A polyethersulfone humidifying membrane with symmetrical structure and preparation method thereof

By designing a polyethersulfone humidification film with a symmetrical structure, the problems of irregular structure and low separation efficiency of the existing membrane are solved, and the effects of high mechanical strength, gas resistance and water flux are achieved.

CN115463550BActive Publication Date: 2024-11-29TIANJIN CNCLEAR ENVIRONMENTAL PROTECTION SCI & TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211036326.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-28
Publication Date
2024-11-29
Estimated Expiration
2042-08-28

AI Technical Summary

Technical Problem

The existing polyethersulfone film has irregular structure, low separation efficiency and small flux, and a polyethersulfone humidification film with a symmetrical structure is needed.

Method used

A structure combining the intermediate cavern layer, an outer and inner support layer and a separation layer is adopted, and a symmetrical structure of the inner and outer double filter layer and a double-layer finger-like support layer is formed by the preparation and spinning of the polyethersulfone membrane liquid.

Benefits of technology

The symmetrical structural design of the polyethersulfone humidification film is realized, which improves the mechanical strength, bubble point pressure and water flux of the film, while maintaining gas resistance at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115463550B_ABST
    Figure CN115463550B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyethersulfone humidifying membranes, and in particular, a polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof, including an intermediate sponge layer, and an outer supporting layer is provided on one side of the intermediate sponge layer. The polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof, with polyethersulfone as a film-forming polymer, adding a porogen, a hydrophilic polymer and an organic solvent, and preparing a polyethersulfone homogeneous membrane liquid. During spinning, the air bath and the internal and external coagulation baths are the inner and external surfaces of the membrane liquid that rapidly separate into dense layers, slowing down the double diffusion inside the membrane liquid. The polyethersulfone humidifying membrane with a symmetrical structure is prepared by regulating the air bath time, the temperature of the internal and external coagulation baths and the composition of the membrane liquid, so that the polyethersulfone humidifying membrane prepared by the present invention presents a symmetrical structure of an inner and outer double filter layer and a double-layer finger-shaped hole supporting layer, and the inner and outer filter layers both have a separation pore size of 0.002-0.02 μm, and have high mechanical strength, bubble point pressure, and water flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyethersulfone humidifying membranes, and in particular to a polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof. Background Art

[0002] Polyethersulfone is a thermoplastic polymer material with excellent comprehensive properties and is one of the few special engineering plastics that have been applied. It has excellent heat resistance, physical and mechanical properties, insulation properties, etc., especially the outstanding advantages of being able to be used continuously at high temperatures and maintaining stable performance in environments with rapid temperature changes. It has been widely used in many fields.

[0003] According to the Chinese patent with publication number CN1951550A, a large-pore polyethersulfone membrane and its preparation method are disclosed, wherein 9-15% polyethersulfone and 5-10% polyvinylpyrrolidone are dissolved in an organic solvent to prepare a casting solution; then the casting solution is scraped and finally formed into a membrane in a gel water bath. The obtained poly-sealed microfiltration membrane has an irregular structure, low separation efficiency, and small flux, so a polyethersulfone humidification membrane with a symmetrical structure and its preparation method are needed. Summary of the invention

[0004] Based on the existing technical problems, the present invention proposes a polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof.

[0005] The present invention proposes a polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof, comprising a middle sponge layer, an outer supporting layer is arranged on one side of the middle sponge layer, an outer separation layer is arranged on one side of the outer supporting layer, an inner supporting layer is arranged on the other side of the middle sponge layer, and an inner separation layer is arranged on one side of the inner supporting layer.

[0006] Preferably, step 1, preparation of polyethersulfone membrane solution;

[0007] Step 2: Processing of membrane fibers;

[0008] Step 3: Preparation of humidifying membrane.

[0009] Preferably, the materials for preparing the polyethersulfone membrane solution in step 1 include the following materials, such as polyethersulfone polymer, porogen, hydrophilic polymer and organic solvent.

