting method and 60% relative to the baseline from DOW.

[0114] Example 5: Citric Acid (CA) Crosslinker

[0115] In an attempt to further improve the flux, citric acid was added to the PVA solution as a cross-linking agent or pore former.

[0116] The PVA solution prepared as described above was supplemented with 0.42% by weight of citric acid, which, when reacting with the available OH groups of the PVA, corresponds to a 50% degree of crosslinking. The PVA was applied by a spray method and allowed to react for 10 s, after which the excess PVA solution was removed with an air knife. The results are shown in Table 8 below.

[0117] Table 8:

[0118] Citric Acid A[LMH / Bar] Retention rate [%] PVA 4.5 99.1 PVA+CA(50%) 4.9 99.1

[0119] Test conditions: 2000ppm NaCl feed, 15.5 bar, 1.8 LPM flow rate

[0120] The results showed that about 9% flux improvement could be obtained by adding citric acid to the PVA solution.

[0121] The surface roughness Ra (nm), contact angle and zeta potential (mV) of PVA films and PVA+CA (50%) were studied and compared with control films not treated with PVA. The results are shown in Table 9 below.

[0122] Table 9:

[0123] Average roughness(nm) Contact angle Zeta potential (mV) PVA 35.6 70.4 -9.00 PVA+CA(50%) 22.4 61.2 -6.33 Comparison 53.9 55.3 -22.05

[0124] The results in Table 9 show that when the film is coated with a PVA layer, the average roughness is reduced. A further reduction in roughness is obtained by adding citric acid to the PVA solution. In addition, when citric acid is added to the PVA solution, the contact angle and zeta potential are significantly reduced. Low surface roughness and zeta potential are generally considered to improve the antifouling properties of the film. The fact that the surface charge tends to be neutral when citric acid is added to the PVA solution is also considered to improve the antifouling performance.

[0125] Further experiments were designed to compare 50% and 100% cross-linking. The 100% cross-linking PVA solution contained 0.84% ​​by weight citric acid. The results are shown in Table 10 below.

[0126] Table 10:

[0127] Citric Acid A[LMH / Bar] Retention rate [%] PVA+CA(50%) 4.6 99.3±0.2 PVA+CA(100%) 5.0 99.2±0.2

[0128] Test conditions: 2000ppm NaCl feed, 15.5 bar, 1.8 LPM flow rate

[0129] The results shown in Table 10 show that when the amount of citric acid in the PVA solution is increased from 50% cross-linking to 100% cross-linking, an improved flux of about 9% can be obtained.

[0130] Various aspects and implementations have been described in conjunction with various embodiments herein. However, other variations to the disclosed embodiments may be understood and effected by those skilled in the art in practicing the claimed subject matter, by studying the disclosure and the appended claims. In the claims, the word "comprising" does not exclude other elements or steps, and the indefinite article "a" or "an" does not exclude a plurality.

Claims

1. An antifouling semipermeable membrane comprising a porous support layer, a thin film composite TFC layer formed on the surface of the support layer, and a cross-linked polyvinyl alcohol (PVA) layer formed on top of the TFC layer, wherein the cross-linked PVA layer is a reaction product of PVA and a cross-linking agent, the cross-linking agent is a polyacid comprising three or more acid groups or a precursor thereof, the precursor of the acid group being selected from the group comprising aldehydes, acyl halides and alkali metal salts of carboxylic acids, It is characterized in that An aqueous glycerol solution is applied to the support layer surface of the TFC membrane prior to applying the cross-linked PVA layer.

2. The antifouling semipermeable membrane according to claim 1, wherein the viscosity of the PVA measured as a 4% aqueous solution at 20°C is between 30 mPa·s and 80 mPa·s.

3. The antifouling semipermeable membrane according to claim 1, wherein the viscosity of the PVA measured as a 4% aqueous solution at 20°C is between 30 mPa·s and 60 mPa·s.

4. The antifouling semipermeable membrane according to any one of the preceding claims, wherein the TFC layer comprises aquaporin water channels. The antifouling semipermeable membrane according to claim 4 , wherein the aquaporin water channel is present in a vesicle. The antifouling semipermeable membrane according to claim 5 , wherein the vesicles are polymer vesicles comprising one or more polymers.

7. The antifouling semipermeable membrane according to claim 1, wherein the PVA is derived from the hydrolysis of polyvinyl acetate, and the degree of hydrolysis of the polyvinyl acetate is 90% to 99.9%. 8 . The antifouling semipermeable membrane according to claim 1 , wherein the polyacid is selected from the group consisting of citric acid, 1,2,3,4-butanetetracarboxylic acid, 2,3,5-hexanetricarboxylic acid, and 1,2,3-butanetricarboxylic acid.

9. A method for preparing an antifouling semipermeable membrane, comprising the following steps: a. providing a semipermeable membrane comprising a porous support layer, the porous support layer having a thin film composite TFC layer formed on its surface, b. applying a layer of an aqueous PVA mixture of polyvinyl alcohol and a crosslinking agent to the surface of the TFC layer of the membrane, and c. reacting the mixture, wherein the crosslinking agent is a polyacid having three or more acid groups or a precursor thereof, the precursor of the acid groups being selected from the group consisting of aldehydes, acid halides and alkali metal salts of carboxylic acids, It is characterized in that An aqueous glycerol solution is applied to the support layer surface of the TFC membrane prior to applying the aqueous PVA mixture.

10. The method of claim 9, wherein the PVA is derived from the hydrolysis of polyvinyl acetate, the degree of hydrolysis of the polyvinyl acetate being 90% to 99.9%.

11. The method of claim 9, wherein the viscosity of the PVA measured as a 4% aqueous solution at 20°C is between 30 mPa·s and 80 mPa·s.

12. The method according to claim 9, wherein the concentration of glycerol in the aqueous glycerol solution is 13% by weight to 80% by weight.

13. The method of claim 12, wherein the polyacid is selected from the group consisting of citric acid, 1,2,3,4-butanetetracarboxylic acid, 2,3,5-hexanetricarboxylic acid, and 1,2,3-butanetricarboxylic acid.

14. The method of claim 9, wherein the concentration by weight of the polyacid is equal to or higher than the concentration by weight of the PVA in the aqueous PVA mixture.

15. The method of claim 13, wherein the concentration by weight of the citric acid is at least twice the concentration of the PVA in the aqueous PVA mixture.