[0010] Preferably, the mass percentages of the components of the material are selected as follows: 10%-30% of polyethersulfone polymer, 0.5%-8% of porogen, 3%-15% of hydrophilic polymer and 40%-80% of organic solvent.

[0011] Preferably, the porogen is one or more of titanium dioxide, silicon dioxide or aluminum chloride, the hydrophilic polymer is one or more of polyethylene glycol, polymethyl methacrylate or cellulose acetate, and the organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylpyrrolidone, dimethylformamide or dimethylacetamide.

[0012] Preferably, the preparation step of the polyethersulfone membrane liquid in step one is as follows: Sa1, at 70°C-90°C, add the polyethersulfone polymer, porogen, hydrophilic polymer and organic solvent in a certain proportion into a reaction kettle, stir at a speed of 30-60 rpm, and stir at 70-90°C for 10 hours to dissolve the polymer into a homogeneous membrane liquid.

[0013] Preferably, Sa2, then cool to 30-65°C, stir for 5-10h, and stir at a speed of 20-40 rpm to allow the membrane liquid to fully dissolve and mature during the cooling process to obtain the spinning membrane liquid.

[0014] Preferably, the processing of the membrane filaments in step 2: Sb1, pouring the membrane liquid into a spinning kettle, vacuum degassing at -0.1 MPa for 15-24 hours, and the degassing temperature is 50-65°C; the membrane liquid is extruded through a spinneret and enters an air bath with a humidity of 30-80%, and the air bath length is 2-20 cm.

[0015] Preferably, after Sb2 is initially solidified, the membrane liquid enters an aqueous solution containing 15-50% dimethylformamide DMAc, the coagulation bath temperature is 30-70°C, and the stretching speed is 8-20m / min, so that the membrane filaments are solidified and formed to form a humidifying membrane after initial solidification.

[0016] Preferably, in the preparation of the humidifying membrane in step three, the humidifying membrane after preliminary curing is immersed in deionized water at 30-40° C. for 24 hours to remove residual additives and solvents, thereby preparing a polyethersulfone humidifying membrane with a symmetrical structure.

[0017] The beneficial effects of the present invention are:

[0018] 1. In the present invention, polyethersulfone is used as a film-forming polymer, and a porogen, a hydrophilic polymer and an organic solvent are added to prepare a polyethersulfone homogeneous membrane liquid. During spinning, the air bath and the internal and external coagulation baths are used to rapidly separate the inner and external surfaces of the membrane liquid into dense layers, which slows down the double diffusion inside the membrane liquid and is conducive to the formation of finger-like pores. By regulating the air bath time, the temperature and composition of the internal and external coagulation baths of the membrane liquid, a polyethersulfone humidification membrane with a symmetrical structure is prepared, so that the polyethersulfone humidification membrane prepared by the present invention presents a symmetrical structure of an inner and outer double filter layer and a double-layer finger-like pore support layer, and the inner and outer filter layers both have a separation pore size of 0.002-0.02μm, and have high mechanical strength, bubble point pressure, and water flux.

[0019] 2. The membrane has a symmetrical structure of double separation layers and support layers. The inner and outer surface structures are dense, and the membrane tube can still maintain good gas resistance when operating at high temperatures; the support layer is composed of double-layer finger-shaped holes with high porosity, which makes the membrane have high water vapor permeability. When water enters the finger-shaped holes, it is conducive to its storage, preventing the gas from overflowing from the pores in the membrane, and improving the gas resistance of the membrane tube to a certain extent. The preparation method of the membrane tube adopts the immersion phase inversion preparation technology, which has good process controllability and mature technology, can effectively reduce production costs and ensure the quality of membrane tubes, and has broad application prospects in humidification systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic diagram of a basic performance test table of a polyethersulfone humidifying membrane having a symmetrical structure and a preparation method thereof;

[0021] Figure 2 The present invention is a cross-sectional scanning electron microscope image of a polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof at a magnification of 60 times.

[0022] In the figure: 1. middle sponge layer; 2. outer support layer; 3. outer separation layer; 4. inner support layer; 5. inner separation layer. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0024] Reference Figure 1-2 A polyethersulfone humidifying membrane with a symmetrical structure and a preparation method thereof, comprising an intermediate sponge layer 1, an outer supporting layer 2 is arranged on one side of the intermediate sponge layer 1, an outer separation layer 3 is arranged on one side of the outer supporting layer 2, an inner supporting layer 4 is arranged on the other side of the intermediate sponge layer 1, and an inner separation layer 5 is arranged on one side of the inner supporting layer 4.

[0025] The membrane has a symmetrical structure of double separation layers and a support layer. The inner and outer surface structures are dense, and the membrane tube can still maintain good gas resistance when operating at high temperatures; the support layer is composed of double-layer finger-shaped holes with high porosity, which makes the membrane have high water vapor permeability. When water enters the finger-shaped holes, it is conducive to its storage, preventing the gas from overflowing from the pores in the membrane, and improving the gas resistance of the membrane tube to a certain extent. The preparation method of the membrane tube adopts the immersion phase inversion preparation technology, which has good process controllability and mature technology, can effectively reduce production costs and ensure the quality of membrane tubes, and has broad application prospects in humidification systems.

[0026] Step 1, preparation of polyethersulfone membrane solution; the selection of materials for the preparation of polyethersulfone membrane solution includes the following selected materials, such as polyethersulfone polymer, porogen, hydrophilic polymer and organic solvent.

[0027] The mass percentage contents of the selected material components are: 10%-30% of polyethersulfone polymer, 0.5%-8% of porogen, 3%-15% of hydrophilic polymer and 40%-80% of organic solvent.

[0028] The porogen is one or more of titanium dioxide, silicon dioxide or aluminum chloride, the hydrophilic polymer is one or more of polyethylene glycol, polymethyl methacrylate or cellulose acetate, and the organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylpyrrolidone, dimethylformamide or dimethylacetamide.

[0029] Preparation steps of polyethersulfone membrane liquid: Sa1, at 70°C-90°C, add polyethersulfone polymer, porogen, hydrophilic polymer and organic solvent in a certain proportion into a reaction kettle, stir at a speed of 30-60 rpm, and stir at 70-90°C for 10 hours to dissolve the polymer into a homogeneous membrane liquid;

[0030] Sa2. Then cool down to 30-65°C, stir for 5-10 hours, and stir at a speed of 20-40 rpm to allow the membrane liquid to fully dissolve and mature during the cooling process to obtain the spinning membrane liquid.

[0031] Step 2, membrane processing; Sb1, pour the membrane liquid into the spinning kettle, vacuum degassing at -0.1MPa for 15-24h, degassing temperature 50-65°C; the membrane liquid is extruded through the spinneret and enters an air bath with a humidity of 30-80%, and the air bath length is 2-20cm;

[0032] Sb2. After preliminary solidification, the membrane liquid enters into an aqueous solution containing 15-50% dimethylformamide DMAc, the coagulation bath temperature is 30-70°C, and the stretching speed is 8-20m / min, so that the membrane filaments are solidified and formed to form a humidifying membrane after preliminary solidification.

[0033] Step 3: Preparation of humidification membrane: soak the preliminarily cured humidification membrane in deionized water at 30-40° C. for 24 hours to remove residual additives and solvents, thereby obtaining a polyethersulfone humidification membrane with a symmetrical structure.

[0034] In the present invention, polyethersulfone is used as a film-forming polymer, and a porogen, a hydrophilic polymer and an organic solvent are added to prepare a polyethersulfone homogeneous membrane liquid. During spinning, the air bath and the internal and external coagulation baths are used to rapidly separate the inner and external surfaces of the membrane liquid into dense layers, which slows down the double diffusion inside the membrane liquid and is conducive to the formation of finger-like pores. A polyethersulfone humidifying membrane with a symmetrical structure is prepared by regulating the air bath time, the temperature and composition of the internal and external coagulation baths of the membrane liquid, so that the polyethersulfone humidifying membrane prepared by the present invention presents a symmetrical structure of an inner and outer double filter layer and a double-layer finger-like pore support layer, and the inner and outer filter layers both have a separation pore size of 0.002-0.02μm, and have high mechanical strength, bubble point pressure, and water flux.

[0035] Embodiment 1

[0036] In a stirring kettle at 90°C, add 300g of PES and 1057.5g of DMF. After stirring for 1h, add 120g of polyethylene glycol and 22.5g of silica, and continue stirring for 9h at a stirring speed of 30 rpm. Lower the temperature in the kettle to 50°C and stir for 10h to make a homogeneous membrane liquid. After pouring into the spinning kettle, vacuum degassing is carried out at 50°C for 20h. After degassing, the membrane liquid is extruded from the spinneret of the double-ring flow channel, and the spinning temperature is controlled at 40°C. Use 30% DMAc aqueous solution as the inner coagulation bath, and enter the outer coagulation bath after a 15cm range and 80% humidity air bath. The outer coagulation bath is 20% DMAc aqueous solution, the temperature is 30°C, the spinning speed is 10m / min, and after passing through the water washing tank, it is wound into a bundle and solidified to obtain a PES hollow fiber humidification membrane.

[0037] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a polyethersulfone humidifying membrane with a symmetrical structure, characterized in that: The polyethersulfone humidifying membrane with a symmetrical structure comprises a middle sponge layer (1), an outer supporting layer (2) is arranged on one side of the middle sponge layer (1), an outer separation layer (3) is arranged on one side of the outer supporting layer (2), an inner supporting layer (4) is arranged on the other side of the middle sponge layer (1), and an inner separation layer (5) is arranged on one side of the inner supporting layer (4); The preparation method comprises the following steps: At 70-90°C, polyethersulfone polymer, porogen, hydrophilic polymer and organic solvent are added into a reaction kettle in a certain proportion, stirred at a speed of 30-60 rpm, and stirred at 70-90°C for 10 hours to dissolve the polymer into a homogeneous membrane liquid; Then cool down to 30-65°C, stir for 5-10h, and stir at 20-40 rpm to make the membrane solution fully dissolved and matured during the cooling process to obtain the spinning membrane solution; Pour the membrane liquid into the spinning kettle and degas under vacuum at -0.1MPa for 15-24h, the degassing temperature is 50-65℃; the membrane liquid is extruded through the spinneret and enters the air bath with a humidity of 30-80% and a length of 2-20cm; After preliminary solidification, the membrane liquid enters into an aqueous solution containing 15-50% dimethylformamide DMAc, the solidification bath temperature is 30-70°C, and the stretching speed is 8-20m / min, so that the membrane filaments are solidified and formed to form a humidifying membrane after preliminary solidification; The preliminarily cured humidifying membrane is immersed in deionized water at 30-40°C for 24 hours to remove residual additives and solvents, thereby obtaining a polyethersulfone humidifying membrane with a symmetrical structure; The mass percentages of the selected material components are: polyethersulfone polymer 10%-30%, porogen 0.5%-8%, hydrophilic polymer 3%-15% and organic solvent 40%-80%; The porogen is one or more of titanium dioxide, silicon dioxide or aluminum chloride, the hydrophilic polymer is one or more of polyethylene glycol, polymethyl methacrylate or cellulose acetate, and the organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylpyrrolidone, dimethylformamide or dimethylacetamide.

2. A polyethersulfone humidifying membrane with a symmetrical structure, characterized in that: Prepared by the method described in claim 1.

Citation Information

Patent Citations

  • Large aperture polyethersulfone film, preparation method and usage thereof

    CN1951550A

  • Preparation method of asymmetric polyether sulfone hollow fiber nanofiltration membrane

    CN105233710A

  • Polyether sulfone hollow fiber ultrafiltration membrane with symmetrical structure and preparation method thereof